A zero-shrinkage and micro-expansion solid waste concrete suitable for grassland and sandy land environment and a preparation method thereof

By combining modified water-reducing agents with solid waste-based sulfoaluminate cementitious materials and gypsum-bonded aeolian sand composite fine aggregate, the problems of large shrinkage deformation and poor durability of concrete in grassland sandy environments were solved, and concrete with excellent workability, high volume stability and strong durability was prepared.

CN123151663APending Publication Date: 2026-11-24INNER MONGOLIA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611666088.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Concrete shrinks and deforms greatly in grassland and sandy environments. Existing water-reducing agents have reduced dispersion in high-alkali and high-sulfate systems, resulting in poor concrete workability, easy cracking, and difficulty in meeting the requirements for volume stability and durability.

Method used

By combining modified water-reducing agents with solid waste-based sulfoaluminate cementitious materials and gypsum-bonded aeolian sand composite fine aggregate, the modified water-reducing agents maintain good fluidity in high-alkali and high-sulfate systems, and the gypsum-bonded aeolian sand composite fine aggregate improves the aggregate gradation, thus controlling the length change rate of concrete during the hardening process within the range of zero shrinkage to slight expansion.

Benefits of technology

In grassland and sandy environments, concrete exhibits good workability, rapid early strength development, continuous strength growth in later stages, high compressive strength, good volume stability, and excellent durability, reducing the risk of cracking and meeting the requirements of road, foundation and other engineering projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123151663A_ABST
    Figure CN123151663A_ABST
Patent Text Reader

Abstract

This invention relates to the field of concrete technology, specifically to a zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments and its preparation method. The method includes mixing coarse aggregates of sand and gravel with ungranulated aeolian sand, adding solid waste-based sulfoaluminate cementitious materials, continuing dry mixing, adding a modified water-reducing agent, adding gypsum-bonded aeolian sand composite fine aggregate and water, stirring to obtain a mixture, pouring the mixture into a mold and vibrating it to form the final product, covering it with a film for moisture retention and curing, thus obtaining zero-shrinkage, micro-expansion solid waste concrete. In this invention, the modified water-reducing agent is stably dispersed in the high-alkali, high-sulfate system of the solid waste-based sulfoaluminate cementitious materials. Using it in concrete mixing allows the mixture to maintain good fluidity at a low water-cement ratio, exhibiting good cohesiveness and water retention, and preventing bleeding and segregation. When used in conjunction with gypsum-bonded aeolian sand composite fine aggregate, it improves aggregate gradation, reduces the amount of slurry required, and makes the concrete easier to pour and vibrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of concrete technology, specifically to a zero-shrinkage, micro-expansion solid waste concrete suitable for grassland and sandy environments and its preparation method. Background Technology

[0002] Studies have shown that as the amount of aeolian sand increases, the shrinkage deformation of aeolian sand concrete gradually increases. At the same time, the grassland sandy areas are dry and windy, with large diurnal temperature differences, frequent freeze-thaw cycles, and strong wind and sand erosion. The internal moisture of the concrete is rapidly lost, which further aggravates the risk of shrinkage cracking and puts forward stringent requirements on the volume stability and durability of concrete.

[0003] Existing polycarboxylic acid, naphthalene-based, or aliphatic water-reducing agents tend to exhibit reduced dispersion in high-alkali, high-sulfate systems composed of carbide slag, desulfurized gypsum, and coal gangue, resulting in rapid slump loss and difficulty in ensuring concrete workability. When ordinary water-reducing agents are combined with gypsum-bonded aeolian sand composite fine aggregates, they may further exacerbate localized sulfate concentrations, leading to uneven expansion or later cracking. Therefore, to address the problems described above, this invention proposes a zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments and its preparation method. Summary of the Invention

[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide a zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments and its preparation method, so as to solve the problems mentioned in the background art.

[0005] To achieve the above objectives, the present invention provides the following technical solution: A zero-shrinkage, micro-expansion solid waste concrete suitable for grassland and sandy environments and its preparation method, comprising the following steps: S1. Mix the coarse aggregate of sand and gravel and the ungranulated aeolian sand for 30-60 seconds, add the solid waste-based sulfoaluminate cementitious material, continue to dry mix for 60-120 seconds, add the modified water-reducing agent, stir for 60-120 seconds, add the gypsum-bonded aeolian sand composite fine aggregate and water, and stir for 60-120 seconds to obtain the mixture.

[0006] S2. Pour the mixture into a mold and vibrate it to form the desired shape. Cover it with a film to keep it moist and cured for 24-36 hours to obtain zero-shrinkage, micro-expansion solid waste concrete.

[0007] The modified water-reducing agent is prepared through the following steps: S11. The hydroxyl-terminated hyperbranched polyester is dissolved in pyridine and subjected to azeotropic dehydration at 110-120℃ under nitrogen protection. After dehydration, 4-dimethylaminopyridine and hydroquinone are added at 30-40℃, while methacrylic anhydride solution is added dropwise. After the addition is complete, the reaction is carried out at 50-60℃ for 6-8 h. After the reaction is completed, the mixture is cooled to room temperature to obtain the precursor monomer.

