Low-viscosity anti-cracking dispersant suitable for high-strength concrete ultra-thin member and preparation method thereof

By leveraging the synergistic effect of selective dispersants for cement particles and silica fume particles with instant shrinkage-reducing components, the problems of high slurry plastic viscosity and insufficient early crack resistance in ultra-thin high-strength concrete components are solved, achieving efficient casting and early strength enhancement.

CN123151633APending Publication Date: 2026-11-24CHINA RAILWAY NO 19TH BUREAU GROUP NANCHANG WANWOXIN MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611320210.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-24

Smart Images

  • Figure CN123151633A_ABST
    Figure CN123151633A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of concrete admixtures and high-performance cement-based materials. It discloses a low-viscosity, crack-resistant dispersant suitable for ultra-thin high-strength concrete components and its preparation method. The dispersant includes a cement particle-selective polycarboxylate superplasticizer mother liquor, a silica fume particle-selective shrinkage-reducing polycarboxylate superplasticizer mother liquor, a polycarboxylate-stabilized hydrated calcium silicate nanocrystal seed liquor, an instant shrinkage-reducing component, an antifoaming agent, and water. The preparation method includes the preparation of hydrolyzable shrinkage-reducing monomers, the synthesis of two types of superplasticizer mother liquors, the preparation of the nanocrystal seed liquor, staged dispersion, and filtration. By forming steric hindrance layers on cement particles and silica fume particles respectively to reduce plastic viscosity, utilizing instant shrinkage reduction and hydrolytic slow release to reduce the surface tension of the pore solution, and utilizing nanocrystal seed to promote the formation of a continuous skeleton, the dispersant achieves synergistic improvement in flow retention, early strength, and crack resistance, reducing pores, fiber aggregation, and shrinkage cracks in ultra-thin components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of concrete admixtures and high-performance cement-based materials, and particularly relates to a low-viscosity crack-resistant dispersant suitable for ultra-thin high-strength concrete components and its preparation method. Background Technology

[0002] High-strength concrete ultra-thin components are characterized by small component thickness, high load-bearing requirements per unit section, and limited molding space. To obtain higher strength and dense structure, the mixture usually adopts a low water-cement ratio and incorporates silica fume, quartz powder, and steel fibers. This results in an increase in the specific surface area of ​​the cementitious material, a decrease in free water content, and an increase in the flow resistance of the slurry. At the same time, ultra-thin sections are more sensitive to autogenous shrinkage and early temperature and humidity changes. Therefore, it is necessary to use a composite dispersant that takes into account low viscosity dispersion, flow retention, shrinkage control, and early strength development.

[0003] One issue requiring improvement in the existing technology is that existing polycarboxylate superplasticizers mainly use a single molecular structure to disperse both cement particles and silica fume particles. They do not address the differences in particle size, specific surface area, and surface adsorption characteristics between cement particles and silica fume particles by configuring different anchoring densities and side chain lengths. Silica fume easily competes to adsorb polycarboxylate molecules and consumes effective dispersing components, leading to cement particle flocculation, increased plastic viscosity of the slurry, and accelerated loss of fluidity. In ultra-thin cavities, this can easily result in incomplete filling, localized voids, and steel fiber aggregation.

[0004] The second problem to be improved in the existing technology is that the existing crack-resistant treatment usually adds free shrinkage reducing agents or expansion components directly to the concrete. Free shrinkage reducing agents act in the early stage of mixing, which can easily increase the air content and delay hydration. The volume compensation period of expansion components is difficult to accurately match with the shrinkage development period of ultra-thin components. At the same time, simple compounding of nanocrystalline seeds is prone to agglomeration and sedimentation, making it difficult to simultaneously achieve shrinkage reduction in the plastic stage, continuous shrinkage reduction in the early stage of hardening, and early strength compensation. Summary of the Invention

[0005] This invention aims to solve the technical problems of high-strength concrete ultrathin components under conditions of low water-cement ratio, high silica fume content and high solid volume fraction, such as high slurry plastic viscosity, uneven particle dispersion, difficulty in casting and filling, concentration of self-shrinkage, insufficient early tensile strength and high risk of through cracks. It provides a low-viscosity crack-resistant dispersant suitable for high-strength concrete ultrathin components and its preparation method.

[0006] To solve the above-mentioned technical problems, the low-viscosity crack-resistant dispersant provided by the present invention comprises, by weight, 35-48 parts of cement particle selective polycarboxylate superplasticizer mother liquor, 25-38 parts of silica fume particle selective shrinkage-reducing polycarboxylate superplasticizer mother liquor, 5-12 parts of polycarboxylate stabilized hydrated calcium silicate nanocrystal seed liquor, 1.0-3.0 parts of instant shrinkage-reducing component, 0.05-0.20 parts of polyether modified organosilicon defoamer, and 10-25 parts of water, with the total weight of all components being 100 parts.

[0007] The mother liquor of the cement particle selective polycarboxylate superplasticizer is formed by copolymerization of methoxy polyethylene glycol methacrylate, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and hydroxyethyl acrylate. It adopts relatively short polyethylene glycol side chains and high carboxyl anchoring density, so that polycarboxylate molecules are preferentially adsorbed on the surface of cement particles and form a steric hindrance layer, which reduces the initial yield stress caused by cement particle agglomeration.

