Low-conductivity antistatic functional glass and preparation method thereof
By constructing a composite oxide layer and a density gradient conductive micro-region structure on the surface of a glass substrate, the problem of unifying low electrical conductivity and antistatic properties in functional glass was solved, achieving high surface resistivity, rapid electrostatic dissipation, and excellent light transmittance and hygrothermal stability.
Patent Information
- Application Number
- CN202611386335.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-24
AI Technical Summary
Existing functional glass cannot achieve a balance between low electrical conductivity and antistatic properties, resulting in static electricity accumulation that affects light transmission and electrical conductivity stability, and its performance deteriorates in high temperature and high humidity environments.
A composite oxide layer, a functional layer, and a composite dielectric layer are constructed on the surface of a glass substrate. By controlling the spatial distribution and density gradient structure of conductive micro-units, discrete conductive micro-regions are formed and conductive networks are isolated, thereby regulating the electric field distribution and electrostatic relaxation process.
It achieves a balance between high surface resistivity and antistatic properties, maintains good light transmittance and long-term environmental stability, and avoids instability and performance degradation of conductive networks.
Smart Images

Figure CN123151618A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional glass manufacturing technology, specifically relating to a low-conductivity antistatic functional glass and its preparation method. Background Technology
[0002] With the rapid development of display devices, architectural glass, photovoltaic modules, and smart terminals, glass materials increasingly need to possess antistatic properties in addition to good light transmittance. Ordinary glass is a typical insulating material with a generally high surface resistivity, making it prone to accumulating static electricity during transportation, processing, and use due to friction and contact separation. This accumulated static electricity not only easily attracts dust particles from the air, affecting the cleanliness and light transmittance of the glass surface, but also, in applications such as electronic displays, precision optics, and semiconductor manufacturing, can cause electrostatic discharge, damaging electronic components. Therefore, developing functional glass with both high light transmittance and antistatic properties has become an important research direction in the field of glass deep processing in recent years.
[0003] Currently, technologies for improving the antistatic properties of glass mainly include conductive oxide transparent conductive films, conductive polymer coatings, and nano-conductive filler composite films. To achieve higher conductivity, it is usually necessary to increase the content of the conductive phase or form a continuous conductive network. With increased conductive phase content and the formation of a continuous conductive network, the absorption and scattering of light by the film layer are enhanced, leading to a decrease in the optical properties of the glass. Simultaneously, due to the significant differences in elastic modulus and thermal expansion coefficients between the conductive film layer and the glass substrate, stress accumulation at the interface between the film layer and the substrate is prone to occur under long-term humid and hot conditions, causing problems such as film cracking and peeling, and resulting in a decrease in conductivity. Furthermore, the conductive films in existing conductive functional glasses typically adopt a single-layer structure or a uniformly distributed conductive material, lacking effective control over charge transport paths and electric field distribution. When static charge accumulates on the glass surface, the charge tends to migrate and concentrate along local conductive areas, causing uneven local current distribution. This may lead to a decrease in the stability of the conductive network during long-term operation, thus affecting the stability of the conductive film layer. Especially in complex environments such as high temperature and high humidity, conductive particles are prone to contact, migration, or aggregation, further deteriorating the electrical and optical properties of the film layer.
[0004] To address the problem that existing functional glasses cannot achieve a balance between low electrical conductivity and antistatic properties, this invention provides a low electrical conductivity antistatic functional glass and its preparation method. Summary of the Invention
[0005] The purpose of this invention is to provide a low-conductivity antistatic functional glass and its preparation method, thereby solving the problem that existing functional glasses cannot achieve a balance between low conductivity and antistatic properties. This invention sequentially constructs a composite oxide layer, a conductive structure layer, and a composite dielectric layer on the surface of a glass substrate. By controlling the spatial distribution and contact state of the conductive micro-units, the conductive phase exists in isolated micro-regions, forming a density gradient structure along the thickness direction of the functional layer. Without forming a continuous conductive network, this structure can alter the local electric field distribution inside and on the surface of the functional film layer, and influence the relaxation process of static charges in the film layer, thereby reducing the surface potential decay time. The specific charge transport behavior is related to the film layer structure parameters, environmental conditions, and test boundary conditions. This results in a glass that possesses both high surface resistivity and good antistatic properties.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A low-conductivity antistatic functional glass and its preparation method, comprising the following steps: Unless otherwise specified, the parts in this invention refer to parts by mass.