[0008] S12. Add methyl methacrylate polyoxyethylene and precursor monomer to deionized water, stir and dissolve at 45-48℃ under nitrogen protection, add hydrogen peroxide aqueous solution, and keep warm for 5-10 min to obtain a mixed solution.

[0009] S13. Mix hydroxyethyl methacrylate and hydroquinone monomethyl ether evenly, add phosphorus pentoxide at 45-55℃, raise the temperature to 80-85℃ and keep it at that temperature for 5-6 h, cool to room temperature after the reaction is complete to obtain the mixture.

[0010] S14. Dissolve acrylic acid, hydroxyethyl acrylate, a mixture, 2-acrylamide-2-methylpropanesulfonic acid, and methacryloyloxyethyltrimethylammonium chloride in deionized water and mix thoroughly to obtain solution A. Dissolve L-ascorbic acid and mercaptoacetic acid in deionized water and mix thoroughly to obtain solution B. Simultaneously add solution A and solution B dropwise to the mixed solution at 45-50℃. After the addition is complete, continue the reaction at this temperature for 1-1.5 h. Cool to room temperature and adjust the pH to 6-7 with NaOH aqueous solution to obtain the modified water-reducing agent.

[0011] Furthermore, the gypsum-bonded aeolian sand composite fine aggregate in S1 is obtained through the following steps: A1. Dry mix aeolian sand and β-type hemihydrate desulfurization gypsum for 1-3 minutes, add water by spraying, and granulate for 10-20 minutes to obtain composite particles.

[0012] A2. Place the composite particles in an environment with a temperature of 15-35℃ and a relative humidity of 80-85% for 24-48 hours, and then dry them at 40-60℃ for 1-2 hours to obtain gypsum-bonded aeolian sand composite fine aggregate.

[0013] The preparation process of β-type hemihydrate desulfurization gypsum is as follows: The original desulfurized gypsum was crushed and sieved. After sieving, it was pre-dried at 40-60℃ and then calcined at 140-170℃ for 1-3 hours. After calcination, it was cooled to room temperature to obtain β-type hemihydrate desulfurized gypsum.

[0014] Furthermore, the solid waste-based sulfoaluminate cementitious material in S1 is prepared through the following steps: B1. Crush, dry, and ball-mill the coal gangue, and pass it through a 200-mesh sieve to obtain coal gangue powder. Dry the carbide slag and desulfurized gypsum, and grind and pass them through a 200-mesh sieve respectively to obtain carbide slag powder and desulfurized gypsum powder.

[0015] B2. Mix coal gangue powder, carbide slag powder and desulfurized gypsum powder for 5-10 minutes, then add water to wet mix to obtain wet mixture. Granulate the wet mixture into 5-15 mm particles and dry at 100-110℃ for 2-4 hours to obtain raw material particles.

[0016] B3. Heat the raw material particles to 300-400℃ and hold for 30-50 minutes. Then, heat to 750-850℃ and hold for 40-60 minutes. Finally, heat to 1200-1280℃ and hold for 40-60 minutes. After calcination, cool to room temperature, crush and grind to obtain solid waste-based sulfoaluminate cementitious material.

[0017] The mass ratio of coal gangue powder, carbide slag powder, desulfurized gypsum powder and water is 1:(0.78-1.67):(0.33-0.83):(0.2-0.5).

[0018] Furthermore, in S1, the mass ratio of coarse aggregate, ungranulated aeolian sand, solid waste-based sulfoaluminate cementitious material, modified water-reducing agent, gypsum-bonded aeolian sand composite fine aggregate to water is 1: (0.25-0.35): (1.2-1.4): (0.01-0.02): (0.5-0.7): (0.5-0.7).

[0019] Furthermore, the mass ratio of the S11 terminal hydroxyl hyperbranched polyester, pyridine, 4-dimethylaminopyridine, hydroquinone and methacrylic anhydride solution is 1:(2-4):(0.01-0.03):(0.0005-0.0009):(0.2-0.3).

[0020] Furthermore, the mass ratio of methyl methacrylate polyoxyethylene ether, precursor monomer, deionized water and hydrogen peroxide aqueous solution in S12 is 1:(0.04-0.06):(2-3):(0.02-0.06).

[0021] Furthermore, the mass ratio of hydroxyethyl methacrylate, hydroquinone monomethyl ether, and phosphorus pentoxide in S13 is 1:(0.002-0.005):(0.5-0.6).

[0022] Furthermore, in S14, the mass ratio of acrylic acid, hydroxyethyl acrylate, mixture, 2-acrylamide-2-methylpropanesulfonic acid, methacryloyloxyethyltrimethylammonium chloride to deionized water is 1:(0.6-1.2):(0.2-0.4):(0.25-0.75):(0.2-0.4):(4-8), the mass ratio of L-ascorbic acid, mercaptoacetic acid to deionized water is 1:(2-5):(20-30), and the mass ratio of mixed solution, liquid A to liquid B is 1:(0.3-0.6):(0.1-0.2).

