Polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and preparation method thereof
By using a composite foam stabilizer made of polyethylene glycol, fatty alcohol polyoxyethylene ether, and polyvinyl alcohol with silica fume, the problem of the single function of traditional foam stabilizers has been solved, and efficient foam stabilization and performance improvement of autoclaved aerated concrete have been achieved.
Patent Information
- Application Number
- CN202611545885.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional foam stabilizers cannot simultaneously reduce surface tension, enhance the bubble film, adjust slurry consistency, and support the green body, resulting in poor quality of autoclaved aerated concrete products.
A composite foam stabilizer was prepared by mixing polyethylene glycol as the bubble film reinforcing component, fatty alcohol polyoxyethylene ether as the surfactant, polyvinyl alcohol as the thickening and stabilizing component, and silica fume as the pore wall reinforcing component in a stirred tank, forming a synergistic and efficient foam stabilizing system.
It significantly improves the quality of autoclaved aerated concrete (AAC) products, resulting in finer and more uniform pores, fewer interconnected pores, increased compressive strength, and reduced drying shrinkage. It is suitable for various raw material systems and features a simple process with no waste emissions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of building material additives technology, specifically relating to a polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method. Background Technology
[0002] Autoclaved aerated concrete (AAC) is a porous, lightweight new type of building material. It is an artificial stone with a certain strength, synthesized by mixing various materials such as siliceous materials, calcareous materials, air-entraining agents, and foam stabilizers in a certain proportion, and then casting, molding, and curing under high-pressure steam. One of the key technologies in manufacturing AAC is air entrainment and foam stabilization. Foam stabilization refers to reducing the surface tension of the three-phase system composed of solid, liquid, and gas, increasing the mechanical strength of the bubble film in the system, and preventing the slurry from boiling and collapsing due to bubble rupture, thus achieving the purpose of molding. Therefore, selecting a suitable foam stabilizer has always been a hot topic in the AAC industry. Traditional foam stabilization systems often use single polyvinyl alcohol or cellulose ether, which is difficult to achieve simultaneously the functions of reducing surface tension, strengthening the bubble film, adjusting slurry consistency, and supporting the green body. Polyethylene glycol has good wettability, film-forming properties, and interface strengthening effects. When compounded with surfactants, thickening and foam-stabilizing components, and pore wall strengthening components, it can form a synergistic and efficient foam stabilization system, significantly improving the quality of finished autoclaved aerated concrete. Summary of the Invention
[0003] Purpose of the invention: The purpose of this invention is to provide a polyethylene glycol-based composite foam stabilizer with clearly defined components, clear functions, stable effects, and suitable for industrial production.
[0004] Technical solution: A polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method, comprising, by weight: Polyethylene glycol is used as a bubble film reinforcing component in the amount of 15-35 parts, fatty alcohol polyoxyethylene ether is used as a surfactant in the amount of 8-18 parts, polyvinyl alcohol is used as a thickening and stabilizing component in the amount of 5-12 parts, silica fume is used as a pore wall reinforcing component in the amount of 3-8 parts, and water is used in the amount of 45-65 parts.
[0005] Furthermore, the number-average molecular weight of the polyethylene glycol is 400-6000, and it can be a single type of polyethylene glycol within this molecular weight range, or a blend of multiple polyethylene glycols with different molecular weights.
[0006] Furthermore, the number-average molecular weight of the fatty alcohol polyoxyethylene ether is 550-620.
[0007] Furthermore, the polyvinyl alcohol has a number-average molecular weight of 72,600-81,400 and a degree of hydrolysis of 86%-90%.
[0008] Furthermore, the aforementioned polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method include the following steps: (1) Each component is prepared according to the following proportions: 15-35 parts of polyethylene glycol as bubble film reinforcing component, 8-18 parts of fatty alcohol polyoxyethylene ether as surfactant, 5-12 parts of polyvinyl alcohol as thickening and stabilizing component, 3-8 parts of silica fume as pore wall reinforcing component, and 45-65 parts of water. (2) Add water to the mixing tank and control the stirring speed to 300-600 r / min; add polyethylene glycol and stir until completely dissolved; then add fatty alcohol polyoxyethylene ether and stir until the system is uniform and transparent; then add polyvinyl alcohol and stir until there are no solid particles; increase the speed to 800-1200 r / min and add silica fume for high-speed dispersion for 15-30 min; filter out the material and cool to room temperature to obtain liquid composite foam stabilizer. The whole process is carried out at room temperature and pressure.