[0007] The low-conductivity antistatic functional glass of the present invention comprises a glass substrate, on the surface of which a composite functional film system is formed. The composite functional film system includes a composite oxide layer, a functional layer, and a composite dielectric layer. The composite oxide layer is formed by alternating layers of a first oxide layer and a second oxide layer, with an alternation period of 10-60 layers. The functional layer includes a continuously distributed insulating oxide substrate and a plurality of conductive microregions dispersed within the insulating oxide substrate, with each conductive microregion isolated from the insulating oxide substrate. Each conductive microregion includes at least one conductive microunit and an insulating oxide shell covering the conductive microunit. The conductive microregions are discretely distributed along the surface of the glass substrate and form a density gradient distribution along the thickness direction of the conductive structural layer. The composite dielectric layer continuously covers the surface of the functional layer.
[0008] Preferably, the first oxide layer is a SiO2 layer; the second oxide layer is one of an Al2O3 layer, a TiO2 layer, or a ZrO2 layer. Preferably, the thickness of the first oxide layer is 1-6 nm; the thickness of the second oxide layer is 1-4 nm. Preferably, the conductive micro-unit comprises conductive oxide particles formed from one or more of ATO, AZO, ITO, SnO2, or ZnO; Preferably, the insulating oxide shell layer comprises one or more of SiO2, Al2O3, or TiO2; the thickness of the insulating oxide shell layer is 1-10 nm. Preferably, the average particle size of the conductive micro-unit is 10-30 nm; the average edge spacing of the adjacent conductive micro-regions is 5-30 nm. Preferably, the composite dielectric layer comprises one or more of SiO2, MgF2, SiOC and Al2O3, and has a thickness of 20-200 nm.
[0009] Preparation method of low conductivity antistatic functional glass: S1. A composite oxide layer is formed by alternately depositing a first oxide layer and a second oxide layer on the surface of a glass substrate using physical vapor deposition or chemical vapor deposition. S2. An insulating oxide matrix is deposited on the surface of the composite oxide layer, and multiple conductive micro-units are formed by intermittent deposition, so that the conductive micro-units are distributed in the insulating oxide matrix; S3. An insulating oxide shell is formed on the outside of the conductive micro-unit, and an insulating oxide matrix is deposited to embed the conductive micro-unit covered with the insulating oxide shell into the insulating oxide matrix, forming conductive micro-regions that are isolated from each other. S4. Adjust the deposition rate, deposition time, reaction atmosphere, or raw material supply rate of the conductive micro-units during the deposition process to form a density gradient distribution along the thickness direction of the functional layer in the conductive micro-regions. S5. A composite dielectric layer is formed on the surface of the functional layer, and after heat treatment, the low conductivity antistatic functional glass is obtained.
[0010] Preferably, in S1, SiO2 and Al2O3 layers are deposited alternately by magnetron sputtering, so that one SiO2 layer and one Al2O3 layer form a stacking cycle, and a composite oxide layer is formed by repeated deposition; Preferably, in step S3, SiO2 insulating oxide is continuously deposited, while ATO conductive micro-units are intermittently deposited using pulsed magnetron sputtering, so that the ATO conductive micro-units are distributed in a discrete state in the SiO2 insulating oxide substrate, thus avoiding the formation of a continuous conductive film layer. Preferably, in step S4, the functional layer is deposited in stages along the thickness direction. By adjusting the deposition rate, deposition time, or pulse duty cycle of the ATO conductive micro-units, the deposition amount of ATO conductive micro-units in each stage changes sequentially, thereby forming a density gradient along the thickness direction of the film layer. Preferably, in step S5, SiO2 and MgF2 are deposited on the surface of the functional layer by co-sputtering to form a composite dielectric layer, and then heat-treated to improve the structural stability of the film layer and the bonding performance between the film layers.
[0011] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention provides a composite functional film system on the surface of a glass substrate, comprising a composite oxide layer, a functional layer, and a composite dielectric layer. The functional layer includes a continuously distributed insulating oxide matrix and multiple conductive microregions dispersed therein. These conductive microregions are isolated from each other by the insulating oxide matrix and are discretely distributed along the surface of the glass substrate. This structure restricts the formation of a continuous conductive network between the conductive microregions. Compared to structures using continuous conductive films, this invention achieves electrostatic dissipation while maintaining high surface resistivity and also provides good light transmittance.
