A highly stable BaTiO3-based ceramic capacitor dielectric material and its preparation method
By using Ti-site Ca-doped BaTiO₃-based ceramic capacitor dielectric materials, combined with MgO, Re₂O₃, and MO sintering aids, the dielectric properties and reduction resistance characteristics are optimized, solving the stability and reliability problems of BaTiO₃-based dielectric materials under high temperature and high pressure environments, and realizing ceramic capacitor dielectric materials with high dielectric constant and wide temperature range.
Patent Information
- Application Number
- CN202510663521.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing BaTiO₃-based dielectric materials suffer from problems such as reduced dielectric constant, poor DC bias stability, and insufficient resistance to reduction in terms of high specific capacitance, wide temperature range, and high reliability, making it difficult to meet the requirements for long-term stable operation under high temperature and high pressure environments.
By employing non-stoichiometric control of Ti-site Ca-doped BaTiO₃ as the main component, combined with MgO, Re₂O₃ and MO sintering aids, and through specific heat treatment and sintering processes, the dielectric properties and reduction resistance are optimized to form an inverted core-shell structure, thereby improving the material's high dielectric constant, DC bias stability and temperature stability.
A highly stable BaTiO₃-based ceramic capacitor dielectric material with a dielectric constant higher than 1500, dielectric loss lower than 0.01, excellent DC bias stability, and good resistance to reduction was achieved under the X7R standard, making it suitable for long-term stable operation under high temperature and high pressure environments.
Smart Images

Figure CN123151684A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electronic ceramic materials technology, specifically relating to a highly stable BaTiO3-based ceramic capacitor dielectric material and its preparation method. Background Technology
[0002] Multilayer ceramic capacitors (MLCCs) are key components in electronic circuits, widely used in cutting-edge fields such as 5G / 6G communications, advanced weaponry, artificial intelligence, and new energy vehicles. With the rapid development of smart hardware, autonomous driving, and high-frequency communications, MLCCs are being continuously optimized for higher specific capacitance, wider temperature range, and higher reliability. Taking automotive MLCCs as an example, they need to operate stably for extended periods under extreme environments such as high temperature and high voltage, which places higher demands on their dielectric materials, including high dielectric constant, excellent DC bias stability, wide temperature range stability, and long-term reliability.
[0003] High-specific-capacitance MLCCs typically employ BaTiO3-based type II dielectric ceramics, with their high specific capacity primarily achieved by reducing the dielectric layer thickness and increasing the number of dielectric layers. However, as the thickness decreases, the dielectric layer must withstand a higher operating electric field, leading to a significant reduction in the dielectric constant. This results in the effective capacitance of the MLCC being far below its nominal capacitance, causing challenges in MLCC selection and application. To improve the DC bias stability of BaTiO3-based dielectric materials, various material modification methods have been proposed, such as reducing grain size, optimizing the core-shell structure using chemical methods, and elemental doping. While these methods can improve DC bias stability, they typically significantly reduce the dielectric constant, leading to a decrease in capacitance density. Using materials with different crystal structures, such as tungsten bronze, can improve DC bias stability, but this results in a lower initial dielectric constant, leading to a still low absolute value of the dielectric constant. Using bismuth- or lead-containing material systems presents challenges such as difficulty in co-firing with base metal electrodes (e.g., nickel), a narrow range of optimal sintering conditions, and easy evaporation during sintering, leading to significant fluctuations in sintering and electrical properties, and substantial differences in characteristics between individual materials.
[0004] Besides bias stability and dielectric constant, temperature stability is another crucial performance characteristic of MLCCs during long-term service. Traditional MLCC dielectric materials control their dielectric temperature profiles by constructing a "core-shell" structure, typically using BaTiO3 as the core (determining the dielectric properties at high temperatures) and alkaline earth oxides, rare earth oxides, and sintering aids reacting with BaTiO3 as the shell (affecting the dielectric properties at low temperatures). However, the strong ferroelectric core results in relatively poor dielectric bias stability. Furthermore, to match the current mainstream nickel metal internal electrode co-firing process, MLCC dielectric materials are also required to possess excellent reduction resistance under reducing atmosphere sintering conditions. Summary of the Invention
[0005] To address the aforementioned technical problems, the present invention aims to provide a highly stable BaTiO3-based ceramic capacitor dielectric material and its preparation method that possesses high dielectric constant, high DC bias stability, good anti-reduction properties, and meets the X7R standard.
