Ceramic matrix composite friction pair, method for manufacturing and use thereof

The method for preparing ceramic matrix composite friction pairs by gradient design solves the problems of insufficient contact matching and unclear functional division of Ti, Al and carbon sources in MAX phase modified C/C or C/C-SiC friction materials, and achieves the synergistic effect of load bearing and wear resistance and interface stability of friction pairs.

CN123151701APending Publication Date: 2026-11-24CENT SOUTH UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611685723.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-29
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing MAX phase modified C/C or C/C-SiC friction materials suffer from problems such as insufficient contact matching of Ti, Al and carbon sources, uneven distribution of MAX phase, insufficient strengthening of the friction working surface, and unclear functional division on both sides of the friction pair.

Method used

A method for preparing friction pairs using gradient ceramic matrix composites containing MAX phases was adopted. By matching different C/C preform structures, Ti/TiAl@carbon source core-shell reactive powder compositions, phenolic resin content, and infiltration agent compositions, hard ceramic phase-enriched friction disks and MAX phase-enriched friction disks were prepared respectively, so that the pairing of the two could achieve a synergistic improvement in load-bearing capacity, wear resistance, and interface stability.

Benefits of technology

The system achieves a friction pair where the hard ceramic phase friction disk focuses on hard load-bearing and wear resistance, while the MAX phase friction disk focuses on interface stability and friction film retention. It is suitable for friction service scenarios such as high-energy braking, clutches, and wear-resistant structural components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123151701A_ABST
    Figure CN123151701A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of ceramic matrix composite technology, specifically disclosing a ceramic matrix composite friction pair, its preparation method, and its application. The friction pair of this invention consists of a hard ceramic phase-enriched friction disk A and a MAX phase-enriched friction disk B. The hard ceramic phase-enriched friction disk A uses a sandwich-structured porous C / C preform as a reinforcing skeleton, and its friction working surface is a relatively enriched region of TiC and SiC hard ceramic phases. The MAX phase-enriched friction disk B uses a puncture-structured porous C / C preform as a reinforcing skeleton, and its friction working surface is a relatively enriched region of Ti2AlC and / or Ti3AlC2. This invention achieves a synergistic improvement in load-bearing capacity, wear resistance, and interface stability by matching different C / C preform structures, different Ti / TiAl@carbon source core-shell reactive powder compositions, different boron-modified phenolic resin contents, and different infiltration agent compositions in the prepared paired friction pair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic matrix composites technology, and in particular to a ceramic matrix composite friction pair, its preparation method, and its application. Background Technology

[0002] Continuous carbon fiber reinforced ceramic matrix composites possess characteristics such as low density, high temperature resistance, thermal shock resistance, and high specific strength, making them valuable for applications in aerospace thermal protection, advanced friction braking, and nuclear energy equipment. When used as high-energy friction braking materials, they not only require high load-bearing capacity and thermal stability, but also must maintain a stable coefficient of friction, low wear rate, and good resistance to oxidation and wear under wide temperature range friction environments.

[0003] MAX phase ceramics are a class of ternary layered compounds. Among them, Ti-based MAX phases such as Ti3AlC2, Ti2AlC, and Ti3SiC2 combine the high-temperature stability of ceramic phases with the characteristics of layered structure, exhibiting good thermal conductivity, thermal shock resistance, damage resistance, and certain self-lubricating properties. Introducing them into C / C or C / C-SiC composites helps improve interfacial bonding, promote crack deflection and energy dissipation, and enhance the stability of friction films. Currently, MAX phase-modified C / C or C / C-SiC composites are mainly achieved through methods such as adding MAX phase powder, in-situ reaction of Ti / Al / C mixed powders, or reactive melting. Added MAX phase powders are easily affected by slurry stability, pore size, and powder agglomeration, making it difficult to distribute uniformly within porous C / C preforms. While in-situ reaction of Ti / Al / C mixed powders can generate MAX phases, the Ti, Al, and carbon sources are mostly mixed mechanically, resulting in large reactant contact scales. At high temperatures, this can easily lead to problems such as particle segregation, Al volatilization, localized over-reaction, and uneven MAX phase distribution.