[0012] 2. The functional layer of this invention comprises a continuously distributed insulating oxide matrix and a plurality of conductive microregions dispersed therein. Each conductive microregion includes at least one conductive microunit and an insulating oxide shell covering the outside of the conductive microunit. The conductive microregions form a density gradient distribution along the thickness direction of the functional layer. The insulating oxide shell reduces direct contact between conductive microunits, lowering the likelihood of conductive particle agglomeration and the formation of continuous conductive pathways. The density gradient distribution can regulate the local dielectric response and charge accumulation state in different regions of the functional layer, enabling faster potential decay response of static charges under the influence of an applied electric field and environmental conditions. Compared with existing structures where conductive particles are uniformly dispersed or form a continuous conductive network, this invention improves antistatic properties, conductive stability, and operational stability under humid and hot environments while maintaining a high surface resistivity.
[0013] 3. This invention forms a composite functional film system on the surface of a glass substrate, consisting of a composite oxide layer, a functional layer, and a composite dielectric layer. The composite oxide layer is formed by alternating layers of a first oxide layer and a second oxide layer, and the composite dielectric layer continuously covers the surface of the functional layer. The alternating layers of the composite oxide layer improve the film structure and are associated with enhanced film adhesion and environmental stability. The composite dielectric layer protects the functional layer and improves the overall optical performance of the film. Compared with existing technologies using a single oxide substrate or a single protective film, the composite functional film system constructed in this invention exhibits higher film bonding stability, better resistance to damp heat, and good light transmittance. Attached Figure Description
[0014] Figure 1 This is a flowchart of the preparation method of the present invention.
[0015] Figure 2 This is a schematic diagram of the surface resistivity and electrostatic decay time of the present invention. Detailed Implementation
[0016] The technical solution of the present invention will be clearly and completely described below through some embodiments and experimental examples. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0017] The raw material information used in the embodiments and comparative examples of this invention is as follows: The glass substrate is float soda-lime-silicon glass, purchased from China Southern Glass Holding Co., Ltd., with a glass thickness of 2.0 mm; SiO2 is purchased from Jiangyin Tongchuang Vacuum Coating Materials Co., Ltd.; Al2O3 is purchased from Jiangyin Tongchuang Vacuum Coating Materials Co., Ltd.; TiO2 is purchased from Beijing GRINM Advanced Materials Co., Ltd., CAS number: 13463-67-7; ZrO2 is purchased from Beijing GRINM Advanced Materials Co., Ltd., CAS number: 1314-23-4; ATO conductive oxide is a conductive oxide target for magnetron sputtering, used to form conductive micro-units; AZO, ITO, SnO2 and ZnO are optional conductive oxide materials; bis(diethylamino)silane was purchased from Merck Sigma-Aldrich as a precursor for SiO2 insulating oxide shell deposition; MgF2 was purchased from Jiangyin Tongchuang Vacuum Coating Materials Co., Ltd., CAS No.: 7783-40-6; high-purity argon was purchased from Hangzhou Hangyang Co., Ltd. as the working gas for magnetron sputtering; high-purity oxygen was purchased from Hangzhou Hangyang Co., Ltd. as the reaction gas; anhydrous ethanol was purchased from Sinopharm Chemical Reagent Co., Ltd., CAS No.: 64-17-5; acetone was purchased from Sinopharm Chemical Reagent Co., Ltd., CAS No.: 67-64-1.
[0018] Reference Figure 1 The process flow diagram shown illustrates that this invention provides a low-conductivity antistatic functional glass and its preparation method. The technical solution is as follows: Example
[0019] 1. Raw materials and formula The low-conductivity antistatic functional glass comprises a glass substrate and a composite oxide layer, a functional layer, and a composite dielectric layer sequentially disposed on the surface of the glass substrate. The composite oxide layer is formed by alternating layers of SiO2 and Al2O3, with a total of 20 SiO2 / Al2O3 stacking cycles. Each SiO2 layer is 3 nm thick, and each Al2O3 layer is 2 nm thick, for a total composite oxide layer thickness of 100 nm. The functional layer has a total thickness of 60 nm and consists of a continuously distributed SiO2 insulating oxide substrate and ATO conductive micro-units. During deposition, the distribution of ATO conductive micro-units in the SiO2 substrate is controlled by pulsed magnetron sputtering and subsequent SiO2 coating processes. The process objective is to form discrete conductive micro-regions isolated by the SiO2 insulating oxide substrate and to suppress the formation of a continuous conductive film layer of ATO. The design controls the average particle size of the ATO conductive micro-units to be 25 nm, the designed thickness of the SiO2 insulating oxide coating layer to be 3 nm, and the designed edge spacing between adjacent conductive micro-regions to be 20 nm. The functional layer forms a three-layer gradient structure along its thickness: a first deposition region near the composite oxide layer, a second deposition region in the middle, and a third deposition region near the composite dielectric layer. Each deposition region is 20 nm thick. Based on the total deposition amount of ATO and SiO2, the nominal deposition ratios of ATO in the three regions are set to 12%, 20%, and 28%, respectively, thus creating a density gradient distribution of conductive micro-regions from low to high along the thickness of the functional layer. The composite dielectric layer is composed of SiO2 and MgF2, with a mass ratio of 70:30, and a total thickness of 80 nm.