[0008] The mother liquor of the selective shrinkage-reducing polycarboxylate superplasticizer for silica fume particles is copolymerized from isopentenyl polyoxyethylene ether, acrylic acid, sodium vinyl sulfonate and hydrolyzable shrinkage-reducing monomer. The relatively long polyoxyethylene side chain is used to improve the coverage of polycarboxylate molecules on the surface of silica fume particles with high specific surface area. The hydrolyzable shrinkage-reducing monomer is obtained by esterification of polyoxypropylene monobutyl ether with maleic anhydride and is incorporated into the polycarboxylate backbone. In the alkaline pore solution of concrete, the polyoxypropylene shrinkage-reducing chain segments are gradually hydrolyzed and released.

[0009] The polycarboxylate stabilized hydrated calcium silicate nanocrystal seed solution is formed by the reaction of calcium source, silicon source and polycarboxylate stabilizer in alkaline aqueous phase. The polycarboxylate stabilizer is adsorbed on the surface of hydrated calcium silicate nanocrystal seed to limit the agglomeration of nanocrystal seed and maintain the suspension stability of the seed in the dispersant. After the dispersant enters the concrete, the nanocrystal seed provides heterogeneous nucleation sites for hydration products, accelerating the early hydration structure formation of ultrathin components.

[0010] The instant shrinkage-reducing component is polyoxypropylene monobutyl ether with a number average molecular weight of 300-600. The instant shrinkage-reducing component reduces the surface tension of the pore solution in the early stage of mixing and can delay the release of polyoxypropylene shrinkage-reducing segments in the hydrolyzed shrinkage-reducing monomer during the hydration process. This forms a staged shrinkage control mechanism that connects instant shrinkage in the early stage of mixing with continuous shrinkage in the early stage of hardening.

[0011] The present invention also provides a method for preparing a low-viscosity anti-crack dispersant, comprising the following steps.

[0012] Step S1: Polyoxypropylene monobutyl ether, maleic anhydride, esterification catalyst and polymerization inhibitor are added to the reaction vessel, and the esterification reaction is carried out under nitrogen protection and at 70-85°C to obtain a decondensing monomer with unsaturated double bonds and hydrolyzable ester bonds.

[0013] Step S2: Add methoxy polyethylene glycol methacrylate to water, and add acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, hydroxyethyl acrylate, chain transfer agent and redox initiator dropwise at 40-50°C. After the reaction is complete, adjust the pH to obtain the mother liquor of cement particle selective polycarboxylate superplasticizer.

[0014] In step S3, isopentenyl alcohol polyoxyethylene ether is added to water, and acrylic acid, sodium vinyl sulfonate, the hydrolyzable shrinkage-reducing monomer obtained in step S1, chain transfer agent and redox initiator are added dropwise at 30-42°C. After the reaction is completed, the pH is adjusted to obtain the mother liquor of silica fume selective shrinkage-reducing polycarboxylate superplasticizer.

[0015] In step S4, the polycarboxylic acid stabilizer is added to the sodium silicate solution, and calcium nitrate solution is added under stirring conditions. The pH of the reaction system is controlled at 11.5-12.5 and the temperature is controlled at 20-30℃. The reaction forms a polycarboxylic acid stabilized hydrated calcium silicate nanocrystal seed solution.

[0016] Step S5: Mix the cement particle selective polycarboxylate superplasticizer mother liquor and the silica fume particle selective shrinkage-reducing polycarboxylate superplasticizer mother liquor according to the mass fraction. After adding the instant shrinkage-reducing component, perform the first stage dispersion. Then, slowly add the polycarboxylate stabilized hydrated calcium silicate nanocrystal seed liquid for the second stage dispersion.

[0017] Step S6: Add polyether-modified silicone defoamer and water to the mixture obtained in step S5, adjust the pH, and then filter to obtain a low-viscosity, crack-resistant dispersant.

[0018] The prepared low-viscosity crack-resistant dispersant has a solid content of 30% to 38%, a viscosity of 80 to 220 mPa·s at 25℃, and a pH of 6.0 to 7.5. The dosage of the low-viscosity crack-resistant dispersant in high-strength concrete is 0.8% to 1.5% of the mass of the cementitious material.

[0019] The beneficial effects of this invention are as follows: (1) By matching cement particles with selective polycarboxylate superplasticizer mother liquor and silica fume particles with selective shrinkage-reducing polycarboxylate superplasticizer mother liquor respectively, cement and silica fume can form effective adsorption and steric hindrance layers, thereby achieving synergistic dispersion of particle gradation in high solid phase and low water-cement ratio mixtures, reducing plastic viscosity and yield stress, and solving the problems of high casting resistance, local material shortage and fiber aggregation in ultra-thin high-strength concrete components.

[0020] (2) By reducing the surface tension of the pore solution in the early stage of mixing by the instant shrinkage-reducing component, and then by the hydrolyzable shrinkage-reducing segments grafted into the polycarboxylic acid molecules gradually released during the hydration process, continuous shrinkage control is achieved in the plastic stage and the early stage of hardening. At the same time, the increase in gas content and early strength loss caused by the one-time addition of free shrinkage-reducing agent are reduced, thus solving the problems of shrinkage concentration and early cracking of ultra-thin components.

[0021] (3) By providing stable heterogeneous nucleation sites through polycarboxylic acid stabilized hydrated calcium silicate nanocrystals, cement hydration products can be rapidly formed into a continuous skeleton in the early stage of the component, which can compensate for the early hydration delay caused by shrinkage components, improve the early compressive strength and flexural strength of ultra-thin components, and solve the problem of insufficient early crack resistance of ultra-thin components with low water-cement ratio. Attached Figure Description

[0022] The accompanying drawings are provided to further understand the present invention and form part of the specification. They are used together with the embodiments of the present invention to explain the invention and do not constitute a limitation thereof.

