A magnesium-silicon-based high-frequency ceramic material with a wide sintering temperature window, a preparation method and applications thereof
By introducing Ni²⁺ ions into magnesium-silicon-based ceramic materials and optimizing the sintering process, the problems of low quality factor and narrow sintering temperature were solved, achieving high dielectric properties and wide temperature range sintering in high-frequency communication systems.
Patent Information
- Application Number
- CN202611391171.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing magnesium-silicon-based ceramic materials suffer from insufficient quality factor and narrow sintering temperature range in high-frequency applications, which affects their application in 5G/6G communication and IoT devices.
By introducing an appropriate amount of Ni²⁺ ions into magnesium-silicon-based ceramic materials and combining solid-state reaction processes, the sintering process, including ball milling, pre-firing, granulation, and sintering, is optimized to broaden the sintering temperature window and improve dielectric properties.
It achieves high quality factor, high dielectric constant and wide temperature range sintering, improves the density and dielectric properties of ceramics, and is suitable for high frequency communication systems.
Smart Images

Figure CN123151679A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of microwave dielectric ceramic materials technology, specifically to a magnesium-silicon-based high-frequency ceramic material with a wide sintering temperature window, its preparation method, and its applications. Background Technology
[0002] Driven by the development of artificial intelligence and high-speed communication technologies, global wireless data transmission is experiencing explosive growth, propelling the rapid evolution of communication frequency bands towards centimeter-wave and millimeter-wave domains. This trend places more stringent performance requirements on microwave dielectric ceramic materials. Magnesium silicate ( Ceramics, due to their moderate dielectric constant and near-zero temperature coefficient, have become ideal candidate materials for high-frequency applications. However, this material faces two major technical bottlenecks: one is the quality factor (…). First, insufficient signal strength leads to significant signal loss; second, the narrow sintering temperature range severely impacts production yield and product consistency. These defects significantly restrict production. Applications of ceramics in high-end information circuits such as 5G / 6G communication and IoT devices.
[0003] To address this issue, there is an urgent need in this field to develop a novel magnesium-silicon-based ceramic that, while maintaining its existing advantages, also achieves high quality factor, high dielectric constant, and wide-temperature-range sintering properties to meet the pressing demands of future communication technologies for high-performance microwave ceramics.
[0004] The information disclosed in this background section is intended only to enhance the understanding of the overall background of the invention and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention
[0005] Purpose of the invention: The technical problem to be solved by the present invention is to address the shortcomings of the prior art by providing a magnesium-silicon-based high-frequency ceramic material with a wide sintering temperature window, its preparation method and application, while maintaining the original advantages, and simultaneously achieving high quality factor, high dielectric constant and wide temperature range sintering characteristics, so as to meet the urgent needs of future communication technologies for high-performance microwave ceramics.
[0006] To address the aforementioned technical problems, this invention discloses a magnesium-silicon-based high-frequency ceramic material with a wide sintering temperature window, the general formula of which is: ,in This indicates the A-site equivalent ion, selected as Ni, 0.02≤ ≤0.10.
[0007] Specifically, when When the dielectric constant is 0.06, the dielectric properties of the material are: =6.54, =62525GHz, =-22.9ppm / °C (13.109GHz).
[0008] The present invention also provides a method for preparing the magnesium-silicon-based high-frequency ceramic material according to claim 1, the method comprising the following steps:
[0009] Step a. Weighing: According to Weigh the magnesium source, silicon source, and A-site equivalent ion source after drying and pretreatment according to the nominal stoichiometry or non-stoichiometry of each cation element. Raw materials; the aforementioned Choose you;
[0010] Step b. Initial ball milling: Mix these raw materials with volatile ball milling media and grinding media and ball mill to achieve uniform mixing and obtain ball mill slurry;
[0011] Step c. Drying and sieving: The ball mill slurry is dried and sieved to obtain a uniform powder from which volatile ball milling media have been completely removed;
[0012] Step d. Pre-calcination: The sieved powder is pre-calcined to form the target phase or precursor phase;
[0013] Step e. Secondary ball milling: The pre-calcined material is crushed and ball-milled a second time to control the particle size distribution;
[0014] Step f. Granulation: Add the binder to the powder after secondary ball milling and granulate to obtain granulated powder;
[0015] Step g. Pressing and molding: Press the granulated powder into a raw blank;
[0016] Step h. Sintering: The green blank is sintered according to a temperature program that includes debinding and sintering sections to densify the green blank, and then slowly cooled to room temperature to obtain magnesium-silicon-based high-frequency ceramic material.