[0020] 2. Preparation method (1) Pretreatment of glass substrate: Float soda-lime silica glass with a thickness of 2 mm was selected as the substrate and ultrasonically cleaned for 10 minutes each in acetone, anhydrous ethanol, and deionized water to remove contaminants from the glass surface. After cleaning, it was dried with high-purity nitrogen and placed in a 120℃ forced-air drying oven for 30 minutes to remove moisture from the glass surface. Subsequently, the glass substrate was placed in the magnetron sputtering deposition chamber and evacuated to a background vacuum level not exceeding 5×10⁻⁶. -4 Pa, before deposition, uses argon plasma to treat the glass surface for 5 minutes to improve the adhesion between the film and the glass substrate.
[0021] (2) Preparation of the composite oxide layer: SiO2 and Al2O3 layers were alternately deposited on the glass substrate surface using a dual-target magnetron sputtering process. During the deposition process, SiO2 ceramic targets and Al2O3 ceramic targets were used as sputtering targets, respectively, and argon gas was used as the working gas. The working pressure was controlled at 0.8 Pa, the argon flow rate was 40 sccm, and the substrate temperature was maintained at 100℃. A SiO2 layer with a thickness of 3 nm and an Al2O3 layer with a thickness of 2 nm were deposited sequentially. One SiO2 layer and one Al2O3 layer constituted a deposition cycle, and a total of 20 deposition cycles were repeated to form a composite oxide layer with a total thickness of 100 nm.
[0022] (3) Preparation of the functional layer: The functional layer was prepared on the surface of the composite oxide layer by a combination of magnetron sputtering and plasma-enhanced atomic layer deposition. First, ATO conductive micro-units were intermittently deposited by pulsed magnetron sputtering while continuously depositing the SiO2 insulating oxide substrate. Before deposition, the deposition amount of ATO and SiO2 per unit time under the same deposition conditions was calibrated, and the deposition time and deposition cycle of ATO and SiO2 were controlled according to the calibration results, so that ATO was deposited in the SiO2 insulating oxide substrate in an intermittent manner to avoid the formation of a continuous ATO film. The functional layer is divided into a first deposition region, a second deposition region and a third deposition region along the thickness direction, and the thickness of each deposition region is 20 nm. Based on the total deposition amount of ATO and SiO2, the nominal deposition ratio of ATO in the three deposition regions was set to 12%, 20% and 28% respectively, so that the ATO deposition amount increases stepwise along the thickness direction of the functional layer. After the ATO conductive micro-units were formed in each deposition stage, the ATO deposition was paused, and the ATO conductive micro-units were coated with SiO2 by plasma-enhanced atomic layer deposition. Using bis(diethylamino)silane as the silicon source and oxygen-containing plasma as the oxygen source, the SiO2-coated region was designed to have a thickness of 3 nm by controlling the number of atomic layer deposition cycles. Subsequently, a SiO2 insulating oxide substrate was deposited, dispersing the SiO2-coated ATO conductive micro-units within the continuous SiO2 insulating oxide substrate. The deposition of the first, second, and third deposition regions was completed sequentially in the above manner, resulting in a functional layer with a total thickness of 60 nm. The ATO deposition amount gradually increased from the side closer to the composite oxide layer towards the side closer to the composite dielectric layer.