[0023] Furthermore, the mass ratio of aeolian sand, β-type hemihydrate desulfurization gypsum and water in A1 is 1:(0.2-0.4):(0.2-0.4).

[0024] Furthermore, a zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments is prepared according to the aforementioned preparation method.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The modified water-reducing agent in this invention is stable in the high-alkali and high-sulfate system of solid waste-based sulfoaluminate cementitious materials. When used in concrete mixing, it can maintain good fluidity of the mixture at a low water-cement ratio, with good cohesiveness and water retention, and is not prone to bleeding and segregation. When used in combination with gypsum-bonded aeolian sand composite fine aggregate, it can improve aggregate gradation, reduce the amount of slurry required, make the concrete easy to pour and vibrate, and meet the construction performance requirements of grassland sandy land engineering.

[0026] 2. This invention combines a modified water-reducing agent with solid waste-based sulfoaluminate cementitious materials and gypsum-bonded aeolian sand composite fine aggregate, thereby controlling the length change rate of concrete within the range of zero shrinkage to slight expansion during the hardening process. This effectively compensates for drying shrinkage and autogenous shrinkage, reduces the risk of cracking, and provides good volume stability. Simultaneously, the early strength of the concrete develops rapidly, and its later strength continues to increase. The compressive strength meets the requirements of engineering projects such as roads, foundations, and slope protection. The hardened body has high density, and the aggregate and paste have good bonding. It exhibits excellent durability and a long service life in dry, windy, and freeze-thaw environments in grasslands and sandy areas. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the preparation process of zero-shrinkage micro-expansion solid waste concrete in this invention; Figure 2 This is a schematic diagram of the preparation process of the modified water-reducing agent in this invention; Figure 3 This is a schematic diagram of the preparation process of gypsum-bonded aeolian sand composite fine aggregate in this invention; Figure 4 This is a schematic diagram of the preparation process of the solid waste-based sulfoaluminate cementitious material in this invention; Figure 5 The XRD patterns of zero-shrinkage, micro-expansion solid waste concrete cured at different ages (1d, 3d, 7d, 28d, 90d) in Example 1 are shown. Figure 6 This is a SEM microstructure image of the zero-shrinkage, micro-expansion solid waste concrete cured for 1 day in Example 1. Figure 7 This is a SEM microstructure image of the zero-shrinkage, micro-expansion solid waste concrete cured for 3 days in Example 1. Figure 8 This is a SEM microstructure image of the zero-shrinkage, micro-expansion solid waste concrete cured for 7 days in Example 1. Figure 9 This is a SEM microstructure image of the zero-shrinkage, micro-expansion solid waste concrete cured for 28 days in Example 1. Figure 10 This is a SEM microstructure image of the zero-shrinkage, micro-expansion solid waste concrete cured for 90 days in Example 1. Detailed Implementation

[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0029] Please see Figures 1-10 The present invention provides a technical solution: In the following examples and comparative examples, the particle size range of the base raw materials used is as follows: Aeolian sand is taken from the original aeolian sand of grassland sandy land. Before use, it is sieved to remove plant roots, soil clods and impurities with a particle size greater than 1.18mm. The main particle size is 0.19-1.18mm.

[0030] Ungranulated aeolian sand is the fine part of aeolian sand after removing particles larger than 0.60mm, with a particle size of 0.125-0.60mm.

[0031] The coarse aggregate of sand and gravel is divided into two sizes: 5-10 mm and 10-20 mm, with a mass ratio of 30:70.

[0032] Example 1: A method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments includes the following steps: I. Preparation of solid waste-based sulfoaluminate cementitious materials: B1. Crush, dry, and ball-mill the coal gangue, and pass it through a 200-mesh sieve to obtain coal gangue powder. Dry the carbide slag and desulfurized gypsum, and grind and pass them through a 200-mesh sieve respectively to obtain carbide slag powder and desulfurized gypsum powder.

[0033] B2. Weigh 1000g of coal gangue powder, 780g of calcium carbide slag powder, and 330g of desulfurized gypsum powder, mix for 5 minutes, add 200g of water to wet mix, granulate into 5mm particles, and dry at 100℃ for 2 hours to obtain raw material particles.

[0034] B3. Place the raw material pellets in a high-temperature furnace, heat to 300℃ and hold for 30 minutes, then continue heating to 750℃ and hold for 40 minutes, then continue heating to 1200℃ and hold for 40 minutes. After calcination, rapidly cool to below 500℃, then cool to room temperature, crush and ball-mill to a specific surface area of ​​500 m². 2 / kg yields solid waste-based sulfoaluminate cementitious material.

[0035] II. Preparation of β-type hemihydrate desulfurized gypsum: Take an appropriate amount of undisturbed desulfurized gypsum, crush and sieve it to a particle size ≤0.15mm, pre-dry it at 40℃ to a free water content ≤3%, calcine it at 140℃ for 1 hour, cool it to room temperature, and store it in a sealed container to obtain β-type hemihydrate desulfurized gypsum.

[0036] III. Preparation of gypsum-bonded aeolian sand composite fine aggregate: A1. Weigh 1000g of aeolian sand and 200g of β-type hemihydrate desulfurized gypsum, dry mix for 1min, start the drum granulator (speed 25r / min), add 200g of water by spraying, granulate for 10min, and obtain composite granules.

