A bismuth magnesium niobate doped with bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material and a preparation method thereof
By introducing bismuth magnesium niobate into the bismuth scandate-lead titanate system, high-temperature piezoelectric ceramics doped with bismuth magnesium niobate were prepared, solving the problem of insufficient piezoelectric performance of lead zirconate titanate-based ceramics under high-temperature conditions. This achieved a combination of high piezoelectric performance and high Curie temperature, making it suitable for high-temperature transducers and sensors.
Patent Information
- Application Number
- CN202611344043.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lead zirconate titanate-based piezoelectric ceramics have insufficient piezoelectric properties at high temperatures, making it difficult to meet the application requirements of high-temperature transducers and sensors.
Bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramics were developed by introducing bismuth magnesium niobate into the bismuth scandate-lead titanate system, controlling the composition and optimizing the preparation process, including steps such as ball milling, drying, calcination, cold isostatic pressing and sintering, to form bismuth magnesium niobate-doped ternary high-temperature piezoelectric ceramics.
It achieves high piezoelectric performance with a piezoelectric coefficient of 570pC/N at 430℃, while also having a high Curie temperature, low material cost, simple and easy process, and good product repeatability.
Smart Images

Figure CN123151685A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of piezoelectric ceramics technology, and in particular to a bismuth magnesium niobate-doped bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material and its preparation method. Background Technology
[0002] Piezoelectric ceramics are functional materials capable of exchanging electrical and mechanical energy. Due to their excellent electromechanical coupling effect and large-scale fabrication capabilities, they are widely used in sensors, actuators, and transducers. With the rapid development of industries such as aerospace, automotive, and energy exploration, higher demands are being placed on piezoelectric ceramics in high-tech applications, requiring them to meet the needs of high-temperature environments. Therefore, researching and preparing high-performance high-temperature piezoelectric ceramic materials helps promote technological and industrial upgrading and aligns with key national strategic development directions.
[0003] Traditional commercial lead zirconate titanate (PZT)-based piezoelectric ceramics have limited applications in high-temperature fields due to their relatively low operating temperature, generally not exceeding 300℃. In recent years, researchers both domestically and internationally have discovered that the bismuth scandate-lead titanate (BiScO3-PbTiO3) system possesses both a high Curie temperature (450℃) and a high piezoelectric coefficient (460 pC / N) at the quasi-isomorphic phase boundary (x=0.64). Therefore, BiScO3-PbTiO3 piezoelectric ceramics are considered one of the most competitive high-temperature piezoelectric ceramic materials in the 200–400℃ temperature range. However, in practical applications, it has been found that further optimization of the piezoelectric properties of this system is needed to meet the requirements of high-temperature transducers and sensors.
[0004] Therefore, developing a novel doping system that can significantly enhance piezoelectric properties while maintaining a high Curie temperature is of great scientific and engineering significance for promoting the practical application of high-temperature piezoelectric ceramics. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material and its preparation method. The ternary bismuth scandate-lead titanate-bismuth magnesium niobate high-temperature piezoelectric ceramic of this invention exhibits a piezoelectric coefficient di at a Curie temperature of 430°C. 33 It can reach 570pC / N, while achieving both high Curie temperature and high voltage performance.
[0006] The technical solution of the present invention is as follows: The first aspect of this invention protects a bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material, wherein the general formula of the high-temperature piezoelectric ceramic material is: 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg 2 / 3 Nb 1 / 3)O3, Where: 0.00 < x ≤ 0.07.
[0007] The second aspect of this invention protects a method for preparing the high-temperature piezoelectric ceramic material described in the first aspect, comprising the following steps: S1: Weigh Bi₂O₃, Sc₂O₃, PbO, TiO₂, MgO, and Nb₂O₅ according to stoichiometric ratio, mix them to obtain a mixture, ball mill, dry, and calcine to obtain 0.36BiScO₃-(0.64-x)PbTiO₃-xBi(Mg 2 / 3 Nb 1 / 3 )O3 powder; S2: 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg) from S1 2 / 3 Nb 1 / 3 O3 powder is subjected to secondary ball milling and drying to obtain powder material; S3: Add binder to the powder in S2, grind and then form a blank to obtain a blank; S4: After debinding and cold isostatic pressing of the blank from S3, sintering is performed to obtain the bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material.
[0008] Preferably, in S1, the mass ratio of the mixture, grinding balls, and milling media is 1:5:2; The ball mill rotates at a speed of 300-400 r / min; and / or, The ball milling time is 12-24 hours.