[0023] (4) Preparation and heat treatment of the composite dielectric layer: A composite dielectric layer was formed on the surface of the functional layer by co-sputtering of SiO2 and MgF2. Before deposition, the deposition rates of SiO2 and MgF2 under corresponding sputtering conditions were calibrated by adjusting the sputtering power of the two targets. Based on the calibration results, the deposition power and deposition time of the two targets were adjusted to maintain the mass ratio of SiO2 to MgF2 in the resulting composite dielectric layer at 70:30, and deposition continued until the total film thickness reached 80 nm. After film deposition, the sample was placed in a nitrogen protective atmosphere and heated to 450 °C at a heating rate of 5 °C / min, and held at this temperature for 30 minutes to release the internal stress of the film. This process improves the bonding strength between the various film layers and promotes the stability of the microstructure of the functional layer. After the heat preservation is completed, the glass is cooled to room temperature with the furnace to obtain the low conductivity antistatic functional glass.
[0024] Examples 2-5 differ from Example 1 in operating parameters, but the other process steps and the range of raw material selection are the same.
[0025] The specific changes in operating parameters are summarized in Table 1.
[0026] Table 1. Parameter variations in Examples 1-5 Example 1 Example 2 Example 3 Example 4 Example 5 Number of composite oxide layer cycles 20 10 40 20 30 <![CDATA[SiO2 layer thickness (nm)]]> 3 6 1.5 3 2 <![CDATA[Al2O3 layer thickness (nm)]]> 2 4 1 2 1.5 Conductive micro-unit particle size (nm) 25 15 30 30 20 <![CDATA[SiO2 shell thickness (nm)]]> 3 1 8 5 3 Nominal ATO deposition percentage (%) in the three sedimentary zones: 12:20:28 8:18:28 15:22:29 10:20:30 15:20:25 Conductive layer thickness (nm) 60 40 80 60 70 Dielectric layer thickness (nm) 80 40 150 100 60 Comparative Example 1 Unlike Example 1, this comparative example does not use a composite oxide layer formed by alternating layers of a first oxide layer and a second oxide layer. Instead, a single-layer SiO2 film with a thickness of 100 nm is directly deposited on the surface of the glass substrate. The remaining process parameters are the same as in Example 1.
[0027] Comparative Example 2 Unlike Example 1, in this comparative example, the functional layer does not form a density gradient of conductive micro-regions. During the deposition of the functional layer, the nominal deposition ratio of ATO in each deposition area is set to 20% to ensure that the conductive micro-regions are evenly distributed along the thickness direction of the functional layer. The remaining process parameters are the same as in Example 1.
[0028] Comparative Example 3 Unlike Example 1, in this comparative example, after the ATO conductive micro-units are formed, they are not coated with a SiO2 insulating oxide shell. Instead, a SiO2 insulating oxide substrate is directly deposited to form a functional layer. The remaining process parameters are the same as in Example 1.
[0029] Comparative Example 4 Unlike Example 1, this comparative example uses continuous magnetron sputtering to deposit the ATO conductive layer, so that the ATO forms a continuous conductive film and does not form discrete conductive micro-regions isolated by the insulating oxide substrate. The other process parameters are the same as those in Example 1.
[0030] Comparative Example 5 Unlike Example 1, in this comparative example, the nominal ATO deposition ratios in the first, second, and third deposition regions of the functional layer are 4%, 20%, and 36%, respectively, and the difference in the nominal ATO deposition ratio between adjacent deposition regions is 16 percentage points, which creates a large density gradient in the conductive micro-regions along the thickness direction of the functional layer. The remaining process parameters are the same as in Example 1.
[0031] Comparative Example 6 Unlike Example 1, in this comparative example, the average particle size of the ATO conductive microcells is controlled at 15 nm, the average edge spacing between adjacent conductive microregions is controlled at 25 nm, and the remaining process parameters are the same as in Example 1.
[0032] Comparative Example 7 Unlike Example 1, in this comparative example, a SiO2 inner shell layer and an Al2O3 outer shell layer are sequentially deposited on the surface of the ATO conductive micro-unit. The total thickness of the two layers is maintained at 3 nm, with the SiO2 inner shell layer having a thickness of 1 nm and the Al2O3 outer shell layer having a thickness of 2 nm. The remaining process parameters are the same as in Example 1.
[0033] Experimental Example 1 The results of surface resistivity, electrostatic decay time, visible light transmittance, haze, film adhesion, and surface resistivity change rate after damp heat of the low-conductivity antistatic functional glass prepared in Examples 1-5 and Comparative Examples 1-7 are summarized in Table 2.
