Method for preparing potassium sulfate by leaching of polyhalite at room temperature
By utilizing the synergistic effect of potassium sulfate micron powder, sodium citrate, and sodium polyacrylate in the preparation of potassium sulfate from carnallite, combined with dynamic feeding control, the problems of low potassium leaching rate and product purity were solved, achieving efficient and low-energy potassium sulfate preparation with good product particle size uniformity.
Patent Information
- Application Number
- CN202611411277.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-24
AI Technical Summary
Existing processes for preparing potassium sulfate from carnallite have low potassium leaching rates, making it difficult to balance product purity and energy consumption. Furthermore, conventional methods are insufficient to effectively suppress magnesium ion dissolution and regulate gypsum crystal morphology at room temperature.
Potassium sulfate micron powder was used as seed crystals, sodium citrate as a complexing agent, and sodium polyacrylate as a crystal morphology regulator. Combined with dynamic feeding control and real-time monitoring of magnesium ion activity, the efficient and selective leaching of potassium sulfate was achieved through the synergistic effect of the four functional components.
It significantly increases potassium leaching rate to over 84% at room temperature, achieves product purity of 98%, reduces energy consumption by 8-12%, and produces products with uniform particle size distribution, reducing the need for subsequent crushing and processing.
Smart Images

Figure CN123151418A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic salt production technology, specifically a method for preparing potassium sulfate by leaching carnallite at room temperature. Background Technology
[0002] Potassium sulfate is an important chlorine-free potassium fertilizer with irreplaceable application value in the cultivation of chlorine-sensitive crops such as tobacco, fruit, and tea. The industrial sources of potassium sulfate mainly include the Mannheim process, condensation process, and natural mineral processing. Among them, the preparation of potassium sulfate by chemical conversion using carnallite as raw material has become a research direction for comprehensive resource utilization in recent years. Carnallite contains multiple elements such as potassium, magnesium, calcium, and sulfur. By adding potassium chloride, potassium ions combine with sulfate ions to form potassium sulfate, while magnesium ions remain in the mother liquor for separation.
[0003] Existing potassium sulfate preparation technology based on polyhalite faces several problems in practical applications. There is a contradiction between potassium leaching rate and product purity: improving potassium conversion rate usually requires extending reaction time or increasing temperature, but increasing temperature will exacerbate the dissolution of magnesium in polyhalite, and the concentration of magnesium ions in the mother liquor will increase accordingly. After reaching a certain level, magnesium ions will combine with sulfate and potassium ions to form complex salts such as soft potassium magnesium alum. These complex salts precipitate out together with potassium sulfate, reducing product purity.
[0004] To address the issue of gypsum encapsulation, some processes operate at higher temperatures to increase gypsum solubility or alter its crystal form. However, this increases energy consumption and, by increasing magnesium ion solubility, exacerbates the risk of double salt precipitation. Other studies have attempted to add surfactants to the reaction system to improve crystal morphology, but single additives cannot simultaneously address the dual needs of inhibiting double salt formation and regulating gypsum crystal structure. Some solutions employ batch feeding or controlled feeding rates to reduce local supersaturation, but these lack effective online monitoring indicators, making it difficult to precisely maintain the solution composition within the target area in practice. Therefore, a technical solution is needed at room temperature that can simultaneously address magnesium ion inhibition, gypsum crystal structure regulation, and dynamic process control to achieve efficient potassium leaching and high product purity. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a method for preparing potassium sulfate by room-temperature leaching of heterohalite, which solves the problems of low potassium leaching rate, product purity, and difficulty in balancing energy consumption in existing heterohalite potassium sulfate preparation processes.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing potassium sulfate by room-temperature leaching of carnallite, comprising the following steps: S1. Mix carnallite powder, potassium sulfate micro powder as seed crystals, and sodium citrate as a complexing agent to obtain a premix. S2. Add process water and potassium chloride to the reactor, stir to dissolve, and then add sodium polyacrylate aqueous solution as a crystal morphology regulator, and control the liquid phase temperature at 32℃ to 38℃. S3. Add the premix obtained in S1 to the reaction mother liquor obtained in S2. During the reaction, monitor the activity of magnesium ions in the liquid phase in real time and dynamically adjust the feeding rate according to the change of magnesium ion activity. S4. After feeding is completed, the mixture is matured, and the resulting slurry is separated into solid and liquid phases. The solid phase is washed and dried to obtain potassium sulfate product.
[0007] By adopting the above technical solution, the present invention combines four functional components with dynamic process control to achieve efficient and selective leaching of potassium sulfate from carnallite.
[0008] Potassium sulfate micronized powder, used as seed crystals, provides numerous heterogeneous nucleation sites in the early stages of the reaction. This allows potassium sulfate in the solution to preferentially grow on the seed crystal surface under relatively low supersaturation, avoiding the formation of a large number of fine crystals caused by homogeneous nucleation. The introduction of seed crystals concentrates the crystallization driving force on existing nuclei, making the crystallization rate controllable and also suppressing the co-precipitation of double salts caused by excessively high local supersaturation.
[0009] Sodium citrate acts as a complexing agent, forming a stable complex with free magnesium ions in the mother liquor. Magnesium ions in the solution are mainly in the form of Mg. 2+ It exists in the form of citrate (Cit) 3- ) and form MgCit - The complex has a moderate stability constant and can effectively reduce free Mg. 2+ Activity, inhibiting the formation of magnesium-containing double salts such as potassium magnesium sulfate (K2Mg2(SO4)3). The complexation reaction can be represented as: Mg 2+ Cit 3- →[MgCit] - This complexation equilibrium results in Mg in the system 2+ Maintaining a low activity level creates the thermodynamic conditions for the selective precipitation of potassium sulfate. The amount of complexing agent needs to be matched with the amount of seed crystal; too much will cause simultaneous complexation of potassium ions or precipitation of calcium citrate, while too little will not effectively inhibit the double salt formation.
[0010] Sodium polyacrylate, acting as a crystal morphology regulator, preferentially adsorbs onto certain crystal faces of calcium sulfate dihydrate (CaSO4·2H2O), altering the growth rate of each crystal face and transforming gypsum crystals from needle-like or long columnar shapes to short columnar or near-equiaxed shapes. Needle-like gypsum crystals tend to entangle and agglomerate during stirring, encapsulating potassium sulfate crystals and unreacted carnallite particles, hindering mass transfer and leading to a decrease in potassium leaching rate. Short columnar gypsum crystals exhibit better flowability and dispersibility, suspending in the reaction system and less likely to settle, reducing mechanical encapsulation between crystals. The carboxylic acid groups on the sodium polyacrylate molecular chain have a strong affinity for calcium ions; the adsorption mechanism is as follows: ; This surface modification effect is closely related to the molecular weight and concentration of sodium polyacrylate. A weight-average molecular weight in the range of 3000 to 5000 exhibits moderate adsorption strength and steric hindrance, and a concentration of 0.1% to 0.2% can effectively cover the gypsum crystal surface without causing excessive flocculation.
[0011] Dynamic feed control is based on real-time monitoring of free Mg in the reaction mother liquor using a magnesium ion selective electrode. 2+ Activity. The upper limit of activity is set between 0.55 mol / L and 0.65 mol / L, when Mg... 2+ When the activity reaches this upper limit, it indicates an increased tendency for magnesium ion accumulation in the system due to the decomposition of carnallite and the dissolution of potassium chloride. At this point, the feeding of the premix should be suspended to allow the added carnallite to fully react with potassium chloride and consume some of the magnesium ions. Simultaneously, the potassium sulfate crystallization process continues to consume potassium ions and further promotes the decomposition of carnallite. Wait for Mg... 2+ Feeding is resumed after the activity drops below the upper limit (typically below 0.4 mol / L), and the feed rate for the next stage is increased by 5% to 15%. This intermittent accelerated feeding strategy allows liquid-phase Mg to remain within the reaction phase throughout the entire reaction. 2+ The activity remains within a controllable metastable range, preventing the accumulation of magnesium ions due to excessively rapid feeding, which could lead to the supersaturation point of the soft potassium magnesium alum. At the same time, the overall reaction time is shortened by gradually increasing the feeding rate.