[0009] Preferably, in S1, the drying temperature is 100~120℃, and / or, The drying time is 4 to 6 hours.
[0010] Preferably, in S1, the calcination is carried out by heating at 3~5℃ / min and then holding at that temperature; Preferably, the calcination is carried out by heating to 700-800°C at a rate of 3-5°C / min and then holding at that temperature; More preferably, the heat preservation time is 4 to 6 hours.
[0011] Preferably, in S2, during the secondary ball milling, the 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg) 2 / 3 Nb 1 / 3 The mass ratio of O3 powder, grinding balls and milling media is 1:5:2; The ball mill rotates at a speed of 300-400 r / min; and / or, The ball milling time is 12-24 hours; The drying temperature is 100~120℃, and / or, The drying time is 4 to 6 hours.
[0012] Preferably, in step S3, the mass ratio of the powder to the binder is 10:1; The adhesive comprises an aqueous solution of polyvinyl alcohol; Preferably, the mass concentration of the polyvinyl alcohol aqueous solution is 5-10%.
[0013] Preferably, in S3, the blank preparation is achieved by pressing and holding pressure; Preferably, the pressing pressure is 8~10MPa, and the holding time is 1~3min.
[0014] Preferably, in step S4, the temperature of the glue discharge is 500~600℃, the heating rate is 1~3℃ / min, and the holding time is 4~6h.
[0015] Preferably, in step S4, the pressure of the cold isostatic pressing is 100~120MPa, and the holding time is 10~30min; The sintering temperature is 1000~1200℃, the heating rate is 3~5℃ / min, and the holding time is 2~4h.
[0016] The beneficial technical effects of this invention are as follows: This invention uses a binary bismuth scandate-lead titanate matrix as the substrate and introduces a third component, bismuth magnesium niobate, to obtain a bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material. Specifically, the A-site is composed of Bi... 3+ For Pb 2+ Donor substitution, in order to maintain electroneutrality, creates cation vacancies in the material. The presence of cation vacancies disrupts the original periodic arrangement of the crystal, resulting in a reduction in domain size. Smaller domains are more prone to movement and rearrangement under an external electric field, which helps to enhance the intrinsic piezoelectric contribution. The B site is composed of two anisovalent ions, Mg... 2+ 、Nb 5+ For Ti 4+ Substitution and the construction of locally non-uniform structures also contribute to the improvement of piezoelectric properties. This third-component doping strategy fully leverages the advantages of the A and B sites, achieving a significant improvement in piezoelectric activity and providing a novel approach and method for preparing high-performance high-temperature piezoelectric ceramics.
[0017] This invention improves the piezoelectric coefficient of the prepared piezoelectric ceramics through component control and process optimization. d 33 It can reach 570 pC / N and Curie temperature 430℃. At the same time, the piezoelectric ceramic of the present invention uses low-cost raw materials, and the process steps are simple, easy to operate, have good repeatability, and high yield. Attached Figure Description
[0018] Figure 1 The X-ray diffraction patterns are shown for the ceramic materials prepared in the embodiments and comparative examples of this invention.
[0019] In the figure: (a) is the X-ray diffraction pattern tested at room temperature, with a test range of 20°~80°, and (b) is a magnified view of a local area within the range of 44°~46°.
[0020] Figure 2 The diagram shows the piezoelectric coefficients of the ceramic materials prepared in the embodiments and comparative examples of this invention.
[0021] Figure 3 The dielectric temperature spectrum of the ceramic materials prepared in the embodiments and comparative examples of the present invention is shown. Detailed Implementation
[0022] The present invention will now be described in detail with reference to the embodiments.
[0023] To address the problem that existing high-temperature piezoelectric ceramics cannot meet the requirements of high-voltage piezoelectric applications, this invention proposes a bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material and its preparation method to solve the above problems.
[0024] The first aspect of this invention provides a bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material, wherein the general formula of the high-temperature piezoelectric ceramic is: 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg 2 / 3 Nb 1 / 3 O3, Where: 0.00 < x ≤ 0.07.
[0025] It is understood that this invention dops bismuth magnesium niobate into a bismuth scandate-lead titanate system and controls the doping ratio of bismuth magnesium niobate to obtain a ternary bismuth scandate-lead titanate-bismuth magnesium niobate high-temperature piezoelectric ceramic with superior overall performance. The piezoelectric coefficient of the prepared piezoelectric ceramic is... d 33 At a temperature of 430℃, the Curie temperature reaches 570pC / N, exhibiting superior overall performance.