[0034] (1) Surface resistivity test method: The test was conducted in accordance with GB / T31838.3-2019. The specific test method is as follows: The prepared glass sample was conditioned for 24 hours in an environment with a temperature of 23℃±2℃ and a relative humidity of 50%±5%. The surface resistivity of the sample coating surface was measured using a high resistance meter in conjunction with a surface resistivity test electrode. During the test, the electrode was brought into full contact with the surface of the composite dielectric layer. After maintaining the specified DC test voltage for 60 seconds, the stable resistance value was read. Five test positions were randomly selected for each group of samples for measurement, and the average value was taken as the surface resistivity test result of the sample.
[0035] (2) Electrostatic decay time test method: The prepared glass sample was conditioned for 24 hours in an environment with a temperature of 23℃±2℃ and a relative humidity of 50%±5%. The coated surface of the sample was facing the charging electrode of the electrostatic decay tester. The sample surface potential was raised to +1000V by corona charging. After charging was stopped, the time required for the sample surface potential to decay from 1000V to 100V was recorded. The test was then repeated at -1000V. The positive and negative voltages were tested 3 times each, and the average value of the 6 test results was taken as the electrostatic decay time.
[0036] (3) Visible light transmittance test method: The test shall be conducted in accordance with GB / T2410-2008. The specific test method is as follows: The spectral transmittance of the sample shall be tested using an ultraviolet-visible spectrophotometer. Uncoated soda-lime silica glass shall be used as a reference. The spectral transmittance of the sample shall be scanned in the wavelength range of 380-780nm, and the average transmittance shall be calculated according to the visible light band. Five parallel samples shall be tested for each group of samples, and the average value shall be taken as the visible light transmittance.
[0037] (4) Haze Test Method: A haze meter is used to test the samples. The coated surface of the sample faces the incident light direction. The total transmitted light flux and the scattered transmitted light flux of the sample are measured, and the haze is calculated. Five different locations are randomly tested for each group of samples, and the average value of the test results is taken. The haze calculation formula is as follows: H=T d / T t ×100% Where: H is haze (%); T d T represents diffuse luminous flux. t This represents the total transmitted light flux.
[0038] (5) Film adhesion test method: Perform a cross-cut treatment on the coated surface of the sample, so that the scratches penetrate the film to the glass substrate. Adhesive tape with specified adhesion performance is pasted into the cross-cut area and compacted. Then, the tape is peeled off at a stable speed in the specified direction. The peeling of the film in the cross-cut area is observed, and the adhesion performance is evaluated according to the degree of peeling. Five parallel samples are tested for each group of samples.
[0039] (6) Test method for surface resistivity change rate after damp heat treatment: Place the sample in a constant temperature and humidity test chamber at 85℃±2℃ and 50%±5% relative humidity for 500 hours. After completion, remove the sample and adjust it in an environment at 23℃±2℃ and 50%±5% relative humidity for 24 hours. Test the surface resistivity and visible light transmittance of the sample according to the above method, and calculate the surface resistivity change rate before and after damp heat treatment. The formula for surface resistivity change rate is as follows: ΔR = |R1−R0| / R0 × 100% Where: ΔR is the rate of change of surface resistivity; R1 is the surface resistivity after humidification; R0 is the surface resistivity before humidification.