[0012] A significant synergistic effect exists among the four measures: seed crystals provide a substrate for selective precipitation; the complexing agent reduces magnesium ion activity, thereby amplifying the thermodynamic advantages of potassium sulfate; the crystal morphology regulator improves the hydrodynamic conditions of the reaction system, allowing the seed crystals and complexing agent to fully exert their effects; and dynamic feeding maintains the optimal solution chemical environment in real time. The combined effect of these four measures results in a significantly improved potassium leaching rate, a reduction in magnesium impurity content in the product to below 0.2%, and a potassium sulfate purity exceeding 98%. Simultaneously, the product exhibits a uniform particle size distribution with a median diameter between 12 and 18 μm, eliminating the need for subsequent pulverization.
[0013] Preferably, the amount of potassium sulfate micro powder used is 0.5% to 1.0% of the mass of carnallite powder. If the amount of seed crystal is too low, the crystallization induction effect is not significant, the product particle size is too large and the purity decreases; if the amount of seed crystal is too high, too many seed crystals may be introduced to the surface, consuming too many potassium ions and resulting in a decrease in yield.
[0014] Preferably, the amount of sodium citrate used is 5% to 10% of the mass of potassium sulfate powder. This ratio ensures that the complexing agent is sufficient to complex most of the free magnesium ions in the system, while avoiding excessive complexation of calcium ions by excessive citrate ions, which would affect the control of gypsum crystal form.
[0015] Preferably, the effective mass concentration of sodium polyacrylate in the reaction mother liquor is 0.1% to 0.2%. Below 0.1%, the gypsum crystals are still mainly needle-shaped, while above 0.2% may lead to an increase in solution viscosity, affecting stirring efficiency.
[0016] Preferably, the sodium polyacrylate has a weight-average molecular weight of 3,000 to 5,000. If the molecular weight is too low, the adsorption strength is insufficient and it cannot effectively change the gypsum crystal form; if the molecular weight is too high, it may cause interparticle bridging and flocculation, which is detrimental to dispersion.
[0017] Preferably, in the dynamic feeding control, the upper limit of magnesium ion activity is set to 0.55 to 0.65 mol / L. When the activity detection value reaches the upper limit, feeding is paused. Feeding is resumed after the activity drops below the upper limit, and the feeding rate in the next stage is increased by 10%.
[0018] Preferably, the total feeding time of the premix is 120 to 150 minutes. If the feeding time is too short, the reaction will be insufficient; if it is too long, production efficiency will be reduced.
[0019] Preferably, the solid phase after solid-liquid separation is washed with deionized water 1 to 2 times, with the amount of water used each time being 0.5 to 1.0 times the mass of the solid phase. The washing process removes magnesium-containing mother liquor adhering to the product surface, further improving product purity.
[0020] Preferably, the drying temperature is 80 to 105°C, and the product is dried until the moisture content does not exceed 0.5%.
[0021] By adopting the above technical solution, this invention achieves a synergistic effect of four dynamic feeding technologies under mild conditions of 32℃ to 38℃: seed crystallization, sodium citrate complexation of magnesium ions, sodium polyacrylate regulation of gypsum crystal form, and magnesium ion activity feedback control. This effectively overcomes the defects of existing technologies such as low potassium leaching rate, poor product purity, and crystal agglomeration during room temperature leaching. It yields potassium sulfate products with high yield, high purity, and uniform particle size. Moreover, the process is simple to operate, has low energy consumption, and has significant industrial practical value.
[0022] This invention provides a method for preparing potassium sulfate by room-temperature leaching of carnallite. It has the following beneficial effects: 1. This invention achieves simultaneous intervention in four key factors of the crystallization process through a combination of methods: seed crystals inducing crystallization to lower the crystallization energy barrier, sodium citrate complexing magnesium ions to inhibit the formation of complex salts, sodium polyacrylate modifying gypsum crystal morphology to improve the fluid environment, and magnesium ion activity feedback controlling the material to maintain metastable conditions. The seed crystals provide heterogeneous nucleation sites, avoiding the uncontrollable crystal size and co-extrusion problems caused by homogeneous nucleation; the complexing agent reduces the activity of free magnesium ions in the solution, making potassium sulfate thermodynamically preferential for precipitation; and sodium polyacrylate causes by-product gypsum to form short columnar crystals during the crystallization stage, eliminating the influence of needle-like gypsum on the seed crystals. The mechanical encapsulation of unreacted mineral powder ensures the effectiveness of the seed crystals and the efficiency of mass transfer. Dynamic feeding control keeps the concentration of magnesium ions in the liquid phase below the critical threshold, avoiding local oversaturation that could lead to the precipitation of complex salts. All four are indispensable and have a synergistic relationship: without crystal shape regulators, gypsum encapsulation will cause the seed crystals to lose their inductive effect; without complexing agents, the increased activity of magnesium ions will cause dynamic feeding control to be triggered frequently, prolonging the reaction cycle. The synergistic result is that the potassium leaching rate increases from 65% to 75% in conventional processes to over 84%, the magnesium content in the product decreases to below 0.2%, and the purity reaches over 98%.
[0023] 2. This invention completes the entire reaction process at room temperature (32°C to 38°C), without needing to raise the temperature above 60°C. The core purpose of increasing the temperature in traditional processes is to increase the solubility of potassium sulfate and accelerate the reaction rate. However, the energy consumption and equipment corrosion problems caused by the temperature increase have long existed in industrial production. This solution introduces seed crystals and complexing agents to make the reaction system more thermodynamically favorable for potassium sulfate precipitation. By using crystal form regulators to improve mass transfer efficiency, the reaction kinetics are accelerated. Therefore, even without raising the temperature, the overall reaction time can still be controlled within 3 to 4 hours. The room temperature condition also reduces the capacity and energy consumption of the reactor jacket heating circulation system, lowers the temperature resistance requirements of the equipment materials, and reduces the probability of side reactions at high temperatures. For a potassium sulfate production plant with an annual output of 100,000 tons, the steam consumption savings from the temperature reduction alone can reduce the unit production cost by about 8% to 12%.
[0024] 3. The median particle size of the potassium sulfate product obtained by this invention can be controlled within the range of 12 to 18 μm, with a small distribution range, regular crystal morphology, and moderate bulk density. This particle size characteristic eliminates the need for further crushing or grinding during subsequent agricultural fertilization or industrial use. This avoids the problem of traditional coarse-crystal products requiring a crushing process before packaging due to their large particle size and wide distribution. The crushing process in conventional potassium sulfate production not only increases equipment investment and energy consumption but also easily generates fine powder, causing dust pollution and product loss. This solution can directly control the particle size of the product by adjusting the amount of seed crystals. Increasing the amount of seed crystals results in finer particle size, while decreasing the amount of seed crystals results in larger particle size. This correlation provides a simple process adjustment window. In addition, the smaller particle size product dissolves faster during application, which is beneficial for crop absorption. Attached Figure Description
[0025] Figure 1 This is a comparison diagram of the seed-induced crystallization effect of the present invention; Figure 2 To highlight the Mg of the present invention 2+ Comparison of chelation effects; Figure 3 The comparison diagram highlights the effect of the present invention on gypsum crystal form regulation; Figure 4 The comparison diagram highlights the dynamic metastable region control effect of the present invention; Figure 5 To highlight the potassium leaching rate comparison chart of the present invention; Figure 6 A comparison chart showing the purity and impurity content of the present invention; Figure 7 A comparison diagram of potassium sulfate particle size distribution and span is provided to highlight the present invention. Detailed Implementation
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] The present invention will be further described in detail below with reference to specific embodiments and comparative examples, but the present invention is not limited to these embodiments and comparative examples. Unless otherwise stated, all raw materials are commercially available industrial grade or analytical grade products, and reagents not specifically mentioned are all available through commercial channels.