[0026] Understandably, bismuth magnesium niobate, compared to other tertiary components, has the advantage of significantly improving piezoelectric properties while maintaining a high Curie temperature, thus enabling it to... d 33 , T C A good balance is achieved among multiple parameters; when bismuth magnesium niobate is not doped, its high energy barrier results in a high piezoelectric coefficient. d 33The optimal value cannot be achieved; when the doping amount of bismuth magnesium niobate is too large, the internal lattice is excessively distorted, the internal stress increases, and the material structure deviates from the optimal quasi-isomorphic phase boundary MPB state, thus its overall performance will decrease.
[0027] The second aspect of this invention provides a method for preparing the bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material described in the first aspect above, comprising the following steps: S1: 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg) 2 / 3 Nb 1 / 3 The stoichiometric ratio of O3 (where 0.00 < x ≤ 0.07) was determined by weighing Bi2O3, Sc2O3, PbO, TiO2, MgO, and Nb2O5. The raw materials were then mixed to obtain a mixture, ball milling media were added, and the mixture was dried and calcined to obtain 0.36BiScO3-(0.64-x)PbTiO3-xBi(MgO) 2 / 3 Nb 1 / 3 )O3 powder; S2: The 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg) prepared in S1 2 / 3 Nb 1 / 3 The O3 powder was ball-milled again and dried to obtain the powder. S3: Add binder to the powder in S2, grind thoroughly, and then form a blank to obtain a green body; S4: After removing the binder from the blank of S3, a dense blank is obtained by cold isostatic pressing. The blank is placed in a sealed crucible, covered with the powder prepared in S2, and then sintered to obtain a ternary bismuth scandate-lead titanate-bismuth magnesium niobate high-temperature piezoelectric ceramic, that is, bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material.
[0028] In some implementations, in steps S1 and S2, the ball milling process satisfies at least one of the following conditions: (1) The mass ratio of the grinding media to the grinding media is 1:5:2; (2) The rotation speed of the ball mill is 300~400 r / min; (3) The ball milling time is 12~24h.
[0029] The ball milling speed includes, but is not limited to, 300 r / min, 350 r / min, and 400 r / min; the ball milling time includes, but is not limited to, 12 h, 18 h, and 24 h.
[0030] It is understood that the ball milling conditions in steps S1 and S2 may be the same or different. The ball milling media include, but are not limited to, alcohol. This invention does not limit the type of grinding ball; any grinding ball capable of achieving the objectives of this invention is within the scope of protection of this invention.
[0031] In some embodiments, in steps S1 and S2, the drying temperature is 100~120℃, including but not limited to 100℃, 110℃, and 120℃; and / or, the drying time is 4~6h, including but not limited to 4h, 5h, and 6h.
[0032] In some embodiments, in step S1, the calcination is performed by heating at 3~5℃ / min and then holding at that temperature.
[0033] In some embodiments, the calcination involves heating to 700-800°C at a rate of 3-5°C / min and then holding at that temperature. The heating rate includes, but is not limited to, 3°C / min, 4°C / min, and 5°C / min; the heating temperature includes, but is not limited to, 700°C, 750°C, and 800°C.
[0034] In some embodiments, the heat preservation time is 4 to 6 hours, including but not limited to 4 hours, 5 hours, and 6 hours.
[0035] In some embodiments, in step S3, the adhesive comprises an aqueous solution of polyvinyl alcohol.
[0036] In some embodiments, the mass concentration of the polyvinyl alcohol aqueous solution is 5-10%, including but not limited to 5%, 8%, and 10%.
[0037] In some implementations, step S3 involves pressing and holding the blank during the blanking process.
[0038] In some embodiments, the pressing pressure is 8~10MPa, including but not limited to 8MPa, 9MPa, and 10MPa; the holding time is 1~3min, including but not limited to 1min, 2min, and 3min.
[0039] In some embodiments, in step S4, the temperature of the adhesive discharge is 500~600℃, including but not limited to 500℃, 550℃, and 600℃; the heating rate is 1~3℃ / min, including but not limited to 1℃ / min, 2℃ / min, and 3℃ / min; and the heat preservation time is 4~6h, including but not limited to 4h, 5h, and 6h.
[0040] Understandably, excessively high debinding temperatures can lead to significant thermal stress within and on the surface of the green body due to temperature gradients. Because organic matter rapidly volatilizes and decomposes at high temperatures, the excessively rapid gas expulsion from the green body, if not evenly diffused in time, creates a pressure difference, causing deformation such as bending and twisting. Conversely, excessively low debinding temperatures prevent the organic binder and other organic materials from fully decomposing and volatilizing, leaving residues in the green body. These residues form pores during subsequent sintering, reducing the ceramic's density. Low-density piezoelectric ceramics exhibit weak grain bonding, affecting charge transfer and polarization, thus reducing piezoelectric properties.