[0023] Figure 1 This is a flowchart of the preparation method of the low-viscosity anti-crack dispersant of the present invention; Figure 2 This is a schematic diagram illustrating the selective dispersion of cement particles and silica fume particles according to the present invention. Figure 3 This is a schematic diagram illustrating the synergistic mechanism of the low-viscosity, crack-resistant dispersant of the present invention. Detailed Implementation

[0024] To make the objectives, technical solutions, and technical effects of the present invention clearer, the present invention will be described in detail below with reference to the embodiments. Obviously, the following embodiments are only some embodiments of the present invention, not all embodiments. Other implementation methods obtained by those skilled in the art based on the technical concept of the present invention are all within the protection scope of the present invention.

[0025] In the embodiments provided in this specification, operations without specific technical conditions are carried out in accordance with conventional technical conditions in the field of concrete admixtures and polymer synthesis, and raw materials and equipment without specified manufacturers are all industrial-grade products obtained through legitimate channels.

[0026] This invention provides a low-viscosity crack-resistant dispersant suitable for ultra-thin high-strength concrete components. The low-viscosity crack-resistant dispersant includes a selective dispersing mother liquor for cement particles, a selective shrinkage-resistant mother liquor for silica fume particles, a polycarboxylate-stabilized hydrated calcium silicate crystal nucleation liquid, an instant shrinkage-reducing component, an antifoaming component, and deionized water.

[0027] The selective dispersion mother liquor for cement particles forms a rapid adsorption structure through medium side chain length, high anionic group density and controlled main chain length. During the concrete mixing stage, it preferentially adsorbs onto the surface of cement particles and early hydration products, and breaks down cement flocs through electrostatic repulsion and steric hindrance.

[0028] The selective anti-shrinkage mother liquor for silica fume particles covers the surface of silica fume particles with a long polyoxyethylene side chain and introduces hydrolyzable anti-shrinkage side segments containing polyoxypropylene segments into the polymer backbone, so that the silica fume particles remain dispersed in the low water-to-binder ratio slurry, while the hydrolyzable anti-shrinkage side segments gradually release polyoxypropylene shrinkage-reducing components in the alkaline pore liquid.

[0029] The polycarboxylate-stabilized calcium silicate hydrate nucleation solution includes sheet-like calcium silicate hydrate nanocrystals and a polycarboxylate stabilizing layer coated on the surface of the calcium silicate hydrate nanocrystals. The polycarboxylate stabilizing layer restricts the agglomeration of the calcium silicate hydrate nanocrystals in the low-viscosity crack-resistant dispersant and provides hydration nucleation sites after concrete mixing.

[0030] The immediate shrinkage-reducing component lowers the surface tension of the pore fluid during the plastic stage of concrete, while the hydrolyzable shrinkage-resistant side gradually releases the shrinkage-reducing component during the setting and early hardening stages of concrete, thus forming a two-stage shrinkage-resistant process that connects the immediate shrinkage reduction during the plastic stage and the delayed shrinkage reduction during the hardening stage.

[0031] By weight, the low-viscosity crack-resistant dispersant includes 35-48 parts of selective dispersion mother liquor for cement particles, 25-38 parts of selective shrinkage-resistant mother liquor for silica fume particles, 5-12 parts of polycarboxylate stabilized hydrated calcium silicate crystal nucleation liquid, 1.0-3.0 parts of instant shrinkage-reducing component, 0.05-0.20 parts of defoaming component, and 10-25 parts of deionized water, with the total weight of all components being 100 parts.

[0032] The solid content of the selectively dispersed mother liquor for cement particles is 38%–42%, the weight-average molecular weight is 18,000–35,000, the number-average molecular weight of the polyethylene oxide side chains is 1,000–1,500, and the carboxylic acid monomer accounts for 18%–28% of the total mass of polymerizable monomers.

[0033] The solid content of the selective anti-shrinkage mother liquor containing silica fume particles is 35%–40%, the weight-average molecular weight is 25,000–50,000, the number-average molecular weight of the polyethylene oxide side chains is 2,400–3,000, and the hydrolyzable anti-shrinkage side segments account for 7%–15% of the total mass of polymerizable monomers.

[0034] The solid content of the polycarboxylate-stabilized hydrated calcium silicate crystal nuclei solution is 10%–16%, the median particle size of the hydrated calcium silicate nanocrystals is 80–180 nm, and the calcium-silicon molar ratio is 1.2–1.6.

[0035] The immediate shrinkage reducing component is polyoxypropylene monobutyl ether with a number average molecular weight of 300-600, and the defoaming component is a polyether-modified silicone defoamer.

[0036] The low-viscosity crack-resistant dispersant has a dynamic viscosity of 80–220 mPa·s at 25℃, a solid content of 30%–38%, a pH value of 6.0–7.5, and an adsorption amount of 0.8%–1.5% of the mass of the cementitious material.

[0037] The present invention also provides a method for preparing the aforementioned low-viscosity anti-crack dispersant, comprising the following steps.

[0038] Step S1: Prepare a hydrolyzable anti-condensation monomer. Polyoxypropylene monobutyl ether (300-600 number average molecular weight), maleic anhydride, p-toluenesulfonic acid, and hydroquinone are added to a reactor equipped with a condenser and a nitrogen inlet. The molar ratio of polyoxypropylene monobutyl ether to maleic anhydride is 1:0.95 to 1:1.05. The amount of p-toluenesulfonic acid added is 0.10% to 0.30% of the total mass of the reactants, and the amount of hydroquinone added is 0.02% to 0.05% of the total mass of the reactants. The reaction is carried out at 70-85°C under nitrogen protection for 2-4 hours to obtain a hydrolyzable anti-condensation monomer containing maleic acid monoester structure and polyoxypropylene segments.