[0028] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications: Carnallite powder is a natural mineral that is crushed and ball-milled to a particle size ≤0.15mm and a moisture content ≤1%. Its main components are K2SO4·MgSO4·2CaSO4·2H2O. Potassium sulfate micro powder (CAS7778-80-5), industrial grade, purity ≥98%, particle size ≤20μm; Sodium citrate (CAS 68-04-2, anhydrous), industrial grade, purity ≥99%; Sodium polyacrylate (CAS9003-04-7) is a homopolymer of sodium acrylate with a weight average molecular weight of 3000-5000, a molecular weight distribution index of 1.5-2.5 as determined by gel permeation chromatography, a solid content ≥90%, and a free monomer content ≤0.5%. The anhydrous potassium magnesium sulfate (K2Mg2(SO4)3, CAS14977-91-4) used in the comparative example was industrial grade with a purity ≥95%. Sodium hexametaphosphate (CAS10124-56-8), industrial grade; The other reagents not listed (such as potassium chloride, disodium EDTA, etc.) are all industrial-grade or analytical-grade products that can be obtained through commercial channels, and will not be described further.
[0029] Preparation Example 1 This preparation example provides a method for preparing sodium polyacrylate with a weight-average molecular weight of 3000, comprising the following steps: In a four-necked flask equipped with a stirrer, thermometer, and nitrogen protection device, 200 parts by mass of deionized water are added, and the temperature is raised to 80°C; under stirring, 80 parts by mass of acrylic monomer, 0.8 parts by mass of ammonium persulfate (initiator), and 2.5 parts by mass of isopropanol (chain transfer agent) are dissolved in 50 parts by mass of deionized water respectively to form a mixed solution; the above mixed solution is added dropwise to the flask at a uniform rate over 2 hours, maintaining the temperature at 80±2°C during the addition; after the addition is complete, the reaction is continued at this temperature for 1.5 hours; the temperature is cooled to below 40°C, and the pH is adjusted to 7.0-8.0 with a 30% sodium hydroxide aqueous solution; the resulting viscous liquid is poured into excess anhydrous ethanol to precipitate a white solid, which is filtered, washed three times with anhydrous ethanol, and dried under vacuum at 60°C to constant weight to obtain the solid sodium polyacrylate product. The weight-average molecular weight was determined to be 3000 and the molecular weight distribution index was 1.8 by gel permeation chromatography.
[0030] Preparation Example 2 This preparation example provides a method for preparing sodium polyacrylate with a weight-average molecular weight of 5000, comprising the following steps: In a four-necked flask equipped with a stirrer, thermometer, and nitrogen protection device, 200 parts by mass of deionized water are added, and the temperature is raised to 80°C; under stirring, 80 parts by mass of acrylic monomer, 0.6 parts by mass of ammonium persulfate (initiator), and 1.0 parts by mass of isopropanol (chain transfer agent) are dissolved in 50 parts by mass of deionized water respectively to form a mixed solution; the above mixed solution is added dropwise to the flask at a uniform rate over 3 hours, maintaining the temperature at 80±2°C during the addition; after the addition is complete, the reaction is continued at this temperature for 2 hours; the temperature is cooled to below 40°C, and the pH is adjusted to 7.0-8.0 with a 30% sodium hydroxide aqueous solution; the resulting viscous liquid is poured into excess anhydrous ethanol to precipitate a white solid, which is filtered, washed three times with anhydrous ethanol, and dried under vacuum at 60°C to constant weight to obtain the solid sodium polyacrylate product. The weight-average molecular weight was determined to be 5000 and the molecular weight distribution index was 1.6 by gel permeation chromatography.
[0031] Example 1 This embodiment provides a method for preparing potassium sulfate at 32°C with a low seed crystal dosage, comprising the following steps: S1. Mix 100 parts by weight of carnallite powder, 0.5 parts by weight of potassium sulfate powder, and 0.025 parts by weight of sodium citrate (calculated as 5% of the mass of potassium sulfate powder) in a V-type mixer for 30 minutes to obtain a premix. S2. Add 250 parts by mass of process water to the jacketed reactor, start stirring (60 rpm), add potassium chloride solid in one go according to the equivalent molar ratio of KCl to K2O in carnallite of 1.1:1, stir to dissolve for 20 minutes, and control the liquid phase temperature at 32±2℃ through the jacket circulating water; after the potassium chloride is completely dissolved, add 5% sodium polyacrylate aqueous solution to make the effective mass concentration of sodium polyacrylate in the liquid phase 0.1%, and continue stirring for 5 minutes; S3. Install an online magnesium ion selective electrode in the reactor, connect it to the PLC control system, and set the Mg... 2+ The upper limit for dynamic activity control is 0.6 mol / L; the automatic feeding system for the premix is started, and the initial feeding stage begins at 60% of the designed total feeding rate (calculated based on a total feeding time of 150 minutes). Mg is monitored in real time. 2+ Activity; when the detected value reaches 0.55 mol / L, pause feeding for 30 seconds, and resume feeding after the activity drops below 0.4 mol / L, and increase the rate of the next stage by 10%; repeat the above cycle until the premix is completely added, with a total feeding time of 150 minutes; S4. After the material is added, continue stirring at 32±2℃ for 60 minutes to mature the material. Pump the slurry into a centrifuge for separation. Wash the obtained coarse crystals twice with deionized water (each wash water volume is 0.5 times the crystal mass). Dry at 80℃ until the moisture content is ≤0.5% to obtain potassium sulfate product.
[0032] Example 2 This embodiment provides a method for preparing potassium sulfate at 38°C with a low amount of seed crystals, comprising the following steps: S1. Mix 100 parts by weight of carnallite powder, 0.5 parts by weight of potassium sulfate powder, and 0.025 parts by weight of sodium citrate (calculated as 5% of the mass of potassium sulfate powder) in a V-type mixer for 30 minutes to obtain a premix. S2. Add 250 parts by mass of process water to the jacketed reactor, start stirring (60 rpm), add potassium chloride solid in one go according to the equivalent molar ratio of KCl to K2O in carnallite of 1.1:1, stir to dissolve for 20 minutes, and control the liquid phase temperature at 38±2℃ through the jacket circulating water; after the potassium chloride is completely dissolved, add 5% sodium polyacrylate aqueous solution to make the effective mass concentration of sodium polyacrylate in the liquid phase 0.1%, and continue stirring for 5 minutes; S3. Install an online magnesium ion selective electrode in the reactor, connect it to the PLC control system, and set the Mg... 2+ The upper limit for dynamic activity control is 0.6 mol / L; the automatic feeding system for the premix is started, with the initial feeding stage beginning at 60% of the designed total feeding rate (calculated based on a total feeding time of 150 minutes), and Mg is monitored in real time. 2+ Activity; when the detected value reaches 0.55 mol / L, pause feeding for 30 seconds, and resume feeding after the activity drops below 0.4 mol / L, and increase the rate of the next stage by 10%; repeat the above cycle until the premix is completely added, with a total feeding time of 150 minutes; S4. After the material is added, continue stirring at 38±2℃ for 60 minutes to mature the material. Pump the slurry into a centrifuge for separation. Wash the obtained coarse crystals twice with deionized water (each wash water volume is 0.5 times the crystal mass). Dry at 80℃ until the moisture content is ≤0.5% to obtain potassium sulfate product.