[0041] In some embodiments, in step S4, the pressure of cold isostatic pressing is 100~120MPa, including but not limited to 100MPa, 110MPa, and 120MPa; and the holding time is 10~30min, including but not limited to 10min, 20min, and 30min.
[0042] In step S4, the green body is placed in a sealed crucible and covered with the same composition powder prepared in S2 for sintering. This helps to form a relatively stable local sintering atmosphere around the green body, reduces the loss of volatile components such as Bi and Pb during high-temperature sintering, thereby reducing the stoichiometric deviation caused by volatilization, which helps to maintain the stability of the target composition and phase structure, and reduces the risk of local composition inhomogeneity and the formation of a second phase.
[0043] In some embodiments, in step S4, the sintering temperature is 1000~1200℃, including but not limited to 1000℃, 1100℃, and 1200℃; the heating rate is 3~5℃ / min, including but not limited to 3℃ / min, 4℃ / min, and 5℃ / min; and the holding time is 2~4h, including but not limited to 2h, 3h, and 4h.
[0044] For the introduction of Bi(Mg) in this invention 2 / 3 Nb 1 / 3For bismuth scandate-lead titanate-based ceramics with O3 as the tertiary component, the tertiary component needs to diffuse sufficiently and dissolve as uniformly as possible during calcination and sintering, while maintaining relative stability of the local composition and defect state at the A / B sites. Therefore, if the sintering temperature is too low, the diffusion and solid-state reaction of Bi, Mg, and Nb components may be insufficient, easily leading to inhomogeneity in local composition and grain size, and increasing the risk of residual second phase, which is detrimental to densification and piezoelectric response. If the sintering temperature is too high, it may exacerbate the volatilization of Bi / Pb-containing components, changes in defect concentration, and abnormal grain growth or local compositional segregation, causing the phase structure and defect state to deviate from the range favorable to piezoelectric response. If the heating rate is too fast, densification, grain growth, and the diffusion process of the tertiary component are difficult to coordinate sufficiently, easily forming temperature gradients and inhomogeneity in local composition; if the heating rate is too slow, it will prolong the high-temperature exposure time, increasing the risk of volatilization and grain coarsening. Therefore, controlling the sintering temperature and heating rate within the range defined by this invention is beneficial to obtaining a more uniform solid solution state, microstructure and phase structure, thereby maintaining better piezoelectric properties.
[0045] The present invention will be further described below through examples and other means.
[0046] Example 1 (x = 0.01) A bismuth magnesium niobate-doped bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material with the chemical formula 0.36BiScO3-0.63PbTiO3-0.01Bi(Mg) 2 / 3 Nb 1 / 3 O3, its preparation method includes the following steps: S1: According to 0.36BiScO3-0.63PbTiO3-0.01Bi(Mg) 2 / 3 Nb 1 / 3 Based on the stoichiometric ratio of O3, weigh all raw materials, mix with alcohol, ball mill for 24 hours, dry in an oven at 100℃ for 4 hours, then calcine at 700℃ with a heating rate of 3℃ / min for 4 hours to obtain 0.36BiScO3-0.63PbTiO3-0.01Bi(Mg) 2 / 3 Nb 1 / 3 O3 powder. The raw materials include Bi2O3, Sc2O3, PbO, TiO2, MgO, and Nb2O5.
[0047] S2: The 0.36BiScO3-0.63PbTiO3-0.01Bi(Mg)O3 obtained in step S1 is... 2 / 3 Nb 1 / 3 O3 powder was ball-milled twice for 12 hours and dried in an oven at 100°C for 4 hours to obtain powder.
[0048] In steps S1 and S2, the ball milling conditions are as follows: the mass ratio of ball milling powder, grinding balls and alcohol is 1:5:2, and the rotation speed of the ball mill is 300 r / min.
[0049] S3: Add a 7wt% polyvinyl alcohol aqueous solution to the powder obtained in step S2, grind thoroughly, and then press into a blank; wherein, the mass ratio of powder to polyvinyl alcohol aqueous solution is 10:1, the pressing pressure is 10MPa, and the holding time is 1min.