[0040] Table 2. Performance test results of the low-conductivity antistatic functional glasses prepared in Examples 1-5 and Comparative Examples 1-7. Surface resistivity (Ω / sq) Electrostatic decay time (s) Visible light transmittance (%) Haze (%) Film adhesion Surface resistivity change rate after damp heat / % Example 1 <![CDATA[3.6×10 9 ]]> 0.42 89.2 0.56 Level 0 4.7 Example 2 <![CDATA[7.4×10 9 ]]> 1.18 87.8 0.91 Level 1 9.3 Example 3 <![CDATA[2.8×10 10 ]]> 2.46 83.7 1.63 Level 0 7.1 Example 4 <![CDATA[9.6×10 9 ]]> 0.93 86.5 0.83 Level 0 5.9 Example 5 <![CDATA[5.8×10 9 ]]> 0.71 88.0 0.72 Level 0 7.6 Comparative Example 1 <![CDATA[4.1×10 9 ]]> 0.79 85.6 1.18 Level 2 16.8 Comparative Example 2 <![CDATA[2.7×10 9 ]]> 0.61 87.0 0.96 Level 0 11.7 Comparative Example 3 <![CDATA[6.3×10 7 ]]> 0.16 83.9 2.28 Level 1 20.6 Comparative Example 4 <![CDATA[8.5×10 5 ]]> 0.035 75.4 4.83 Level 1 25.9 Comparative Example 5 <![CDATA[1.8×10 9 ]]> 0.31 86.7 1.21 Level 0 12.6 Comparative Example 6 <![CDATA[1.6×10 10 ]]> 1.74 89.0 0.49 Level 0 8.8 Comparative Example 7 <![CDATA[6.7×10 9 ]]> 0.76 87.3 0.88 Level 1 10.4 As shown in Table 2, the low-conductivity antistatic functional glasses prepared in Examples 1-5 and Comparative Examples 1-7 exhibit significant differences in surface resistivity, electrostatic decay time, visible light transmittance, haze, film adhesion, and surface resistivity change rate after damp heat. Example 1 employs an alternating layered composite oxide layer, a functional layer with a thickness-direction density gradient, a silica insulating oxide shell encapsulating ATO conductive microunits, and a composite dielectric layer in a synergistic design. This results in a functional glass with high surface resistivity, fast electrostatic dissipation, and long-term environmental stability, achieving optimal overall performance.
[0041] Comparing Examples 1-5, it can be seen that different combinations of structural parameters affect the surface resistivity, electrostatic decay time, optical performance, and damp-heat stability of the functional glass. Each example involves variations in multiple parameters, including the number of composite oxide layer cycles, conductive micro-unit particle size, SiO2 shell thickness, ATO gradient ratio, and functional layer thickness. Therefore, this set of experiments is primarily used to evaluate the overall performance differences of different structural combinations and cannot be used to determine the independent contribution of a single structural parameter to performance changes. Specific parameter influence patterns need to be verified through single-factor control experiments or further statistical analysis.
[0042] Firstly, comparing Example 1 and Comparative Example 1, it can be seen that Comparative Example 1 eliminated the composite oxide layer formed by alternating layers of the first and second oxide layers. Instead, a single-layer SiO2 film with a thickness of 100 nm was directly deposited on the surface of the glass substrate. While the surface resistivity did not change significantly, the visible light transmittance decreased from 89.2% to 85.6%, the haze increased from 0.56% to 1.18%, and the film adhesion decreased from level 0 to level 2. The rate of change in surface resistivity after humid heat increased from 4.7% to 16.8%. This indicates that the alternatingly layered composite oxide layer can reduce interfacial stress, improve the bonding ability between the film layer and the glass substrate, and improve the optical uniformity and humid heat stability of the film layer, enabling the functional glass to maintain good optical performance and electrical stability during long-term use.
[0043] Further comparison of Example 1 and Comparative Example 2 shows that Comparative Example 2 eliminated the density gradient along the thickness direction of the functional layer in the conductive microregions, and the ATO volume fraction in each deposition region remained at 20%. The data shows that its surface resistivity decreased to 2.7 × 10⁻⁶. 9 The electrostatic decay time was extended to 0.61 seconds, indicating a decrease in the electrostatic decay rate. However, the surface resistivity change rate and haze both increased after humid heating, indicating that although uniformly distributed ATO can improve conductivity continuity and thus increase the electrostatic decay rate, the lack of thickness gradient control makes it easy for local conductive concentration areas to form between conductive micro-regions, leading to a decrease in overall conductivity stability.
[0044] Comparing Example 1 and Comparative Example 3, it can be seen that Comparative Example 3 eliminated the SiO2 insulating oxide shell layer on the outside of the ATO conductive microunit, and directly deposited the SiO2 insulating oxide substrate to form a functional layer, which reduced the surface resistivity to 6.3 × 10⁻⁶. 7 While the electrostatic decay time was shortened to 0.16 seconds, the visible light transmittance decreased to 83.9%, and the haze increased to 2.28%. Simultaneously, the surface resistivity change rate after damp heat reached 20.6%, indicating that without the SiO2 insulating oxide shell, ATO conductive micro-units are prone to direct contact and even localized aggregation. Although a strong conductive network is formed, this weakens the insulation between conductive micro-regions and reduces environmental stability. This invention constructs a uniform SiO2 insulating oxide shell on the surface of the ATO conductive micro-units, isolating each conductive micro-region from the others. This avoids the formation of a continuous conductive network while maintaining good optical performance and long-term stability.