[0009] Invention Principle: Polyethylene glycol (PEG) acts as a bubble film reinforcing component, forming a continuous and flexible protective film on the surface of the bubble liquid film, improving the film's toughness and inhibiting bubble breakage and coalescence. Fatty alcohol polyoxyethylene ether (FAE), as a surfactant, reduces the gas-liquid interfacial tension of the slurry, promoting the generation of numerous fine bubbles. This non-ionic component exhibits good stability in the strongly alkaline slurry environment of aerated concrete. Polyvinyl alcohol (PVA), as a thickening and foam-stabilizing component, increases the slurry's plastic viscosity, providing physical support for the bubbles and slowing down the liquid film drainage rate, thus matching the gas generation process with the slurry thickening process. Silica fume, as a pore wall reinforcing component, fills the micropores in the pore walls. During the autoclaving stage, it can react with calcium hydroxide in the system to generate hydrated calcium silicate, further reinforcing the pore walls. Water, as a dispersion medium, ensures uniform mixing of all components, resulting in a homogeneous liquid product. The components work synergistically to achieve the effects of stabilizing bubbles, regulating pore structure, and enhancing product performance.
[0010] Beneficial Effects: Compared with existing technologies, the polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete (AAC) of this invention exhibits superior foam stabilization performance. Polyethylene glycol and fatty alcohol polyoxyethylene ether synergistically strengthen the bubble liquid film, polyvinyl alcohol adjusts the slurry consistency to prevent mold collapse, and silica fume enhances the mechanical properties of the pore walls. The finished product has fine and uniform pores, a low proportion of interconnected pores, improved compressive strength, and significantly reduced drying shrinkage. This invention is prepared entirely at room temperature and pressure, with a simple process, no waste emissions, and is compatible with existing AAC production lines. The product is suitable for various raw material systems, including fly ash-based, sand-based, and stone powder-based materials. When using, the foam stabilizer dosage is only 0.03%-0.1% of the total mass of the raw materials used in preparing AAC to achieve the desired effect. Detailed Implementation
[0011] The present invention will be further described below with reference to specific embodiments.
[0012] The polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete comprises the following components in parts by weight: 15-35 parts polyethylene glycol as a bubble film reinforcing component, 8-18 parts fatty alcohol polyoxyethylene ether as a surfactant, 5-12 parts polyvinyl alcohol as a thickening and foam stabilizing component, 3-8 parts silica fume as a pore wall reinforcing component, and 45-65 parts water.
[0013] Furthermore, the number-average molecular weight of the polyethylene glycol is 400-6000, and it can be a single type of polyethylene glycol within this molecular weight range, or a blend of multiple polyethylene glycols with different molecular weights; the number-average molecular weight of the fatty alcohol polyoxyethylene ether is 550-620; and the number-average molecular weight of the polyvinyl alcohol is 72600-81400, with a degree of alcoholysis of 86%-90%.
[0014] Furthermore, the aforementioned polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method include the following steps: (1) Each component is prepared according to the specified proportions; (2) Add water to the mixing tank and control the stirring speed to 300-600 r / min; add polyethylene glycol and stir until completely dissolved; then add fatty alcohol polyoxyethylene ether and stir until the system is uniform and transparent; then add polyvinyl alcohol and stir until there are no solid particles; increase the speed to 800-1200 r / min and add silica fume for high-speed dispersion for 15-30 min; filter out the material and cool to room temperature to obtain liquid composite foam stabilizer. The whole process is carried out at room temperature and pressure.
[0015] Example 1 The raw materials used in this embodiment to prepare the polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete include the following components in parts by weight: 20 parts of polyethylene glycol 1000 as a bubble film reinforcing component, 10 parts of fatty alcohol polyoxyethylene ether AEO-9 as a surfactant, 6 parts of polyvinyl alcohol 1788 as a thickening and foam stabilizing component, 4 parts of silica fume as a pore wall reinforcing component, and 60 parts of water.
[0016] Among them, polyethylene glycol has a number average molecular weight of 1000; fatty alcohol polyoxyethylene ether is model AEO-9; and polyvinyl alcohol is model 1788.
[0017] Preparation process: Water is added to a mixing tank and stirred at 400 rpm; polyethylene glycol 1000 is added and stirred to dissolve; AEO-9 is added and stirred until transparent; polyvinyl alcohol type 1788 is added and stirred until completely dissolved; the stirring speed is increased to 1000 rpm and silica fume is added and dispersed for 20 minutes; the mixture is filtered and cooled to room temperature to obtain a liquid foam stabilizer. The application dosage is 0.05% of the total mass of raw materials for preparing autoclaved aerated concrete.