[0006] In a first aspect, the present invention provides a highly stable BaTiO3-based ceramic capacitor dielectric material, wherein the chemical formula of the highly stable BaTiO3-based ceramic capacitor dielectric material is 100BaTi 1-x Ca x O 3-x -yBaTiO3-zMgO-mRe2O3-nMO, where Re2O3 is a rare earth oxide and MO is a sintering aid; wherein BaTi 1-x Ca x O 3-x The main component is BaTiO3, with BaTiO3, MgO, and Re2O3 as secondary components.
[0007] Preferably, Re2O3 includes at least one of Dy2O3, Y2O3, Yb2O3, and Ho2O3, and MO includes at least one of SiO2, Al2O3, MnO2, ZrO2, TiO2, and WO3.
[0008] Preferably, the value of y is in the range of 10 to 70 and not 10, and more preferably 20 to 50; the value of z is in the range of 0 to 8, and more preferably 3 to 6; the value of m is in the range of 0 to 10; and the value of n is in the range of 0.2 to 7.
[0009] Preferably, the BaTi 1-x Ca x O 3-x In this process, the molar ratio of Ba, Ti, and Ca satisfies Ba / (Ti+Ca)=1, and the Ca doping amount x satisfies 0.02<x≤0.06, preferably 0.04≤x≤0.05.
[0010] Secondly, the present invention provides a method for preparing the above-mentioned highly stable BaTiO3-based ceramic capacitor dielectric material, the preparation method comprising the following steps: (1) The raw materials BaCO3, TiO2, and CaCO3 were weighed and mixed according to the stoichiometric ratio, and then calcined and ground to obtain the main component BaTi. 1-x Ca x O 3-x ; (2) BaTiO3, MgO and Re2O3 are mixed in proportion and subjected to heat treatment to obtain the by-products; (3) Weigh the main component, secondary component and sintering aid MO according to the proportion, mix them and then form and sinter them to obtain the high-stability BaTiO3-based ceramic capacitor dielectric material.
[0011] Preferably, in step (1), the calcination temperature is 1100-1300℃ and the time is 2-4h.
[0012] Preferably, in step (2), the temperature of the heat treatment is 500-1000℃ and the holding time is 1-4h.
[0013] Preferably, in step (3), the sintering temperature is 1150-1350℃, more preferably 1200-1300℃, and the holding time is 1min-3h; preferably, the sintering atmosphere is air, nitrogen atmosphere or reducing atmosphere, wherein the reducing atmosphere is a nitrogen-hydrogen mixture.
[0014] Beneficial effects This invention uses a Ca-doped BaTiO3-based material at Ti sites as the main component, controlled by non-stoichiometric regulation, and a mixture of BaTiO3, MgO, and Re2O3 as the secondary component. The reaction and densification of the main and secondary components are controlled by selecting appropriate additives, heat treatment methods, and sintering regimes. As a result, while the dielectric properties of the dielectric ceramic meet the requirements of X7R, its dielectric constant and DC bias stability are synergistically optimized. This preparation method provides a new process route for designing highly stable ceramic capacitor dielectric materials. Attached Figure Description
[0015] Figure 1 , 2 These are schematic diagrams of a traditional core-shell structure for dielectric materials and a reverse core-shell structure for the dielectric material of this invention, respectively. Detailed Implementation
[0016] The present invention will be further illustrated by the following embodiments. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the present invention.