[0045] Comparing Example 1 and Comparative Example 4, it can be seen that Comparative Example 4 uses continuous magnetron sputtering to deposit the ATO conductive layer, so that ATO forms a continuous conductive film and does not form discrete conductive micro-regions isolated by the insulating oxide substrate, and its surface resistivity is further reduced to 8.5 × 10⁻⁶. 5 The electrostatic decay time and visible light transmittance both decreased, while the haze increased to 4.83%, and the film adhesion decreased. This indicates that although the continuous ATO film has high conductivity, the continuous conductive network easily causes increased light absorption and light scattering. At the same time, the interface stress concentration significantly reduces the film's resistance to damp heat. This invention adopts a discrete conductive micro-region structure isolated by a continuous SiO2 insulating oxide matrix, which effectively avoids the problems of decreased transmittance and reduced stability caused by continuous conductive films while ensuring rapid dissipation of static electricity.
[0046] In summary, this invention constructs alternating layers of composite oxide layers, discrete core-shell conductive microregions, and a thickness-direction density gradient conductive structure, while combining the effect of a composite dielectric layer. This enables the glass to maintain high surface resistivity while achieving rapid electrostatic dissipation, and also takes into account high visible light transmittance, low haze, excellent film adhesion, and hygrothermal stability, thus achieving a balance between low conductivity and antistatic performance.
Claims
1. A low-conductivity antistatic functional glass, comprising a glass substrate, characterized in that: A composite functional film system is formed on the surface of the glass substrate. The composite functional film system includes a composite oxide layer, a functional layer, and a composite dielectric layer. The composite oxide layer is formed by alternating layers of a first oxide layer and a second oxide layer, with an alternation period of 10-60. The functional layer includes a continuously distributed insulating oxide matrix and a plurality of conductive microregions dispersed in the insulating oxide matrix, with each conductive microregion isolated from the insulating oxide matrix. Each conductive microregion includes at least one conductive microunit and an insulating oxide shell covering the outside of the conductive microunit. The conductive microregions are discretely distributed along the surface of the glass substrate and form a density gradient distribution along the thickness direction of the functional layer. The composite dielectric layer continuously covers the surface of the functional layer.
2. The low conductivity antistatic functional glass according to claim 1, characterized in that: The first oxide layer is a SiO2 layer; the second oxide layer is one of an Al2O3 layer, a TiO2 layer, or a ZrO2 layer; the single-layer thickness of the first oxide layer is 1-6 nm; the single-layer thickness of the second oxide layer is 1-4 nm.
3. The low conductivity antistatic functional glass according to claim 1, characterized in that: The conductive micro-units include conductive oxide particles formed from one or more of ATO, AZO, ITO, SnO2, or ZnO.
4. The low conductivity antistatic functional glass according to claim 1, characterized in that: The insulating oxide shell includes one or more of SiO2, Al2O3 or TiO2; the thickness of the insulating oxide shell is 1-10 nm.
5. The low conductivity antistatic functional glass according to claim 3, characterized in that: The average particle size of the conductive micro-unit is 10-30 nm; the average edge spacing of the adjacent conductive micro-regions is 5-30 nm.
6. A low-conductivity antistatic functional glass according to claim 1 or 2, characterized in that: The composite dielectric layer includes one or more of SiO2, MgF2, SiOC and Al2O3, with a thickness of 20-200 nm.
7. A method for preparing a low-conductivity antistatic functional glass according to claims 1-6, characterized in that: The preparation method is as follows: S1. A composite oxide layer is formed by alternately depositing a first oxide layer and a second oxide layer on the surface of a glass substrate using physical vapor deposition or chemical vapor deposition. S2. An insulating oxide matrix is deposited on the surface of the first composite oxide layer, and multiple conductive micro-units are formed by intermittent deposition, so that the conductive micro-units are distributed in the insulating oxide matrix; S3. An insulating oxide shell is formed on the outside of the conductive micro-unit, and an insulating oxide matrix is deposited to embed the conductive micro-unit covered with the insulating oxide shell into the insulating oxide matrix, forming conductive micro-regions that are isolated from each other. S4. Adjust the deposition rate, deposition time, reaction atmosphere, or raw material supply rate of the conductive micro-units during the deposition process to form a density gradient distribution along the thickness direction of the functional layer in the conductive micro-regions. S5. A composite dielectric layer is formed on the surface of the functional layer, and after heat treatment, the low conductivity antistatic functional glass is obtained.