[0004] Existing research has explored MAX phase-modified C / C or C / C-SiC composites. For example, Zhao Huan, in his study "Process and Performance Research of MAX Phase Modified C / C Composites Prepared by Reactive Melting Method," prepared C / C-SiC-Ti3Al(Si)C2 composites using TiC, Ti, Si, and Al powders at 1400–1600℃. This method can introduce the MAX phase into the C / C matrix, but due to the use of mixed powders in the reaction, the matching between Ti, Al, and the carbon source is limited, and there is still room for optimization in the distribution of the MAX phase and the reaction process. Chinese patent CN118206384B discloses a method for preparing MAX phase-toughened SiC_f / SiC composites using a staged melting method, which generates toughening phases such as Ti3AlC2 through stepwise melting of TiAl and Si. This method is mainly used for matrix toughening of SiC_f / SiC systems, but it does not construct a ceramic phase gradient structure on the friction surface to meet the service requirements of C / C friction disks, nor does it involve the pairing design of friction disks enriched with hard ceramic phases and friction disks enriched with MAX phases.

[0005] Furthermore, existing friction disc modification methods mostly focus on a single friction disc material, typically pursuing overall ceramic phase content or single-phase reinforcement effects, lacking paired designs that address the functional differences between the two friction discs in a friction pair. In actual friction processes, one side of the friction pair requires a high-hardness ceramic phase to provide load-bearing and wear resistance, while the other side needs good interface stability, anti-delamination, and friction film retention. If both friction discs use the same structure and component design, it is difficult to simultaneously achieve high load-bearing capacity, low wear, and friction stability.

[0006] Therefore, it is necessary to develop a gradient MAX phase ceramic matrix composite material and its preparation process for the overall pairing design of friction pairs, so as to meet the application requirements in friction service scenarios such as high-energy braking, clutches and wear-resistant structural components. Summary of the Invention

[0007] This invention aims to address at least the problems of insufficient contact matching of Ti, Al, and carbon sources, uneven distribution of the MAX phase, insufficient strengthening of the friction working surface, and unclear functional division on both sides of the friction pair in existing MAX phase-modified C / C or C / C-SiC friction materials. To this end, this invention provides a gradient MAX phase-containing ceramic matrix composite friction pair and its preparation method. This invention prepares hard ceramic phase-enriched friction disks and MAX phase-enriched friction disks by matching different C / C preform structures, different Ti / TiAl@carbon source core-shell reactive powder compositions, different boron-modified phenolic resin contents, and different infiltration agent compositions, respectively, achieving a synergistic improvement in load-bearing capacity, wear resistance, and interface stability after pairing.

[0008] In a first aspect, the present invention provides a method for preparing a ceramic matrix composite friction pair, comprising the following steps:

[0009] S1. The first Ti / TiAl@carbon source core-shell reactive powder is introduced into the sandwich structure porous C / C preform, and the second Ti / TiAl@carbon source core-shell reactive powder is introduced into the puncture structure porous C / C preform. After cross-linking curing and pyrolysis-reaction treatment, the first C / C-TiC-MAX preform and the second C / C-TiC-MAX preform are obtained.

[0010] S2. The first C / C-TiC-MAX green body is subjected to pressure reaction melting treatment using the first melting agent to obtain a hard ceramic phase enriched friction disk A; the second C / C-TiC-MAX green body is subjected to pressure reaction melting treatment using the second melting agent to obtain a MAX phase enriched friction disk B.

[0011] S3. Pair the hard ceramic phase enriched friction disk A and the MAX phase enriched friction disk B to obtain the ceramic matrix composite friction pair.