[0017] First, this invention provides a highly stable BaTiO3-based ceramic capacitor dielectric material. The chemical formula of the highly stable BaTiO3-based ceramic capacitor dielectric material can be 100BaTi 1-x Ca x O 3-x -yBaTiO3-zMgO-mRe2O3-nMO, where Re2O3 may include at least one rare earth oxide such as Dy2O3, Y2O3, Yb2O3, Ho2O3, etc., and MO may include at least one rare earth oxide such as SiO2, Al2O3, MnO2, ZrO2, TiO2, WO3; wherein, BaTi 1-x Ca x O 3-x The main component is BaTiO3, MgO, and Re2O3, which are secondary components, and MO is a firing aid component.
[0018] The dielectric material provided by this invention features Ca substitution at Ti sites in its main component, unlike conventional materials where Ca substitutes at Ba sites. The different substitution positions of Ca have a significant impact on its dielectric properties. This invention promotes Ca substitution at Ti sites through stoichiometric control, thereby improving the dielectric constant at low temperatures, as well as its bias stability and reduction resistance. In this invention, MgO, Re₂O₃, and MO primarily function to regulate the degree of reaction between the main and secondary components, rather than reacting with BaTiO₃ to form a shell.
[0019] In some implementations, the value of y can be 10 to 70 and not 10, preferably 20 to 50; the value of z can be 0 to 8, preferably 3 to 6; the value of m can be 0 to 10; and the value of n can be 0.2 to 7.
[0020] Inappropriate BaTiO3 content can affect the overall high-temperature stability of the material. Low MgO content can hinder the formation of the core-shell structure, while excessive MgO content can impair the compactness of the dielectric ceramic. Re2O3 is expensive, and high content will increase costs. Insufficient MO content will lead to excessively high sintering temperatures, while excessive MO content will affect the formation of the core-shell structure.
[0021] In some implementations, the BaTi 1-x Ca x O 3-x In this mixture, the molar ratio of Ba, Ti, and Ca can satisfy Ba / (Ti+Ca)=1, and the Ca doping amount x can satisfy 0.02<x≤0.06, preferably 0.04≤x≤0.05; BaTi 1- x Ca x O 3-x The particle size of the powder can be ≤500nm, preferably <300nm.
[0022] Because the ionic radii of Ca and Ti differ significantly, stoichiometric control is needed to induce Ca substitution at Ti sites. If Ba / (Ti+Ca) < 1, additional Ti vacancies will be generated while inducing Ca substitution, potentially leading to decreased material reliability. Furthermore, Ca substitution at Ti sites introduces additional oxygen vacancies. During sintering in a reducing atmosphere, these oxygen vacancies can reduce electronic conductivity, giving the dielectric material good resistance to reduction.
[0023] At the same time, too low a Ca doping level will lead to an excessively high Curie temperature, while too high a doping level will exceed the solid solution limit, resulting in the appearance of a second phase.
[0024] In some embodiments, the particle size of the BaTiO3 powder can be 50–300 nm, preferably 50–200 nm. BaTiO3 is mainly used to improve the dielectric constant at high temperatures, thereby optimizing the overall temperature stability of the material and ensuring that its capacitance change rate is within ±15% in the range of -55 to 125°C.
[0025] In some embodiments, the particle size of the MgO can be 50–500 nm, preferably 50–100 nm. Adding MgO can suppress grain growth, broaden the temperature profile, and improve temperature stability.
[0026] In some embodiments, the particle size of the Re2O3 can be 50–500 nm, preferably 50–100 nm. The particle size of BaTi can be controlled by adding rare earth elements. 1-x Ca x O 3-x The reaction rate with BaTiO3 was increased, and the dielectric temperature curve was further broadened.
[0027] In some embodiments, the particle size of the MO can be 30–500 nm, preferably 50–100 nm. The addition of the sintering aid MO helps to lower the sintering temperature and further broaden the dielectric temperature profile.
[0028] In some embodiments, the dielectric material of the high-stability BaTiO3-based ceramic capacitor meets the X7R standard (capacitance temperature coefficient TCC = ±15% (-55~125℃)), the dielectric constant at room temperature (25℃) can be >1500, the dielectric loss at room temperature (25℃) can be <0.01, and the absolute value of dielectric compatibility under a 25kV / cm DC bias electric field is <10%.