[0017] Specifically, the magnesium source is Silicon source is The raw material of the A-site equivalent ion source is the oxide corresponding to the A-site equivalent ion.
[0018] Specifically, in step a, 0.02 ≤ ≤0.10.
[0019] Specifically, in step b, the initial ball milling uses ethanol as the volatile ball milling medium and zirconia balls as the grinding media, with a mass ratio of raw material, zirconia balls and ethanol of 1:3:1.2.
[0020] Specifically, in step b, the ball mill speed for the initial ball milling is 300 r / min, and the ball milling time is 8 hours.
[0021] Specifically, in step c, the drying temperature is 80°C and the drying time is 24 hours.
[0022] Specifically, in step c, the sieve mesh size is 120 mesh.
[0023] Specifically, in step d, the preheating temperature is approximately 1300°C, and the holding time is 3 hours.
[0024] Specifically, in step e, the secondary ball milling uses deionized water as the volatile ball milling medium and zirconia balls as the grinding media, with a mass ratio of raw material, zirconia balls and deionized water of 1:4:1.
[0025] Specifically, in step e, the ball mill speed for the secondary ball mill is 300 r / min, and the ball milling time is 15–18 hours.
[0026] Specifically, in step e, the particle size distribution D50 of the powder after the secondary ball milling is 1.8μm-2.1μm.
[0027] Specifically, in step f, the adhesive is a PVA solution.
[0028] Specifically, the step h of sintering the green blank according to a temperature program including debinding and sintering sections includes the following process: the green blank is placed on fused magnesium powder, first heated to 600°C at 2°C / min and held for 2 hours to debind, then heated to the sintering temperature at a rate of 10°C / min to complete densification, and then slowly cooled to room temperature at a rate of 3°C / min.
[0029] Specifically, the sintering temperature range is 1410°C to 1480°C.
[0030] The present invention also discloses the aforementioned magnesium-silicon-based high-frequency ceramic material or the magnesium-silicon-based high-frequency ceramic material prepared by the aforementioned method as a dielectric material in high-frequency or microwave electronic systems.
[0031] Specifically, the high-frequency or microwave electronic system is a communication system, preferably a 5G mobile communication system.
[0032] Specifically, the dielectric material is used to manufacture at least one of a dielectric resonator, a dielectric filter, or an antenna substrate.
[0033] Specifically, the microwave frequency band is the millimeter wave frequency band above 24 GHz.
[0034] Beneficial effects:
[0035] Tradition Ceramics suffer from drawbacks such as poor sintering characteristics, low quality factor, and difficulty in eliminating secondary phases. Appropriate Ni...2+ Substitution can effectively eliminate at lower temperatures. Phase, suppressing monoclinic Phase formation effectively improved The sintering characteristics of ceramics significantly reduced the sintering temperature, decreased the distortion of the [Mg(2)O6] octahedron, and improved... Density and dielectric properties. (0.02≤ ≤0.1 ceramics at the corresponding optimal sintering temperature have a bulk density from The value of 2.8919 g / cm³ at =0 increased to The Ni concentration was 3.0392 g / cm³ at a value of 0.06, and the sintering temperature decreased by 20°C. With the increase of Ni... 2+ As the content increases, the lattice parameter decreases. When When = 0.06, the composition ( It exhibits the best dielectric properties: =6.54, =62525GHz, =-22.9ppm / °C (13.109GHz). Attached Figure Description
[0036] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, and the advantages of the present invention in the above and / or other aspects will become clearer.