[0012] Wherein, the mass ratio of Ti powder to TiAl powder in the first Ti / TiAl@carbon source core-shell reaction powder is greater than the mass ratio of Ti powder to TiAl powder in the second Ti / TiAl@carbon source core-shell reaction powder;

[0013] Both the first and second infiltrating agents include Si powder and TiAl powder, and the mass ratio of Si powder to TiAl powder in the first infiltrating agent is greater than the mass ratio of Si powder to TiAl powder in the second infiltrating agent.

[0014] The core of this invention lies not in introducing the MAX phase alone, but in combining a sandwich-structured porous C / C preform, Ti-rich core-shell reactive powder, and Si-rich infiltrator to prepare friction disk A, which emphasizes hard load-bearing and wear resistance; simultaneously, combining a puncture-structured porous C / C preform, TiAl-rich core-shell reactive powder, and TiAl-rich infiltrator to prepare friction disk B, which emphasizes interface stability and friction film retention. The two types of friction disks are used in pairs to form a friction pair with functional division of labor.

[0015] According to some embodiments of the present invention, both the first Ti / TiAl@carbon source core-shell reactive powder and the second Ti / TiAl@carbon source core-shell reactive powder include a Ti / TiAl mixed powder core, an inner carbon source layer formed by in-situ curing and coating, and an outer carbon source layer formed by chemical vapor deposition.

[0016] The inner carbon source layer designed in this invention is used to enable phenolic resin to be deposited, cured, and pre-carbonized in situ on the surface of Ti / TiAl mixed powder, forming an initial carbon source coating; the outer carbon source layer is used to further improve the continuity and uniformity of the carbon source layer; by constructing Ti / Al / C short-range reaction units through the inner and outer carbon source layers, the reaction diffusion distance of Ti-C and Ti-Al-C can be shortened, reducing the risk of component segregation and local reaction inhomogeneity during the high-temperature reaction of ordinary mixed powders.

[0017] According to some embodiments of the present invention, the preparation methods of the first Ti / TiAl@carbon source core-shell reactive powder and the second Ti / TiAl@carbon source core-shell reactive powder include the following steps:

[0018] Ti powder and TiAl powder are mixed and added to phenolic resin. After ball milling and dispersion, the mixture is filtered and then subjected to in-situ curing and coating treatment at 90-220℃. Following this, a pre-carbonization treatment is performed at 600-900℃ to form an inner carbon source layer on the powder surface. Subsequently, an outer carbon source layer is formed by fluidized bed chemical vapor deposition at 500-700℃, yielding Ti / TiAl@carbon source core-shell reactive powder. Preferably, the phenolic resin is an alcohol-soluble phenolic resin.

[0019] According to some embodiments of the present invention, the in-situ solidification coating treatment time is 2-6 hours, the pre-carbonization treatment time is 0.5-2 hours, the fluidized bed chemical vapor deposition time is 5-60 minutes, and the gaseous carbon source used in the fluidized bed chemical vapor deposition includes acetylene.

[0020] The in-situ curing and coating process of this invention enables phenolic resin to be cured and coated on the powder surface in situ, thereby reducing the risk of local separation of Ti powder, TiAl powder, and carbon source during slurry preparation, impregnation, and heat treatment. Subsequent carbonization treatment transforms the organic carbon source precursor into a more stable carbonaceous coating layer, providing a base surface for subsequent fluidized bed chemical vapor deposition (FCVD). FCVD further improves the continuity and uniformity of the carbon source layer on the powder surface; when the powder is in a fluidized state, the gaseous carbon source is more likely to contact and deposit on the particle surface, reducing the potential for insufficient local coating or agglomeration problems in simple liquid-phase coating. The combination of in-situ curing and coating with FCVD enables the Ti / TiAl core and carbon source layer to form a more stable core-shell reaction structure and reduces the introduction of exogenous impurities, thereby improving the reaction compatibility of subsequent in-situ generation of TiC and MAX phases.