[0029] Figure 1 , 2 The figures show schematic diagrams of a traditional core-shell dielectric material and the reverse core-shell structure of the dielectric material of this invention. As can be seen from the figures, the traditional core-shell structure uses BaTiO3 as the core (possessing a high dielectric constant at high temperatures), and a solid solution formed by the reaction of rare earth elements with BaTiO3 as the shell (enhancing the dielectric constant at low temperatures). This invention uses Ti-site Ca-doped BaTiO3 as the main component (possessing a high dielectric constant at low temperatures), and pre-heat-treated BaTiO3, Re2O3, and MgO materials as secondary components (possessing high dielectric constants at high temperatures). The combination of the main and secondary components improves temperature stability. Because the Ti-site Ca-doped BaTiO3 material has good reduction resistance and DC bias stability, its reaction with the high Curie temperature secondary components achieves synergistic optimization of dielectric constant, DC bias stability, temperature stability, and reduction resistance.
[0030] The following is an exemplary description of a method for preparing the highly stable BaTiO3-based ceramic capacitor dielectric material provided by the present invention. The preparation method may include the following steps: (1) The raw materials BaCO3, TiO2, and CaCO3 were weighed and mixed according to the stoichiometric ratio, and then calcined and ground to obtain the main component BaTi. 1-x Ca x O 3-x ; (2) BaTiO3, MgO and Re2O3 are mixed in proportion and subjected to heat treatment to obtain the by-products; (3) Weigh the main component, secondary component and sintering aid MO according to the proportion, mix them and then form and sinter them to obtain the high-stability BaTiO3-based ceramic capacitor dielectric material.
[0031] In some embodiments, in step (1), the calcination temperature can be 1100–1300°C, and the time can be 2–4 hours. If the calcination temperature is too low, some Ca ions will replace Ba sites; if the calcination temperature is too high, the reactivity of the main component will be reduced, which is not conducive to the densification of the ceramic.
[0032] It should be noted that, due to the significant difference in ionic radii between Ca and Ti, Ca has a higher capacity to enter Ba sites than Ti sites. This invention effectively promotes Ca ion entry into Ti sites by controlling the stoichiometry and calcination temperature. This pretreatment process promotes Ca substitution at Ti sites, thereby affecting the performance of the main component.
[0033] In some embodiments, in step (1), the grinding method may include planetary grinding, sand grinding, or stirring grinding; the grinding medium may be anhydrous ethanol; and the grinding time may be 30 min to 24 h.
[0034] In some embodiments, in step (2), the heat treatment temperature can be 500–1000°C, and the holding time can be 1–4 hours. Heat treatment can promote the reaction of some Re2O3 or MgO+Re2O3 with BaTiO3, thereby affecting the reaction rates of the main and secondary components, and thus achieving control over the overall temperature stability. Excessive heat treatment temperature reduces the subsequent reaction activity of the mixed powder and affects its high-temperature dielectric properties.
[0035] In some embodiments, in step (3), the sintering temperature can be 1150–1350°C, preferably 1200–1300°C, the holding time is 1 min–3 h, and the sintering atmosphere can be air, nitrogen, or a reducing atmosphere. The reducing atmosphere can be a nitrogen-hydrogen mixture (hydrogen / hydrogen volume ratio of 3%–10%). If the sintering temperature is too low, the ceramic cannot be densified; if the sintering temperature is too high, it will lead to abnormal grain growth and is not conducive to further co-firing with the base metal electrode.
[0036] Traditional preparation methods typically involve reacting rare earth elements with BaTiO3 to form a core-shell structure, thereby optimizing overall temperature stability. In this reaction, shell formation and core shrinkage occur simultaneously, and the dielectric constants at high and low temperatures also influence each other. This invention primarily employs a composite of Ti-doped Ca-coated BaTiO3 material with a high dielectric constant at low temperatures and BaTiO3 material with a high dielectric constant at high temperatures to improve temperature stability. This method allows for separate control of the dielectric constants at high and low temperatures; furthermore, the Ca doping at the Ti sites enhances resistance to reduction and bias voltage stability.