[0050] S4: After removing the binder from the green body, cold isostatic pressing is performed to obtain a dense green body. The dense green body is placed in a sealed crucible, and the green body is covered with the powder prepared in step S2 and then sintered to obtain the ternary bismuth scandate-lead titanate-bismuth magnesium niobate high temperature piezoelectric ceramic.
[0051] The debinding temperature was 600℃, the heating rate was 2℃ / min, and the holding time was 4h. The cold isostatic pressing pressure was 120MPa, and the holding time was 30min. The sintering temperature was 1000℃, the heating rate was 5℃ / min, and the holding time was 2h.
[0052] Example 2 (x = 0.03) A bismuth magnesium niobate-doped bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material with the chemical formula 0.36BiScO3-0.61PbTiO3-0.03Bi(Mg) 2 / 3 Nb 1 / 3 O3, its preparation method includes the following steps: S1: According to 0.36BiScO3-0.61PbTiO3-0.03Bi(Mg) 2 / 3 Nb 1 / 3 Based on the stoichiometric ratio of O3, weigh all raw materials, mix with alcohol, ball mill for 24 hours, dry in an oven at 100℃ for 4 hours, then heat to 700℃ at a rate of 3℃ / min and hold for 4 hours to complete calcination, yielding 0.36BiScO3-0.61PbTiO3-0.03Bi(Mg) 2 / 3 Nb 1 / 3 O3 powder; wherein the raw materials include Bi2O3, Sc2O3, PbO, TiO2, MgO, and Nb2O5.
[0053] S2: The 0.36BiScO3-0.61PbTiO3-0.03Bi(Mg)O3 obtained in step S1 2 / 3 Nb 1 / 3 O3 powder was ball-milled twice for 12 hours and dried in an oven at 100°C for 4 hours to obtain powder.
[0054] In steps S1 and S2, the ball milling conditions are as follows: the mass ratio of ball milling powder, grinding balls and alcohol is 1:5:2, and the rotation speed of the ball mill is 300 r / min.
[0055] S3: Add a 7wt% polyvinyl alcohol aqueous solution to the powder obtained in step S2, grind thoroughly, and press into a blank. The mass ratio of powder to polyvinyl alcohol aqueous solution is 10:1, the pressing pressure is 10MPa, and the holding time is 1min.
[0056] S4: After removing the binder from the green body, cold isostatic pressing is performed to obtain a dense green body; the dense green body is placed in a sealed crucible, and the green body is covered with the powder prepared in step S2 and then sintered to obtain the ternary bismuth scandate-lead titanate-bismuth magnesium niobate high temperature piezoelectric ceramic.
[0057] The debinding temperature was 600℃, the heating rate was 2℃ / min, and the holding time was 4h. The cold isostatic pressing pressure was 120MPa, and the holding time was 30min. The sintering temperature was 1000℃, the heating rate was 5℃ / min, and the holding time was 2h.
[0058] Example 3 (x = 0.05) A bismuth magnesium niobate-doped bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material with the chemical formula 0.36BiScO3-0.59PbTiO3-0.05Bi(Mg) 2 / 3 Nb 1 / 3 O3, its preparation method includes the following steps: S1: According to 0.36BiScO3-0.59PbTiO3-0.05Bi(Mg) 2 / 3 Nb 1 / 3 Based on the stoichiometric ratio of O3, weigh all raw materials, mix with alcohol, ball mill for 24 hours, dry in an oven at 100℃ for 4 hours, then calcine at 700℃ with a heating rate of 3℃ / min for 4 hours to obtain 0.36BiScO3-0.59PbTiO3-0.05Bi(Mg) 2 / 3 Nb 1 / 3 O3 powder. The raw materials include Bi2O3, Sc2O3, PbO, TiO2, MgO, and Nb2O5.
[0059] S2: The 0.36BiScO3-0.59PbTiO3-0.05Bi(Mg)O3 obtained in step S1 2 / 3 Nb 1 / 3 O3 powder was ball-milled twice for 12 hours and dried in an oven at 100°C for 4 hours to obtain powder.
[0060] In steps S1 and S2, the ball milling conditions are as follows: the mass ratio of ball milling powder, grinding balls and alcohol is 1:5:2, and the rotation speed of the ball mill is 300 r / min.
[0061] S3: Add a 7wt% polyvinyl alcohol aqueous solution to the powder obtained in step S2, grind thoroughly, and then press into a blank; wherein, the mass ratio of powder to polyvinyl alcohol aqueous solution is 10:1, the pressing pressure is 10MPa, and the holding time is 1min.