[0037] Figure 1 The preparation process of magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window is disclosed in one embodiment of the present invention;
[0038] Figure 2 This is a schematic diagram of the sample XRD pattern disclosed in Embodiment 1 of the present invention.
[0039] Figure 3 This is a schematic diagram of the crystal structure after A-ion substitution disclosed in Example 1 of the present invention.
[0040] Figure 4 The embodiments 1-5 and Comparative Example 1 of the present invention are disclosed A schematic diagram showing the density changes at different sintering temperatures.
[0041] Figure 5 The embodiments 1-5 and Comparative Example 1 of the present invention are disclosed SEM images of samples at the optimal sintering temperature, where (a) Comparative Example 1; (b) Example 1; (c) Example 2; (d) Example 3; (e) Example 4; (f) Example 5.
[0042] Figure 6The embodiments 1-5 and Comparative Example 1 of the present invention are disclosed A schematic diagram showing the change in dielectric properties at different sintering temperatures, where (a) is the dielectric constant and (b) is the quality factor.
[0043] Figure 7 These are physical images of the ceramic materials prepared in Examples 1-5 and Comparative Example 1 of the present invention. Detailed Implementation
[0044] This invention relates to the field of functional ceramic materials technology, and discloses a magnesium-silicon-based high-frequency ceramic sintered over a wide temperature range and its preparation method. The method is based on a typical solid-state reaction process, firstly by drying and pretreating the raw materials, followed by sequential processes including ball milling, pre-firing, secondary ball milling, granulation, pressing, and sintering. Silicate ceramics. By controlling the particle size and magnesium-silicon stoichiometry of the pre-fired powder, the sintering behavior and microstructure of the ceramics were significantly optimized. Finally, using A-site equivalent ion substitution technology, ceramics with high density and excellent dielectric properties were successfully prepared. Ceramic-based materials.
[0045] The first aspect of the present invention provides a magnesium-silicon-based high-frequency ceramic material with a wide sintering temperature window, the general formula of which is: ,in Indicates the A-site equivalent ion and selects Ni, 0.02≤ ≤0.10.
[0046] In one embodiment, the ceramic material has a low dielectric constant and a near-zero temperature coefficient, when When = 0.06, the composition ( It exhibits the best dielectric properties: =6.54, =62525GHz, =-22.9ppm / °C (13.109GHz).
[0047] A second aspect of the present invention provides a method for preparing magnesium-silicon-based high-frequency ceramic materials having a wide sintering temperature window, comprising the following steps:
[0048] Step a. Weighing: According to The nominal stoichiometric ratios of each cation element in the sample were determined by weighing the dried pretreated magnesium source, silicon source, and A-site equivalent ion source. Raw materials; the aforementioned Ni was selected;
[0049] By pre-drying each raw material before weighing, the effects of moisture absorption by the raw materials can be avoided.
[0050] In a specific embodiment, a 0.0005g analytical balance can be used to weigh the sample, ensuring the weighing accuracy is controlled within ±0.0005g. Care should be taken to prevent cross-contamination during operation, and the sample should be sealed immediately after weighing.
[0051] Step b. Initial ball milling: Mix these raw materials with volatile ball milling media and grinding media and ball mill to achieve uniform mixing and obtain ball mill slurry;
[0052] In practice, the raw materials, volatile ball milling media, and grinding media are loaded into the ball mill jar together.