[0037] A2. The composite particles are cured in an environment of 15℃ and 80% relative humidity for 24 hours, dried at 40℃ for 1 hour, and sieved into three particle sizes of 0.6-1.18mm, 1.18-2.36mm and 2.36-4.75mm. They are then mixed in a mass ratio of 30%, 40% and 30% respectively to obtain gypsum-bonded aeolian sand composite fine aggregate.

[0038] IV. Preparation of Modified Water-Reducing Agents: S11. Weigh 100g of hydroxyl-terminated hyperbranched polyester and dissolve it in 200g of pyridine. Under nitrogen protection, dehydrate it azeotropically at 110℃. Cool to 30℃, add 1g of 4-dimethylaminopyridine and 0.05g of hydroquinone, and add 20g of methacrylic anhydride dropwise. After the addition is complete, react at 50℃ for 6h and cool to room temperature to obtain the precursor monomer.

[0039] S12. Weigh 100g of methyl methacrylate polyoxyethylene ether and 4g of precursor monomer, add 200g of deionized water, stir and dissolve at 45℃ under nitrogen protection, add 2g of hydrogen peroxide aqueous solution, and keep warm for 5min to obtain a mixed solution.

[0040] S13. Weigh 100g of hydroxyethyl methacrylate and 0.2g of hydroquinone monomethyl ether, mix them evenly, add 50g of phosphorus pentoxide in batches at 45℃, heat to 80℃ and keep the temperature for 5h, cool to room temperature to obtain the mixture.

[0041] S14. Weigh 10g of acrylic acid, 6g of hydroxyethyl acrylate, 2g of a mixture, 2.5g of 2-acrylamide-2-methylpropanesulfonic acid, and 2g of methacryloyloxyethyltrimethylammonium chloride, and dissolve them in 40g of deionized water to prepare solution A. Weigh 1g of L-ascorbic acid and 2g of mercaptoacetic acid, and dissolve them in 20g of deionized water to prepare solution B. Place 100g of the mixed solution in a reaction vessel, and simultaneously add 30g of solution A and 10g of solution B at 45℃. After the addition is complete, keep the temperature for 1 hour, cool to room temperature, and adjust the pH to 6 with NaOH aqueous solution to obtain the modified water-reducing agent.

[0042] V. Preparation of Zero-Shrinkage Micro-Expansion Solid Waste Concrete: S1. Weigh 1000g of coarse aggregate and 250g of ungranulated aeolian sand, add them to a forced mixer and mix for 30s. Add 1200g of solid waste-based sulfoaluminate cementitious material and continue dry mixing for 60s. Add 10g of modified water-reducing agent and mix for 60s. Add 500g of gypsum-bonded aeolian sand composite fine aggregate and 500g of water and mix for 60s to obtain the mixture.

[0043] S2. Pour the mixture into a mold, vibrate it to form the desired shape, cover it with a film, and cure it at 25°C for 24 hours. After demolding, cure it according to standard to the specified age to obtain zero-shrinkage micro-expansion solid waste concrete.

[0044] Example 2: A method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments includes the following steps: I. Preparation of solid waste-based sulfoaluminate cementitious materials: B1. Crush, dry, and ball-mill the coal gangue, and pass it through a 200-mesh sieve to obtain coal gangue powder. Dry the carbide slag and desulfurized gypsum, and grind and pass them through a 200-mesh sieve respectively to obtain carbide slag powder and desulfurized gypsum powder.

[0045] B2. Weigh 1000g of coal gangue powder, 1225g of carbide slag powder, and 580g of desulfurized gypsum powder, mix for 7.5 minutes, add 350g of water to wet mix, granulate into 10mm particles, and dry at 105℃ for 3 hours to obtain raw material particles.

[0046] B3. Place the raw material pellets in a high-temperature furnace, heat to 350℃ and hold for 40 minutes, then continue heating to 800℃ and hold for 50 minutes, then continue heating to 1240℃ and hold for 50 minutes. After calcination, rapidly cool to below 500℃, then cool to room temperature, crush and ball-mill to a specific surface area of ​​500 m².2 / kg yields solid waste-based sulfoaluminate cementitious material.

[0047] II. Preparation of β-type hemihydrate desulfurized gypsum: Take an appropriate amount of undisturbed desulfurized gypsum, crush and sieve it to a particle size ≤0.15mm, pre-dry it at 50℃ to a free water content ≤3%, calcine it at 155℃ for 2 hours, cool it to room temperature, and store it in a sealed container to obtain β-type hemihydrate desulfurized gypsum.

[0048] III. Preparation of gypsum-bonded aeolian sand composite fine aggregate: A1. Weigh 1000g of aeolian sand and 300g of β-type hemihydrate desulfurization gypsum, dry mix for 2 minutes, start the drum granulator (speed 25r / min), add 300g of water by spraying, granulate for 15 minutes to obtain composite granules.

