Chemical removal agent, method of making and use thereof

The chemical removal agent prepared by the hydrothermal-ball milling multi-level loading method utilizes the synergistic effect of iron-manganese phosphate composite materials to solve the difficulties in removing complex pollution and the risk of secondary pollution in the treatment of heavy metal pollution, and achieves efficient and stable heavy metal removal and immobilization effects.

CN123151503APending Publication Date: 2026-11-24HUNAN PROVINCIAL URBAN GEOLOGICAL SURVEY & MONITORING INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611666203.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing heavy metal pollution control technologies face challenges such as difficulty in synergistic removal of complex pollution, drastic fluctuations in operating conditions, and high risks of secondary pollution. In particular, when dealing with multiple heavy metal ions and soil pollution, existing methods are inefficient, unstable, and pose a risk of secondary pollution.

Method used

Chemical removal agents were prepared by a hydrothermal-ball milling multi-level loading method. Iron and manganese sources were used to form Lewis acid sites and glucose hydroxyl functional groups in a weakly alkaline environment. Combined with the slow-release reaction of phosphate and the adsorption of hydroxyl groups on the surface of iron oxide, the adsorption-precipitation and coordination fixation of heavy metals were achieved, forming a highly stable active component loading structure.

Benefits of technology

It achieves a high-efficiency synergistic removal rate (≥95%) and stabilization rate (>50%) for multiple heavy metal ions, maintains stable performance under dynamic fluctuation conditions, reduces the risk of secondary pollution, and is adaptable to different heavy metal pollution scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123151503A_ABST
    Figure CN123151503A_ABST
Patent Text Reader

Abstract

This invention relates to the field of heavy metal polluted wastewater treatment technology, and discloses a chemical removal agent, its preparation method, and its application. A complexing agent solution is mixed with a solution containing a source M, and glucose is added under stirring to obtain a mixture. Through the synergistic effect of Lewis acidic sites and hydroxyl functional groups, adsorption-precipitation and coordination fixation of heavy metal cations are simultaneously achieved in a weakly alkaline environment. The mixture is reacted under hydrothermal conditions and dried to obtain a reaction precursor. The reaction precursor and phosphate are ball-milled in a ball mill to obtain a product. A multi-level loading method involving hydrothermal treatment and ball milling is used to achieve uniform loading of carbon-based and iron-based active components and phosphate on a carrier material. The obtained product is annealed at high temperature under an inert atmosphere to obtain the chemical removal agent. By controlling the ratio of iron to manganese sources and the annealing temperature, the pore structure and crystallinity of the active components are optimized, giving the material high stability and anti-interference ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heavy metal polluted wastewater treatment technology, and in particular, to a chemical removal agent, its preparation method, and its application. Background Technology

[0002] With rapid industrialization, heavy metal pollutants emitted from industries such as mining, metal smelting, and new energy battery manufacturing have become a significant source of environmental pollution. These pollutants have complex origins, are difficult to treat, and pose a serious threat to the ecological environment and human health.

[0003] Industrial production is a major source of heavy metal pollution. During mining operations, wastewater containing heavy metals such as cadmium (Cd) and lead (Pb) generated from waste rock leaching can reach concentrations of 0.5 mg / L to 15 mg / L. In acidic wastewater (pH < 3) discharged from the metallurgical industry, the proportion of active heavy metal ions such as copper (Cu) and zinc (Zn) exceeds 70%, making them highly susceptible to diffusion via surface runoff. Furthermore, the rapid development of the new energy industry has led to an average annual increase of 17% in the demand for metals such as cobalt (Co), nickel (Ni), and manganese (Mn) for power battery production; however, due to an imperfect recycling system, approximately 30% of these metals ultimately enter the environment. The long-term application of fertilizers and pesticides containing cadmium and arsenic (As) in agricultural activities, as well as the weathering and release of heavy metals due to improper disposal of electronic waste, further exacerbate multi-media pollution problems in soil and water bodies.

[0004] Currently, the treatment of heavy metal pollution mainly relies on physicochemical methods and bioremediation technologies.

[0005] Physicochemical methods include chemical precipitation, adsorption, ion exchange, and membrane separation.

[0006] Chemical precipitation method: Heavy metals are precipitated as hydroxides by adding alkali. It is low cost, but it produces a large amount of sludge containing heavy metals. Moreover, the sludge solidification rate is less than 60%, which poses a risk of secondary pollution.

[0007] Adsorption method: Adsorbents such as activated carbon and nanomaterials are used to retain heavy metal ions, but the adsorbent materials are difficult to regenerate, have poor economic efficiency, and the removal efficiency drops significantly in high-concentration complex pollution systems.

[0008] Ion exchange method: It uses resin to selectively replace heavy metal ions, but the resin is easily saturated and high-salt wastewater will reduce the exchange efficiency.

[0009] Membrane separation technologies (such as reverse osmosis and nanofiltration) can efficiently remove heavy metal pollutants, but they can lead to the concentration of heavy metal pollutants, and the concentration of heavy metals in the concentrate can be up to 10 times that of the original water, making subsequent treatment difficult.

[0010] Among them, bioremediation technology uses hyperaccumulating plants (such as centipede grass to accumulate arsenic) or microorganisms (such as sulfate-reducing bacteria to fix cadmium) for ecological restoration, but the restoration cycle is as long as 3 to 5 years, and the harvested organisms need to be further processed, otherwise it may cause secondary release of heavy metals.

[0011] The main technical challenges in heavy metal pollution control: 1. Difficulty in synergistic removal of complex pollutants: Actual wastewater usually contains 5 to 8 kinds of heavy metal ions (such as Zn, Cu, Cd, etc.), and the competitive adsorption effect between ions will lead to a 15% to 25% decrease in removal rate; Soil pollution also commonly contains at least 3 kinds of complex pollution, and existing technologies are difficult to achieve efficient synergistic removal.

[0012] 2. Drastic fluctuations in operating conditions: The quality and quantity of industrial wastewater fluctuate greatly. For example, the temperature of metal smelting wastewater can vary from 30℃ to 80℃, and existing treatment processes are difficult to stably adapt to such drastic fluctuations.

[0013] 3. Significant risk of secondary pollution: Chemical precipitation generates more than 20 million tons of heavy metal sludge annually, of which less than 60% is effectively solidified; if the concentrate produced by membrane technology is not properly disposed of, it can easily cause leachate pollution and exacerbate environmental risks. Summary of the Invention

[0014] This invention provides a chemical removal agent, its preparation method, and its applications. A hydrothermal-ball milling multi-layer loading method achieves uniform loading of carbon-based and iron-based active components and phosphate stabilizers on a carrier material. Based on the iron-phosphorus slow-release mechanism, through a dual pathway of phosphoric acid slow-release reaction and hydroxyl adsorption on the surface of iron oxides, it can simultaneously remove 5-8 heavy metal ions such as lead, cadmium, copper, and zinc from wastewater (removal rate ≥95%), and achieve heavy metal stabilization in soil remediation (conversion rate >50%). The prepared chemical removal agent can be applied to the simultaneous treatment of wastewater contaminated with multiple types of metals and the simultaneous remediation of soil contaminated with multiple types of metals. In the wastewater treatment field, the chemical removal agent can treat complex wastewater with pH 3-10 and heavy metal concentration fluctuations ranging from three orders of magnitude through adsorption test batches. In soil remediation, using an in-situ addition method (addition amount 3wt%-7wt%), it can simultaneously immobilize multiple heavy metals. This addresses the technical problems of low treatment efficiency, poor operational stability, and high risk of secondary pollution in existing heavy metal pollution treatment technologies.

[0015] According to one aspect of the present invention, a method for preparing a chemical removal agent is provided, comprising the following steps: S100, mixing a complexing agent solution with a solution containing a source M, and then adding glucose under stirring to obtain a mixture; the source M is an iron source and a manganese source; the molar ratio of iron to manganese is 1:0.2~0.5; the complexing agent in the complexing agent solution is at least one of oxalic acid and citric acid, and the concentration of the complexing agent is 0.01mol / L-0.5mol / L; through the synergistic effect of Lewis acidic sites and hydroxyl functional groups, in a weakly alkaline environment... Simultaneously, the adsorption-precipitation and coordination fixation of heavy metal cations are achieved. In step S200, the mixture is reacted under hydrothermal conditions at a temperature of 200℃-280℃, and then dried to obtain a reaction precursor. In step S300, the reaction precursor and phosphate are ball-milled in a ball mill to obtain the product. Through a multi-level loading method involving hydrothermal treatment and ball milling, uniform loading of carbon-based and iron-based active components and phosphate on the carrier material is achieved. In step S400, the obtained product is annealed at high temperature under an inert atmosphere at a temperature of 500℃~800℃ for 30~120 min, with a heating rate of 10℃ / min-20℃ / min, to obtain a chemical removal agent. By adjusting the ratio of iron to manganese sources and the annealing temperature, the pore structure and crystallinity of the active components are optimized, endowing the material with high stability and anti-interference ability.

[0016] Furthermore, the manganese source is at least one of manganese chloride and manganese nitrate; and / or the iron source is at least one of ferric chloride and ferric nitrate nonahydrate.

[0017] Furthermore, in the solution containing source M, the concentration of element M is 0.01 mol / L to 0.5 mol / L.

[0018] Further, the glucose is anhydrous glucose and / or glucose monohydrate, and the mass ratio of glucose dosage to complexing agent is 60:1 to 10:1. Preferably, the mass ratio of glucose dosage to complexing agent is 50:1 to 25:1.

[0019] Furthermore, in the mixture, the ratio of complexing agent to element M is 1.2 to 2.2:1, measured by molar ratio.

[0020] Further, the mass ratio of the reaction precursor to the phosphate is 1:0.01 to 0.1; the phosphate is at least one selected from hydroxyapatite, calcium hydrogen phosphate, or potassium dihydrogen phosphate. Preferably, the mass ratio of the reaction precursor to the phosphate is 1:0.03 to 1:0.07.

[0021] Furthermore, the inert atmosphere is nitrogen or argon.

[0022] According to another aspect of the present invention, a chemical removal agent is also provided, which is prepared by the above-described method for preparing a chemical removal agent.