[0053] Step c. Drying and sieving: The ball mill slurry is dried and sieved to obtain a uniform powder from which volatile ball milling media have been completely removed;
[0054] Step d. Pre-calcination: The sieved powder is pre-calcined to form the target phase or precursor phase;
[0055] Step e. Secondary ball milling: The pre-calcined material is crushed and ball-milled a second time to control the particle size distribution;
[0056] Step f. Granulation: Mix the powder after secondary ball milling and the binder evenly and granulate to obtain granulated powder;
[0057] This step involves adding an appropriate amount of binder to the powder, mixing it thoroughly, and then sieving it to improve the powder's flowability and pressing performance.
[0058] Step g. Pressing and molding: Press the granulated powder into a raw blank;
[0059] Step h. Sintering: The green blank is sintered according to a temperature program that includes debinding and sintering sections to densify the green blank, and then slowly cooled to room temperature to obtain magnesium-silicon-based high-frequency ceramic material.
[0060] In one embodiment, the magnesium source is Silicon source is The raw material of the A-site equivalent ion source is the oxide corresponding to the A-site equivalent ion.
[0061] In one embodiment, in step a, 0.02 ≤ ≤0.10.
[0062] In one embodiment, the drying pretreatment step is to dry in a drying oven for 24 hours.
[0063] In one embodiment, in step b, the initial ball milling uses ethanol as the volatile milling medium and zirconia balls as the grinding media. The mass ratio of zirconium oxide spheres to ethanol is 1:3:1.2.
[0064] In one embodiment, in step b, the ball mill speed for the initial ball milling is 300 r / min, and the ball milling time is 8 hours.
[0065] In one embodiment, in step c, the drying temperature is 80°C and the drying time is 24 hours.
[0066] In one embodiment, in step c, the sieve mesh size is 120 mesh.
[0067] In one embodiment, in step d, the preheating temperature is approximately 1300°C, and the holding time is 3 hours.
[0068] In one embodiment, in step e, the secondary ball milling uses deionized water as the volatile milling medium and zirconia balls as the grinding media. The mass ratio of zirconium oxide balls to deionized water is 1:4:1.
[0069] In one embodiment, in step e, the ball mill speed of the secondary ball mill is 300 r / min, and the ball milling time is 15–18 hours.
[0070] In one embodiment, in step e, the particle size distribution D50 of the powder after secondary ball milling is 1.8 μm-2.1 μm.
[0071] In one embodiment, in step g, the pressed blank is a cylindrical blank with a diameter of 12mm × 6mm.
[0072] In one embodiment, in step g, pressure is maintained for about 1 minute, and castor oil is used for lubrication during demolding.
[0073] In one embodiment, in step f, the adhesive is a PVA solution.
[0074] In one embodiment, in step f, the amount of PVA solution added as the adhesive is 10%-12%.
[0075] In one embodiment, the step h of sintering the green blank according to a temperature program including debinding and sintering sections includes the following process: the green blank is placed on fused magnesium powder, first heated to 600°C at 2°C / min and held for 2 hours to debind, then heated to the sintering temperature at a rate of 10°C / min to complete densification, and then slowly cooled to room temperature at a rate of 3°C / min.
[0076] In one embodiment, the sintering temperature ranges from 1410°C to 1480°C.
[0077] A third aspect of the present invention provides a magnesium-silicon-based high-frequency ceramic material, or a magnesium-silicon-based high-frequency ceramic material prepared by the above-described preparation method, for use as a dielectric material in a high-frequency or microwave electronic system.
[0078] In one embodiment, the high-frequency or microwave electronic system is a communication system, preferably a 5G mobile communication system.
[0079] In one embodiment, the dielectric material is used to manufacture at least one of a dielectric resonator, a dielectric filter, or an antenna substrate.
[0080] In one embodiment, the microwave frequency band is a millimeter wave band above 24 GHz.
[0081] The present invention will be further illustrated by the following examples.
[0082] Example 1
[0083] This embodiment improves upon... The sintering characteristics of the material are improved, broadening the sintering window and enhancing the dielectric properties of the ceramic, thus providing a method for preparing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window. Its general formula is: ,in For Ni, =0.02.