[0037] The preparation method provided by this invention achieves synergistic optimization of the dielectric constant, DC bias stability, temperature stability, and reduction resistance of the dielectric material. By controlling the stoichiometry and preparation process, Ca is encouraged to enter the Ti sites. The reaction rate and extent of the main and secondary components are controlled through pretreatment and sintering processes, ultimately producing a dielectric material with high stability, high dielectric constant, and reduction resistance under both DC bias and temperature fields. As a result, while meeting the X7R dielectric properties, the DC bias stability and reduction resistance of the dielectric ceramic are significantly improved.
[0038] The following examples further illustrate the present invention in detail. It should also be understood that the following examples are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make appropriate selections within the range based on the description herein, and are not intended to be limited to the specific values in the examples below. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.
[0039] Example 1
[0040] The method for preparing the highly stable BaTiO3-based ceramic capacitor dielectric material provided in this embodiment includes the following steps: (1) The raw materials BaCO3, TiO2, and CaCO3 are mixed according to the stoichiometric ratio BaTi 0.96Ca 0.04 O 2.96 (BTC4) was weighed and mixed, and then ground for 6 hours using a wet process. After drying at 80°C, it was sieved to obtain a uniformly mixed powder material. The uniformly mixed powder material was calcined in air at 1200°C for 2 hours. The calcined powder was then ground again for 6 hours to obtain the main component BTC4. (2) Weigh a certain amount of each raw material in the proportion of 30 mol BaTiO3, 2.4 mol Y2O3 and 5.6 mol MgO. The particle size of BaTiO3 is 200 nm. Wet grinding is carried out for 6 h. After drying at 80 °C, the powder material is sieved to obtain a uniformly mixed powder material. The powder is heat-treated in air at 800 °C for 2 h to obtain the secondary component 30BT-2.4Y-5.6Mg. (3) Weigh out each raw material in the following proportions: 100 mol of main component BTC4, 30 mol of BaTiO3, 2.4 mol of Y2O3, 5.6 mol of MgO, 2 mol of sintering aid SiO2, and 0.1 mol of sintering aid MnO2. Grind and mix thoroughly for 6 hours. Dry the uniformly mixed powder material at 80°C and shape it. Sinter it in air at 1275°C for 2 hours to obtain the high-stability BaTiO3-based ceramic capacitor dielectric material, denoted as 100BTC4-30BT-2.4Y-5.6Mg-2Si-0.1Mn.
[0041] Example 2
[0042] The preparation method of the highly stable BaTiO3-based ceramic capacitor dielectric material provided in this embodiment is the same as that in Example 1, with the main difference being: In step (1), the raw materials BaCO3, TiO2, and CaCO3 are mixed according to the stoichiometric ratio BaTi 0.956 Ca 0.044 O 2.956 (BTC4.4) Weigh and mix; In step (2), a certain amount of each raw material is weighed in the proportion of 30 mol BaTiO3, 2.4 mol Y2O3 and 3.8 mol MgO. The powder obtained after mixing is heat-treated in air at 800℃ for 2 hours. The secondary component is denoted as 30BT-2.4Y-3.8Mg. In step (3), each raw material is weighed in the proportion of 100 mol BTC4.4, 30 mol BaTiO3, 2.4 mol Y2O3 and 3.8 mol MgO and 2 mol SiO2 as the sintering aid. The sintering temperature is 1275℃ and the holding time is 2 hours in air. The high-stability BaTiO3-based ceramic capacitor dielectric material obtained is denoted as 100BTC4.4-30BT-2.4Y-3.8Mg-2Si.