[0039] Step S2: Prepare a selective dispersion mother liquor for cement particles. Add methoxy polyethylene glycol methacrylate, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, hydroxyethyl acrylate, mercaptoethanol, and deionized water to a polymerization reactor. Under nitrogen protection and at 40–50°C, add hydrogen peroxide solution and ascorbic acid solution dropwise over 2.5–3.5 hours. After the addition is complete, maintain the temperature for 1–2 hours. Then, adjust the pH to 6.2–6.8 using a 30% sodium hydroxide solution and adjust the solid content to 38%–42% using deionized water to obtain the selective dispersion mother liquor for cement particles.

[0040] Step S3: Prepare a selective anti-shrinkage mother liquor for silica fume particles. Add isopentenyl alcohol polyoxyethylene ether, acrylic acid, sodium vinyl sulfonate, the hydrolyzable anti-shrinkage monomer obtained in step S1, mercaptoethanol, and deionized water to a polymerization reactor. Under nitrogen protection and at 30-42°C, add hydrogen peroxide solution and ascorbic acid solution dropwise over 3-4 hours. After the addition is complete, keep the temperature for 1-2 hours. Then adjust the pH to 6.0-6.8 and the solid content to 35%-40% to obtain the selective anti-shrinkage mother liquor for silica fume particles.

[0041] Step S4: Prepare polycarboxylate-stabilized hydrated calcium silicate crystal nucleation solution. Selectively dispersed cement particles mother liquor is added to sodium silicate solution to form a silicon source mixture. Calcium nitrate solution is added dropwise to the silicon source mixture at 20–30℃ and 500–800 r / min, controlling the calcium-silicon molar ratio at 1.2–1.6 and the pH of the reaction system at 11.5–12.5. After the addition is complete, stirring is continued for 1–3 hours. The solution is then filtered through a membrane to reduce the soluble salt content and the solid content is adjusted to 10%–16% to obtain the polycarboxylate-stabilized hydrated calcium silicate crystal nucleation solution.

[0042] Step S5: Perform graded compounding. Add the selective dispersion mother liquor of cement particles and the selective anti-shrinkage mother liquor of silica fume particles into the compounding kettle and stir for 15-25 minutes at 25-35℃ and 300-500 r / min. Then add the instant shrinkage reduction component and stir for 10-20 minutes. Subsequently, add the polycarboxylate stabilized hydrated calcium silicate crystal nucleation liquid into the compounding kettle at a uniform flow rate for 20-40 minutes.

[0043] Step S6: Add defoaming components and deionized water, stir at 200-350 r / min for 20-30 min, adjust the pH value to 6.0-7.5, and obtain a low-viscosity crack-resistant dispersant suitable for ultra-thin high-strength concrete components after filtration through a 100-mesh filter.

[0044] Example 1: This example describes the preparation of a low-viscosity, crack-resistant dispersant suitable for ultra-thin high-strength concrete components.

[0045] In step S1, 100 kg of polyoxypropylene monobutyl ether with a number average molecular weight of 400, 24.5 kg of maleic anhydride, 0.25 kg of p-toluenesulfonic acid and 0.04 kg of hydroquinone were added to the reactor. The temperature was raised to 78°C under nitrogen protection and the reaction was carried out for 3 hours. Heating was stopped after the acid value of the reaction product reached 86 mg KOH / g to obtain a hydrolyzable anti-condensation monomer.

[0046] In step S2, 100 kg of methoxy polyethylene glycol methacrylate with a side chain number average molecular weight of 1200, 28 kg of acrylic acid, 3 kg of 2-acrylamido-2-methylpropanesulfonic acid, 4 kg of hydroxyethyl acrylate, 0.8 kg of mercaptoethanol, and 180 kg of deionized water were added to the polymerization reactor. At 45°C, 8 kg of 10% hydrogen peroxide solution and 6 kg of 5% ascorbic acid solution were added dropwise over 3 hours. After the addition was completed, the temperature was maintained for 1.5 hours. The pH value was adjusted to 6.5 and the solid content was adjusted to 40% to obtain a selective dispersion mother liquor of cement particles with a weight average molecular weight of 26400.

[0047] In step S3, 100 kg of isopentenyl alcohol polyoxyethylene ether with a side chain number average molecular weight of 2800, 16 kg of acrylic acid, 2.5 kg of sodium vinyl sulfonate, 15 kg of hydrolyzable anti-shrinkage monomer, 0.6 kg of mercaptoethanol, and 190 kg of deionized water were added to the polymerization reactor. At 36°C, 7 kg of 10% hydrogen peroxide solution and 5 kg of 5% ascorbic acid solution were added dropwise over a period of 3.5 h. After the addition was completed, the temperature was maintained for 1.5 h. The pH value was adjusted to 6.4 and the solid content was adjusted to 38%, resulting in a selective anti-shrinkage mother liquor of silica fume particles with a weight average molecular weight of 37200.

[0048] Step S4: 10 kg of selectively dispersed mother liquor of cement particles is added to 100 kg of sodium silicate solution with a mass concentration of 12%. Calcium nitrate solution is added dropwise at 25℃ and 650 r / min, with the calcium-silicon molar ratio controlled at 1.45 and the pH value controlled at 12.0. After the addition is completed, the mixture is stirred for 2 hours. After membrane filtration and concentration adjustment, a polycarboxylate-stabilized hydrated calcium silicate crystal nucleation solution with a solid content of 12% and a median particle size of 118 nm is obtained.