[0084] The second aspect of this embodiment provides a method for preparing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window, comprising the following steps:
[0085] Step a. Weighing: Weigh the dried and pretreated magnesium source, silicon source, and A-site equivalent ion source according to the nominal or non-stoichiometric ratio of each cation element in the general formula of this embodiment. raw material;
[0086] In this embodiment, the Source is Silicon source is The A-site equivalent ion source raw material is In a specific embodiment, a 0.0005g analytical balance can be used to weigh the sample, ensuring the weighing accuracy is controlled within ±0.0005g. Care should be taken to prevent cross-contamination during operation, and the sample should be sealed immediately after weighing.
[0087] In this embodiment, the drying pretreatment step involves drying in a drying oven for 24 hours. By performing a drying pretreatment on each raw material before weighing, the effects of moisture absorption by the raw materials can be avoided.
[0088] Step b. Initial ball milling: Mix these raw materials with volatile ball milling media and grinding media and ball mill to achieve uniform mixing and obtain ball mill slurry;
[0089] In practice, the raw materials, volatile ball milling media, and grinding media are loaded into the ball mill jar together.
[0090] In this embodiment, in step b, the initial ball milling uses ethanol as the volatile ball milling medium and zirconia balls as the grinding media, with a mass ratio of raw material, zirconia balls and anhydrous ethanol of 1:3:1.2.
[0091] In this embodiment, in step b, the ball mill speed for the initial ball milling is 300 r / min, and the ball milling time is 8 hours.
[0092] Step c. Drying and sieving: The ball mill slurry is dried and sieved to obtain a uniform powder from which volatile ball milling media have been completely removed;
[0093] In this embodiment, in step c, the drying temperature is 80°C and the drying time is 24 hours.
[0094] In this embodiment, in step c, the sieve mesh size is 120 mesh.
[0095] Step d. Pre-calcination: The sieved powder is pre-calcined to form the target phase or precursor phase;
[0096] Step e. Secondary ball milling: The pre-calcined material is crushed and ball-milled a second time to control the particle size distribution;
[0097] In this embodiment, in step d, the preheating temperature is approximately 1300°C, and the holding time is 3 hours.
[0098] In this embodiment, in step e, the secondary ball milling uses deionized water as the volatile ball milling medium and zirconia balls as the grinding media, with a mass ratio of raw material, zirconia balls and deionized water of 1:4:1.
[0099] In this embodiment, in step e, the ball mill speed of the secondary ball mill is 300 r / min, and the ball milling time is 15–18 hours.
[0100] In this embodiment, in step e, the particle size distribution D50 of the powder after secondary ball milling is 2 μm.
[0101] Step f. Granulation: Add the binder to the powder after secondary ball milling and granulate to obtain granulated powder;
[0102] This step involves adding an appropriate amount of binder to the powder, mixing it thoroughly, and then sieving it to improve the powder's flowability and pressing performance.
[0103] In this embodiment, the adhesive in step f is a PVA solution.
[0104] Step g. Pressing and molding: Press the granulated powder into three identical preforms;
[0105] In this embodiment, the blank obtained by pressing in step g is a cylindrical blank with a diameter of 12mm × 6mm.
[0106] In this embodiment, in step g, the pressure is maintained for about 1 minute, and castor oil is used for lubrication during demolding.
[0107] Step h. Sintering: Each of the green blanks is sintered according to the corresponding temperature program including the debinding and sintering sections to densify the green blanks, and then slowly cooled to room temperature to obtain the corresponding magnesium-silicon-based high-frequency ceramic material.
[0108] In this embodiment, the three green blanks are placed on corresponding fused magnesium powder, heated to 600°C at 2°C / min and held for 2 hours to remove the binder, and then heated to 1410°C, 1430°C and 1450°C respectively at a relatively fast rate of 10°C / min to complete densification, and then slowly cooled to room temperature at a rate of 3°C / min to obtain the corresponding magnesium-silicon based high-frequency ceramic materials.