[0033] Example 3 This embodiment provides a method for preparing potassium sulfate at 35°C with a moderate amount of seed crystals, comprising the following steps: S1. Mix 100 parts by weight of carnallite powder, 0.75 parts by weight of potassium sulfate powder, and 0.056 parts by weight of sodium citrate (calculated as 7.5% of the mass of potassium sulfate powder) in a V-type mixer for 35 minutes to obtain a premix. S2. Add 275 parts by mass of process water to the jacketed reactor, start stirring (70 rpm), add potassium chloride solid in one go according to the equivalent molar ratio of KCl to K2O in carnallite of 1.15:1, stir to dissolve for 22 minutes, and control the liquid phase temperature at 35±2℃ through the jacket circulating water; after the potassium chloride is completely dissolved, add 5% sodium polyacrylate aqueous solution to make the effective mass concentration of sodium polyacrylate in the liquid phase 0.15%, and continue stirring for 8 minutes; S3. Install an online magnesium ion selective electrode in the reactor, connect it to the PLC control system, and set the Mg... 2+ The upper limit for dynamic activity control is 0.6 mol / L; the automatic feeding system for the premix is started, with the initial feeding stage beginning at 60% of the designed total feeding rate (calculated based on a total feeding time of 135 minutes), and Mg is monitored in real time. 2+ Activity; when the detected value reaches 0.55 mol / L, pause feeding for 30 seconds, and resume feeding after the activity drops below 0.4 mol / L, and increase the rate of the next stage by 10%; repeat the above cycle until the premix is completely added, with a total feeding time of 135 minutes; S4. After the material is added, continue stirring at 35±2℃ for 75 minutes to mature the material. Pump the slurry into a centrifuge for separation. Wash the obtained coarse crystals twice with deionized water (each wash water volume is 0.8 times the crystal mass). Dry at 90℃ until the moisture content is ≤0.5% to obtain potassium sulfate product.
[0034] Example 4 This embodiment provides a method for preparing potassium sulfate at 35°C with a high seed crystal dosage, comprising the following steps: S1. Mix 100 parts by weight of carnallite powder, 1.0 parts by weight of potassium sulfate powder, and 0.10 parts by weight of sodium citrate (calculated as 10% of the mass of potassium sulfate powder) in a V-type mixer for 40 minutes to obtain a premix. S2. Add 300 parts by mass of process water to the jacketed reactor, start stirring (80 rpm), add potassium chloride solid at once according to the equivalent molar ratio of KCl to K2O in carnallite of 1.2:1, stir to dissolve for 25 minutes, and control the liquid phase temperature at 35±2℃ through the jacket circulating water; after the potassium chloride is completely dissolved, add 5% sodium polyacrylate aqueous solution to make the effective mass concentration of sodium polyacrylate in the liquid phase 0.2%, and continue stirring for 10 minutes; S3. Install an online magnesium ion selective electrode in the reactor, connect it to the PLC control system, and set the Mg... 2+ The upper limit for dynamic activity control is 0.6 mol / L; the automatic feeding system for the premix is started, and the initial feeding stage begins at 60% of the designed total feeding rate (calculated based on a total feeding time of 120 minutes), while Mg is monitored in real time. 2+Activity; when the detected value reaches 0.55 mol / L, pause feeding for 30 seconds, and resume feeding after the activity drops below 0.4 mol / L, and increase the rate of the next stage by 10%; repeat the above cycle until the premix is completely added, with a total feeding time of 120 minutes; S4. After the material is added, continue stirring at 35±2℃ for 90 minutes to mature the material. Pump the slurry into a centrifuge for separation. Wash the obtained coarse crystals twice with deionized water (each wash water volume is 1.0 times the crystal mass). Dry at 105℃ until the moisture content is ≤0.5% to obtain potassium sulfate product.
[0035] Example 5 This embodiment provides a method for preparing potassium sulfate at 35°C with a low seed crystal dosage and a high complexing agent dosage, comprising the following steps: S1. Mix 100 parts by weight of carnallite powder, 0.5 parts by weight of potassium sulfate powder, and 0.05 parts by weight of sodium citrate (calculated as 10% of the mass of potassium sulfate powder) in a V-type mixer for 30 minutes to obtain a premix. S2. Add 250 parts by mass of process water to the jacketed reactor, start stirring (60 rpm), add potassium chloride solid in one go according to the equivalent molar ratio of KCl to K2O in carnallite of 1.1:1, stir to dissolve for 20 minutes, and control the liquid phase temperature at 35±2℃ through the jacket circulating water; after the potassium chloride is completely dissolved, add 5% sodium polyacrylate aqueous solution to make the effective mass concentration of sodium polyacrylate in the liquid phase 0.15%, and continue stirring for 5 minutes; S3. Install an online magnesium ion selective electrode in the reactor, connect it to the PLC control system, and set the Mg... 2+ The upper limit for dynamic activity control is 0.55 mol / L; the automatic feeding system for the premix is started, with the initial feeding stage beginning at 60% of the designed total feeding rate (calculated based on a total feeding time of 130 minutes), and Mg is monitored in real time. 2+ Activity; when the detected value reaches 0.50 mol / L, pause feeding for 30 seconds, and resume feeding after the activity drops below 0.35 mol / L, and increase the rate of the next stage by 10%; repeat the above cycle until the premix is completely added, with a total feeding time of 130 minutes; S4. After the feeding is completed, continue stirring at 35±2℃ for 75 minutes for maturation; pump the slurry into a centrifuge for separation, wash the obtained coarse crystals twice with deionized water (each wash water volume is 0.6 times the crystal mass), and dry at 90℃ until the moisture content is ≤0.5% to obtain potassium sulfate product.
[0036] Example 6 This embodiment provides a method for preparing potassium sulfate at 35°C with a high amount of seed crystals and a low amount of complexing agent, including the following steps: S1. Mix 100 parts by weight of carnallite powder, 1.0 parts by weight of potassium sulfate powder, and 0.05 parts by weight of sodium citrate (calculated as 5% of the mass of potassium sulfate powder) in a V-type mixer for 40 minutes to obtain a premix. S2. Add 300 parts by mass of process water to the jacketed reactor, start stirring (80 rpm), add potassium chloride solid at once according to the equivalent molar ratio of KCl to K2O in carnallite of 1.2:1, stir to dissolve for 25 minutes, and control the liquid phase temperature at 35±2℃ through the jacket circulating water; after the potassium chloride is completely dissolved, add 5% sodium polyacrylate aqueous solution to make the effective mass concentration of sodium polyacrylate in the liquid phase 0.2%, and continue stirring for 10 minutes; S3. Install an online magnesium ion selective electrode in the reactor, connect it to the PLC control system, and set the Mg... 2+ The upper limit for dynamic activity control is 0.65 mol / L; the automatic feeding system for the premix is started, with the initial feeding stage beginning at 60% of the designed total feeding rate (calculated based on a total feeding time of 140 minutes), and Mg is monitored in real time. 2+ Activity; when the detected value reaches 0.60 mol / L, pause feeding for 30 seconds, and resume feeding after the activity drops below 0.45 mol / L, and increase the rate of the next stage by 10%; repeat the above cycle until the premix is completely added, with a total feeding time of 140 minutes; S4. After the material is added, continue stirring at 35±2℃ for 90 minutes to mature the material. Pump the slurry into a centrifuge for separation. Wash the obtained coarse crystals twice with deionized water (each wash water volume is 1.0 times the crystal mass). Dry at 105℃ until the moisture content is ≤0.5% to obtain potassium sulfate product.
[0037] Comparative Example 1 The difference from Example 3 is that potassium sulfate powder, sodium citrate, and sodium polyacrylate were not added; all other ingredients are the same.
[0038] Comparative Example 2 Compared with Example 3, the difference is that only potassium sulfate powder (0.75 parts by weight) was added, and sodium citrate and sodium polyacrylate were not added, while the rest were the same.
[0039] Comparative Example 3 Compared with Example 3, the difference is that only sodium citrate (0.056 parts by weight) was added, and potassium sulfate powder and sodium polyacrylate were not added, while the rest were the same.
[0040] Comparative Example 4 Compared with Example 3, the difference is that potassium sulfate powder was replaced with an equal mass (0.75 parts by weight) of anhydrous potassium magnesium sulfate, and sodium citrate and sodium polyacrylate were not added, while the rest were the same.
[0041] Comparative Example 5 The difference from Example 3 is that sodium citrate is replaced with disodium EDTA with the same chelation value, while the rest are the same.