[0049] A2. The composite particles are cured in an environment of 25℃ and 82.5% relative humidity for 36 hours, dried at 50℃ for 1.5 hours, and sieved into three particle sizes: 0.6-1.18mm, 1.18-2.36mm, and 2.36-4.75mm. They are then mixed in a mass ratio of 30%, 40%, and 30% respectively to obtain gypsum-bonded aeolian sand composite fine aggregate.

[0050] IV. Preparation of Modified Water-Reducing Agents: S11. Weigh 100g of hydroxyl-terminated hyperbranched polyester and dissolve it in 300g of pyridine. Under nitrogen protection, dehydrate it azeotropically at 115℃. Cool to 35℃, add 2g of 4-dimethylaminopyridine and 0.07g of hydroquinone, and add 25g of methacrylic anhydride dropwise. After the addition is complete, react at 55℃ for 7h and cool to room temperature to obtain the precursor monomer.

[0051] S12. Weigh 100g of methyl methacrylate polyoxyethylene ether and 5g of precursor monomer, add 250g of deionized water, stir and dissolve at 46.5℃ under nitrogen protection, add 4g of hydrogen peroxide aqueous solution, and keep warm for 7.5min to obtain a mixed solution.

[0052] S13. Weigh 100g of hydroxyethyl methacrylate and 0.35g of hydroquinone monomethyl ether, mix them evenly, add 55g of phosphorus pentoxide in batches at 50℃, heat to 82.5℃ and keep the temperature for 5.5h, cool to room temperature to obtain the mixture.

[0053] S14. Weigh 10g acrylic acid, 9g hydroxyethyl acrylate, 3g mixture, 5g 2-acrylamide-2-methylpropanesulfonic acid, and 3g methacryloyloxyethyltrimethylammonium chloride and dissolve them in 60g deionized water to prepare solution A. Weigh 1g L-ascorbic acid and 3.5g mercaptoacetic acid and dissolve them in 25g deionized water to prepare solution B. Place 100g of the mixed solution in a reaction vessel, and simultaneously add 45g of solution A and 15g of solution B at 47.5℃. After the addition is complete, keep the temperature for 1.25h, cool to room temperature, and adjust the pH to 6.5 with NaOH aqueous solution to obtain the modified water-reducing agent.

[0054] V. Preparation of Zero-Shrinkage Micro-Expansion Solid Waste Concrete: S1. Weigh 1000g of coarse aggregate and 300g of ungranulated aeolian sand, add them to a forced mixer and mix for 45s. Add 1300g of solid waste-based sulfoaluminate cementitious material and continue dry mixing for 90s. Add 15g of modified water-reducing agent and mix for 90s. Add 600g of gypsum-bonded aeolian sand composite fine aggregate and 600g of water and mix for 90s to obtain the mixture.

[0055] S2. Pour the mixture into a mold, vibrate it to form the desired shape, cover it with a film, and cure it at 25°C for 30 hours. After demolding, cure it according to standard until the specified age to obtain zero-shrinkage, micro-expansion solid waste concrete.

[0056] Example 3: A method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments includes the following steps: I. Preparation of solid waste-based sulfoaluminate cementitious materials: B1. Crush, dry, and ball-mill the coal gangue, and pass it through a 200-mesh sieve to obtain coal gangue powder. Dry the carbide slag and desulfurized gypsum, and grind and pass them through a 200-mesh sieve respectively to obtain carbide slag powder and desulfurized gypsum powder.

[0057] B2. Weigh 1000g of coal gangue powder, 1670g of carbide slag powder, and 830g of desulfurized gypsum powder, mix for 10 minutes, add 500g of water for wet mixing, granulate into 15mm particles, and dry at 110℃ for 4 hours to obtain raw material particles.

[0058] B3. Place the raw material pellets in a high-temperature furnace, heat to 400℃ and hold for 50 minutes, then continue heating to 850℃ and hold for 60 minutes, then continue heating to 1280℃ and hold for 60 minutes. After calcination, rapidly cool to below 500℃, then cool to room temperature, crush and ball-mill to a specific surface area of ​​500 m². 2 / kg yields solid waste-based sulfoaluminate cementitious material.

[0059] II. Preparation of β-type hemihydrate desulfurized gypsum: Take an appropriate amount of undisturbed desulfurized gypsum, crush and sieve it to a particle size ≤0.15mm, pre-dry it at 60℃ to a free water content ≤3%, calcine it at 170℃ for 3 hours, cool it to room temperature, and store it in a sealed container to obtain β-type hemihydrate desulfurized gypsum.

[0060] III. Preparation of gypsum-bonded aeolian sand composite fine aggregate: A1. Weigh 1000g of aeolian sand and 400g of β-type hemihydrate desulfurization gypsum, dry mix for 3 minutes, start the drum granulator (speed 25r / min), add 400g of water by spraying, granulate for 20 minutes to obtain composite granules.

[0061] A2. The composite particles are cured at 35℃ and 85% relative humidity for 48 hours, dried at 60℃ for 2 hours, and sieved into three particle sizes: 0.6-1.18mm, 1.18-2.36mm, and 2.36-4.75mm. They are then mixed in a mass ratio of 30%, 40%, and 30% respectively to obtain gypsum-bonded aeolian sand composite fine aggregate.