[0049] Step S5: By weight, add 42 parts of selective dispersion mother liquor for cement particles and 32 parts of selective anti-shrinkage mother liquor for silica fume particles into the compounding kettle, stir for 20 minutes at 30℃ and 400r / min, then add 1.8 parts of polyoxypropylene monobutyl ether and stir for 15 minutes, and then add 8 parts of polycarboxylic acid stabilized hydrated calcium silicate crystal nucleation solution within 30 minutes.

[0050] In step S6, add 0.12 parts of polyether-modified silicone defoamer and 16.08 parts of deionized water, stir at 280 r / min for 25 min, and filter through 100 mesh to obtain a low-viscosity crack-resistant dispersant. The solid content of the low-viscosity crack-resistant dispersant is 34.7%, the pH value is 6.6, and the dynamic viscosity at 25℃ is 136 mPa·s.

[0051] The selective dispersion mother liquor for cement particles is first adsorbed onto the surface of cement particles and early hydration products. The selective anti-shrinkage mother liquor for silica fume particles uses long polyethylene oxide side chains to cover silica fume particles, thereby reducing the composite flocs formed between cement particles, silica fume particles and quartz powder, so that the low water-binder ratio slurry can obtain a lower plastic viscosity without adding extra mixing water.

[0052] Within the first 2 hours after water is added to the concrete, the shrinkage-reducing component lowers the surface tension of the pore fluid. After the alkalinity of the concrete pore fluid increases, the maleic acid monoester bonds in the shrinkage-resistant side segment can be hydrolyzed and polyoxypropylene segments can be released, so that the shrinkage-reducing effect can continue into the hydration acceleration period and the self-drying formation period.

[0053] After the polycarboxylate-stabilized hydrated calcium silicate crystal nuclei enter the slurry, they remain in a nano-dispersed state and provide hydration nucleation sites. This allows the ultrathin components to form a continuous hydration product skeleton earlier, even under conditions of a large surface area-to-volume ratio and rapid water loss. This improves early tensile strength and reduces the probability that shrinkage stress exceeds the tensile strength at the same time.

[0054] Example 2: This example prepares a high cement compatibility low viscosity crack-resistant dispersant. The difference from Example 1 is that the side chain number-average molecular weight of methoxy polyethylene glycol methacrylate in the selective dispersion mother liquor for cement particles is 1000, the amount of acrylic acid added is 32 kg, the amount of 2-acrylamido-2-methylpropanesulfonic acid added is 4 kg, and the amount of mercaptoethanol added is 1.0 kg. The weight-average molecular weight of the selective dispersion mother liquor for cement particles is 21800.

[0055] The final compounding ratio, by weight, is 46 parts of selective dispersion mother liquor for cement particles, 28 parts of selective anti-shrinkage mother liquor for silica fume particles, 6 parts of polycarboxylate stabilized hydrated calcium silicate crystal nucleation solution, 2.2 parts of instant shrinkage reduction component, 0.15 parts of defoaming component, and 17.65 parts of deionized water.

[0056] This embodiment is suitable for high-strength concrete in which cement accounts for more than 80% of the mass of cementitious materials and silica fume accounts for 10% to 15% of the mass of cementitious materials. The higher density of anionic groups increases the rapid adsorption on the surface of cement particles, and the lower weight-average molecular weight reduces the liquid viscosity caused by polymer chain entanglement.

[0057] Example 3: This example prepares a high silica fume-compatible low viscosity anti-crack dispersant. The difference from Example 1 is that the side chain number-average molecular weight of isopentenyl alcohol polyoxyethylene ether in the silica fume particle selective anti-shrinkage mother liquor is 3000, the amount of acrylic acid added is 13kg, and the amount of hydrolyzable anti-shrinkage monomer added is 17kg, resulting in a silica fume particle selective anti-shrinkage mother liquor with a weight-average molecular weight of 42800.

[0058] The final compounding ratio, by weight, is 38 parts of selective dispersion mother liquor for cement particles, 36 parts of selective anti-shrinkage mother liquor for silica fume particles, 8 parts of polycarboxylate stabilized hydrated calcium silicate crystal nucleation solution, 1.5 parts of instant shrinkage reduction component, 0.10 parts of defoaming component, and 16.40 parts of deionized water.

[0059] This embodiment is suitable for ultra-high strength concrete where silica fume accounts for 15% to 25% of the cementitious material mass. The longer polyoxyethylene side chains form a thicker steric hindrance layer on the silica fume surface, and the increased amount of hydrolyzable shrinkage-resistant monomers improves the release of shrinkage-reducing components during the hardening stage.

[0060] Example 4: This example prepares an early-strength, low-viscosity, crack-resistant dispersant. The difference from Example 1 is that the solid content of the polycarboxylic acid stabilized hydrated calcium silicate crystal nucleus liquid is 15%, and the median particle size of the hydrated calcium silicate nanocrystal nuclei is 92 nm.

[0061] The final compounding ratio, by weight, is 40 parts of selective dispersion mother liquor for cement particles, 30 parts of selective anti-shrinkage mother liquor for silica fume particles, 12 parts of polycarboxylate stabilized hydrated calcium silicate crystal nucleation solution, 1.8 parts of instant shrinkage reduction component, 0.12 parts of defoaming component, and 16.08 parts of deionized water.