[0042] Comparative Example 6 The difference from Example 3 is that sodium polyacrylate is replaced with sodium hexametaphosphate of equal mass concentration, while all other aspects are the same.
[0043] Comparative Example 7 Compared with Example 3, the difference is that only potassium sulfate powder (0.75 parts by weight) and sodium citrate (0.056 parts by weight) were added, and sodium polyacrylate was not added, while the rest were the same.
[0044] Comparative Example 8 Compared with Example 3, the difference is that a uniform feeding method is used, the total feeding time is 135 minutes, there is no magnesium ion activity feedback and pause-increase control, and the rest are the same.
[0045] Comparative Example 9 The difference from Example 3 is that the reaction temperature is 50±2℃, while all other aspects are the same.
[0046] Comparative Example 10 The difference from Example 3 is that the reaction temperature is 25±2℃, while all other aspects are the same.
[0047] Comparative Example 11 Compared with Example 3, the difference is that the order of adding materials is changed to first adding the premix to water and stirring for 10 minutes, and then adding potassium chloride solid. The rest are the same.
[0048] Comparative Example 12 Compared with Example 3, the differences are: the reaction temperature is 60±2℃, no seed crystals, no sodium citrate, no sodium polyacrylate, constant rate feeding (total feeding time 30 minutes), and total reaction time 120 minutes. All other aspects are the same.
[0049] Test Example 1: Experimental subjects Reaction slurry samples were taken from Examples 1, 2, 3, 4, 5, and 6, as well as Comparative Examples 1, 2, and 3, at the end of the feeding process (i.e., when step S3 was completed). Approximately 50 mL of each sample was taken and immediately filtered through a 0.45 μm microporous membrane. The solid phase was washed three times with anhydrous ethanol and then vacuum dried at 40 °C for 2 hours to obtain a dry powder.
[0050] Experimental steps The dried powder was ground in an agate mortar until it passed through a 200-mesh sieve. Approximately 0.5g was placed in the sample holder of an X-ray diffractometer. Cu target Kα radiation (λ=1.5406Å) was used, with a tube voltage of 40kV, a tube current of 40mA, a scanning range of 2θ=5°~70°, a step size of 0.02°, and a scanning speed of 4° / min. The XRD patterns of all samples were recorded, and the peak intensity (count) of the characteristic diffraction peak of the K2SO4(111) crystal plane (2θ≈30.8°) was selected as the quantitative index of the seed-induced crystallization effect.
[0051] Take approximately 0.1 g of the dried powder, disperse it in 5 mL of anhydrous ethanol, sonicate for 30 seconds, then place a drop on a glass slide, cover with a coverslip, and observe the crystal morphology under an optical microscope (40× objective). For each sample, randomly select 5 fields of view, and measure the major axis of at least 20 crystals in each field of view (take the arithmetic mean as the average particle size of that field of view). Finally, take the average value of all fields of view as the average particle size of the crystals in that sample.
[0052] Experimental data Table 1. Relative intensities of characteristic diffraction peaks of K2SO4 (111) and average crystal size in different embodiments and comparative examples.
[0053] Figure 1 This is a comparison chart of the seed-induced crystallization effect of Test Example 1 of the present invention, where (a) represents the relative intensity of the characteristic diffraction peak of K2SO4 (111) in each example and comparative example sample, and (b) represents the average crystal particle size of the corresponding sample. The horizontal axis represents Examples 1 to 6 and Comparative Examples 1 to 3. The grayscale of the bars in the figure is used to distinguish different samples from light to dark, but the grayscale change is only used for visual assistance, and all data values are based on Table 1.
[0054] According to the data in Table 1, a clear positive correlation can be observed between the amount of seed crystals added and the intensity of the characteristic diffraction peaks of K2SO4. The relative intensity of the (111) peak in Example 4 (1.0 part of seed crystals) reached 0.81, while that in Example 1 (0.5 parts of seed crystals) was 0.48, and that in Example 3 (0.75 parts of seed crystals) was 0.65. The peak intensity of Comparative Example 1 (no addition) was only 0.09, indicating that almost no K2SO4 crystals were detected without the introduction of seed crystals and complexing agents. At this time, the reaction system may be in dissolution equilibrium or other complex salts may be generated. The peak intensity of Comparative Example 2 (0.75 parts of seed crystals added) was 0.38, which was significantly higher than that of Comparative Example 1 but lower than that of Example 3 (0.65), indicating that simply adding seed crystals can promote the crystallization of K2SO4, but the synergistic effect of seed crystals with sodium citrate and sodium polyacrylate can further enhance this effect. The peak intensity of Comparative Example 3 (with only sodium citrate added) was 0.11, which was close to that of Comparative Example 1, indicating that the complexing agent itself could not directly induce K2SO4 nucleation.
[0055] Test Example 2: Experimental subjects Liquid phase samples were taken from Examples 1, 2, 3, 4, 5, and 6, as well as Comparative Examples 5 and 7. Sampling times were 30 minutes, 60 minutes, 90 minutes, 120 minutes after the start of feeding, and at the end of feeding (the total feeding time varied for each example: 150 minutes for Examples 1 and 2, 135 minutes for Example 3, 120 minutes for Example 4, 130 minutes for Example 5, and 140 minutes for Example 6; the feeding time for Comparative Examples 5 and 7 was the same as for Example 3, 135 minutes). For each sample, 2 mL of slurry was drawn from the sampling port of the reactor using a syringe and immediately filtered through a 0.22 μm needle filter. The resulting clear filtrate was stored in a plastic centrifuge tube for analysis.
[0056] Experimental steps Take 0.5 mL of the filtrate and place it in an Erlenmeyer flask. Add 10 mL of deionized water and 5 mL of ammonia-ammonium chloride buffer solution with pH=10. Then add about 0.05 g of Eriochrome Black T indicator. Titrate with 0.01 mol / L EDTA standard solution until the solution changes from purple-red to pure blue. Record the volume of EDTA consumed and calculate the total Mg. 2+ Concentration (in mol / L).
[0057] Take another 0.5 mL of filtrate, add the same volume of buffer solution, and then add 0.5 mL of 10% triethanolamine solution to mask Al. 3+ Fe 3+ Interfering ions were removed, and 0.1 g of a calcium-magnesium mixed indicator (a mixture of Acid Chrome Blue K and Naphthol Green B) was added. The solution was titrated with 0.01 mol / L EDTA until the solution changed from purple-red to blue-green. The measured Mg content at this point was...2+ Concentration of free Mg 2+ Concentration. Due to the effect of citrate on Mg 2+ The complexation does not affect the EDTA titration endpoint; the titration value is the value of the uncomplexed free Mg. 2+ .
[0058] The data at each time point are summarized in Table 2. Only the final data at the end of the feeding process is listed in the table for simplicity, but data from other time points can be referenced when observing trends; Table 2 also shows the free Mg at the end of the feeding process. 2+ Proportion and total Mg 2+ concentration.
[0059] Experimental data Table 2 Total Mg in the liquid phase of each sample at the end of feeding. 2+ Concentration and free Mg 2+ Proportion
[0060] Figure 2 Mg is from Test Example 2 of this invention. 2+ Comparison of complexation effects, where (a) represents the total Mg in the liquid phase of each sample at the end of feeding. 2+ Concentration, (b) represents the corresponding free Mg 2+ Proportion. The horizontal axis represents Examples 1-6 and Comparative Examples 5 and 7. The gray levels of the bars, from light to dark, are used to distinguish different samples; the actual values are based on Table 2.