[0023] According to another aspect of the present invention, an application of a chemical removal agent is also provided, wherein the chemical removal agent is used for the treatment of wastewater contaminated with a single heavy metal or metalloid; or for the treatment of wastewater contaminated with multiple heavy metals and / or metalloids.

[0024] The present invention has the following beneficial effects: 1. Highly efficient synergistic removal of multiple heavy metals: Through the coordination synergistic effect of Lewis acidic sites formed by iron and manganese sources in a weakly alkaline environment and glucose hydroxyl functional groups, the chemical removal agent simultaneously possesses the adsorption-precipitation and coordination fixation capabilities of heavy metal cations, significantly improving the simultaneous removal efficiency of multiple heavy metals (such as Cd, Pb, Cu, Zn, etc.) in complex pollution systems, overcoming the problem of decreased removal rate caused by competitive adsorption in traditional technologies.

[0025] 2. Enhanced material stability and anti-interference properties: The hydrothermal reaction combined with high-temperature annealing process directionally regulates the pore structure and crystallinity of the iron oxide, manganese oxide and phosphate composite material, forming a highly stable active component loading structure, so that the chemical removal agent can maintain stable heavy metal removal performance under dynamic fluctuation conditions (such as temperature changes and high salt environment).

[0026] 3. Reduce the risk of secondary pollution: By introducing phosphate and high-temperature annealing, heavy metals form stable phosphate precipitates or solid solutions on the surface of the removal agent, significantly reducing the risk of heavy metal re-dissolution; at the same time, the construction of the carbon-based framework avoids the problem of generating a large amount of sludge in traditional chemical precipitation methods, and achieves permanent immobilization of heavy metals.

[0027] 4. Optimize the adjustability of material functions: By adjusting the ratio of iron source to manganese source and annealing temperature, the distribution of surface active sites and pore size characteristics of chemical removal agents can be precisely controlled, making them suitable for different heavy metal pollution scenarios (such as high-concentration wastewater or low-concentration soil leachate), thereby improving the versatility and engineering application potential of the materials.

[0028] 5. Unlike existing hydrothermal-ball milling multi-layered loading methods, this invention achieves a higher density of active sites through the synergistic effect of Lewis acidic sites and surface –OH groups in Fe / Mn oxides, as well as by controlling the iron / manganese ratio and annealing temperature. Simultaneously, the Fe-Mn-phosphate ternary system brings complementary effects from precipitation, complexation, and ion exchange mechanisms, significantly improving adsorption capacity and stability. This synergistic effect results in higher removal rates and lower re-dissolution rates.

[0029] In addition to the objectives, features, and advantages described above, the present invention has other objectives, features, and advantages. The invention will now be described in further detail with reference to the figures. Attached Figure Description

[0030] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a scanning electron microscope image of the chemical removal agent (BC-Fe / P) obtained in preferred embodiment 1 of the present invention, wherein... Figure 1 (a) is a SEM image at the 5μm level. Figure 1 (b) is a SEM image at the 10μm level; Figure 2 This is the FTIR spectrum of the chemical removal agent (BC-Fe / P) obtained in the preferred embodiment 1 of the present invention; Figure 3 This is a graph showing the removal effect of the chemical removal agent (BC-Fe / P) prepared in Example 1 on Pb, Cd, Zn and Cu in lead-cadmium-zinc-copper composite polluted wastewater, which is a preferred verification example of the present invention. Figure 4 This is a graph showing the removal effect of the chemical removal agent (BC-Fe / P) prepared in Example 1 on arsenic-contaminated wastewater in the preferred verification example 2 of the present invention.

[0031] Figure 5 This is a graph showing the removal effect of the chemical removal agent (BC-Fe / P) prepared in Example 1 on lead, cadmium, zinc, copper and arsenic polluted wastewater in the preferred verification example 3 of the present invention; Figure 6 This is a graph showing the removal effect of the chemical removal agent (BC-Fe / P) prepared in Example 1 on As in wastewater contaminated with different concentrations, as described in the preferred verification example 4 of this invention. Figure 7 This is a graph showing the stabilization effect of the chemical removal agent (BC-Fe / P) prepared in Example 1 on Pb, Cd, Zn, Cu, and As in soil contaminated with lead, cadmium, zinc, copper, and arsenic in the preferred verification example 5 of this invention. Figure 8 This is a scanning electron microscope image of the chemical removal agent (BC-Fe-Mn / P) obtained in preferred embodiment 2 of the present invention, wherein... Figure 8 (a) is a SEM image at the 5μm level. Figure 8 (b) is a SEM image at the 50μm level; Figure 9 This is the FTIR spectrum of the chemical removal agent (BC-Fe-Mn / P) obtained in preferred embodiment 2 of the present invention; Figure 10 This is a graph showing the removal effect of the chemical removal agent (BC-Fe-Mn / P) prepared in Example 2 on lead, cadmium, zinc, copper and arsenic polluted wastewater in the preferred verification example 6 of the present invention; Figure 11This is a diagram showing the stabilization effect of the chemical removal agent (BC-Fe-Mn / P) prepared in Example 2 on Pb, Cd, Zn, Cu, and As in soil contaminated with lead, cadmium, zinc, copper, and arsenic in the preferred verification example 7 of the present invention. Figure 12 This is the NH3-TPD diagram of the preferred embodiment 2 (BC-Fe-Mn / P) and comparative examples 1 (BC-P) and 2 (BC-Mg-P) of the present invention. The diagram includes a comparison curve of the desorption peaks of the three chemical removal agents of embodiment 2 (BC-Fe-Mn / P) and comparative examples 1 (BC-P) and 2 (BC-Mg-P). Figure 13 This is an FTIR image of the preferred embodiment 2 (BC-Fe-Mn / P) and comparative examples 1 (BC-P) and 2 (BC-Mg-P) of the present invention. The image includes a comparison curve of the infrared spectra of the three chemical removal agents of embodiment 2 (BC-Fe-Mn / P) and comparative examples 1 (BC-P) and 2 (BC-Mg-P). Figure 14 The bar chart shows the removal efficiency of three chemical removal agents prepared by preferred embodiment 2 (BC-Fe-Mn / P) and comparative examples 1 (BC-P) and 2 (BC-Mg-P) of the present invention, corresponding to verification example 8, for the removal of Pb, Cd, Zn, Cu and As from wastewater contaminated with lead, cadmium, zinc, copper and arsenic. Figure 15 The bar chart shows the removal efficiency of the chemical removal agents prepared in Preferred Example 3 (BC-Fe-Mn / P-2, BC-Fe-Mn / P-3, BC-Fe-Mn / P-4, BC-Fe-Mn / P-5, Fe:Mn=1:0.2~1:0.5) and Example 2 (Fe:Mn≈1:0.49) of this invention, corresponding to Verification Example 9, for the removal of Pb, Cd, Zn, Cu and As in wastewater with combined lead, cadmium, zinc, copper and arsenic pollution. Figure 16 This is a bar chart showing the removal efficiency of chemical removal agents prepared in preferred embodiment 4 of the present invention (BC-Fe-Mn / P-T1, BC-Fe-Mn / P-T2, BC-Fe-Mn / P-T3, BC-Fe-Mn / P-T4, annealing temperatures 500℃ / 550℃ / 600℃ / 650℃), corresponding to verification example 10, for the removal of Pb, Cd, Zn, Cu, and As from lead-cadmium-zinc-copper-arsenic composite polluted wastewater; Figure 17 This is a bar chart showing the removal efficiency of chemical removal agents prepared in Comparative Example 3 (BC-Fe-Mn, without phosphorus source), Comparative Example 1 (BC-P), and Example 2 (BC-Fe-Mn / P) of the present invention, corresponding to Verification Example 11, for the removal of Pb, Cd, Zn, Cu, and As from wastewater contaminated with lead, cadmium, zinc, copper, and arsenic. Detailed Implementation

[0032] The embodiments of the present invention will be described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below. Unless otherwise stated, the raw materials and reagents used in the following embodiments are commercially available or can be prepared by known methods.

[0033] The preparation method of the chemical removal agent in this embodiment includes the following steps: S100, mixing the complexing agent solution with a solution containing source M, and then adding glucose under stirring to obtain a mixture; source M is an iron source and a manganese source; the molar ratio of iron to manganese is 1:0.2~0.5; the complexing agent in the complexing agent solution is at least one of oxalic acid and citric acid, and the concentration of the complexing agent is 0.01mol / L-0.5mol / L; through the synergistic effect of Lewis acidic sites and hydroxyl functional groups, simultaneous action is achieved in a weakly alkaline environment. The process involves the adsorption-precipitation and coordination fixation of heavy metal cations. In step S200, the mixture is reacted under hydrothermal conditions at 200℃-280℃, and then dried to obtain a reaction precursor. In step S300, the reaction precursor and phosphate are ball-milled in a ball mill to obtain the product. A multi-layered loading method combining hydrothermal and ball milling is used to achieve uniform loading of carbon-based and iron-based active components and phosphate on a carrier material. In step S400, the obtained product is annealed at high temperature under an inert atmosphere at 500℃-800℃ for 30-120 min at a heating rate of 10℃ / min-20℃ / min to obtain a chemical removal agent. By adjusting the ratio of iron to manganese sources and the annealing temperature, the pore structure and crystallinity of the active components are optimized, resulting in high stability and anti-interference capabilities. This invention's method for preparing a chemical removal agent effectively addresses the problems of difficult removal of complex pollution, poor adaptability to operating conditions, and high risk of secondary pollution in existing heavy metal pollution control technologies through process steps and synergistic effects of components. Through the synergistic coordination of Lewis acidic sites formed by iron and manganese sources in a weakly alkaline environment with glucose hydroxyl functional groups, the chemical removal agent simultaneously possesses the adsorption-precipitation and coordination fixation capabilities for heavy metal cations. This significantly improves the simultaneous removal efficiency of multiple heavy metals (such as Cd, Pb, Cu, Zn, etc.) in complex pollution systems, overcoming the problem of decreased removal rates caused by competitive adsorption in traditional technologies. Hydrothermal reaction combined with high-temperature annealing directionally regulates the pore structure and crystallinity of the iron oxide, manganese oxide, and phosphate composite material, forming a highly stable active component loading structure. This allows the chemical removal agent to maintain stable heavy metal removal performance even under dynamic fluctuations (such as temperature changes and high-salt environments). The introduction of phosphate and high-temperature annealing treatment enable the heavy metals to form stable phosphate precipitates or solid solutions on the surface of the removal agent, significantly reducing the risk of heavy metal re-dissolution. Simultaneously, the construction of the carbon-based framework avoids the problem of generating large amounts of sludge in traditional chemical precipitation methods, achieving permanent immobilization of heavy metals. By adjusting the ratio of iron to manganese sources and the annealing temperature, the distribution of surface active sites and pore size characteristics of chemical removal agents can be precisely controlled, making them suitable for different heavy metal pollution scenarios (such as high-concentration wastewater or low-concentration soil leachate), thereby improving the versatility and engineering application potential of the materials.Unlike existing hydrothermal-ball milling multi-layered loading methods, this invention achieves a higher density of active sites through the synergistic effect of Lewis acidic sites and surface –OH groups in Fe / Mn oxides, as well as by controlling the iron / manganese ratio and annealing temperature. Simultaneously, the Fe-Mn-phosphate ternary system brings complementary effects from precipitation, complexation, and ion exchange mechanisms, significantly improving adsorption capacity and stability. This synergistic effect results in higher removal rates and lower re-dissolution rates. The chemical remover prepared by this invention combines highly efficient adsorption-precipitation synergy, structural stability, and environmental friendliness, providing a solution for the remediation of complex heavy metal pollution. Preferably, in step S400, the annealing temperature is 500℃~650℃.