[0062] This embodiment is suitable for ultra-thin precast components with a demolding time of no more than 24 hours. Increasing the number of hydrated calcium silicate nanocrystal nuclei can shorten the hydration induction period and improve the compressive strength and splitting tensile strength of concrete from 12 hours to 24 hours.

[0063] Example 5: This example prepares a low-air-entraining, low-viscosity, crack-resistant dispersant. The difference from Example 1 is that the amount of the instant shrinkage-reducing component added is 1.0 part, the amount of the defoaming component added is 0.20 parts, and the amount of the hydrolyzable shrinkage-resistant monomer added to the silica fume particle selective shrinkage-resistant mother liquor is 18 kg.

[0064] This embodiment reduces the amount of free polyoxypropylene monobutyl ether added and increases the proportion of polymer-bound anti-shrinkage side segments, so that the shrinkage-reducing components are gradually released during the hydration process, thereby reducing the increase in gas content caused by the accumulation of immediate shrinkage-reducing components at the gas-liquid interface during the stirring stage.

[0065] Example 6: In this example, the low-viscosity crack-resistant dispersant prepared in Example 1 is applied to a high-strength concrete ultrathin slab with a thickness of 20mm.

[0066] Each cubic meter of concrete includes 850 kg of silicate cement, 150 kg of silica fume, 100 kg of quartz powder, 1050 kg of quartz sand with a particle size of 0.1-0.6 mm, 180 kg of water, 120 kg of copper-plated steel fiber with a length of 13 mm and a diameter of 0.2 mm, and 12 kg of low-viscosity crack-resistant dispersant, with a water-cement ratio of 0.18.

[0067] Step S1: Add silicate cement, silica fume, quartz powder and quartz sand to a forced mixer and dry mix for 2 minutes.

[0068] Step S2: Add the low-viscosity anti-crack dispersant to the mixing water to form a liquid component. Add the liquid component to a forced mixer within 60 seconds, and stir at 60 r / min for 2 minutes, then at 120 r / min for 3 minutes.

[0069] Step S3: Add copper-plated steel fibers evenly to the slurry within 2 minutes and continue stirring for 2 minutes to obtain a high-strength concrete mixture.

[0070] Step S4: Pour the high-strength concrete mixture into a slab mold with a length of 1000mm, a width of 300mm, and a thickness of 20mm. Do not perform high-frequency vibration; instead, apply low-amplitude vibration for 30 seconds to the outside of the mold to remove air bubbles from the edges and corners.

[0071] Step S5: Curing in the mold for 24 hours at 20℃ and 95% relative humidity. After demolding, continue curing at 20℃ and 95% relative humidity for 7 days, and then transfer to an environment at 20℃ and 60% relative humidity for 28 days.

[0072] No through-holes were found inside the prepared ultrathin plate. The steel fibers were able to pass through the 20mm thick mold cavity and remain evenly distributed. No plastic shrinkage cracks or through-early cracks appeared on the plate surface.

[0073] Example 7: In this example, the low-viscosity crack-resistant dispersant prepared in Example 3 is applied to a 15mm thick high-silica fume concrete decorative panel. Each cubic meter of concrete includes 800kg of silicate cement, 200kg of silica fume, 120kg of quartz powder, 1020kg of quartz sand, 175kg of water, 90kg of stainless steel fiber with a length of 8mm and a diameter of 0.16mm, and 13kg of low-viscosity crack-resistant dispersant.

[0074] The preparation process was carried out according to steps S1 to S5, with a demolding time of 30 hours. The resulting high silica fume concrete decorative panel had an intact surface, with no missing material or honeycomb in the corner areas, and a 28-day compressive strength of 162.8 MPa.

[0075] Comparative Example 1: This comparative example uses a conventional isopentenyl alcohol polyoxyethylene ether type polycarboxylate water-reducing agent with a solid content of 35%, without adding silica fume particle selective anti-shrinkage mother liquor, polycarboxylate stabilized hydrated calcium silicate crystal nucleation liquid and instant shrinkage reduction component. The water-reducing agent dosage is the same as in Example 1.

[0076] Comparative Example 2: This comparative example uses cement particle selective dispersion mother liquor as the only polycarboxylic acid component, without adding silica fume particle selective anti-shrinkage mother liquor, and the other components and dosages are the same as in Example 1.

[0077] Comparative Example 3: This comparative example uses a selectively dispersed cement particle mother liquor and a long-chain polycarboxylic acid mother liquor without the introduction of hydrolyzable shrinkage-resistant monomers, and adds the same instant shrinkage-reducing component and polycarboxylic acid stabilized hydrated calcium silicate crystal nucleation solution as in Example 1.

[0078] Comparative Example 4: This comparative example uses a combination of selective dispersion mother liquor for cement particles and selective anti-shrinkage mother liquor for silica fume particles, without adding polycarboxylate stabilized hydrated calcium silicate crystal nucleation solution. The remaining components and dosages are the same as in Example 1.

[0079] Comparative Example 5: This comparative example uses a conventional isopentenyl alcohol polyoxyethylene ether type polycarboxylate superplasticizer, and adds the same amount of free polyoxypropylene monobutyl ether as the instant shrinkage reduction component and hydrolyzable anti-shrinkage side segment in Example 1, without introducing polymer-bound anti-shrinkage side segment.

[0080] Experimental Example 1: This experimental example examines the effects of Examples 1 to 5 and Comparative Examples 1 to 5 on the rheological properties, dispersion retention properties, and air content of high-strength concrete paste. The mix proportions of each concrete group are the same as those in Example 6, and the admixture dosage is 1.2% of the mass of cementitious materials.