[0062] S4: After removing the binder from the green body, cold isostatic pressing is performed to obtain a dense green body. The dense green body is placed in a sealed crucible, and the green body is covered with the powder prepared in step S2 and then sintered to obtain the ternary bismuth scandate-lead titanate-bismuth magnesium niobate high temperature piezoelectric ceramic.
[0063] The debinding temperature was 600℃, the heating rate was 2℃ / min, and the holding time was 4h. The cold isostatic pressing pressure was 120MPa, and the holding time was 30min. The sintering temperature was 1000℃, the heating rate was 5℃ / min, and the holding time was 2h.
[0064] Example 4 (x = 0.07) A bismuth magnesium niobate-doped bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material with the chemical formula 0.36BiScO3-0.57PbTiO3-0.07Bi(Mg) 2 / 3 Nb 1 / 3 O3, its preparation method includes the following steps: S1: According to 0.36BiScO3-0.57PbTiO3-0.07Bi(Mg) 2 / 3 Nb 1 / 3 Based on the stoichiometric ratio of O3, weigh all raw materials, mix with alcohol, ball mill for 24 hours, dry in an oven at 100℃ for 4 hours, then calcine at 700℃ with a heating rate of 3℃ / min for 4 hours to obtain 0.36BiScO3-0.57PbTiO3-0.07Bi(Mg) 2 / 3 Nb 1 / 3 O3 powder. The raw materials include Bi2O3, Sc2O3, PbO, TiO2, MgO, and Nb2O5.
[0065] S2: The 0.36BiScO3-0.57PbTiO3-0.07Bi(Mg)O3 obtained in step S1 2 / 3 Nb 1 / 3 O3 powder was ball-milled twice for 12 hours and dried in an oven at 100°C for 4 hours to obtain powder.
[0066] In steps S1 and S2, the ball milling conditions are as follows: the mass ratio of ball milling powder, grinding balls and alcohol is 1:5:2, and the rotation speed of the ball mill is 300 r / min.
[0067] S3: Add a 7wt% polyvinyl alcohol aqueous solution to the powder obtained in step S2, grind thoroughly, and then press into a blank; wherein, the mass ratio of powder to polyvinyl alcohol aqueous solution is 10:1, the pressing pressure is 10MPa, and the holding time is 1min.
[0068] S4: After removing the binder from the green body, cold isostatic pressing is performed to obtain a dense green body. The dense green body is placed in a sealed crucible, and the green body is covered with the powder prepared in step S2 and then sintered to obtain the ternary bismuth scandate-lead titanate-bismuth magnesium niobate high temperature piezoelectric ceramic.
[0069] The debinding temperature was 600℃, the heating rate was 2℃ / min, and the holding time was 4h. The cold isostatic pressing pressure was 120MPa, and the holding time was 30min. The sintering temperature was 1000℃, the heating rate was 5℃ / min, and the holding time was 2h.
[0070] Comparative Example 1 (x=0) A bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material, with the chemical formula 0.36BiScO3-0.64PbTiO3, is prepared by the following steps: S1: Weigh the raw materials according to the stoichiometric ratio of 0.36BiScO3-0.64PbTiO3, mix with alcohol, ball mill for 24 hours, dry in an oven at 100℃ for 4 hours, then calcine at 700℃ with a heating rate of 3℃ / min for 4 hours to obtain 0.36BiScO3-0.64PbTiO3 powder. The raw materials include Bi2O3, Sc2O3, PbO, and TiO2.
[0071] S2: The 0.36BiScO3-0.64PbTiO3 powder obtained in step S1 is ball-milled twice for 12 hours and dried in an oven at 100℃ for 4 hours to obtain the powder.
[0072] In steps S1 and S2, the ball milling conditions are as follows: the mass ratio of ball milling powder, grinding balls and alcohol is 1:5:2, and the rotation speed of the ball mill is 300 r / min.
[0073] S3: Add a 7wt% polyvinyl alcohol aqueous solution to the powder obtained in step S2, grind thoroughly, and then press into a blank; wherein, the mass ratio of powder to polyvinyl alcohol aqueous solution is 10:1, the pressing pressure is 10MPa, and the holding time is 1min.
[0074] S4: After removing the binder from the green body, cold isostatic pressing is performed to obtain a dense green body. The dense green body is placed in a sealed crucible, and the green body is covered with the powder prepared in step S2 and then sintered to obtain the binary bismuth scandate-lead titanate high-temperature piezoelectric ceramic.
[0075] The debinding temperature was 600℃, the heating rate was 2℃ / min, and the holding time was 4h. The cold isostatic pressing pressure was 120MPa, and the holding time was 30min. The sintering temperature was 1000℃, the heating rate was 5℃ / min, and the holding time was 2h.