[0034] Heavy metal and metalloid polluted wastewater is an important type of wastewater classified in environmental engineering based on its physicochemical properties and ecotoxicity. Its pollutants include typical heavy metal elements (such as cadmium (Cd), lead (Pb), copper (Cu), and zinc (Zn)) and metalloid elements (such as arsenic (As). These pollutants can exist in water bodies in free ionic, colloidal / particulate, or complexed forms (e.g., forming coordination complexes with cyanide, ammonia, or EDTA). Complexed forms often enhance environmental mobility and increase the difficulty of remediation, making them a key target for control.

[0035] In this embodiment, the manganese source is at least one of manganese chloride and manganese nitrate; and / or the iron source is at least one of ferric chloride and ferric nitrate nonahydrate. By selecting specific manganese sources (manganese chloride, manganese nitrate) and iron sources (ferric chloride, ferric nitrate nonahydrate), the preparation process of the chemical removal agent and its heavy metal removal performance can be optimized. Manganese chloride (MnCl2), manganese nitrate (Mn(NO3)2), ferric chloride (FeCl3), and ferric nitrate nonahydrate (Fe(NO3)3·9H2O) are all highly soluble metal salts that can be fully dissociated in aqueous solution, ensuring that iron (Fe) 3+ ) and manganese (Mn 2+ / Mn 3+ The ions are uniformly dispersed, thus forming an active component of iron-manganese oxide with abundant Lewis acidic sites during hydrothermal and annealing processes, enhancing the adsorption and fixation capacity for heavy metals. Chlorides and nitrates can decompose during high-temperature annealing to produce gases (such as HCl, NO). x This helps to form a porous structure, increasing the specific surface area and heavy metal adsorption capacity of chemical removal agents; at the same time, the oxidizing properties of nitrates can promote the formation of high valence states of iron and manganese (such as Fe). 3+ Mn 3 +The selected iron and manganese sources exhibit stable properties, enhancing the redox stability of the material in a weakly alkaline environment. Their coordination ability with the hydroxyl groups of glucose is moderate, enabling them to inhibit premature precipitation of metal ions through complexation and effectively combine with phosphates under hydrothermal conditions to form a stable iron / manganese-phosphate-carbon composite structure. This achieves long-term immobilization of heavy metals and reduces the risk of secondary release. Manganese chloride, manganese nitrate, ferric chloride, and ferric nitrate nonahydrate are all commonly used industrial reagents, inexpensive, and readily available for large-scale production, ensuring the economic efficiency and reproducibility of chemical removal agent preparation and meeting the raw material requirements of practical pollution control projects. The use of these specific manganese and iron sources synergistically improves the active site density, structural stability, and heavy metal removal efficiency of the chemical removal agent, while also considering both feasibility and economic viability.

[0036] In this embodiment, the concentration of element M in the solution containing source M is 0.01 mol / L-0.5 mol / L. By limiting the concentration range to 0.01~0.5 mol / L, the high dispersion of iron / manganese oxides on the carbon-based support can be ensured, forming abundant surface active sites. Within this concentration range, the coordination reaction rate between iron / manganese ions and glucose hydroxyl groups is moderate, which can stabilize metal ions through complexation and avoid local supersaturation precipitation, while also fully combining with phosphate under hydrothermal conditions to form a stable heavy metal immobilization structure. This concentration range matches the hydrothermal reaction (200℃~280℃) and high-temperature annealing (500℃~800℃) processes, ensuring that the metal precursor is effectively converted into a highly crystalline iron / manganese-phosphate active phase during carbonization, while avoiding material pore blockage or sintering due to excessive concentration. The chemical removal agent prepared within this concentration range has a repeatable pore structure and surface chemical properties, and can stably cope with different concentrations of heavy metal pollution scenarios (such as low-concentration soil leachate or high-concentration industrial wastewater). When the concentration of element M is below 0.01 mol / L, the loading of the iron / manganese active components is insufficient, resulting in an excessively low density of Lewis acidic sites in the material, which affects the heavy metal adsorption capacity. When the concentration of element M is above 0.5 mol / L, metal ions are prone to aggregation or premature precipitation, reducing the dispersibility of the active components and hindering uniform complexation with glucose and phosphate. By controlling the concentration of element M between 0.01 mol / L and 0.5 mol / L, the distribution of active components, structural stability, and heavy metal removal efficiency of the chemical removal agent can be synergistically optimized.

[0037] In this embodiment, the iron:manganese ratio is 1:0.2–0.5 according to the molar ratio. This ratio ensures optimal electronic synergy in the formation of iron-manganese oxides, enhancing the simultaneous removal of multiple heavy metals. This ratio range is also beneficial for forming a stable iron-manganese composite oxide crystal structure, avoiding lattice distortion of single metal oxides during high-temperature processing. Appropriate manganese doping can suppress excessive growth of iron oxide particles, maintaining the material's high specific surface area and pore structure. The introduction of manganese can construct Fe... 2+ / Fe 3+ and Mn 2+ / Mn 3+ / Mn 4+ Multivalent redox systems enhance the material's resistance to variable-valence heavy metals (such as Cr). 6+ As 3+ The ratio of manganese to manganese (e.g., iron) enhances the conversion and fixation capacity of iron and manganese, achieving a synergistic adsorption-oxidation effect. The composite metal oxides formed under this ratio exhibit stronger resistance to pH fluctuations and competing ion interference, maintaining stable heavy metal removal efficiency even in complex water environments. When the manganese ratio is below 0.2, the valence state regulation effect of manganese in the material is insufficient, making it difficult to form abundant Mn. 3+ / Mn 4 + Redox active sites: When the manganese ratio is higher than 0.5, excessive manganese will inhibit the formation of iron active sites and reduce the material's selective adsorption capacity for specific heavy metals. Controlling the iron-manganese molar ratio to 1:0.2–0.5 can synergistically optimize the material's crystal structure, surface chemical properties, and heavy metal removal performance.

[0038] In this embodiment, the complexing agent in the complexing agent solution is at least one of oxalic acid and citric acid, and the concentration of the complexing agent is 0.01 mol / L-0.5 mol / L. Both oxalic acid and citric acid are polydentate ligands, capable of reacting with iron (Fe²⁺). 3+ ), manganese (Mn) 2+ / Mn 3+ This process forms stable, soluble complexes, preventing premature hydrolysis and precipitation of metal ions and ensuring their uniform dispersion in solution. This results in highly dispersed active components during hydrothermal and annealing processes. Oxalic acid and citric acid can be partially carbonized under high-temperature hydrothermal and annealing conditions, forming a carbon-based framework rich in oxygen-containing functional groups, enhancing the material's specific surface area and heavy metal adsorption capacity. A complexing agent concentration range of 0.01 mol / L to 0.5 mol / L ensures uniform decomposition of the metal-organic precursor during carbonization, preventing excessive carbon skeleton thickness from clogging active sites due to excessive complexing agent. The carboxylic acid groups (-COOH) of oxalic acid and citric acid can be partially deprotonated (-COO₂) under weakly alkaline conditions. -), and heavy metal cations (such as Cd²⁺) + Pb² + Cu² + (e.g., oxalic acid and citric acid) form a stable coordination structure, improving the heavy metal immobilization efficiency of the material; they can balance the coordination ability of the complexing agent and the precipitation effect of phosphate, achieving synergistic removal of heavy metals through adsorption and precipitation; oxalic acid and citric acid are both inexpensive and readily available industrial raw materials, and have high solubility and stability within this concentration range, facilitating large-scale preparation and ensuring the consistency and economy of the chemical removal agent. When the concentration of the complexing agent is below 0.01 mol / L, the complexing ability is insufficient, and metal ions are prone to local aggregation or precipitation; when the concentration is above 0.5 mol / L, excessive complexing agent may hinder the subsequent loading of phosphate, affecting the structural stability of the material. Using oxalic acid and / or citric acid as complexing agents, and controlling their concentration within 0.01 mol / L~0.5 mol / L, can synergistically optimize the dispersibility of the active components, carbon skeleton structure, and heavy metal removal performance of the chemical removal agent, providing an efficient and stable solution for the treatment of complex heavy metal pollution.