[0021] According to some embodiments of the present invention, in step S1, the method of introducing the Ti / TiAl@carbon source core-shell reactive powder into the porous C / C preform is as follows: the Ti / TiAl@carbon source core-shell reactive powder is mixed with boron-modified phenolic resin, dispersant and solvent to obtain a reactive impregnation slurry, and the porous C / C preform is placed in the reactive impregnation slurry and impregnated under vacuum-pressure; preferably, the boron-modified phenolic resin is an alcohol-soluble thermosetting boron-modified phenolic resin, the dispersant is an alcohol-soluble polymeric dispersant, and the solvent is anhydrous ethanol;

[0022] The first Ti / TiAl@ carbon source core-shell reactive powder is mixed with boron-modified phenolic resin, dispersant and solvent in a mass ratio of 5: (9~14): (1~2): (1~3) to obtain the first reactive impregnation slurry, which is used to impregnate sandwich structure porous C / C preforms.

[0023] The second Ti / TiAl@ carbon source core-shell reactive powder is mixed with boron-modified phenolic resin, dispersant and solvent in a mass ratio of 5:(4~8):(1~2):(1~3) to obtain a second reactive impregnation slurry, which is used to impregnate porous C / C preforms with puncture structure.

[0024] The boron-modified phenolic resin used in this invention exhibits high thermal stability and char residue. Its pyrolysis-formed boron-containing carbonaceous structure helps improve the heat resistance of the friction working layer and the stability of the friction film. The first reactive impregnation slurry has a high boron-modified phenolic resin content, providing more active carbon sources for subsequent pyrolysis, which is beneficial for the formation of hard ceramic phases such as TiC and SiC, thus improving the load-bearing and wear-resistant capabilities of friction disk A. The second reactive impregnation slurry has a relatively low boron-modified phenolic resin content, which ensures powder fixation and carbon source supply while avoiding excessive TiC formation induced by excessive carbon source, thus facilitating the formation and regulation of the Ti-Al-C MAX phase.

[0025] According to some embodiments of the present invention, in step S1, the pyrolysis-reaction treatment includes two stages: the first stage is pyrolysis at 800~1000℃ for 0.5~2h, and the second stage is reaction at 1200~1500℃ for 1~2h.

[0026] The impregnation, cross-linking curing, and pyrolysis treatments are repeated 2 to 4 times; the densities of both the first C / C-TiC-MAX preform and the second C / C-TiC-MAX preform are 1.20–1.60 g / cm³. 3 The open area ratio is 15% to 40%.

[0027] This invention utilizes cross-linking curing to fix the positions of Ti / TiAl@carbon source core-shell reactive powder and resin carbon source within a porous C / C preform. During pyrolysis, boron-modified phenolic resin is converted into activated carbon and reacts in situ with the Ti / TiAl@carbon source core-shell reactive powder to generate TiC, Ti2AlC, and / or Ti3AlC2. Through multiple cross-linking curing and pyrolysis cycles, a C / C-TiC-MAX pre-reactive framework can be formed within the pores of the C / C preform, while retaining the pore channels required for subsequent pressure reaction melting and infiltration.

[0028] According to some embodiments of the present invention, in step S2, the temperature of the pressure reaction melting infiltration treatment is 1450-1750°C, the holding time is 1-2.5h, and in the last hour of holding, the pressure is increased to 5-15MPa at a pressurization rate of 0.15-0.4MPa / min, and then the pressure is maintained until the end of the holding time, and finally the temperature is reduced under pressure.