[0062] IV. Preparation of Modified Water-Reducing Agents: S11. Weigh 100g of hydroxyl-terminated hyperbranched polyester and dissolve it in 400g of pyridine. Under nitrogen protection, dehydrate it azeotropically at 120℃. Cool to 40℃, add 3g of 4-dimethylaminopyridine and 0.09g of hydroquinone, and add 30g of methacrylic anhydride dropwise. After the addition is complete, react at 60℃ for 8h and cool to room temperature to obtain the precursor monomer.

[0063] S12. Weigh 100g of methyl methacrylate polyoxyethylene ether and 6g of precursor monomer, add 300g of deionized water, stir and dissolve at 48℃ under nitrogen protection, add 6g of hydrogen peroxide aqueous solution, and keep warm for 10min to obtain a mixed solution.

[0064] S13. Weigh 100g of hydroxyethyl methacrylate and 0.5g of hydroquinone monomethyl ether, mix them evenly, add 60g of phosphorus pentoxide in batches at 55℃, heat to 85℃ and keep the temperature for 6h, cool to room temperature to obtain the mixture.

[0065] S14. Weigh 10g acrylic acid, 12g hydroxyethyl acrylate, 4g mixture, 7.5g 2-acrylamide-2-methylpropanesulfonic acid, and 4g methacryloyloxyethyltrimethylammonium chloride, and dissolve them in 80g deionized water to prepare solution A. Weigh 1g L-ascorbic acid and 5g mercaptoacetic acid, and dissolve them in 30g deionized water to prepare solution B. Place 100g of the mixed solution in a reaction vessel, and simultaneously add 60g of solution A and 20g of solution B at 50℃. After the addition is complete, keep the temperature for 1.5h, cool to room temperature, and adjust the pH to 7 with NaOH aqueous solution to obtain the modified water-reducing agent.

[0066] V. Preparation of Zero-Shrinkage Micro-Expansion Solid Waste Concrete: S1. Weigh 1000g of coarse aggregate and 350g of ungranulated aeolian sand, add them to a forced mixer and mix for 60s. Add 1400g of solid waste-based sulfoaluminate cementitious material and continue dry mixing for 120s. Add 20g of modified water-reducing agent and mix for 120s. Add 700g of gypsum-bonded aeolian sand composite fine aggregate and 700g of water and mix for 120s to obtain the mixture.

[0067] S2. Pour the mixture into a mold, vibrate it to form the desired shape, cover it with a film, and cure it at 25°C for 36 hours. After demolding, cure it according to standard until the specified age to obtain zero-shrinkage, micro-expansion solid waste concrete.

[0068] Comparative Example 1: Comparative Example 1 differs from Example 1 in that the modified water-reducing agent is replaced with an equal mass of polycarboxylate water-reducing agent, while the remaining steps are exactly the same as in Example 1.

[0069] The following performance tests were conducted on the zero-shrinkage, micro-expansion solid waste concrete prepared in Examples 1-3 and Comparative Example 1: I. Mechanical property testing: 1. Compressive strength: The test was conducted according to GB / T 50081 "Standard for Test Methods of Physical and Mechanical Properties of Concrete". Three 100mm×100mm×100mm cubic specimens were used in each group. After molding, the specimens were covered with a thin film, left to stand at 20±2℃ for 24 hours before demolding, and then cured according to standard (20±2℃, RH≥95%). The compressive strength was measured at 1d, 3d, 7d, 28d and 90d respectively.

[0070] 2. Flexural strength: According to GB / T 50081, a 100mm×100mm×400mm prism specimen was used, and the loading rate was controlled according to the standard to determine the flexural strength after 28 days.

[0071] 3. Static compressive modulus of elasticity: According to GB / T 50081, the 28-day static compressive elastic modulus was determined using a 150mm×150mm×300mm prism specimen.

[0072] II. Volume stability test: 1. Self-shrinkage (early stage): According to ASTM C1698, "Standard Test Method for Self-Strain of Cement Paste and Mortar", a φ29mm×420mm polyethylene hollow corrugated pipe was used. After the mixture was formed and sealed, it was placed in an environment of 20±2℃, and the length change rate was measured at 30min, 6h, 1d, 7d, and 28d.

[0073] 2. Drying shrinkage: According to GB / T 50082 "Standard for Test Methods of Long-Term Performance and Durability of Ordinary Concrete", 100mm×100mm×515mm prism specimens were used, with probes pre-embedded at both ends. After the specimens were formed, they were cured under standard conditions for 3 days, and then placed in an environment with a temperature of 20±2℃ and a relative humidity of 60±5% to measure the length change rate at 1d, 3d, 7d, 14d and 28d respectively.

[0074] 3. Limit expansion rate: According to GB / T 23439 "Concrete Expansion Agent", 100mm×100mm×300mm specimens were used, and the longitudinal reinforcement ratio was set according to the standard. The length change rate was measured after 28 days of curing in water and 28 days in dry air.