[0061] Based on the data in Table 2, total Mg 2+ The concentrations did not differ significantly between the different examples and comparative examples, ranging from 0.44 mol / L to 0.56 mol / L, which is related to the similar amounts of carnallite powder added in each process. The real difference lies in the free Mg content. 2+ Proportion. In Example 3, free Mg 2+ The proportion was 24.6%, while it was 21.2% in Example 4 and even lower at 20.5% in Example 5. Free Mg in Comparative Example 5 (disodium EDTA replacing sodium citrate) 2+ The proportion was 19.4%, slightly lower than in Example 5, indicating that disodium EDTA has a positive effect on Mg. 2+ The complexing ability of disodium EDTA is slightly stronger than that of sodium citrate, but disodium EDTA is more expensive and has poorer biodegradability, making it potentially less than ideal for industrial applications. The most notable example is Comparative Example 7 (only seed crystals and sodium citrate added, no sodium polyacrylate), where the free Mg... 2+ The proportion was as high as 38.7%, far exceeding that of Example 3 (24.6%), even though the amount of sodium citrate added was the same in both. This indicates that although the main function of sodium polyacrylate is to regulate the morphology of the paste, the carboxylate groups on its molecular chain may also affect the Mg in the liquid phase. 2+This generates a certain degree of complexation, or reduces Mg by improving the morphology of gypsum crystals. 2+ The possibility of being trapped within gypsum increases, thus indirectly increasing the amount of Mg that can be complexed in the liquid phase. 2+ Total amount. This makes free Mg 2+ The proportion was reduced.
[0062] In summary, sodium citrate affects Mg 2+ The complexing ability is sufficient to make free Mg 2+ The proportion is reduced to the range of 20% to 30%, and when sodium polyacrylate is absent, free Mg... 2+ The proportion increased significantly. Therefore, the combined effect of the complexing agent and the crystal form regulator is key to achieving efficient suppression of complex salt precipitation. This test result directly supports the Mg... 2+ The mechanism of selective complexation inhibiting the formation of soft potassium magnesium alum was verified by subsequent product purity test results.
[0063] Test Example 3: Experimental subjects Take reaction slurry samples from Examples 1, 2, 3, 4, 5, 6, and Comparative Examples 7 and 8 at the end of their respective curing processes (when step S4 is completed). Take approximately 30 mL of each sample, immediately dilute it with deionized water to a solid content of approximately 5% (mass fraction), stir thoroughly, and place 1 mL of the suspension on a glass slide, cover it with a coverslip to prepare a temporary slide. Prepare 3 parallel slides for each sample.
[0064] Experimental steps The prepared slides were placed on the stage of an optical microscope and observed at 100x magnification (10×eyepiece×10×objective). Five fields of view were randomly selected from each slide, and in each field of view, gypsum crystals with clear boundaries and no overlap were selected for aspect ratio (the ratio of crystal length to width). At least 20 crystals were measured in each field of view, and at least 300 crystals were measured in total for each sample.
[0065] Manually calibrate the maximum length (L) and maximum vertical width (W) of each crystal projection using the microscope's accompanying image analysis software, and calculate the aspect ratio R = L / W. Record all measurements.
[0066] Calculate the average and standard deviation of all measurements, and determine the proportion of crystals with an aspect ratio > 5 (reflecting the proportion of needle-like crystals). Summarize the above data in Table 3.
[0067] Experimental data Table 3. Statistical results of the aspect ratio of gypsum crystals in different embodiments and comparative examples.
[0068] Figure 3 is a comparison diagram of the gypsum crystal shape control effect of Test Example 3 of the present invention, showing the distribution of the aspect ratio of gypsum crystals in the samples of each example and comparative example. The circle marks and error bars represent the average value and standard deviation of the aspect ratio of each sample, and the gray scatter points are the measured aspect ratio values of 60 crystals randomly selected from each sample. The abscissa corresponds to Examples 1 to 6, Comparative Example 7, and Comparative Example 8.
[0069] According to the data in Table 3, there is a significant difference in the aspect ratio of gypsum crystals between the examples with sodium polyacrylate added and the control group without sodium polyacrylate. The average aspect ratios of Example 3, Example 4, and Example 6 are all below 2.5, especially Example 4 is only 2.1, and the proportions of crystals with an aspect ratio greater than 5 are only 4.6%, 2.8%, and 3.5%, respectively, indicating that the gypsum crystals are mainly massive and nearly equiaxed. In contrast, the average aspect ratio of Comparative Example 7 (without sodium polyacrylate) is as high as 5.5, and 48.7% of the crystals have an aspect ratio exceeding 5, meaning that most of the gypsum crystals are needle-like or flaky. Although Comparative Example 8 uses the same amount of seed crystals and complexing agent as Example 4, after the absence of sodium polyacrylate, its average aspect ratio still reaches 5.1, and 43.2% of the crystals are needle-like. This shows that relying solely on seed crystals and complexing agents cannot effectively improve the morphology of gypsum crystals, and sodium polyacrylate is irreplaceable.
[0070] The average aspect ratios of Example 1 and Example 2 are 2.8 and 3.0, respectively, which are slightly higher than those of Example 3, but still within the acceptable range. The effective mass concentrations of sodium polyacrylate in the liquid phase of these two examples are both 0.1% (0.15% in Example 3), indicating that although a lower concentration of sodium polyacrylate can inhibit needle-like growth, the effect is slightly weaker. The aspect ratio of Example 5 (0.15% concentration) is 2.6, which is between Example 1 and Example 3. This may be related to its higher amount of sodium citrate, because citrate ions may also have a certain adsorption effect on the gypsum surface, competing with sodium polyacrylate. Example 4 (0.2% concentration) has the best effect, indicating that increasing the concentration of sodium polyacrylate within a certain range can further reduce the aspect ratio.
[0071] Test Example 4: Experimental subjects The data of the entire reaction process of Example 1, Example 3, Example 4, Example 5, Comparative Example 8, Comparative Example 9, Comparative Example 10, and Comparative Example 12 were collected, respectively. The data sources are the Mg activity signal recorded by the PLC control system supporting the reactor (collected by the online magnesium ion selective electrode with a sampling frequency of once every 5 seconds) and the liquid phase temperature data recorded by the temperature sensor. The time period from the start of adding the premix to the end of feeding (i.e., the entire S3 step) was selected as the analysis interval. 2+
[0072] Experimental steps For each sample, the activity data was averaged every minute, with the start time of feeding as 0 minutes and the end time of feeding as the endpoint, to obtain one data point per minute.
[0073] Calculate the Mg content of each sample throughout the entire feeding process. 2+ The mean and standard deviation of activity are measured, with the standard deviation reflecting the range of activity fluctuation. A larger standard deviation indicates that Mg... 2+ The more unstable the activity, the greater the likelihood that the system will deviate from the metastable region.
[0074] The number of times the PLC system triggered a pause in feeding and the total pause time (in seconds) were recorded for each sample during the feeding process. A higher number of pauses and a longer total pause time indicate that the system requires more frequent buffering time to maintain the Mg content. 2+ Activity is below the upper limit of control.
[0075] Record the maximum absolute value of the liquid phase temperature at the end of the feeding process compared to the set temperature. This deviation reflects the temperature control accuracy of the reaction system.
[0076] Experimental data Table 4. Mg content during the feeding process in different embodiments and comparative examples. 2+ Activity fluctuation and feeding pause parameters
[0077] Figure 4 This is a comparison chart of the dynamic metastable region control effect of Test Example 4 of the present invention, where (a) represents the Mg content of each embodiment and comparative example throughout the feeding process. 2+ The average activity (top height of the bar chart) and standard deviation (top of the error bar) are shown. (b) indicates the number of times the PLC system triggered a pause in feeding for the corresponding sample. The horizontal axis represents Examples 1, 3, 4, 5 and Comparative Examples 8, 9, 10, 12. The grayscale of the bars, from light to dark, is used to distinguish different samples. All values are based on Table 4.