[0043] Example 3
[0044] The preparation method of the highly stable BaTiO3-based ceramic capacitor dielectric material provided in this embodiment is the same as that in Example 1, with the main difference being: In step (1), the raw materials BaCO3, TiO2, and CaCO3 are mixed according to the stoichiometric ratio BaTi 0.956 Ca 0.044 O 2.956 (BTC4.4) Weigh and mix; In step (2), a certain amount of each raw material is weighed in the proportion of 30 mol BaTiO3, 1.8 mol Y2O3, 1.8 mol Yb2O3 and 3.8 mol MgO. The particle size of BaTiO3 is 150 nm. The resulting byproduct is recorded as 30BT-1.8Y-1.8Yb-3.8Mg. In step (3), each raw material is weighed in the following proportions: 100 mol of main component BTC4.4, 30 mol of secondary components BaTiO3, 1.8 mol of Y2O3, 1.8 mol of Yb2O3, 3.8 mol of MgO, and 2 mol of sintering aid SiO2. The sintering temperature is 1275℃ and the holding time is 2h under air atmosphere. The resulting high-stability BaTiO3-based ceramic capacitor dielectric material is denoted as 100BTC4.4-30BT-1.8Y-1.8Yb-3.8Mg-2Si.
[0045] Example 4
[0046] The preparation method of the highly stable BaTiO3-based ceramic capacitor dielectric material provided in this embodiment is the same as that in Example 1, with the main difference being: In step (3), after the powder material is formed, it is sintered in a mixed atmosphere of 4% hydrogen / nitrogen by volume, the sintering temperature is 1280℃, and the holding time is 1h. The resulting high-stability BaTiO3-based ceramic capacitor dielectric material is denoted as N2-100BTC4-30BT-2.4Y-5.6Mg-2Si-0.1Mn.
[0047] Example 5
[0048] The preparation method of the highly stable BaTiO3-based ceramic capacitor dielectric material provided in this embodiment is the same as in Embodiment 2, with the main difference being: In step (3), after the powder material is formed, it is sintered in a mixed atmosphere of 4% hydrogen / nitrogen by volume, the sintering temperature is 1280℃, and the holding time is 1h. The resulting high-stability BaTiO3-based ceramic capacitor dielectric material is denoted as N2-100BTC4.4-30BT-2.4Y-3.8Mg-2Si.
[0049] Comparative Example 1
[0050] The method for preparing the ceramic dielectric material provided in this comparative example includes the following steps: The raw materials BaCO3, TiO2, and CaCO3 are mixed according to the stoichiometric ratio BaTi 0.956 Ca 0.044 O 2.956 (BTC4.4) Weigh and mix, then grind using a wet process for 6 hours. After drying at 80°C, sieve to obtain a uniformly mixed powder material. Calcinate the mixed powder in air at 1200°C for 2 hours. Grind the calcined powder a second time for 6 hours, dry at 80°C, and sieve to obtain a uniformly mixed powder material. Press into shape and sinter in air at 1325°C for 2 hours to obtain the ceramic dielectric material, denoted as BTC4.4.
[0051] Comparative Example 2
[0052] The method for preparing the ceramic dielectric material provided in this comparative example includes the following steps: A certain amount of each raw material was weighed in the proportion of 30 mol BaTiO3, 2.4 mol Y2O3, and 5.6 mol MgO. The BaTiO3 particle size was 200 nm. The raw materials were wet-milled by planetary milling for 6 hours, dried at 80°C, and sieved to obtain a uniformly mixed powder material. The powder was then heat-treated in air at 800°C for 2 hours. The powder was then thoroughly mixed by planetary milling for 6 hours, dried at 80°C, and then shaped. Finally, it was sintered in air at 1325°C for 2 hours to obtain the ceramic dielectric material, denoted as 30BT-2.4Y-5.6Mg.