[0075] III. Durability Testing: 1. Freeze resistance: According to the rapid freezing method of GB / T 50082, 100mm×100mm×400mm prism specimens were used. After standard curing for 28 days, freeze-thaw cycles were started. The mass loss rate and relative dynamic elastic modulus were measured every 25 cycles.

[0076] 2. Impermeability: According to the GB / T 50082 permeability test method, a frustum specimen with a top diameter of 175 mm, a bottom diameter of 185 mm, and a height of 150 mm was used. After standard curing for 28 days, the permeability grade was determined by gradually increasing the pressure using the water pressure method. The specific test results are shown in the table below.

[0077] Table 1: Performance Test Table for Zero-Shrinkage and Micro-Expansion Solid Waste Concrete As can be seen from the data in Table 1, the zero-shrinkage micro-expansion solid waste concrete prepared in the examples is significantly superior to the comparative example in terms of mechanical properties, volume stability, and durability. In terms of mechanical properties, the early, late, and long-term compressive strength, flexural strength, and compressive modulus of elasticity of the examples are all higher than those of the comparative example, with Example 2 showing the best performance, followed by Examples 1 and 3. In terms of volume stability, the examples are in a state of zero shrinkage to micro-expansion in terms of autogenous shrinkage, drying shrinkage, and restricted expansion rate, which can effectively compensate for shrinkage, while the comparative example continues to shrink, and its volume stability is obviously insufficient. In terms of durability, the examples have less mass loss, higher relative dynamic modulus of elasticity, and better impermeability after freeze-thaw cycles, indicating that they have stronger freeze-thaw resistance and impermeability. In summary, the modified water-reducing agent, solid waste-based sulfoaluminate cementitious material, and gypsum-bonded aeolian sand composite fine aggregate work synergistically to significantly improve the mechanical properties, volume stability, and durability of concrete, and the mix proportion of Example 2 is the best, verifying the effectiveness and superiority of the technical solution of the present invention.

[0078] Figure 5The XRD patterns of zero-shrinkage, micro-expansion solid waste concrete cured at different ages (1d, 3d, 7d, 28d, 90d) in Example 1 are shown. The main crystalline phases of the samples at 1d, 3d, 7d, 28d, and 90d were AFt (ettringite), Ye'elimite (calcium sulfoaluminate), Anhydrite, Belite, and Quartz. With increasing age, the characteristic peaks of Ye'elimite and Anhydrite generally weakened, indicating that they gradually participated in the hydration reaction and were consumed. The characteristic peak of AFt at 1d... The presence of peak d indicates that hydrated products such as ettringite were formed in the early stages and the hydration process continued. The Quartz peak remained relatively stable at each age, mainly originating from aggregate components such as aeolian sand, and did not participate in hydration. The Belite peak changed relatively slowly, indicating that its hydration reaction was slow. Overall, the spectrum reflects the process of gradual consumption of sulfoaluminate clinker minerals and the formation and continued existence of hydrated products such as ettringite as the age increases.

[0079] Figures 6-10 The SEM images mainly reflect the evolution of the microstructure of concrete over time, 1 day ( Figure 6 At 7 days, granular and flocculent hydration products and unreacted particles are visible, with a relatively loose structure and obvious pores and interparticle voids, indicating that hydration has just begun and the products are few. Figure 8 Needle-like crystals intertwine with flocculent gel, filling some pores, enhancing interparticle connections, and initially forming a network structure, 28 days ( Figure 9 At 90 days, the hydration products are more continuous, the gel encapsulates the particles and fills the pores, the macropores are reduced, the bonding between the slurry and aggregate interface is improved, and the structure is significantly densified. Figure 10 The microstructure is more uniform and dense, with fewer defects and pores, and the crystals are tightly bonded to the gel, indicating that long-term hydration continues. Overall, with increasing age, the hydration products increase, the structure becomes denser, the porosity decreases, and the interface is strengthened. This is consistent with the results in the document showing increased strength, excellent volume stability, and good durability.

[0080] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland and sandy environments, characterized in that, Includes the following steps: S1. Mix the coarse aggregate of sand and gravel and the ungranulated aeolian sand for 30-60 seconds, add solid waste-based sulfoaluminate cementitious material, continue dry mixing for 60-120 seconds, add modified water-reducing agent, stir for 60-120 seconds, add gypsum-bonded aeolian sand composite fine aggregate and water, and stir for 60-120 seconds to obtain the mixture. S2. Pour the mixture into a mold and vibrate it to form a shape. Cover it with a film to keep it moist and cure for 24-36 hours to obtain zero-shrinkage micro-expansion solid waste concrete. The modified water-reducing agent is prepared through the following steps: S11. The hydroxyl-terminated hyperbranched polyester is dissolved in pyridine and subjected to azeotropic dehydration at 110-120℃ under nitrogen protection. After dehydration, 4-dimethylaminopyridine and hydroquinone are added at 30-40℃, while methacrylic anhydride solution is added dropwise. After the addition is complete, the reaction is carried out at 50-60℃ for 6-8 h. After the reaction is completed, the mixture is cooled to room temperature to obtain the precursor monomer. S12. Add methyl methacrylate polyoxyethylene ether and precursor monomer to deionized water, stir and dissolve at 45-48℃ under nitrogen protection, add hydrogen peroxide aqueous solution, and keep warm for 5-10 min to obtain a mixed solution. S13. Mix hydroxyethyl methacrylate and hydroquinone monomethyl ether evenly, add phosphorus pentoxide at 45-55℃, heat to 80-85℃ and keep the temperature for 5-6 h, cool to room temperature after the reaction is completed to obtain a mixture; S14. Dissolve acrylic acid, hydroxyethyl acrylate, a mixture, 2-acrylamide-2-methylpropanesulfonic acid, and methacryloyloxyethyltrimethylammonium chloride in deionized water and mix thoroughly to obtain solution A. Dissolve L-ascorbic acid and mercaptoacetic acid in deionized water and mix thoroughly to obtain solution B. Simultaneously add solution A and solution B dropwise to the mixed solution at 45-50℃. After the addition is complete, continue the reaction at this temperature for 1-1.5 h. Cool to room temperature and adjust the pH to 6-7 with NaOH aqueous solution to obtain the modified water-reducing agent.

2. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, The gypsum-bonded aeolian sand composite fine aggregate in S1 is prepared through the following steps: A1. Dry mix aeolian sand and β-type hemihydrate desulfurization gypsum for 1-3 minutes, add water by spraying, and granulate for 10-20 minutes to obtain composite particles. A2. Place the composite particles in an environment with a temperature of 15-35℃ and a relative humidity of 80-85% for 24-48 hours, and then dry them at 40-60℃ for 1-2 hours to obtain gypsum-bonded aeolian sand composite fine aggregate. The preparation process of β-type hemihydrate desulfurization gypsum is as follows: The original desulfurized gypsum was crushed and sieved. After sieving, it was pre-dried at 40-60℃ and then calcined at 140-170℃ for 1-3 hours. After calcination, it was cooled to room temperature to obtain β-type hemihydrate desulfurized gypsum.

3. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, The solid waste-based sulfoaluminate cementitious material in S1 is prepared through the following steps: B1. Crush, dry, and ball-mill the coal gangue, and pass it through a 200-mesh sieve to obtain coal gangue powder. Dry the carbide slag and desulfurized gypsum, and grind and pass them through a 200-mesh sieve respectively to obtain carbide slag powder and desulfurized gypsum powder. B2. Mix coal gangue powder, carbide slag powder and desulfurized gypsum powder for 5-10 minutes, then add water to wet mix to obtain wet mixture. Granulate the wet mixture into 5-15 mm particles and dry at 100-110℃ for 2-4 hours to obtain raw meal particles. B3. Heat the raw material particles to 300-400℃ and hold for 30-50 minutes. Then, heat to 750-850℃ and hold for 40-60 minutes. Then, heat to 1200-1280℃ and hold for 40-60 minutes. After calcination, cool to room temperature, crush and grind to obtain solid waste-based sulfoaluminate cementitious material. The mass ratio of coal gangue powder, carbide slag powder, desulfurized gypsum powder and water is 1:(0.78-1.67):(0.33-0.83):(0.2-0.5).

4. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, The mass ratio of coarse aggregate, ungranulated aeolian sand, solid waste-based sulfoaluminate cementitious material, modified water-reducing agent, gypsum-bonded aeolian sand composite fine aggregate to water in S1 is 1: (0.25-0.35): (1.2-1.4): (0.01-0.02): (0.5-0.7): (0.5-0.7).

5. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, The mass ratio of the S11 hydroxyl-terminated hyperbranched polyester, pyridine, 4-dimethylaminopyridine, hydroquinone, and methacrylic anhydride solution is 1:(2-4):(0.01-0.03):(0.0005-0.0009):(0.2-0.3).

6. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, The mass ratio of methyl methacrylate polyoxyethylene ether, precursor monomer, deionized water and hydrogen peroxide aqueous solution in S12 is 1:(0.04-0.06):(2-3):(0.02-0.06).

7. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, The mass ratio of hydroxyethyl methacrylate, hydroquinone monomethyl ether, and phosphorus pentoxide in S13 is 1:(0.002-0.005):(0.5-0.6).

8. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 1, characterized in that, In S14, the mass ratio of acrylic acid, hydroxyethyl acrylate, mixture, 2-acrylamide-2-methylpropanesulfonic acid, methacryloyloxyethyltrimethylammonium chloride to deionized water is 1:(0.6-1.2):(0.2-0.4):(0.25-0.75):(0.2-0.4):(4-8), the mass ratio of L-ascorbic acid, mercaptoacetic acid to deionized water is 1:(2-5):(20-30), and the mass ratio of mixed solution, liquid A to liquid B is 1:(0.3-0.6):(0.1-0.2).

9. The method for preparing zero-shrinkage, micro-expansion solid waste concrete suitable for grassland sandy environments according to claim 2, characterized in that, The mass ratio of aeolian sand, β-type hemihydrate desulfurization gypsum and water in A1 is 1:(0.2-0.4):(0.2-0.4).

10. A zero-shrinkage, micro-expansion solid waste concrete suitable for grassland and sandy environments, characterized in that, Prepared by the method according to any one of claims 1-9.