[0109] The third aspect of this embodiment provides a magnesium-silicon-based high-frequency ceramic material, or a magnesium-silicon-based high-frequency ceramic material prepared by the above-described preparation method, for use as a dielectric material in a high-frequency or microwave electronic system.
[0110] In this embodiment, the high-frequency or microwave electronic system is a communication system, preferably a 5G mobile communication system.
[0111] In this embodiment, the dielectric material is used to manufacture at least one of a dielectric resonator, a dielectric filter, or an antenna substrate.
[0112] In this embodiment, the microwave frequency band is a millimeter wave band above 24 GHz.
[0113] Example 2
[0114] This embodiment improves upon... The sintering characteristics of the material are improved, the sintering window is broadened, and the dielectric properties of the ceramic are enhanced. This provides a method for preparing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window. Compared with Example 1, the difference lies in... =0.04.
[0115] Example 3
[0116] This embodiment improves upon... The sintering characteristics of the material are improved, the sintering window is broadened, and the dielectric properties of the ceramic are enhanced. This provides a method for preparing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window. Compared with Example 1, the difference lies in... =0.06.
[0117] Example 4
[0118] This embodiment improves upon... The sintering characteristics of the material are improved, the sintering window is broadened, and the dielectric properties of the ceramic are enhanced. This provides a method for preparing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window. Compared with Example 1, the difference lies in... =0.08.
[0119] Example 5
[0120] This embodiment improves upon... The sintering characteristics of the material are improved, the sintering window is broadened, and the dielectric properties of the ceramic are enhanced. This provides a method for preparing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window. Compared with Example 1, the difference lies in... =0.1.
[0121] Comparative Example 1
[0122] According to the general formula: The raw materials were prepared with the same composition and content as in Example 1, except for the sintering temperature.
[0123] The differences between the above embodiments and comparative examples in terms of raw material formulation, sintering process parameters, and the properties of the resulting ceramic materials are detailed in Table 1. The performance parameters listed in Table 1 include bulk density and dielectric constant. Quality Factor Value and temperature coefficient of resonant frequency Among them, bulk density is used to evaluate the degree of densification of ceramic materials and reflects the effectiveness of the sintering process; dielectric constant... Used to characterize a material's ability to store electromagnetic energy; The value is used to characterize the dielectric loss characteristics of materials in the microwave frequency band. The higher the value, the lower the dielectric loss. The temperature stability of a material's resonant frequency is characterized by its absolute value being closer to zero, indicating better temperature stability. By comparing the performance data of each embodiment with those of the comparative example, it can be seen that this invention, through the equivalent substitution of A-site cations with Ni²⁺, can broaden the sintering temperature window of the material and synergistically improve the densification degree and microwave dielectric properties of the ceramic material.
[0124] Table 1. Raw material formulations, sintering process parameters, and properties of the resulting ceramic materials used in each embodiment of the present invention and Comparative Example 1.
[0125]
[0126] Table 2. Crystal structure data of ceramic samples sintered at the optimal sintering temperature for Examples 1-5 and Comparative Example 1.
[0127]
[0128] In this application, the optimal sintering temperature is used as the criterion for obtaining the optimal bulk density. Figure 4 As shown in Table 1, Example 1 was sintered at multiple temperatures in the range of 1410-1470℃. The sample sintered at 1450℃ had the highest bulk density, so 1450℃ was defined as the optimal sintering temperature for Example 1.
[0129] Table 3. Comparison of performance parameters of ceramic materials in Examples 1-5 and Comparative Example 1 at the optimal sintering temperature.