[0039] In this embodiment, the glucose is anhydrous glucose and / or glucose monohydrate, and the mass ratio of glucose to complexing agent is 60:1 to 10:1. Preferably, the mass ratio of glucose to complexing agent is 50:1 to 25:1. As a carbon source, the amount of glucose added directly affects the pore structure and mechanical strength of the hydrothermal carbonization products. The hydroxyl groups (-OH) of glucose synergistically work with the complexing agent (oxalic acid / citric acid) to stabilize iron / manganese ions through coordination bonds, preventing their aggregation during the hydrothermal process. This ratio range ensures that glucose provides a sufficient reducing environment (promoting Fe...) 3+ / Mn 3+This method achieves partial reduction without excessive consumption of the complexing agent, maintaining uniform dispersion of metal ions. The glucose-derived carbon skeleton is rich in oxygen-containing functional groups (such as -OH and -COOH), enabling surface complexation with heavy metal ions. Both anhydrous glucose and glucose monohydrate are standardized industrial raw materials with clearly defined dosage ratios, ensuring consistent performance across different batches. The preferred glucose-to-complexing agent mass ratio is 50:1 to 25:1, forming a carbon-based support with high specific surface area and hierarchical pores, while ensuring full exposure of the active components. At this preferred ratio, the composite structure of the carbon skeleton and the iron / manganese-phosphate active phase is more uniform, achieving synergistic effects of physical adsorption (carbon-based) and chemical fixation (metal active sites). This preferred ratio further balances cost and performance, avoiding resource waste caused by excessive glucose. When the glucose ratio is too high (>60:1), the carbon skeleton becomes too thick, potentially blocking iron / manganese active sites and reducing the heavy metal adsorption capacity. Conversely, when the glucose ratio is too low (<10:1), the carbon skeleton lacks sufficient support, resulting in a loose material structure and decreased mechanical strength. Controlling the mass ratio of glucose to complexing agent to be 60:1–10:1 (preferably 50:1–25:1) can synergistically optimize the carbon-based structure, active component dispersibility, and heavy metal removal efficiency of the chemical remover, providing a reliable guarantee for industrial applications.

[0040] In this embodiment, the mixture has a molar ratio of complexing agent to element M of 1.2–2.2:1, ensuring that each iron / manganese ion binds to 1–2 complexing agent molecules to form a soluble complex, thus preventing metal ion aggregation. At this ratio, the complexing agent and glucose work together, with the complexing agent preferentially coordinating with metal ions to inhibit premature precipitation. The remaining carboxyl groups (-COOH) and glucose hydroxyl groups (-OH) condense at high temperature to form a carbon-based framework with metal doping, enhancing the material's mechanical strength. When the complexing agent ratio is appropriate, some unsaturated metal sites are retained in the hydrothermal products, facilitating subsequent binding with phosphate to form a stable iron / manganese-phosphate active phase. Excessive complexing agent will completely block the metal sites, while insufficient complexing agent will lead to uneven phosphate loading. In materials prepared at this ratio, the oxygen-containing functional groups of the carbon skeleton (derived from complexing agents and glucose) provide physical adsorption sites; moderately exposed iron / manganese-phosphate active phases (such as FePO4, Mn3(PO4)2) provide chemical immobilization sites, enabling the adsorption of Cd. 2+ Pb 2+ Synergistic capture of heavy metals. When the molar ratio of complexing agent to element M is <1.2, the complexing agent is insufficient, and some iron / manganese ions cannot be effectively complexed, leading to local hydrolysis and precipitation, which reduces the dispersibility of the active component; when the molar ratio of complexing agent to element M is >2.2, excessive complexing agent may hinder the subsequent loading of phosphate and generate too much organic residue during the hydrothermal process, affecting the pore structure of the material.

[0041] In this embodiment, the mass ratio of the reaction precursor to the phosphate is 1:0.01 to 0.1; the phosphate is at least one selected from hydroxyapatite, calcium hydrogen phosphate, or potassium dihydrogen phosphate. Preferably, the mass ratio of the reaction precursor to the phosphate is 1:0.03 to 1:0.07. Hydroxyapatite (Ca... 10 (PO4)6(OH)2), dicalcium phosphate (CaHPO4) or potassium dihydrogen phosphate (KH2PO4) contain phosphate (PO4) 3- ) and heavy metal ions (such as Pb) 2+ Cd 2+ The reaction generates low-solubility phosphate precipitates (such as Pb3(PO4)2 and Cd3(PO4)2), achieving permanent immobilization. This ratio range ensures that the phosphate can fully cover the active sites without inhibiting the physical adsorption of the carbon-based framework due to excess. The introduction of phosphate can adjust the surface charge characteristics of the material (such as the negative charge of calcium phosphate salts), enhancing the electrostatic adsorption capacity for cationic heavy metals. Hydroxyapatite is suitable for neutral and weakly alkaline environments, potassium dihydrogen phosphate can adjust the pH of the system, and calcium hydrogen phosphate has a slow-release characteristic. The type and ratio of phosphate can be flexibly selected according to the target heavy metal (such as Cd, Pb, As, etc.). When the phosphate ratio is <0.01, the phosphate content in the active component is insufficient, making it difficult to form a stable heavy metal immobilization structure (such as phosphate precipitate or solid solution), leading to an increased risk of heavy metal re-dissolution. When the phosphate ratio is >0.1, excess phosphate may clog the material pores or cover the iron / manganese active sites, reducing the adsorption capacity. Preferably, the mass ratio of the reaction precursor to phosphate is 1:0.03 to 1:0.07, which can form a uniformly distributed phosphate active phase on the material surface, possessing both high heavy metal immobilization capacity and pore permeability. Under preferred ratios, phosphate forms a composite active phase with iron / manganese oxides (such as FePO4, Mn3(PO4)2), synergistically enhancing redox performance (such as Cr...). 6+ →Cr 3+ By controlling the mass ratio of the reaction precursor to phosphate to be 1:0.01 to 0.1 (preferably 1:0.03 to 0.07), the heavy metal immobilization efficiency, structural stability, and environmental adaptability of the chemical removal agent can be synergistically optimized, significantly reducing the risk of secondary pollution.

[0042] In this embodiment, the inert atmosphere is nitrogen or argon.

[0043] The chemical removal agent in this embodiment is prepared using the method described above.

[0044] The application of the chemical removal agent in this embodiment involves using the aforementioned chemical removal agent for the treatment of wastewater contaminated with a single heavy metal or metalloid; or for the treatment of wastewater contaminated with multiple heavy metals and / or metalloids.

[0045] In practice, this invention provides a chemical removal agent for the simultaneous treatment of wastewater contaminated with multiple types of metals and the simultaneous remediation of soil contaminated with multiple types of metals, along with its preparation method and application. The preparation method includes the following steps: mixing a complexing agent solution with a solution containing a source M, then adding glucose under stirring to obtain a mixture; reacting the mixture under hydrothermal conditions and drying it to obtain a reaction precursor, wherein the source M is an iron source + manganese source; ball milling the reaction precursor with phosphate in a ball mill jar to obtain a product; and annealing the obtained product at high temperature (500℃~800℃) under an inert atmosphere to obtain the final product. The chemical removal agent prepared by this invention, when added to wastewater contaminated with lead, cadmium, zinc, copper, and arsenic at a certain mass ratio, achieves lead, cadmium, zinc, and copper removal rates of over 99%, 95%, 95%, and 95%, respectively, and an arsenic removal rate of over 90%. Furthermore, the stabilization rate of lead, cadmium, zinc, copper, and arsenic in soil reaches over 50%. The chemical removal agent described in this invention has a simple, controllable, and low-cost preparation process; moreover, the removal agent prepared by it has a good removal effect on heavy metals and can be used for the treatment of wastewater contaminated with lead, cadmium, zinc, copper, and arsenic.

[0046] The first objective of this invention is to provide a method for preparing materials for the simultaneous treatment of wastewater contaminated with multiple types of metals and the simultaneous remediation of soil contaminated with multiple types of metals. This method achieves uniform loading of carbon-based and iron-based active components and phosphate stabilizers onto a carrier material through a hydrothermal-ball milling multi-layer loading method.

[0047] The hydrothermal-ball milling multi-level loading method is a composite material preparation method that combines hydrothermal synthesis and mechanical ball milling technology. It is used to efficiently and uniformly load multi-level functional particles onto a carrier material. Its core lies in achieving multi-scale dispersion and interface optimization of the loaded particles by stepwise controlling chemical and mechanical interactions.

[0048] Hydrothermal synthesis: In a closed reactor under high temperature and pressure, loaded particles are grown in situ on the surface of a support by utilizing the dissolution-crystallization process of an aqueous solution. Hydrothermal conditions can control the crystal morphology, size, and crystallinity, and enhance the chemical bonding between the support and the active component.

[0049] Ball milling: further disperses hydrothermal products through mechanochemical action (high-energy collision, shearing), breaks up agglomerates, and promotes interfacial fusion between the support and the loaded particles, forming strong interactions (such as defect sites and chemical bonds).

[0050] The steps to implement multi-tiered load balancing: 1. Primary load (hydrothermal stage) The support and the active component precursor are mixed in a hydrothermal reaction system. By controlling parameters such as temperature and time, loaded particles are generated on the surface of the support. The loaded particles are chemically bonded to the support, and are uniformly distributed and highly crystalline.

[0051] 2. Secondary load (ball milling stage) By ball milling hydrothermal products and additional functional components together, mechanical force is used to achieve: physical mixing to uniformly disperse different components; interface modification, where mechanical energy induces surface activation to form new chemical bonds or defect sites; and structural optimization to regulate particle size and porosity and enhance the mechanical stability of the material.

[0052] Hydrothermal methods offer chemical precision, while ball milling compensates for its dispersion limitations, achieving a dual loading of "chemical anchoring + physical enhancement"; it can construct a multi-level system of "carrier-loaded particles-surface modification", suitable for complex functional requirements.

[0053] The hydrothermal-ball milling multi-level loading method solves the problems of particle dispersion and interfacial bonding in traditional methods by integrating chemical and mechanical energy in a stepwise manner, and is particularly suitable for the controllable preparation of high-performance composite materials.

[0054] The second objective of this invention is to provide the application of the material prepared by the above-described method in the simultaneous treatment of wastewater contaminated with multiple types of metals and the simultaneous remediation of soil contaminated with multiple types of metals. Based on the iron-phosphorus slow-release mechanism, this material can simultaneously remove 5-8 heavy metal ions, such as lead, cadmium, copper, and zinc, from wastewater (removal rate ≥95%) through a dual pathway of phosphoric acid slow-release reaction and hydroxyl adsorption on the surface of iron oxides, and achieve heavy metal stabilization in soil remediation (conversion rate >50%).