[0053] Comparative Example 3
[0054] The method for preparing the ceramic dielectric material provided in this comparative example includes the following steps: (1) The raw materials BaCO3, TiO2, and CaCO3 are mixed according to the stoichiometric ratio BaTi 0.956 Ca 0.044 O 2.956 (BTC4.4) was weighed and mixed, and then planetarily ground for 6 hours using a wet process. After drying at 80°C, it was sieved to obtain a uniformly mixed powder material. The mixed powder was calcined in air at 1200°C for 2 hours. The calcined powder was then subjected to a second planetary grinding for 6 hours to obtain the main component BTC4.4. (2) Weigh out each raw material in the proportion of 100 mol of main component BTC4.4, 30 mol of secondary component BaTiO3 with a particle size of 200 nm, and 2 mol of sintering aid component SiO2. Mix thoroughly by planetary milling for 6 h, dry the uniformly mixed powder material at 80 °C and shape it. Sinter at 1275 °C for 2 h in air atmosphere to obtain ceramic dielectric material, denoted as 100BTC4.4-30BT-2Si.
[0055] Comparative Example 4
[0056] The method for preparing the ceramic dielectric material provided in this comparative example includes the following steps: Raw materials BaCO3 and TiO2 were weighed according to a stoichiometric ratio of 1:1, and then wet-milled planetarily for 6 hours. After drying at 80°C, the mixture was sieved to obtain a uniformly mixed powder. The uniformly mixed powder was calcined in air at 1200°C for 2 hours. The calcined powder was then milled a second time for 6 hours, dried at 80°C, and sieved to obtain a uniformly mixed powder. The powder was then pressed into shape and sintered in air at 1325°C for 2 hours to obtain the ceramic dielectric material, denoted as BaTiO3.
[0057] Comparative Example 5
[0058] The preparation method of the ceramic dielectric material provided in this comparative example is the same as that in Comparative Example 2, with the main difference being: The sintering atmosphere was a 4% hydrogen / nitrogen mixture, and the resulting ceramic dielectric material was designated as N2-30BT-2.4Y-5.6Mg.
[0059] Comparative Example 6
[0060] The preparation method of the ceramic dielectric material provided in this comparative example is the same as that in Example 2, with the main difference being: In step (3), each raw material is weighed with the following proportions: 100 mol of main component BTC4.4, 10 mol of secondary component BaTiO3, 2.4 mol of Y2O3, 3.8 mol of MgO, and 2 mol of sintering aid component SiO2. The sintering temperature is 1275℃ and the holding time is 2h under air atmosphere. The resulting BaTiO3-based ceramic capacitor dielectric material is denoted as 100BTC4.4-10BT-2.4Y-3.8Mg-2Si.
[0061] Comparative Example 7
[0062] The preparation method of the ceramic dielectric material provided in this comparative example is the same as that in Example 2, with the main difference being: In step (2), a certain amount of each raw material is weighed in the proportion of 30 mol BaTiO3, 2.4 mol Y2O3 and 10 mol MgO. The powder obtained after mixing is heat-treated in air at 800℃ for 2 hours. The resulting secondary component is denoted as 30BT-2.4Y-10Mg. In step (3), each raw material is weighed in the proportion of 100 mol BTC4.4, 30 mol BaTiO3, 2.4 mol Y2O3 and 10 mol MgO, and 2 mol SiO2 as the sintering aid. The sintering temperature is 1275℃ and the holding time is 2 hours in air. The resulting BaTiO3-based ceramic capacitor dielectric material is denoted as 100BTC4.4-30BT-2.4Y-10Mg-2Si.
[0063] Comparative Example 8
[0064] The preparation method of the ceramic dielectric material provided in this comparative example is the same as that in Example 1, with the main difference being: In step (3), the sintering temperature is 1400℃ and the holding time is 2h.
[0065] Comparative Example 9
[0066] The preparation method of the ceramic dielectric material provided in this comparative example is the same as that in Example 1, with the main difference being: In step (1), the raw materials BaCO3, TiO2, and CaCO3 are mixed according to the stoichiometric ratio BaTi 0.98 Ca 0.02 O 2.98 (BTC2) Weigh and mix; finally obtain BaTiO3-based ceramic capacitor dielectric material, denoted as 100BTC2-30BT-2.4Y-5.6Mg-2Si-0.1Mn.