[0130]
[0131] Figure 2 Tables 1 and 3 present the XRD diffraction patterns, corresponding unit cell parameters, and phase composition data for each embodiment and comparative example that achieved the maximum bulk density at the corresponding sintering temperatures. (This is in conjunction with Table 1 and...) Figure 3 The main diffraction peaks of all samples are consistent with orthorhombic crystal forms. The standard card (PDF#11-0273) matched well, and a weak monoclinic crystal form was also observed in the sample. The diffraction peaks were observed, but no other possible additional phases were detected. etc., indicating that the substitution amount is between 0.02 and 0.1. The system formed a solid solution, i.e., substitution was successful. A schematic diagram of the solid solution crystal is shown below. Figure 3 As shown, the strongest peak (121) shows a shift towards a higher angle. According to Bragg's equation, the peak shift is mainly attributed to the change in their interplanar spacing d, and changes in crystal often lead to changes in dielectric properties.
[0132] Figure 4 The relationship between bulk density and sintering temperature for each embodiment and comparative example is presented. It can be seen that the curves for each embodiment are significantly flatter than those for the comparative example, representing the relationship between Ni and... 2+ It has greatly expanded The sintering window of ceramics.
[0133] Figure 5 SEM images of the ceramic samples from various embodiments and comparative examples at the optimal sintering temperature are presented. The sample of Comparative Example 1 exhibits poor grain continuity and intergranular gaps. All samples with added Ni... 2+ The sample from the examples exhibited well-developed grains and the absence of obvious second phases or atmospheric pores, resulting in good density data. This indicates that the introduction of Ni ions can promote ion diffusion and grain boundary migration, enabling grain growth to fill interstitial spaces and thus improving the density of the ceramic.
[0134] Figure 6 The relationships between dielectric properties and sintering temperature are presented for each embodiment and comparative example. Figure 6 , Figure 6 As can be seen from Table 1, each embodiment The trend of value change and The trends are similar. As the sintering temperature increases, the samples of each component gradually become denser. With the increase in relative density, the ceramic grains grow uniformly to fill the pores. At this stage, densification has a significant impact on… The increase in value played a dominant role. The decline was caused by the monoclinic effect of over-sintering. This is caused by the combined effects of decreased density and grain boundary deterioration in Ni. 2+ The quality factor of the replaced samples was improved when When =0.06, Value from The quality factor increased from 24505 (when =0) to 62525. This increase is due to Ni. 2+ The relative density of the substituted sample increased, the average grain size increased, and the grain boundaries and porosity decreased, resulting in a reduction in defects. Monoclinic The presence of phases in ceramics It can also have negative effects, as shown in Table 2. 2+ Monoclinic degradation was suppressed by both lowering the sintering temperature and enhancing crystal stability. The generation of the phase reduces the monoclinic relatively ceramics Interference from Ni. 2+ The content continues to increase. The value did not continue to increase, when When it exceeds 0.06, the material The values show a decreasing trend. Observation of SEM images reveals that the inhomogeneity of grain size and the lattice distortion caused by the formation of abnormal grains may be the cause. The reason for the drop in value is that the sintering temperature of the undoped Ni comparative example 1 was too high (≥1450°C), and the relative density was too low (≤92.3%). The value is significantly low (≤30000GHz). The deviation from zero is relatively large (≤-24.2ppm / °C). However, the embodiments of this invention can significantly improve the density of the samples relative to the comparative examples within a wide temperature range of 1410–1470°C, and exhibit excellent dielectric properties. When = 0.06, the composition ( It exhibits excellent dielectric properties at microwave frequencies. =6.54, =62525GHz, =-22.9ppm / °C (13.109GHz). This indicates that Ni ion A-site substitution significantly optimizes sintering behavior and microwave dielectric properties. Figure 7 The lower group of products are cylindrical products obtained from the above embodiments and comparative examples, while the upper group is another product obtained from embodiments 1 to 5 using a rectangular mold.
[0135] This invention provides ideas and methods for developing magnesium-silicon-based high-frequency ceramic materials with a wide sintering temperature window, their preparation methods, and applications. Many methods and approaches exist for implementing this technical solution; the above description is merely a preferred embodiment of the invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications should also be considered within the scope of protection of this invention. All components not explicitly stated in this embodiment can be implemented using existing technologies.