[0055] The third objective of this invention is to clarify the engineering application mode of this material. In the field of wastewater treatment, the material can treat complex wastewater with pH 3-10 and heavy metal concentration fluctuations ranging from three orders of magnitude through adsorption test batches; in soil remediation, it can simultaneously immobilize multiple heavy metals by using in-situ addition (addition amount 3wt%-7wt%).

[0056] In this embodiment, the complexing agent is citric acid and oxalic acid, and the concentration of the complexing agent is 0.01 mol / L-0.5 mol / L.

[0057] In this embodiment, the mass ratio of glucose to oxalic acid or citric acid is 60:1 to 10:1, more preferably 50:1 to 25:1. In this embodiment, the concentration of element M in the solution containing source M is 0.01 mol / L to 0.5 mol / L. Preferably, the concentration of element M is 0.05 mol / L to 0.1 mol / L.

[0058] In this embodiment, when the M source is selected as an iron source + manganese source, and measured by molar ratio, the ratio of iron to manganese is 1:0.2 to 1:0.5.

[0059] In this embodiment, the molar ratio of source M to complexing agent is 1:1.2 to 1:2.2. Preferably, the molar ratio of source M to complexing agent is 1:1.3 to 1:1.5.

[0060] In this invention, glucose is added after adding a complexing agent and a metal salt, which can enable the metal elements to form metal-doped carbon materials.

[0061] In this embodiment, the manganese source is selected from at least one of manganese nitrate and manganese chloride.

[0062] In this embodiment, the iron source is selected from at least one of ferric nitrate and ferric chloride.

[0063] In a preferred embodiment, the hydrothermal conditions are 240℃-260℃.

[0064] In this embodiment, the complexing agent in the complexing agent solution is selected from at least one of citric acid and oxalic acid.

[0065] In this embodiment, the reaction is carried out under stirring at a rate of 150-300 rpm, the reaction temperature is room temperature, and the reaction time is 60-120 min.

[0066] In this embodiment, the reaction drying temperature is 105℃~120℃, and the drying time is 12~24h to obtain the reaction precursor.

[0067] In this invention, ball milling of the reaction precursor and phosphate can generate a phosphate-doped material with a slow-release function. Finally, the material is stabilized by high-temperature annealing.

[0068] In this embodiment, the mass ratio of the reaction precursor to phosphate is 1:0.01~0.1. Preferably, the mass ratio of the reaction precursor to phosphate is 1:0.03~1:0.07.

[0069] In this embodiment, the ratio of grinding balls to added materials during the ball milling process is 20:1 to 60:1. Preferably, the ratio of grinding balls to added materials during the ball milling process is 30:1 to 40:1.

[0070] In this embodiment, the ball mill speed is 150~300 rpm during the ball milling process. Preferably, the ball mill speed is 200 rpm during the ball milling process.

[0071] The ball mill mentioned above is a planetary ball mill, and all materials are hard stainless steel. The ball milling process is carried out under vacuum and sealed conditions.

[0072] In this embodiment, the annealing is carried out in a tube furnace, using nitrogen or argon as the protective atmosphere. The annealing temperature is 500~800℃, the annealing time is 60~120min, and the heating rate is 5℃ / min-20℃ / min.

[0073] In actual operation, the annealed product is cooled, washed, dried, ground through a 20-80 mesh sieve, and the material passing through the sieve is taken to obtain the chemical removal agent.

[0074] In this embodiment, the annealing temperature is 600℃ and the heating rate is 15℃ / min.

[0075] In this embodiment, the material was ground through a 60-mesh sieve.

[0076] The present invention also provides a chemical removal agent prepared by the above preparation method.

[0077] The present invention also provides the application of the chemical removal agent prepared by the above preparation method, which is used for the treatment of wastewater contaminated with various metals and the remediation of soil contaminated with various metals.

[0078] The application method is as follows: Add the chemical removal agent to the multi-metal contaminated wastewater, stir until homogeneous, and treat for at least 24 hours. The mass ratio of multi-metal contaminated wastewater to chemical removal agent is 1000:(1-5). In this embodiment, the reaction time is 48h-72h.

[0079] In this embodiment, the heavy metal ions in the heavy metal polluted wastewater include Cd. 2+ Pb 2+ Zn 2+ Cu 2+ AsO4 3- ,HAsO4 2- H2AsO4 1- H3AsO4, HAsO3 2- H2AsO3 1- At least one of H3AsO3.

[0080] The chemical removal agent prepared using this invention can simultaneously remove lead, cadmium, zinc, copper, and arsenic ions from water bodies and stabilize the available components of lead, cadmium, zinc, copper, and arsenic in soil. In water bodies containing lead, cadmium, zinc, copper, and arsenic ions, as well as in soil containing lead, cadmium, zinc, copper, and arsenic, only the chemical removal agent of this invention needs to be added to achieve efficient removal and stabilization.

[0081] This invention relates to a chemical removal agent, its preparation method, and its application for the simultaneous treatment of wastewater contaminated with multiple types of metals and the simultaneous remediation of soil contaminated with multiple types of metals. It has the following beneficial effects: 1. The heavy metal removal agent of this invention achieves the removal of heavy metal cations (Cd) simultaneously in a weakly alkaline environment through the synergistic effect of Lewis acidic sites (iron and manganese oxides) and hydroxyl functional groups. 2+ Pb 2+ Adsorption-precipitation of arsenate (AsO4) and arsenate (AsO4) 3- By fixing the coordination of ions, the limitations of traditional materials in the stepwise treatment of anionic and cationic heavy metals are overcome, and the efficiency of simultaneous removal of multiple pollutants is significantly improved.

[0082] 2. This invention, by adjusting the ratio of iron to manganese sources and the annealing temperature (500℃~800℃), can directionally optimize the pore structure of materials (specific surface area reaching 200m² / g~400m² / g) and the crystallinity of active components (such as the formation of stable FeMnO). X The composite oxide imparts high stability (removal rate still >85% after 5 reuses) and anti-interference ability (maintaining high adsorption efficiency under coexisting ion conditions) to the material. 3. Utilizing the complementary effect of the iron-manganese-phosphate ternary system, the iron component preferentially binds to As and Cd, the manganese component enhances the fixation of Pb and Cu, and the phosphate achieves deep removal by generating heavy metal phosphate precipitates. Ultimately, the removal rate of Pb, Cd, Zn, and Cu in wastewater is >95%, and As is >90%, and it is suitable for high-concentration (<320ppm) pollution scenarios.

[0083] 4. The removal agent described in this invention can convert heavy metal ions in the soil into stable iron-manganese oxide-bound states or phosphate mineral phases through ion exchange between surface hydroxyl groups and heavy metal ions in the soil, thereby reducing the effective state of heavy metals in the soil by more than 85%, and simultaneously solving water and soil pollution problems, achieving a "one agent, two uses" cross-media treatment effect.

[0084] Example 1: This embodiment provides a chemical removal agent (BC-Fe / P composite material), the preparation process of which is as follows: S100, Complexation and Mixing: 70 mL of 0.2 mol / L oxalic acid solution, 65 mL of 0.2 mol / L ferric chloride solution, and 15 mL of 0.2 mol / L manganese chloride solution are thoroughly mixed and stirred at 180 rpm for 60 minutes. Then, 60 g of anhydrous glucose powder is slowly added, and stirring is continued at 180 rpm for 30 minutes to obtain a mixture (Note: In this example, the molar ratio of iron to manganese is 1:0.23; the total molar ratio of complexing agent to M element is approximately 0.875:1; and the mass ratio of glucose to oxalic acid is approximately 42:1).

[0085] S200, Hydrothermal Reaction: The above mixture was placed in a reactor and hydrothermally reacted at 240°C for 4 hours. The product after the reaction was washed with deionized water, filtered, and dried in an oven at 105°C for 12 hours to obtain the reaction precursor.

[0086] S300, Ball Milling Load: Take 10g of dried reaction precursor and 0.3g of potassium dihydrogen phosphate, respectively, and pass them through a 60-mesh sieve. Add grinding balls with a ball-to-material ratio of 35:1 and place them in a ball mill jar. After sealing and evacuating the ball mill jar, ball mill at 300r / min for 3 hours at room temperature, reversing the milling process every 20 minutes. Collect the ball-milled sample.

[0087] S400 Annealing treatment: The ball-milled sample is placed in a tube furnace and heated to 600°C at a rate of 10°C / min under nitrogen protection, and held for annealing for 1 hour. The annealed sample is collected and passed through a 60-mesh sieve to obtain the chemical removal agent (BC-Fe / P composite material).

[0088] Characterization and verification, combined Figure 1 , Figure 2 : The morphology and structure of the chemical removal agent (BC-Fe / P composite material) prepared in this embodiment were characterized. (1) SEM (Scanning Electron Microscopy) analysis: See Figure 1 ,in Figure 1 (a) shows that the material has a sheet-like, layered carrier structure (scale bar 5 μm). Figure 1 (b) (scale bar 10 μm) shows irregular particles uniformly loaded on the carrier surface, presenting a particle-carrier system. The hydrothermal and ball milling processes synergistically promoted the dispersion of the active components. After annealing (600℃), the particles maintained a micron-sized structure and no macroscopic agglomeration occurred, indicating that the material has a high specific surface area, which is beneficial for the adsorption and fixation of heavy metals.

[0089] (2) FTIR (Fourier Transform Infrared Spectroscopy) analysis: See Figure 2 The curves show the functional group changes between the precursor and the BC-Fe / P product. (3400 cm⁻¹) -1 The nearby broad peak corresponds to the OH stretching vibration (surface hydroxyl groups); 1620 cm⁻¹ -1 Nearby corresponding carboxylate / carbon layer vibration; 1085 cm -1 With 1020cm -1 The strong peaks at 875 cm⁻¹ belong to PO bonds and metal -O bonds, confirming the complexation of phosphate with iron-manganese oxide; -1 and 580cm -1The low-frequency region indicates lattice vibrations of metal oxides (such as Fe-O), suggesting the formation of crystalline iron-manganese oxides after annealing. This structure indicates that the material surface possesses abundant hydroxyl groups, Lewis acidic iron-manganese sites, and a phosphate complex phase. During treatment, hydroxyl groups and metal sites synergistically coordinate to fix heavy metals, phosphates induce the precipitation of insoluble phosphates, and the carbon-based support promotes adsorption and enrichment. This multi-stage synergy endows the material with highly efficient removal performance.