[0067] Table 1 below compares the performance of the ceramic capacitor dielectric materials prepared in Examples 1-5 and Comparative Examples 1-9:
[0068] As shown in the table, Examples 1-5 all meet the X7R material requirements, with a room temperature dielectric constant greater than 1500 and a dielectric loss less than 0.008. Compared to Comparative Examples 1-5, temperature stability is significantly improved; at a DC bias electric field of 25kV / vm, the absolute value of dielectric adjustability in Examples 1-5 is less than 10%. Compared to Comparative Examples 1-5, DC bias stability is significantly improved; Examples 4-5 exhibit good resistance to reduction compared to Comparative Example 5. Comparative Examples 6 and 7 demonstrate that a suitable proportion of secondary components is necessary for the overall material performance to meet the X7R standard. Comparative Example 8 shows that excessively high sintering temperatures are detrimental to the formation of core-shell structures and thus hinder the improvement of temperature stability. Comparative Example 9 shows that a low Ca doping content in the main component is detrimental to the improvement of temperature stability.
[0069] Although the present invention has been described in detail through the preferred embodiments above, it should be understood that the above description should not be considered as a limitation of the present invention. Various modifications and substitutions to the present invention will be apparent to those skilled in the art after reading the above description. Therefore, the scope of protection of the present invention should be defined by the appended claims.
Claims
1. A highly stable BaTiO3-based ceramic capacitor dielectric material, characterized in that, The chemical formula of the high-stability BaTiO3-based ceramic capacitor dielectric material is 100BaTi 1-x Ca x O 3-x -yBaTiO3-zMgO-mRe2O3-nMO, where Re2O3 is a rare earth oxide and MO is a sintering aid; wherein BaTi 1-x Ca x O 3-x The main component is BaTiO3, with BaTiO3, MgO, and Re2O3 as secondary components.
2. The high-stability BaTiO3-based ceramic capacitor dielectric material according to claim 1, characterized in that, Re2O3 includes at least one of Dy2O3, Y2O3, Yb2O3, and Ho2O3, and MO includes at least one of SiO2, Al2O3, MnO2, ZrO2, TiO2, and WO3.
3. The highly stable BaTiO3-based ceramic capacitor dielectric material according to claim 1 or 2, characterized in that, The value of y is in the range of 10 to 70 and is not 10, preferably 20 to 50; the value of z is in the range of 0 to 8, preferably 3 to 6; the value of m is in the range of 0 to 10; and the value of n is in the range of 0.2 to 7.
4. The high-stability BaTiO3-based ceramic capacitor dielectric material according to any one of claims 1-3, characterized in that, The BaTi 1-x Ca x O 3-x In this process, the molar ratio of Ba, Ti, and Ca satisfies Ba / (Ti+Ca)=1, and the Ca doping amount x satisfies 0.02<x≤0.06, preferably 0.04≤x≤0.
05.
5. A method for preparing a highly stable BaTiO3-based ceramic capacitor dielectric material according to any one of claims 1-4, characterized in that, The preparation method includes the following steps: (1) The raw materials BaCO3, TiO2, and CaCO3 were weighed and mixed according to the stoichiometric ratio, and then calcined and ground to obtain the main component BaTi. 1-x Ca x O 3-x ; (2) BaTiO3, MgO and Re2O3 are mixed in proportion and subjected to heat treatment to obtain the by-products; (3) Weigh the main component, secondary component and sintering aid MO according to the proportion, mix them and then form and sinter them to obtain the high-stability BaTiO3-based ceramic capacitor dielectric material.
6. The preparation method according to claim 5, characterized in that, In step (1), the calcination temperature is 1100-1300℃ and the time is 2-4h.
7. The preparation method according to claim 5 or 6, characterized in that, In step (2), the heat treatment temperature is 500-1000℃ and the holding time is 1-4h.
8. The preparation method according to any one of claims 5-7, characterized in that, In step (3), the sintering temperature is 1150-1350℃, preferably 1200-1300℃, and the holding time is 1min-3h; preferably, the sintering atmosphere is air, nitrogen atmosphere or reducing atmosphere, and the reducing atmosphere is a nitrogen-hydrogen mixture.