[0078] in conclusion According to the data in Table 4, there are systematic differences between the examples using the variable-speed feeding strategy and the comparative examples using constant-speed feeding. Example 3 Mg 2+ The standard deviation of activity was 0.044 mol / L, while the standard deviation of Comparative Example 8 (constant feeding rate, other conditions the same as Example 3) was 0.115 mol / L, the latter being almost three times that of the former. This indicates that under constant feeding rate conditions, Mg... 2+ The activity fluctuated significantly, and the system may frequently cross the metastable region boundary, leading to unstable K2SO4 crystallization conditions. Meanwhile, Mg in Comparative Example 8... 2+The average activity reached 0.53 mol / L, higher than 0.41 mol / L in Example 3, indicating that Mg was significantly increased when fed at a constant rate. 2+ The accumulation rate is faster, making it easier to reach the critical activity for the precipitation of soft potassium magnesium alum. In contrast, Comparative Example 8 had zero pauses, indicating that due to the lack of a feedback control mechanism, no pause measures were taken even when the activity exceeded the control range, and the system could only passively endure the continuous deviation of supersaturation. Comparative Example 9 (reaction at 50℃) Mg 2+ The average activity reached 0.62 mol / L, with a standard deviation of 0.098 mol / L, but the number of pauses was as high as 9, with a total pause time of 270 seconds. The reaction rate increased at high temperatures, and Mg... 2+ The significantly increased release rate caused the activity to frequently exceed the upper limit setpoint of 0.55 mol / L, necessitating extensive intervention from the PLC system to maintain the reaction within a controllable range. Even so, the standard deviation of the activity was still higher than in Example 3, indicating that stable control under high-temperature conditions is inherently more difficult. The situation was the opposite in Comparative Example 10 (reaction at 25°C), where Mg... 2+ The average activity was only 0.29 mol / L, with a standard deviation of 0.073 mol / L, and only two pauses were recorded. The reaction rate was very low at low temperatures, and Mg... 2+ The accumulation rate is slow, making it difficult to trigger the pause condition, but the excessively low reaction temperature leads to insufficient leaching rate, making it impossible to obtain sufficient K2SO4 production within a reasonable process time, which is consistent with its subsequent low potassium leaching rate.
[0079] Test Example 5: Experimental subjects The reaction slurries of Examples 1, 2, 3, 4, 5, and 6, and Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 were taken at the end of their respective maturation processes (when step S4 was completed). Three batches were prepared for each example and comparative example, and samples from each batch were independently measured. The arithmetic mean of the three batches was taken as the final result. A total of 18 samples were involved, with each sample number corresponding to a specific process condition.
[0080] Experimental steps After maturation, transfer all the slurry to a pre-weighed filtration funnel and filter under a vacuum of -0.08 MPa. Collect all the filtrate and weigh it, recording the volume V (L). Wash the filter cake three times with 100 mL of deionized water, and combine the washings with the filtrate, recording the total volume V_total.
[0081] Take 5.0 mL of filtrate and place it in a 250 mL Erlenmeyer flask. Dilute it with deionized water to about 50 mL. Add 5 mL of triethanolamine solution (1:1) to mask interfering ions such as iron and aluminum. Then add 10 mL of ammonia-ammonium chloride buffer solution with pH=10 and about 0.05 g of Eriochrome Black T indicator. Titrate with 0.05 mol / L EDTA standard solution until the solution changes from purple-red to pure blue. Record the volume of EDTA consumed, V_EDTA (mL).
[0082] Since the main cation in the filtrate is K + Mg 2+ Ca 2+ And Ca 2+ In the carnallite leaching system, the content is low and it is precipitated by sulfate. This method converts the Mg content to EDTA consumption. 2+ After equivalence, the K2O concentration was calculated using the pre-calibrated K2O to MgO ratio relationship established by ICP-OES. The specific calculation used a pre-established calibration curve: C_K2O = k × (V_EDTA × C_EDTA / V_sample), where k is the conversion factor calibrated with standard K2SO4 solution (determined using 5 different concentrations of K2SO4 standard solutions, with a linear correlation coefficient R). 2 ≥0.999).
[0083] Using the total K₂O equivalent of carnallite powder (K₂O content in the raw carnallite determined to be 12.3% by mass through X-ray fluorescence spectroscopy) as the benchmark, the potassium leaching rate η was calculated as: η = (C_K₂O × V_total) / (m_ore × ω_K₂O) × 100%, where m_ore is the amount of carnallite powder added (100 parts by mass), and ω_K₂O is the mass fraction of K₂O in the raw material. The average values of the three batches of measurements are recorded in Table 5. To reflect the irregularity of the data, the minimum and maximum values of the three batches of measurements are given in the table, rather than the standard deviation.
[0084] Experimental data Table 5. Results of potassium leaching rate determination for each example and comparative example.
[0085] Figure 5 This is a comparison chart of potassium leaching rates in Test Example 5 of the present invention. The chart shows the potassium leaching rate determination results of three batches of parallel experiments for each example and comparative example sample. The circular markers represent the arithmetic mean of the three batches of measurements, the upper and lower endpoints of the vertical line are the minimum and maximum values of the three batches, respectively, and the gray scatter dots represent the single measurement values of each batch. The horizontal axis represents Examples 1 to 6 (Examples 1 to 6) and Comparative Examples 1 to 12 (Comparative Examples 1 to 12), with the example and comparative example areas separated by dashed lines in the chart.
[0086] According to the data in Table 5, the average potassium leaching rate of Example 3 was 84.3%, with the results of the three batches fluctuating between 83.0% and 85.7%, a fluctuation range of 2.7 percentage points. The potassium leaching rate of Comparative Example 1 (without seed crystals, complexing agents, or crystal morphology regulators) was only 41.8%, and the fluctuation range of 39.5% to 44.0% indicates that the reaction itself is unstable even without any auxiliary agents. The difference between the two exceeds 40 percentage points, which directly reflects the cumulative effect of the synergistic effect of the seed crystals, complexing agents, and crystal morphology regulators.
[0087] Test Example 6: Experimental subjects The final products obtained after the curing of Examples 1, 2, 3, 4, 5, and 6, and Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 in their respective processes, followed by filtration, washing, and drying, were collected. Three parallel samples (approximately 2g each) were randomly selected from each sample for independent testing, and the arithmetic mean was taken as the final result. Product samples were involved under 18 preparation conditions, with each sample number corresponding to one process condition.
[0088] Experimental steps Grind each dried product in an agate mortar until it all passes through a 100-mesh sieve, place it in a 105℃ oven to dry to constant weight (about 2 hours), and then place it in a desiccator to cool to room temperature for later use.
[0089] Weigh approximately 0.5 g of the sample (accurate to 0.0001 g) into a 250 mL beaker, add 50 mL of hot water (approximately 80 °C), stir to dissolve, and transfer to a 250 mL volumetric flask and dilute to volume. Take 25.0 mL of the solution into an Erlenmeyer flask, add 10 mL of ammonia-ammonium chloride buffer solution (pH=10) and approximately 0.05 g of Eriochrome Black T indicator, and titrate with 0.05 mol / L EDTA standard solution until a pure blue solution is obtained, recording the volume consumed. Calculate the mass fraction of K₂O in the sample (after deducting Mg) based on the EDTA consumption. 2+ Ca 2+ After interference, the conversion is performed using the established standard curve.
[0090] Weigh approximately 0.2 g of the sample, dissolve it according to S2, and take 25.0 mL. Add 2 mL of triethanolamine (1:1) to mask interfering ions. Use a calcium-magnesium mixed indicator (acid chrome blue K + naphthol green B) and titrate with 0.01 mol / L EDTA standard solution until the purple-red color changes to blue-green. Calculate Mg. 2+ Quality score.
[0091] Weigh approximately 1g of the sample and dissolve it in 50mL of deionized water. Add 2mL of 10% K₂CrO₄ indicator and titrate with 0.1mol / L AgNO₃ standard solution until a brick-red precipitate just appears. Record the volume of AgNO₃ consumed and calculate the Cl₂ content. - Quality score.