[0090] Verification Example 1: 100 mL of wastewater contaminated with a mixture of lead, cadmium, zinc, and copper (concentration 40 mg / L) was taken, and 0.3 g of the chemical removal agent (BC-Fe / P composite material) prepared in Example 1 was added and mixed thoroughly. Samples were taken at 60 min, 120 min, 240 min, 480 min, 720 min, 24 h, 48 h, and 72 h to determine the content of lead, cadmium, zinc, and copper in the wastewater. The results showed that after 72 h, the removal rates of lead, cadmium, zinc, and copper were 99%, 95%, 98%, and 96%, respectively. Figure 3 As shown.

[0091] Verification Example 2: Measure 100 mL of arsenic-contaminated wastewater and add 0.3 g of the chemical removal agent (BC-Fe / P composite material) prepared in Example 1 above, and mix thoroughly. Samples were taken at 60 min, 120 min, 240 min, 480 min, 720 min, 24 h, 48 h, and 72 h to determine the arsenic content in the wastewater. The results showed that the arsenic removal rate in the wastewater after 72 h was 99%. Figure 4 As shown.

[0092] Verification Example 3: 100 mL of a mixed solution of lead, cadmium, zinc, copper, and arsenic was taken from the contaminated wastewater, and 0.5 g of the chemical removal agent (BC-Fe / P composite material) prepared in Example 1 was added and mixed thoroughly. Samples were taken at 60 min, 120 min, 240 min, 480 min, 720 min, 24 h, 48 h, and 72 h to determine the content of lead, cadmium, zinc, copper, and arsenic in the wastewater. The results showed that after 72 h, the removal rates of lead, cadmium, zinc, copper, and arsenic in the wastewater were 98%, 95%, 96%, 95%, and 95%, respectively. Figure 5 As shown.

[0093] Verification Example 4: Arsenic-contaminated solutions with different concentration gradients were prepared: 5 mg / L, 10 mg / L, 20 mg / L, 40 mg / L, 80 mg / L, 160 mg / L, and 320 mg / L. 0.3 g of the chemical removal agent (BC-Fe / P composite material) prepared in Example 1 was added to each solution and mixed thoroughly. Samples were taken at 60 min, 120 min, 240 min, 480 min, 720 min, 24 h, 48 h, and 72 h to determine the arsenic content in the wastewater. The results showed that the arsenic removal rates corresponding to concentrations of 5 mg / L, 10 mg / L, 20 mg / L, 40 mg / L, 80 mg / L, 160 mg / L, and 320 mg / L were 100%, 100%, 100%, 99%, 95.5%, 75.3%, and 51.6%, respectively. Figure 6 As shown.

[0094] Verification Example 5: Weigh 100g of the mixed contaminated soil containing lead, cadmium, zinc, copper, and arsenic, add 5g of the chemical removal agent (BC-Fe / P composite material) prepared in Example 1 above, mix thoroughly, and then add 35mL of ultrapure water to bring the water holding capacity to 80% of the maximum field water holding capacity. Maintain two parallel samples per group. Re-weigh the conical flask every three days, always keeping the soil water holding capacity in the conical flask at approximately 80%. Take soil samples every 7 days. Allow the soil to air dry naturally, pass through a 40-mesh sieve, and determine the content of available lead, cadmium, zinc, copper, and arsenic. The results show that after 98 days, the stabilization rate of lead in the soil was 51%, cadmium 55%, zinc 60.3%, copper 62.4%, and arsenic 65%. The results are as follows: Figure 7 .

[0095] Example 2: This embodiment provides a chemical removal agent (BC-Fe-Mn / P composite material), the preparation process of which is as follows: S100, Complexation and Mixing: Mix 100 mL of 0.1 mol / L citric acid solution with 45 mL of 0.1 mol / L ferric chloride solution and 22 mL of 0.1 mol / L manganese chloride solution, and stir at 180 rpm for 60 minutes. Then slowly add 50 g of glucose and continue stirring until the mixture is homogeneous to obtain a mixture (Note: In this example, the molar ratio of iron to manganese is approximately 1:0.49; the total molar ratio of citric acid to manganese is approximately 1.52:1).

[0096] S200, Hydrothermal Reaction: The above mixture was placed in a reactor and hydrothermally reacted at 240°C for 4 hours. The product after the reaction was washed with deionized water, filtered, and dried in an oven at 105°C for 12 hours to obtain the reaction precursor.

[0097] S300, Ball Milling Load: Take 10g of dried reaction precursor and 0.7g of hydroxyapatite, respectively, and pass them through a 60-mesh sieve. Add grinding balls with a ball-to-material ratio of 40:1 and place them in a ball mill jar. After sealing the ball mill jar and evacuating it, perform solid-phase ball milling at 200r / min for 3 hours at room temperature, with reverse rotation every 30 minutes during the process. Collect the ball-milled sample.

[0098] S400, Annealing treatment: The ball-milled sample is placed in a tube furnace and heated to 600℃ at a rate of 15℃ / min under nitrogen protection, and held for annealing for 2 hours. The annealed sample is collected and passed through a 60-mesh sieve to obtain the chemical removal agent (BC-Fe-Mn / P composite material).

[0099] Characterization and verification, combined Figure 8 , Figure 9 , Figure 12 : The morphology and structure of the chemical removal agent (BC-Fe-Mn / P composite material) prepared in this embodiment were characterized. (1) SEM (Scanning Electron Microscopy) analysis: See Figure 8 , Figure 8 (a) shows that the material has a sheet-like stacked carrier structure, with irregular particles attached to the surface of the sheets. Local magnification shows that the surface is rough and the edges are obviously wrinkled. Figure 8 (b) (scale bar 50 μm) shows an overall micron-scale dense sheet-like aggregate with highly curled and interlocked secondary lamellar structures on the surface, forming a dual composite morphology of "dense stacking-curling". This structure is the result of the synergistic effect of hydrothermal carbonization and ball milling: the hydrothermal reaction promotes the formation of flexible sheets on the carbon-based support, and the metal components are distributed on the surface of the sheets in the form of particles / clusters. The ball milling process further promotes the folding and stacking of the sheets, ultimately forming a macroscopically dense and microscopically wrinkled aggregate. The high surface roughness and high edge defect density indicate that the material has a high specific surface area, which is beneficial for the adsorption and fixation of heavy metals.

[0100] (2) FTIR (Fourier Transform Infrared Spectroscopy) analysis: See Figure 9 The curves show the functional group changes between the precursor and the BC-Fe-Mn / P product. (3400 cm⁻¹) -1 The broad peak in the vicinity corresponds to the OH stretching vibration (surface hydroxyl groups and adsorbed water). In the BC-Fe-Mn / P product, this peak is narrower than in the precursor, indicating that some hydroxyl groups dehydrate or form more stable M-OH bonds with iron and manganese metal after annealing; 1620 cm⁻¹ -1 The nearby peak corresponds to the C=O / C=C stretching vibration (aromatic ring conjugated carbonyl / olefin), which is an indicator of the degree of aromatization of biochar. This peak may also be related to Fe. 3+ / Mn 2+ Coordination to form carboxylate (COO)- –M), reflecting the strong interaction between the metal-carbon support; 1523cm -1 The presence of C=C skeletal vibrations indicates further aromatication / graphitization of the carbon skeleton after annealing; 879 cm⁻¹ -1 With 704cm -1 The peaks were attributed to phosphate ester (POC) bond vibrations and phosphate (POP / POM) vibrations, respectively, clearly confirming that phosphorus is complexed with biochar and iron and manganese oxides in the form of phosphate / phosphate ester to form mineral phases such as iron phosphate (FePO4) and manganese phosphate.

[0101] (3) NH3-TPD analysis: See Figure 12 In this embodiment, the NH3 adsorption and desorption peaks of the chemical removal agent (BC-Fe-Mn / P) are mainly located between 250℃ and 400℃. According to the NH3-TPD testing principle, the desorption peaks below 200℃ belong to the physical adsorption of NH3, while the desorption peaks in the 250℃~450℃ temperature range correspond to the chemically adsorbed NH3, i.e., Lewis acidic sites (NH3 acts as a probe molecule, providing lone pair electrons to Lewis acidic sites to form coordination bonds). This result indicates that the surface of the chemical removal agent (BC-Fe-Mn / P) in this embodiment is rich in Lewis acidic iron-manganese sites, providing sufficient active centers for the coordination and fixation of heavy metal ions.

[0102] The above characterization results collectively demonstrate that the chemical removal agent (BC-Fe-Mn / P) of this embodiment possesses abundant hydroxyl functional groups, Lewis acidic iron-manganese sites, and a phosphate / phosphate ester composite phase on its surface. In heavy metal wastewater treatment, hydroxyl groups and metal sites synergistically achieve surface coordination and fixation of heavy metal ions, the phosphate component induces the formation of insoluble heavy metal phosphate precipitates, and the carbon-based support provides a high specific surface area to promote adsorption and enrichment. These three factors work synergistically to endow the material with highly efficient removal performance.

[0103] Verification Example 6: 100 mL of a mixed solution of lead, cadmium, zinc, copper, and arsenic was taken from the contaminated wastewater, and 0.5 g of the chemical removal agent (BC-Fe-Mn / P) prepared in Example 2 was added and mixed thoroughly. Samples were taken at 60 min, 120 min, 240 min, 480 min, 720 min, 24 h, 48 h, and 72 h to determine the content of lead, cadmium, zinc, copper, and arsenic in the wastewater. The results showed that after 72 h, the removal rates of lead, cadmium, zinc, copper, and arsenic were 99%, 96%, 97%, 95%, and 96%, respectively. Figure 10 As shown.