Claims
1. A magnesium-silicon-based high-frequency ceramic material with a wide sintering temperature window, characterized in that, Its general formula is: ,in This indicates the A-site equivalent ion, selected as Ni, 0.02≤ ≤0.
10.
2. The magnesium-silicon-based high-frequency ceramic material according to claim 1, characterized in that, when When the dielectric constant is 0.06, the dielectric properties of the material are: =6.54, =62525GHz, =-22.9ppm / °C (13.109GHz).
3. A method for preparing the magnesium-silicon-based high-frequency ceramic material according to claim 1, characterized in that, Includes the following steps: Step a. Weighing: According to Weigh the magnesium source, silicon source, and A-site equivalent ion source after drying and pretreatment according to the nominal stoichiometry or non-stoichiometry of each cation element. Raw materials; the aforementioned Choose you; Step b. Initial ball milling: Mix these raw materials with volatile ball milling media and grinding media and ball mill to achieve uniform mixing and obtain ball mill slurry; Step c. Drying and sieving: The ball mill slurry is dried and sieved to obtain a uniform powder from which volatile ball milling media have been completely removed; Step d. Pre-calcination: The sieved powder is pre-calcined to form the target phase or precursor phase; Step e. Secondary ball milling: The pre-calcined material is crushed and ball-milled a second time to control the particle size distribution; Step f. Granulation: Add the binder to the powder after secondary ball milling and granulate to obtain granulated powder; Step g. Pressing and molding: Press the granulated powder into a raw blank; Step h. Sintering: The green blank is sintered according to a temperature program that includes debinding and sintering sections to densify the green blank, and then slowly cooled to room temperature to obtain magnesium-silicon-based high-frequency ceramic material.
4. The method according to claim 3, characterized in that, The magnesium source is Silicon source is The raw material of the A-site equivalent ion source is the oxide corresponding to the A-site equivalent ion.
5. The method according to claim 3, characterized in that, In step a, 0.02 ≤ ≤0.
10.
6. The method according to claim 3, characterized in that, In step b, the initial ball milling uses ethanol as the volatile ball milling medium and zirconia balls as the grinding media, with a mass ratio of raw material, zirconia balls and ethanol of 1:3:1.
2.
7. The method according to claim 3, characterized in that, In step b, the initial ball mill rotation speed is 300 r / min, and the ball milling time is 8 hours. In step c, the drying temperature is 80℃ and the drying time is 24 hours; in step c, the sieve mesh size is 120 mesh. In step d, the pre-firing temperature is approximately 1300°C, and the holding time is 3 hours. In step e, the secondary ball milling uses deionized water as the volatile ball milling medium and zirconia balls as the grinding media, with a mass ratio of raw material, zirconia balls and deionized water of 1:4:
1. The particle size distribution D50 of the powder after the secondary ball milling is 1.8μm-2.1μm.
8. The method according to claim 3, characterized in that, The step h, sintering the green blank according to a temperature program that includes a debinding and sintering section, includes the following process: The green blank is placed on fused magnesium powder, heated to 600°C at 2°C / min and held for 2 hours to remove the binder, then heated to the sintering temperature at 10°C / min to complete densification, and then slowly cooled to room temperature at 3°C / min. The sintering temperature range is 1410℃ to 1480℃.
9. The magnesium-silicon-based high-frequency ceramic material according to claim 1 or 2, or the magnesium-silicon-based high-frequency ceramic material prepared by the method according to any one of claims 3 to 8, is used as a dielectric material in a high-frequency or microwave electronic system, characterized in that... The dielectric material is used to manufacture at least one of a dielectric resonator, a dielectric filter, or an antenna substrate, and the high-frequency or microwave electronic system is a communication system, preferably a 5G mobile communication system.
10. The use according to claim 9, characterized in that, The microwave frequency band is the millimeter wave band above 24 GHz.