[0081] The yield stress and plastic viscosity were measured 10 min after mixing using a coaxial cylindrical rheometer. The initial expansion and 60 min expansion were measured using a micro slump expansion test. The gas content was measured using the pressure method. The results are shown in Table 1.

[0082] Table 1. Effects of different dispersants on the rheological properties of high-strength concrete:

[0083] As shown in Table 1, Examples 1 to 5 reduce the degree of composite flocculation in high solid volume fraction slurry by using selective dispersion mother liquor for cement particles and selective anti-shrinkage mother liquor for silica fume particles to cover cement particles and silica fume particles respectively. As a result, the plastic viscosity and yield stress are lower than those of Comparative Example 1 and Comparative Example 2.

[0084] In Comparative Example 5, all shrinkage-reducing components were added at once in a free state. Although this had a certain shrinkage-reducing effect, the free shrinkage-reducing components accumulated at the gas-liquid interface, leading to an increase in gas content. At the same time, it weakened the effective adsorption of polycarboxylic acid on the surface of solid particles, resulting in a higher plastic viscosity than in Example 1.

[0085] Test Example 2: This test example examines the autogenous shrinkage, plastic shrinkage cracking, and constrained cracking properties of concrete prepared in Examples 1 to 5 and Comparative Examples 1 to 5.

[0086] The length change of the self-shrinkage specimen was recorded after final setting; the plastic shrinkage test was conducted for 6 hours at a temperature of 30℃, relative humidity of 40%, and surface wind speed of 3m / s; the constrained cracking test used a ring specimen to record the time of the first visible crack and the maximum crack width at 28 days. The test results are shown in Table 2.

[0087] Table 2. Effects of different dispersants on the shrinkage cracking properties of high-strength concrete:

[0088] As shown in Table 2, Examples 1 to 5 form a two-stage shrinkage reduction effect through the immediate shrinkage reduction component and the hydrolyzable shrinkage-resistant side section, which not only inhibits the surface water loss shrinkage of concrete in the plastic stage, but also reduces the capillary shrinkage pressure generated by the pore liquid meniscus after setting. Therefore, the amount of autogenous shrinkage and the area of ​​plastic cracks are significantly reduced.

[0089] Comparative Example 3 lacks a hydrolyzable shrinkage-resistant side section, and it is difficult to maintain the shrinkage-reducing effect during the hardening stage by relying solely on the immediate shrinkage-reducing component; although Comparative Example 5 adds more free shrinkage-reducing components, the free shrinkage-reducing components cause an increase in gas content and a decrease in early strength, and the restraint cracking performance is still lower than that of Example 1.

[0090] The shrinkage of Comparative Example 4 is close to that of Example 1, but due to the lack of polycarboxylic acid stabilized hydrated calcium silicate crystal nucleation liquid, the early hydration product skeleton formation rate is slower, and the shrinkage stress exceeds the tensile strength at the same time earlier. Therefore, the time of first confined cracking is shorter than that of Example 1.

[0091] Experimental Example 3: This experimental example tests the early strength, later strength, and forming quality of the ultrathin slabs of the concrete prepared in Examples 1, 3, 4, and Comparative Examples 1 to 5.

[0092] Compression specimens, flexural specimens, and an ultrathin plate with a length of 1000 mm, a width of 300 mm, and a thickness of 20 mm were prepared using the mix proportions in Example 6. The porosity of the ultrathin plate was statistically analyzed by cross-sectional images, and the coefficient of variation of the steel fiber mass distribution was detected by the nine-point sampling method. The test results are shown in Table 3.

[0093] Table 3. Effects of different dispersants on strength and forming quality of ultrathin sheets:

[0094] As shown in Table 3, the polycarboxylate stabilized hydrated calcium silicate nucleation solution can improve the 1-day compressive strength and 1-day flexural strength without significantly increasing the plastic viscosity of the slurry. This solves the problem of shrinkage reducing components lowering the surface tension of the pore liquid and delaying the insufficient early crack resistance of some ultrathin components after early hydration.

[0095] Examples 1, 3, and 4 utilize low-plasticity slurry to improve the filling of narrow mold cavities and the dispersion of steel fibers, reducing local agglomeration of steel fibers, material shortage at edges and corners, and internal voids. At the same time, they utilize early hydration nucleation and two-stage shrinkage to improve crack resistance during demolding and handling.

[0096] This invention achieves a continuous synergistic relationship through the selective dispersion of cement particles, selective dispersion of silica fume particles, delayed release of polymer-bound shrinkage-resistant side segments, and early reinforcement of polycarboxylate-stabilized hydrated calcium silicate crystal nuclei. It does not rely on increasing water content to achieve fluidity, nor on large amounts of expansion components to compensate for shrinkage. It is adaptable to water-cement ratios of 0.16–0.22, component thicknesses of 12–35 mm, and cementitious material dosages of 850–1200 kg / m³. 3 High-strength concrete ultra-thin components.

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Any adjustments and equivalent substitutions made by those skilled in the art to the raw material ratio, polymer side chain length, reaction temperature, crystal nucleus particle size and compounding order without departing from the technical concept of the present invention should fall within the scope of protection of the present invention.