[0104] Verification Example 7: Weigh 100g of the mixed contaminated soil containing lead, cadmium, zinc, copper, and arsenic, add 5g of the chemical removal agent (BC-Fe-Mn / P) prepared in Example 2 above, mix thoroughly, and then add 35mL of ultrapure water to bring the water holding capacity to 80% of the maximum field water holding capacity. Maintain two parallel samples per group. Re-measure the weight of the conical flask every three days, always maintaining the soil water holding capacity in the conical flask at approximately 80%. Take soil samples every 7 days. Allow the soil to air dry naturally, pass through a 40-mesh sieve, and determine the content of available lead, cadmium, zinc, copper, and arsenic. The results showed that after 98 days, the stabilization rate of lead in the soil was 53.5%, cadmium 56%, zinc 60%, copper 65%, and arsenic 67.5%. Figure 11 As shown.

[0105] Comparative Example 1: Preparation process of BC-P chemical removal agent: S100, Hydrothermal Carbonization: Add 50g of glucose to 170mL of pure water, stir until dissolved, place in a reaction vessel, and hydrothermally react at 240℃ for 4 hours. After the reaction, the product is washed with deionized water, filtered, and dried in an oven at 105℃ for 12 hours to obtain a pure carbon-based precursor.

[0106] S200, Ball Milling Load: Take 10g of dried pure carbon-based precursor and 0.7g of hydroxyapatite, respectively, and pass them through a 60-mesh sieve. Add grinding balls with a ball-to-material ratio of 40:1 and place them in a ball mill jar. After sealing and evacuating the ball mill jar, ball mill at 200r / min for 3 hours at room temperature, reversing the milling process every 30 minutes. Collect the ball-milled sample.

[0107] S300, Annealing treatment: The ball-milled sample is placed in a tube furnace and heated to 600℃ at a rate of 15℃ / min under nitrogen protection, and held at that temperature for 2 hours. The annealed sample is collected and passed through a 60-mesh sieve to obtain the chemical removal agent, named BC-P chemical removal agent.

[0108] Characterization and validation of BC-P chemical removal agent (combined with Figure 12 , Figure 13 ): (1) NH3-TPD analysis ( Figure 12 The NH3 adsorption and desorption peaks of the BC-P chemical remover in Comparative Example 1 are mainly located between 100℃ and 200℃, which falls within the NH3 physical adsorption temperature range (below 200℃). In contrast, the BC-Fe-Mn / P chemical remover in Comparative Example 2 has NH3 adsorption peaks located between 250℃ and 400℃ (corresponding to Lewis acid sites), indicating that without the introduction of iron and manganese metal, the material surface contains almost no Lewis acid sites.

[0109] (2) FTIR analysis Figure 13): Comparative Example 1: BC-P chemical removal agent at 1085 cm⁻¹ -1 With 1165cm -1 Significant PO4 was observed at the location. 3- The vibrational peaks of POC confirmed that phosphate had been successfully loaded onto the carbon substrate by ball milling, forming a phosphate ester / phosphate composite phase.

[0110] Comparative Example 2: Preparation process of BC-Mg-P chemical removal agent: S100, Complexation and Mixing: Mix 100 mL of 0.1 mol / L citric acid solution with 67 mL of 0.1 mol / L magnesium chloride solution and stir at 180 rpm for 60 minutes. Then slowly add 50 g of glucose and continue stirring until the mixture is homogeneous to obtain the final mixture.

[0111] S200, Hydrothermal Reaction: The above mixture was placed in a reactor and hydrothermally reacted at 240°C for 4 hours. The product after the reaction was washed with deionized water, filtered, and dried in an oven at 105°C for 12 hours to obtain the reaction precursor.

[0112] S300, Ball Milling Load: Take 10g of dried reaction precursor and 0.7g of hydroxyapatite, respectively, and pass them through a 60-mesh sieve. Add grinding balls with a ball-to-material ratio of 40:1 and place them in a ball mill jar. After sealing and evacuating the ball mill jar, ball mill at 200r / min for 3 hours at room temperature, reversing the mill every 30 minutes. Collect the ball-milled sample.

[0113] S400 Annealing Treatment: The ball-milled sample was placed in a tube furnace and heated to 600°C at a rate of 15°C / min under nitrogen protection, and held at that temperature for 2 hours. The annealed sample was collected and passed through a 60-mesh sieve to obtain the chemical removal agent, named BC-Mg-P chemical removal agent.

[0114] Characterization and validation of BC-Mg-P chemical removal agent (combined with...) Figure 12 , Figure 13 ): (1) NH3-TPD analysis ( Figure 12 The NH3 adsorption-desorption peaks of the BC-Mg-P chemical remover in Comparative Example 2 were also mainly located between 100℃ and 200℃, similar to the BC-P chemical remover in Comparative Example 1, and no characteristic peaks of Lewis acidic sites above 250℃ were observed. This further confirms that the introduction of iron and manganese components in the chemical remover (BC-Fe-Mn / P composite material) of Example 2 is key to the formation of Lewis acidic sites.

[0115] (2) FTIR analysis Figure 13 ): Comparative Example 2: BC-Mg-P chemical removal agent at 560 cm⁻¹-1 A weak Mg-O vibrational peak appears at 1020 cm⁻¹. -1 The strong peak at 3400 cm⁻¹ indicates the formation of magnesium oxide and magnesium phosphate mineral phases. Meanwhile, the chemical removal agent (BC-Fe-Mn / P composite material) from Example 2 showed a strong peak at 3400 cm⁻¹. -1 The characteristic peak of (-OH) in the vicinity shifted relative to the peak at the same position as the BC-P chemical remover in Comparative Example 1 and the BC-Mg-P chemical remover in Comparative Example 2, proving that there is a strong interaction (coordination or chemical bonding) between the iron-manganese metal and the surface hydroxyl groups, while the magnesium system did not show a similar hydroxyl shift phenomenon.

[0116] Verification Example 8: Prepare several 100mL portions of wastewater contaminated with a mixed solution of lead, cadmium, zinc, copper, and arsenic. Add 0.5g of the chemical removal agent prepared in Example 2 (BC-Fe-Mn / P composite material), Comparative Example 1 (BC-P), and Comparative Example 2 (BC-Mg-P) to each portion separately, and mix thoroughly. After reacting for 72 hours, determine the residual content of lead, cadmium, zinc, copper, and arsenic in the wastewater. The results show that after 72 hours of reaction, the wastewater treated with the chemical removal agent from Example 2 (BC-Fe-Mn / P composite material) showed a lead removal rate of 99%, a cadmium removal rate of 96%, a zinc removal rate of 97%, a copper removal rate of 95%, and an arsenic removal rate of 96%. The wastewater treated with the chemical removal agent from Comparative Example 1 (BC-P) showed a lead removal rate of 75%, a cadmium removal rate of 56%, a zinc removal rate of 63%, a copper removal rate of 68%, and an arsenic removal rate of 3%. The wastewater treated with the BC-Mg-P chemical removal agent (Comparative Example 2) showed a lead removal rate of 40%, a cadmium removal rate of 23%, a zinc removal rate of 25%, a copper removal rate of 31%, and an arsenic removal rate of 5%. The results are as follows: Figure 14 As shown.

[0117] Comparing the removal rates and set sizes of the three methods Figure 12 (NH3-TPD) and Figure 13FTIR analysis revealed that: the BC-P chemical remover prepared in Comparative Example 1 only possessed a carbon matrix and phosphate composite phase, lacking Lewis acidic metal sites. Its NH3 adsorption peak was located at 100℃~200℃, indicating limited coordination and fixation ability for heavy metals, especially with almost no removal effect on arsenic (only 3%). The BC-Mg-P chemical remover prepared in Comparative Example 2, although incorporating metal components, did not possess typical Lewis acidity (NH3-TPD was also located at 100℃~200℃), and FTIR confirmed that it formed Mg3(PO4)2 rather than iron-manganese phosphate. Therefore, its adsorption-precipitation-coordination synergistic effect on heavy metals was far weaker than that of the iron-manganese system. In contrast, the chemical remover prepared in Example 2 (BC-Fe-Mn / P composite material), rich in Lewis acidic iron-manganese sites (NH3-TPD peak at 250℃~400℃) and exhibiting strong interaction between surface hydroxyl groups and metals (FTIR peak at 3400 cm⁻¹), showed a significant improvement. -1 Peak shifting) enabled the efficient simultaneous removal of five heavy metals and their metalloids (all ≥95%). The above comparison confirms that the introduction of iron-manganese bimetallic compounds and the multi-level loading process of "hydrothermal-ball milling-annealing" are key to achieving efficient removal of the five heavy metals and their metalloids.

[0118] Example 3: Preparation of chemical removal agents with different iron-manganese molar ratios.

[0119] The amount of manganese chloride solution added in Example 2 was adjusted to achieve an iron-manganese molar ratio (Fe:Mn) of 1:0.2, 1:0.3, 1:0.4, and 1:0.5, respectively. All other preparation steps, process parameters, and post-treatment conditions remained the same as in Example 2. The four chemical removal agents obtained were named BC-Fe-Mn / P-2 (Fe:Mn=1:0.2), BC-Fe-Mn / P-3 (Fe:Mn=1:0.3), BC-Fe-Mn / P-4 (Fe:Mn=1:0.4), and BC-Fe-Mn / P-5 (Fe:Mn=1:0.5), respectively.

[0120] Verification Example 9: The effect of different iron-manganese molar ratios on the removal performance of mixed lead, cadmium, zinc, copper and arsenic polluted wastewater.

[0121] Prepare several 100mL portions of wastewater contaminated with a mixed solution of lead, cadmium, zinc, copper, and arsenic (each metal / metal ion concentration is 40mg / L). Add 0.5g of each of the four chemical removal agents prepared in Example 3 (BC-Fe-Mn / P-2, BC-Fe-Mn / P-3, BC-Fe-Mn / P-4, BC-Fe-Mn / P-5) and the chemical removal agent prepared in Example 2 (BC-Fe-Mn / P, Fe:Mn≈1:0.49, as a comparative standard), and mix thoroughly. After reacting for 72 hours, determine the residual content of lead, cadmium, zinc, copper, and arsenic in the wastewater. The results show that after 72 hours of reaction, the removal rate of lead in the wastewater containing the chemical removal agent BC-Fe-Mn / P-2 was 90.2%, the removal rate of cadmium was 86.5%, the removal rate of zinc was 88.7%, the removal rate of copper was 84.9%, and the removal rate of arsenic was 85.1%. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in the wastewater treated with BC-Fe-Mn / P-3 were 94.6%, 91%, 93.1%, and 90.5%, respectively. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in the wastewater treated with BC-Fe-Mn / P-4 were 98.8%, 95.4%, 96.7%, 94.8%, and 95.5%, respectively. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in the wastewater treated with BC-Fe-Mn / P-5 were 99%, 96%, 97%, 95%, and 96%, respectively. The results are as follows: Figure 15 As shown.