[0018] Example 2 The raw materials for preparing the polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete in this embodiment include the following components in parts by weight: 25 parts of polyethylene glycol 4000 as a bubble film reinforcing component, 12 parts of fatty alcohol polyoxyethylene ether AEO-9 as a surfactant, 7 parts of polyvinyl alcohol 1788 as a thickening and foam stabilizing component, 5 parts of silica fume as a pore wall reinforcing component, and 51 parts of water.
[0019] The polyethylene glycol has a number-average molecular weight of 4000; the fatty alcohol polyoxyethylene ether is model AEO-9; and the polyvinyl alcohol is model 1788. The preparation steps are the same as in Example 1, and the dosage is 0.07% of the total mass of the raw materials for preparing autoclaved aerated concrete.
[0020] Example 3 The raw materials for preparing the polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete in this embodiment include the following components in parts by weight: 18 parts of polyethylene glycol 400 as a bubble film reinforcing component, 10 parts of polyethylene glycol 4000 as a bubble film reinforcing component, 9 parts of fatty alcohol polyoxyethylene ether AEO-9 as a surfactant, 6 parts of polyvinyl alcohol 1788 as a thickening and foam stabilizing component, 4 parts of silica fume as a pore wall reinforcing component, and 53 parts of water.
[0021] The polyethylene glycols used were 400 and 4000 in number average molecular weight, respectively; the fatty alcohol polyoxyethylene ether was model AEO-9; and the polyvinyl alcohol was model 1788. The preparation steps were the same as in Example 1, and the dosage was 0.06% of the total mass of the raw materials used to prepare autoclaved aerated concrete.
[0022] Performance testing - mechanical properties The polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete (AAC) prepared in Examples 1-3 and a foam stabilizer system containing only ordinary polyvinyl alcohol (comparative example) were used to prepare AAC under the same conditions for performance testing. The basic mix proportions of the AAC were: cement 15%, quicklime 22%, fly ash 58%, gypsum 5%, and aluminum powder paste 0.06%. The testing standard was GB / T 11969-2020, "Test Methods for Performance of Autoclaved Aerated Concrete".
[0023] Table 1. Mechanical properties of aerated concrete prepared in Examples 1 to 3 and comparative examples.
[0024] As shown in Table 1, under the same basic formulation conditions, the products using the foam stabilizers of Examples 1-3 of this invention have slightly lower bulk density, a compressive strength increase of over 15%, significantly reduced drying shrinkage, and fine, uniform pores without obvious large or interconnected pores. Overall, their performance is superior to the comparative examples using only polyvinyl alcohol as a foam stabilizer. The autoclaved aerated concrete products prepared by this invention meet the relevant national standards for autoclaved aerated concrete blocks.
Claims
1. A polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method, characterized in that, The product is composed of the following components by weight: 15-35 parts polyethylene glycol as a bubble film reinforcing component, 8-18 parts fatty alcohol polyoxyethylene ether as a surfactant, 5-12 parts polyvinyl alcohol as a thickening and stabilizing component, 3-8 parts silica fume as a pore wall reinforcing component, and 45-65 parts water.
2. The polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method according to claim 1, characterized in that: The number average molecular weight of the polyethylene glycol is 400-6000, and it can be a single type of polyethylene glycol within this molecular weight range, or a combination of multiple polyethylene glycols with different molecular weights.
3. The polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method according to claim 1, characterized in that: The number average molecular weight of the fatty alcohol polyoxyethylene ether is 550-620.
4. The polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method according to claim 1, characterized in that: The polyvinyl alcohol has a number-average molecular weight of 72,600-81,400 and a degree of hydrolysis of 86%-90%.
5. A polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete according to any one of claims 1-4, and its preparation method, characterized in that... Includes the following steps: (1) Add water to the mixing vessel, turn on the stirring, and control the stirring speed to 300-600 r / min; (2) Add polyethylene glycol as a bubble film reinforcing component and stir until completely dissolved; (3) Add fatty alcohol polyoxyethylene ether as a surfactant and continue stirring until the system is uniform and transparent; (4) Add polyvinyl alcohol as a thickening and foam-stabilizing component, and stir until completely dissolved and free of particles; (5) Add silica fume as a pore wall reinforcement component, switch to high speed of 800-1200 r / min for uniform dispersion, filter and discharge to obtain the finished product; The entire process is carried out at room temperature and pressure.
6. The application of the polyethylene glycol-based composite foam stabilizer for autoclaved aerated concrete and its preparation method as described in claim 1 in autoclaved aerated concrete, characterized in that: The dosage of foam stabilizer is 0.03% to 0.1% of the total weight of raw materials used in the preparation of autoclaved aerated concrete.