[0076] Test example: The piezoelectric ceramics prepared in the above examples and comparative examples were polished, electrode-attached, and polarized. The polarization electric field was 40~60kV / cm, the polarization time was 30min, and the polarization temperature was 120℃. The piezoelectric properties of each product were measured, and the results are shown in Table 1.
[0077] Table 1 Performance tests of piezoelectric ceramics prepared in the examples and comparative examples
[0078] As can be seen from Table 1, the piezoelectric coefficient of the piezoelectric material prepared through doping in the examples varies with Bi(Mg) 2 / 3 Nb 1 / 3 The doping concentration of O3 initially increases and then decreases with increasing doping concentration, while the Curie temperature gradually decreases with increasing doping concentration. When Bi(Mg) 2 / 3Nb 1 / 3 When the O3 doping amount was increased to 0.03 (Example 2), the overall performance reached its optimal level, with a piezoelectric coefficient of 570 pC / N (approximately 30% higher than Comparative Example 1) and a Curie temperature of 430°C, which is beneficial for high-temperature applications. With the increase of Bi(Mg) doping... 2 / 3 Nb 1 / 3 As the O3 content further increases to x=0.07, the system evolves from a favorable R / T two-phase coexistence region to a trigonal phase region, gradually deviating from the quasi-isomorphic phase boundary region with higher structural responsiveness. Therefore, its piezoelectric coefficient decreases from 570 pC / N in the optimal composition (x=0.03) to 450 pC / N. Simultaneously, with the increase of Bi(Mg) content... 2 / 3 Nb 1 / 3 With the increase of O3 content, the Curie temperature further decreased to 383℃. These results indicate that Bi(Mg) 2 / 3 Nb 1 / 3 There is a suitable range for the addition of O3, with x=0.03 exhibiting the best overall performance.
[0079] Figure 1The X-ray diffraction patterns of the ceramic materials prepared in the embodiments and comparative examples of this invention are shown. The test range is 20°~80°, where x=0.01 corresponds to Example 1, x=0.03 corresponds to Example 2, x=0.05 corresponds to Example 3, x=0.07 corresponds to Example 4, and x=0.00 corresponds to Example 1. As can be seen from the figure, undoped Bi(Mg) 2 / 3 Nb 1 / 3 Comparative Example 1 of O3 exhibits a distinct bimodal characteristic near 45°, indicating that its crystal structure is mainly tetragonal and relatively stable, thus resulting in a relatively low piezoelectric response. With the increase of Bi(Mg) 2 / 3 Nb 1 / 3 The introduction of O3 caused the diffraction peaks near 45° to gradually evolve from bimodal to trimodal. Example 2 exhibited three distinct diffraction peaks near 45°, indicating that its crystal structure is primarily composed of trigonal and tetragonal phases, with the system situated in a quasi-isomorphic phase boundary region. The coexistence of trigonal and tetragonal phases enhances the crystal structure's response to applied electric fields and lowers the energy barrier between different polarization orientations, thereby promoting polarization rotation and non-180° domain response, which is beneficial for improving the piezoelectric properties of the material. With the increase of Bi(Mg) 2 / 3 Nb 1 / 3 With further increase in O3 content, the diffraction peak near 45° gradually shifted from three peaks to a single peak. When x=0.07, Example 4 mainly exhibited a trigonal phase structure, and the system gradually deviated from the quasi-isomorphic phase boundary region where trigonal and tetragonal phases coexisted. The structural responsiveness decreased, and therefore the piezoelectric performance was lower than that of the optimal composition. The above results indicate that the introduction of Bi(Mg2 / 3Nb1 / 3)O3 can effectively regulate the phase structure of bismuth scandate-lead titanate-based ceramics, causing the system to evolve from a tetragonal phase to a trigonal / tetragonal phase coexistence state, and then back to a trigonal phase. Among these factors, an appropriate amount of Bi(Mg2 / 3Nb1 / 3)O3 places the system in a favorable quasi-isomorphic phase boundary region, which is an important structural factor for significantly improving its piezoelectric performance.
[0080] Figure 2 This is a piezoelectric coefficient diagram of the ceramic materials prepared in the embodiments and comparative examples of the present invention. As can be seen from the diagram, with the increase of Bi(Mg)... 2 / 3 Nb 1 / 3 As the O3 doping concentration increases, the piezoelectric coefficient initially increases and then decreases, with the best gain observed when the doping concentration is 0.03 (Example 2). Conversely, without doping, the piezoelectric coefficient decreases significantly.