[0122] Combination Figure 15 It can be seen that as the manganese content in the iron-manganese molar ratio increases (Fe:Mn increases from 1:0.2 to 1:0.5), the removal rates of the five heavy metals and metalloids show a gradual upward trend. When Fe:Mn reaches 1:0.4 or higher, the removal rates of each metal are ≥95%, which is basically the same as the performance of Example 2 (E2, Fe:Mn≈1:0.49). This indicates that the introduction of manganese significantly improves the Lewis acid site density and hydroxyl coordination ability of the material, but excessively high manganese content (above 1:0.5) does not bring further significant improvement. Therefore, the Fe:Mn molar ratio in the claims is preferably 1:0.3~1:0.5, more preferably 1:0.4~1:0.5.

[0123] Example 4: Preparation of chemical removal agents at different annealing temperatures.

[0124] The annealing temperatures in Example 2 were adjusted to 500℃, 550℃, 600℃, and 650℃, respectively. The remaining steps, such as raw material ratio, hydrothermal treatment, ball milling, and annealing time, were the same as in Example 2. Four chemical removal agents were prepared and named BC-Fe-Mn / P-T1 (500℃), BC-Fe-Mn / P-T2 (550℃), BC-Fe-Mn / P-T3 (600℃), and BC-Fe-Mn / P-T4 (650℃), respectively.

[0125] Verification Example 10: Comparison of the removal performance of chemical removal agents with different annealing temperatures on wastewater contaminated with five heavy metals.

[0126] Prepare several 100mL portions of wastewater contaminated with a mixed solution of lead, cadmium, zinc, copper, and arsenic (each metal / metal ion concentration is 40mg / L). Add 0.5g of each of the four chemical removal agents (BC-Fe-Mn / P-T1, BC-Fe-Mn / P-T2, BC-Fe-Mn / P-T3, and BC-Fe-Mn / P-T4) prepared in Example 4 above, and mix thoroughly. After reacting for 72 hours, determine the residual content of lead, cadmium, zinc, copper, and arsenic in the wastewater. The results show that after 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in the wastewater treated with the chemical removal agent BC-Fe-Mn / P-T1 were 93.3%, 90.1%, 91.5%, 89.8%, and 90.4%, respectively. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in wastewater treated with BC-Fe-Mn / P-T2 were 97.8%, 94.2%, 95.3%, 93.7%, and 94%, respectively. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in wastewater treated with BC-Fe-Mn / P-T3 were 99%, 96%, 97%, 95%, and 96%, respectively. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in wastewater treated with BC-Fe-Mn / P-T4 were 84.8%, 84.8%, 87.5%, 85.6%, and 94.6%, respectively. The results are as follows: Figure 16 As shown.

[0127] Combination Figure 16It can be seen that as the annealing temperature increases from 500℃ to 600℃ (BC-Fe-Mn / P-T1 → BC-Fe-Mn / P-T3), the removal rates of the five heavy metals and metalloids gradually increase. Among them, BC-Fe-Mn / P-T3 (600℃) performs best, with a removal rate of ≥95%, consistent with the performance of Example 2. When the temperature rises to 650℃ (BC-Fe-Mn / P-T4), except for arsenic which still maintains a high removal rate (94.6%), the removal rates of lead, cadmium, zinc, and copper decrease significantly (84.8%~87.5%). This indicates that annealing at 600℃ is conducive to the formation of the iron-manganese phosphate phase and the exposure of Lewis acidic sites, while excessively high temperatures (650℃) may lead to pore collapse or sintering of active sites. In summary, the preferred annealing temperature is 550℃~600℃, and more preferably 600℃.

[0128] Comparative Example 3: Preparation of BC-Fe-Mn chemical removal agent (without phosphorus source).

[0129] Based on Example 2, without adding 0.7g of hydroxyapatite, the remaining raw material ratios, hydrothermal treatment, ball milling, and annealing process at 600℃ were exactly the same as in Example 2, and all other steps were also exactly the same. The resulting sample was named BC-Fe-Mn chemical removal agent and was used to verify the synergistic effect of phosphate (hydroxyapatite) in the removal of multiple pollutants.

[0130] Verification Example 11: Comparison of phosphorus source synergistic removal effects, such as Figure 17 As shown.

[0131] Prepare several 100mL portions of wastewater contaminated with a mixed solution of lead, cadmium, zinc, copper, and arsenic (each metal / metal ion concentration is 40mg / L). Add 0.5g of the BC-P chemical removal agent prepared in Comparative Example 1, the chemical removal agent (BC-Fe-Mn / P composite material) prepared in Example 2, and the BC-Fe-Mn chemical removal agent prepared in Comparative Example 3 to each sample, and mix thoroughly. After reacting for 72 hours, determine the residual content of lead, cadmium, zinc, copper, and arsenic in the wastewater. The results show that after 72 hours of reaction, the removal rates of lead in the wastewater with added BC-P chemical removal agent were 75%, cadmium 56%, zinc 63%, copper 68%, and arsenic 3%. After 72 hours of reaction, the removal rates of lead in the wastewater with added BC-Fe-Mn / P chemical removal agent were 99%, cadmium 96%, zinc 97%, copper 95%, and arsenic 96%. After 72 hours of reaction, the removal rates of lead, cadmium, zinc, copper, and arsenic in the wastewater treated with BC-Fe-Mn chemical removal agent were 64%, 47.5%, 48%, 55%, and 91%, respectively. The results are as follows: Figure 17 As shown.

[0132] Combination Figure 17 It can be seen that the chemical removal agent of Example 2 (BC-Fe-Mn / P composite material, complete ternary system) has a removal rate of ≥95% for all five heavy metals and metalloids, which is significantly better than the BC-P chemical removal agent (Fe-Mn deficient) of Comparative Example 1 and the BC-Fe-Mn chemical removal agent (phosphorus-deficient) of Comparative Example 3. Comparative analysis shows that the BC-Fe-Mn chemical removal agent (phosphorus-deficient) of Comparative Example 3 has an excellent removal effect on arsenic (91%) due to the Lewis acidic sites of iron and manganese oxides, but has a low removal rate for heavy metal cations such as lead, cadmium, zinc, and copper (47.5%~64%); while the BC-P chemical removal agent (Fe-Mn deficient) of Comparative Example 1 lacks iron and manganese sites, has almost no removal effect on arsenic (3%), and has limited removal effect on heavy metals. After the introduction of phosphate, the ternary system of the chemical removal agent (BC-Fe-Mn / P composite material) in Example 2 achieves functional complementarity: the iron-manganese component preferentially oxidizes and adsorbs arsenic, while the phosphate forms stable precipitates with lead, cadmium, zinc, and copper. Combined with adsorption on the carbon substrate and coordination with iron-manganese, the efficient and simultaneous removal of five-element mixed pollutants is ultimately achieved. This confirms that the introduction of phosphate and the synergistic effect of the "iron-manganese-phosphorus" ternary system are key to achieving the co-removal of multiple pollutants, demonstrating the necessity of hydroxyapatite (phosphorus source).

[0133] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0134] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.

[0135] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a chemical removal agent, characterized in that, Includes the following steps: S100. Mix the complexing agent solution with the solution containing M source, and then add glucose while stirring to obtain a mixture; M source is an iron source and a manganese source; the molar ratio of iron to manganese is 1:0.2~0.5; the complexing agent in the complexing agent solution is at least one of oxalic acid and citric acid, and the concentration of the complexing agent is 0.01mol / L-0.5mol / L; Through the synergistic effect of Lewis acidic sites and hydroxyl functional groups, adsorption-precipitation and coordination fixation of heavy metal cations can be achieved simultaneously in a weakly alkaline environment. S200. React the mixture under hydrothermal conditions at a temperature of 200℃-280℃, and then dry it to obtain the reaction precursor. S300. The reaction precursor and phosphate are ball-milled in a ball mill jar to obtain the product. A multi-layer loading method involving hydrothermal heating and ball milling was used to achieve uniform loading of carbon-based and iron-based active components and phosphates on a carrier material. S400. The obtained product is annealed at high temperature under an inert atmosphere. The annealing temperature is 500℃~800℃, the time is 30~120min, and the heating rate is 10℃ / min-20℃ / min to obtain the chemical removal agent. By adjusting the ratio of iron to manganese sources and the annealing temperature, the pore structure and crystallinity of the active components of the material are optimized in a targeted manner, thereby endowing the material with high stability and anti-interference ability.

2. The method for preparing the chemical removal agent according to claim 1, characterized in that, The manganese source is at least one of manganese chloride and manganese nitrate; and / or The iron source is at least one of ferric chloride and ferric nitrate nonahydrate.

3. The method for preparing the chemical removal agent according to claim 1, characterized in that, In the solution containing source M, the concentration of element M is 0.01 mol / L-0.5 mol / L.

4. The method for preparing the chemical removal agent according to any one of claims 1 to 3, characterized in that, The glucose is anhydrous glucose and / or glucose monohydrate, and the mass ratio of glucose dosage to complexing agent is 60:1 to 10:

1.

5. The method for preparing the chemical removal agent according to any one of claims 1 to 3, characterized in that, In the mixture, the ratio of complexing agent to element M is 1.2~2.2:1, measured by molar ratio.

6. The method for preparing the chemical removal agent according to any one of claims 1 to 3, characterized in that, The mass ratio of the reaction precursor to phosphate is 1:0.01~0.1; The phosphate is at least one of hydroxyapatite, calcium hydrogen phosphate, or potassium dihydrogen phosphate.

7. A chemical removal agent, characterized in that, It is prepared by the method of any one of claims 1 to 6 for the preparation of the chemical removal agent.

8. The application of a chemical removal agent, characterized in that, The chemical removal agent according to claim 7 can be used for the treatment of wastewater contaminated with a single heavy metal or metalloid; or for the treatment of wastewater contaminated with multiple heavy metals and / or metalloids.