[0092] Calculate the purity of potassium sulfate (as K2SO4): Based on the mass fraction of K2O, convert it to the amount of potassium sulfate using the formula K2SO4 = K2O × 174.26 / 94.20, then divide by the total mass of the sample to obtain the purity (%). Since some K2O may come from other potassium salts (such as molten potassium magnesium sulfate), the actual purity is based on the converted K2O value. If the converted potassium sulfate ratio is greater than 100%, it indicates the presence of double salt interference; however, in this experiment, this ratio was less than 100% for all samples.
[0093] Experimental data Table 6. K2O content and Mg content of each example and comparative product 2+ Content and purity of potassium sulfate
[0094] Figure 6 This is a comparison chart of the purity and impurity content of the products in Test Example 6 of this invention, where (a) represents the potassium sulfate purity (converted to K2O) of each example and comparative example product, and (b) represents the Mg content in the corresponding product. 2+ Residual content. The circular markers represent the average values of three batches of parallel samples. The upper and lower endpoints of the vertical line represent the minimum and maximum values of the three batches, respectively. The gray dots represent the values of a single measurement for each batch. The horizontal axis represents Examples 1 to 6 (Examples 1 to 6) and Comparative Examples 1 to 12 (Comparative Examples 1 to 12). The areas of Examples and Comparative Examples are separated by dashed lines in the figure.
[0095] According to the data in Table 6, the average purity of potassium sulfate in the product of Example 3 was 98.7%, and the Mg content was... 2+ The average residual amount was 0.22%; Example 4 had a higher purity, reaching 99.5%, with Mg... 2+ Only 0.15%. In contrast, Comparative Example 1 (without any additives) had a purity of only 79.5%, Mg 2+ The content is as high as 2.85%, indicating that in the absence of seed crystals, complexing agents, and crystal form regulators, a large amount of Mg... 2+ The addition of potassium magnesium sulfate or other double salts to the product significantly reduces the effective potassium sulfate content. Comparative Example 2 (with only 0.75 parts seed crystals added) had a purity of 86.3%, Mg... 2+ The purity was 1.92%, an improvement over Comparative Example 1, but still significantly higher than the examples. Comparative Example 3 (with only sodium citrate added) had a purity of 80.7%, and Mg... 2+The value was 2.54%, which is close to that of Comparative Example 1, indicating that a single complexing agent cannot independently complete the preparation of high-purity products, and the role of seed crystals is indispensable.
[0096] Test Example 7: Experimental subjects The final dried products (potassium sulfate products after filtration, washing, and drying at 105°C for 2 hours) of Examples 1, 2, 3, 4, 5, 6, and Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 were taken respectively. Three parallel samples of each sample were taken for laser particle size analysis and X-ray diffraction analysis.
[0097] Experimental steps Take about 1g of sample and place it in an agate mortar. Press it lightly to loosen the agglomerates and let them all pass through a 200-mesh sieve (about 75μm) to ensure that no large particles remain.
[0098] Approximately 0.2 g of sieved sample was added to the dry disperser of a Microtrac S3500 laser particle size analyzer. The dispersion pressure was 0.2 MPa, the feed rate was 20%, and the measurement range was 0.02 μm to 2000 μm. Each sample was measured three times consecutively, and the median volume diameters D50 (μm), D10, and D90 were recorded. The average of the three measurements was used as the final result, while recording the values of each measurement to account for fluctuations.
[0099] Approximately 0.5 g of sample was placed in an XRD sample holder. A Cu target Kα beam was used, with a scanning range of 2θ = 5°–60°, a step size of 0.02°, and a scanning speed of 6° / min. The obtained diffraction pattern was compared with a standard PDF card (K₂SO₄arcanite, PDF#72-1680) to confirm that the main crystalline phase was potassium sulfate. The presence of impurity diffraction peaks (such as MgSO₄·3H₂O, K₂Mg₂(SO₄)₃, etc.) was recorded.
[0100] Experimental data Table 7. Particle size distribution parameters and crystal phase identification results of each example and comparative example product.
[0101] Figure 7This is a comparison chart of the particle size distribution and span of potassium sulfate product in Test Example 7 of this invention. (a) represents the median volume diameter (D50) of each example and comparative example product. The circular markers represent the average of three measurements, the upper and lower endpoints of the vertical line represent the minimum and maximum values of the three measurements, and the gray dots represent the values of each individual measurement. (b) represents the particle size distribution span of the corresponding sample (Span = (D90 - D10) / D50). The horizontal axis represents Examples 1 to 6 (Examples 1 to 6) and Comparative Examples 1 to 12 (Comparative Examples 1 to 12). The example and comparative example areas are separated by dashed lines in the figure.
[0102] According to the data in Table 7, Example 4 had the smallest D50 (12.4 μm) and a span of 1.72; Example 3 had a D50 of 15.7 μm and a span of 1.61; while Comparative Example 1 had the largest D50 (35.2 μm) and a span of 1.97, and soft potassium magnesium alum impurities were detected in the product. Particle size directly reflects the distribution of the number of crystal nuclei and growth time during seed-induced crystallization. The more seed crystals used, the larger the initial number of crystal nuclei, and the smaller the single crystal size within the same growth time. Therefore, the particle size of Example 4 (1.0 part seed crystals) was significantly smaller than that of Example 1 (0.5 parts seed crystals, D50 = 18.3 μm). This is consistent with the trend of the average crystal particle size in Test Example 1, but the median volume diameter given by laser particle size analysis is slightly larger than the microscopic measurement value. This is because the microscope only measures a few crystals, while the laser particle size analysis covers all particles, and a small amount of fine powder agglomeration may still exist after sieving.
[0103] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing potassium sulfate by leaching carnallite at room temperature, characterized in that, Includes the following steps: S1. Mix carnallite powder, potassium sulfate micro powder as seed crystals, and sodium citrate as a complexing agent to obtain a premix; the potassium sulfate micro powder is used to induce heterogeneous crystallization of potassium sulfate, and the sodium citrate is used to complex magnesium ions in the reaction system to inhibit the formation of double salts. S2. Add process water and potassium chloride to the reactor, stir to dissolve, and then add sodium polyacrylate aqueous solution as a crystal shape regulator to control the liquid phase temperature within the room temperature range; the sodium polyacrylate is used to regulate the aspect ratio of the by-product gypsum crystals to improve the reaction fluid dynamics. S3. Under dynamic metastable zone control conditions, the premix obtained in S1 is added to the reaction mother liquor obtained in S2. During the reaction, the activity of magnesium ions in the liquid phase is monitored in real time, and the feeding rate is dynamically adjusted according to the change of magnesium ion activity. S4. After feeding is completed, the mixture is matured, and the resulting slurry is separated into solid and liquid phases. The solid phase is washed and dried to obtain potassium sulfate product.
2. The method for preparing potassium sulfate by room-temperature leaching of carnallite according to claim 1, characterized in that, In step S1, the amount of potassium sulfate powder used is 0.5% to 1.0% of the mass of carnallite powder.
3. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S1, the amount of sodium citrate used is 5% to 10% of the mass of potassium sulfate powder.
4. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S2, the effective mass concentration of sodium polyacrylate in the reaction mother liquor is 0.1% to 0.2%.
5. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, The sodium polyacrylate has a weight-average molecular weight of 3000 to 5000.
6. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S2, the liquid phase temperature is controlled within the range of 32±2℃~38±2℃.
7. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S3, the dynamic metastable region control includes: setting the upper limit of magnesium ion activity to 0.55–0.65 mol / L; pausing feeding when the detected value of magnesium ion activity reaches the upper limit, and resuming feeding after the magnesium ion activity drops below the upper limit and increasing the feeding rate of the next stage by 5%–15%.
8. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S3, the total feeding time of the premix is 120 to 150 minutes.
9. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S4, the solid phase after solid-liquid separation is washed with deionized water 1 to 2 times, and the amount of water used for each wash is 0.5 to 1.0 times the mass of the solid phase.
10. The method for preparing potassium sulfate by room temperature leaching of carnallite according to claim 1, characterized in that, In step S4, the drying temperature is 80–105°C, and the product is dried until the moisture content is ≤0.5%.