[0081] Figure 3 The figures show the dielectric temperature spectra of the ceramic materials prepared in the embodiments and comparative examples of the present invention. As can be seen from the figures, with the increase of Bi(Mg)... 2 / 3 Nb 1 / 3 With increasing O3 doping concentration, the Curie temperature of the system gradually decreases and it gradually exhibits relaxation characteristics. Meanwhile, with increasing Bi(Mg) doping concentration...2 / 3 Nb 1 / 3 With increasing O3 content, the temperature corresponding to the dielectric constant peak gradually shifts towards lower temperatures, consistent with the trend in Table 1 where the Curie temperature gradually decreases from 450℃ to 383℃. Simultaneously, the dielectric peak exhibits an overall decreasing and broadening trend, indicating that Bi(Mg) 2 / 3 Nb 1 / 3 The introduction of O3 significantly altered the dielectric response near the ferroelectric phase transition of the material.
[0082] The above description is merely a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It is understood that other improvements and variations that are directly derived or conceived by those skilled in the art without departing from the spirit and concept of the present invention should be considered to be included within the protection scope of the present invention.
Claims
1. A bismuth magnesium niobate-doped bismuth scandate-lead titanate based high-temperature piezoelectric ceramic material, characterized in that, The general formula for the high-temperature piezoelectric ceramic material is: 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg 2 / 3 Nb 1 / 3) O3, Where: 0.00 < x ≤ 0.
07.
2. A method for preparing the high-temperature piezoelectric ceramic material according to claim 1, characterized in that, Includes the following steps: S1: Weigh Bi₂O₃, Sc₂O₃, PbO, TiO₂, MgO, and Nb₂O₅ according to stoichiometric ratio, mix them to obtain a mixture, ball mill, dry, and calcine to obtain 0.36BiScO₃-(0.64-x)PbTiO₃-xBi(Mg 2 / 3 Nb 1 / 3 )O3 powder; S2: 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg) from S1 2 / 3 Nb 1 / 3 O3 powder is subjected to secondary ball milling and drying to obtain powder material; S3: Add binder to the powder in S2, grind and then form a blank to obtain a blank; S4: After debinding and cold isostatic pressing of the blank from S3, sintering is performed to obtain the bismuth magnesium niobate-doped bismuth scandate-lead titanate-based high-temperature piezoelectric ceramic material.
3. The preparation method according to claim 2, characterized in that, In S1, the mass ratio of the mixture, grinding balls and milling media is 1:5:2; The ball mill rotates at a speed of 300-400 r / min; and / or, The ball milling time is 12-24 hours.
4. The preparation method according to claim 2, characterized in that, In S1, the drying temperature is 100~120℃, and / or, The drying time is 4 to 6 hours.
5. The preparation method according to claim 2, characterized in that, In S1, the calcination is achieved by heating at 3~5℃ / min and then holding at that temperature; Preferably, the calcination is carried out by heating to 700-800°C at a rate of 3-5°C / min and then holding at that temperature; More preferably, the heat preservation time is 4 to 6 hours.
6. The preparation method according to claim 2, characterized in that, In S2, during the secondary ball milling, the 0.36BiScO3-(0.64-x)PbTiO3-xBi(Mg) 2 / 3 Nb 1 / 3 The mass ratio of O3 powder, grinding balls and milling media is 1:5:2; The ball mill rotates at a speed of 300-400 r / min; and / or, The ball milling time is 12-24 hours; The drying temperature is 100~120℃, and / or, The drying time is 4 to 6 hours.
7. The preparation method according to claim 2, characterized in that, In S3, the mass ratio of the powder to the binder is 10:1; The adhesive comprises an aqueous solution of polyvinyl alcohol; Preferably, the mass concentration of the polyvinyl alcohol aqueous solution is 5-10%.
8. The preparation method according to claim 2, characterized in that, In S3, the blank preparation is achieved by pressing and holding pressure; Preferably, the pressing pressure is 8~10MPa, and the holding time is 1~3min.
9. The preparation method according to claim 2, characterized in that, In S4, the temperature of the adhesive discharge is 500~600℃, the heating rate is 1~3℃ / min, and the holding time is 4~6h.
10. The preparation method according to claim 2, characterized in that, In S4, the pressure of the cold isostatic pressing is 100~120MPa, and the holding time is 10~30min; The sintering temperature is 1000~1200℃, the heating rate is 3~5℃ / min, and the holding time is 2~4h.