Claims

1. A low-viscosity, crack-resistant dispersant suitable for ultra-thin high-strength concrete components, characterized in that, Based on a total mass of 100 parts, the product includes 35-48 parts of cement particle selective polycarboxylate superplasticizer mother liquor, 25-38 parts of silica fume particle selective shrinkage-reducing polycarboxylate superplasticizer mother liquor, 5-12 parts of polycarboxylate stabilized hydrated calcium silicate nanocrystal seed liquor, 1.0-3.0 parts of instant shrinkage-reducing component, 0.05-0.20 parts of polyether modified organosilicon defoamer, and 10-25 parts of water, with the total mass of all components being 100 parts. The mother liquor of the cement particle selective polycarboxylate superplasticizer is a copolymer solution formed by methoxy polyethylene glycol methacrylate, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and hydroxyethyl acrylate. The mother liquor of the silica fume granules selective shrinkage-reducing polycarboxylate superplasticizer is a copolymer solution formed by isopentenyl alcohol polyoxyethylene ether, acrylic acid, sodium vinyl sulfonate and hydrolyzable shrinkage-reducing monomers. The polycarboxylic acid stabilized hydrated calcium silicate nanocrystal seed solution includes hydrated calcium silicate nanocrystals and a polycarboxylic acid stabilizer adsorbed on the surface of the hydrated calcium silicate nanocrystals.

2. The low-viscosity, crack-resistant dispersant according to claim 1, characterized in that, The solid content of the mother liquor of the selective polycarboxylate superplasticizer for cement particles is 38% to 42%, the weight average molecular weight of the copolymer is 18,000 to 35,000, and the number average molecular weight of the polyethylene glycol side chains of methoxy polyethylene glycol methacrylate is 1,000 to 1,500.

3. The low-viscosity, crack-resistant dispersant according to claim 1, characterized in that, The solid content of the mother liquor of the silica fume selective shrinkage-reducing polycarboxylate superplasticizer is 35% to 40%, the weight average molecular weight of the copolymer is 25,000 to 50,000, the number average molecular weight of the polyoxyethylene side chain of isopentenyl alcohol polyoxyethylene ether is 2,400 to 3,000, the mass of the hydrolyzable shrinkage-reducing monomer is 7% to 15% of the total mass of the comonomer, and the hydrolyzable shrinkage-reducing monomer is obtained by esterification reaction of polyoxypropylene monobutyl ether and maleic anhydride.

4. The low-viscosity, crack-resistant dispersant according to claim 1, characterized in that, The solid content of the polycarboxylic acid stabilized hydrated calcium silicate nanocrystal seed solution is 10% to 16%, the median particle size of the hydrated calcium silicate nanocrystal seeds is 80 to 180 nm, and the calcium-silicon molar ratio of the hydrated calcium silicate nanocrystal seeds is 1.2 to 1.

6.

5. The low-viscosity, crack-resistant dispersant according to claim 1, characterized in that, The instant shrinkage-reducing component is polyoxypropylene monobutyl ether with a number average molecular weight of 300-600, and the low-viscosity anti-crack dispersant has a solid content of 30%-38%, a viscosity of 80-220 mPa·s at 25°C, and a pH of 6.0-7.

5.

6. A method for preparing the low-viscosity anti-crack dispersant according to any one of claims 1 to 5, characterized in that, Includes the following steps: Step S1: Polyoxypropylene monobutyl ether is esterified with maleic anhydride to obtain a hydrolyzable shrinkage-reducing monomer containing unsaturated double bonds and hydrolyzable ester bonds; Step S2: Methoxy polyethylene glycol methacrylate, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, and hydroxyethyl acrylate are free-radical copolymerized to obtain a mother liquor for a cement particle selective polycarboxylate superplasticizer; Step S3: Isopentenyl polyoxyethylene ether, acrylic acid, sodium vinyl sulfonate, and the hydrolyzable shrinkage-reducing monomer obtained in Step S1 are free-radical copolymerized to obtain... Step S4: Calcium source and silicon source react in an alkaline aqueous phase in the presence of polycarboxylic acid stabilizer to obtain polycarboxylic acid stabilized hydrated calcium silicate nanocrystal seed solution; Step S5: Mix cement particle selective polycarboxylic acid superplasticizer mother liquor, silica fume particle selective shrinkage-reducing polycarboxylic acid superplasticizer mother liquor and instant shrinkage-reducing component, and then add polycarboxylic acid stabilized hydrated calcium silicate nanocrystal seed solution; Step S6: Add polyether modified organosilicon defoamer and water, adjust pH and filter to obtain low viscosity crack-resistant dispersant.

7. The preparation method according to claim 6, characterized in that, The esterification reaction in step S1 is carried out under nitrogen protection and at 70-85℃ for 2-4 hours; the free radical copolymerization temperature in step S2 is 40-50℃, and the molecular weight of the copolymer is controlled by chain transfer agent and redox initiator; the free radical copolymerization temperature in step S3 is 30-42℃, and the molecular weight of the copolymer is controlled by chain transfer agent and redox initiator; in step S4, calcium nitrate is used as the calcium source and sodium silicate is used as the silicon source, the reaction temperature is 20-30℃, and the pH of the reaction system is 11.5-12.

5.

8. The preparation method according to claim 6 or 7, characterized in that, Step S5: First, mix the mother liquor of selective polycarboxylate superplasticizer for cement particles with the mother liquor of selective shrinkage-reducing polycarboxylate superplasticizer for silica fume particles, add the instant shrinkage-reducing component for the first stage of dispersion, and then slowly add the polycarboxylate stabilized hydrated calcium silicate nanocrystal seed liquid for the second stage of dispersion; Step S6: Adjust the pH of the mixture to 6.0-7.5, filter it through a 100-mesh sieve, and obtain a low-viscosity crack-resistant dispersant with a solid content of 30%-38% and a viscosity of 80-220 mPa·s at 25℃.