[0029] During the pressure-induced melting process, Si powder forms a liquid phase and enters the pores of the C / C-TiC-MAX green body, reacting with the carbon source to generate SiC, thus increasing the material's densification and the content of hard ceramic phases. TiAl powder is used to supplement the Ti-Al-C reaction components and regulate the formation of MAX phases such as Ti2AlC and / or Ti3AlC2. Pressure enhances the ability of the melting agent to enter the green body pores and promotes the enrichment of ceramic phases in the friction working surface region. Heat preservation ensures that the melting agent fully melts, wets, and reacts with the C / C-TiC-MAX green body. In the last hour of heat preservation, linear pressurization to 5–15 MPa further promotes the liquid phase into the green body pores after the melting agent has formed a stable liquid phase, improving pore filling and reaction uniformity, and promoting the enrichment of ceramic phases in the friction working surface region. Gradual pressure increase avoids instantaneous high pressure causing liquid phase erosion, localized pore blockage, or uneven melting. When the pressure is too low, the driving force for the infiltrator to enter the pores of the green body is insufficient, which can easily lead to insufficient internal infiltration and a large number of residual pores. When the pressure is too high, the infiltrator may excessively enter the core region, weakening the thickness gradient structure and potentially causing pore blockage, free phase residue, matrix microcracks, or material embrittlement. Therefore, controlling the pressure within the range of 5–15 MPa is beneficial for balancing infiltration densification, ceramic phase gradient construction, and the stability of the friction disk structure.

[0030] According to some embodiments of the present invention, the mass ratio of Ti powder to TiAl powder in the first Ti / TiAl@carbon source core-shell reaction powder is (10~20):(1~8); the mass ratio of Ti powder to TiAl powder in the second Ti / TiAl@carbon source core-shell reaction powder is (2~5):(2~7).

[0031] According to some preferred embodiments of the present invention, the mass ratio of Ti powder to TiAl powder in the first Ti / TiAl@carbon source core-shell reaction powder is (12~18):(2~6); the mass ratio of Ti powder to TiAl powder in the second Ti / TiAl@carbon source core-shell reaction powder is (2~4):(4~6).

[0032] According to some embodiments of the present invention, the mass ratio of Si powder to TiAl powder in the first infiltrator is (14~17):(1~3); the mass ratio of Si powder to TiAl powder in the second infiltrator is (12~14):(3~6).

[0033] This invention explores the above-mentioned raw material ratios to form functional differences between two types of friction discs; friction disc A has relatively high levels of Ti and Si sources, which is conducive to the formation of TiC and SiC hard ceramic phases, making its friction working surface focus on load bearing and wear resistance; friction disc B has relatively high levels of TiAl components, which is conducive to the formation of Ti-Al-C system MAX phase, making its friction working surface focus on interface regulation, crack deflection and friction film stability.

[0034] A second aspect of the present invention provides a ceramic matrix composite friction pair, characterized in that it comprises a hard ceramic phase-enriched friction disk A and a MAX phase-enriched friction disk B, which are prepared by the preparation method described in the first aspect of the present invention and are paired with each other.

[0035] The hard ceramic phase enriched friction disk A uses a sandwich-structured porous C / C preform as a reinforcing skeleton, and its friction working surface is a relative enrichment area of ​​TiC and SiC hard ceramic phases.

[0036] The MAX phase-enriched friction disk B uses a puncture-structured porous C / C blank as a reinforcing skeleton, and its friction working surface is a Ti2AlC and / or Ti3AlC2 relatively enriched region.

[0037] This invention utilizes this differentiated preparation method to meet the phase composition matching requirements of different friction pairs or different service positions. The sandwich-structured carbon fiber preform has good pore connectivity and impregnation / melting penetration, which is beneficial for reactive impregnation slurry and melting agent to enter the pores of the preform. Combined with a first Ti / TiAl@carbon source core-shell reactive powder with a high Ti content and a first melting agent with a high Si content, it can promote the formation and enrichment of hard ceramic phases such as TiC and SiC in the friction working area, so that the friction disk focuses on undertaking the hard load-bearing, anti-ploughing and wear-resistant functions in the friction pair. The puncture-structured carbon fiber preform has fiber reinforcement and interlayer constraint in the thickness direction, which is beneficial to improving the interlayer bonding, anti-delamination and peeling ability, and overall stability of the friction disk under thermo-mechanical coupling load. By combining a second Ti / TiAl@carbon source core-shell reactive powder with a high or near-Ti content and a second infiltrator with a high TiAl content, the tendency for Ti-Al-C system MAX phase formation can be adjusted, allowing the friction disk to focus on interface regulation, crack deflection, energy dissipation, and friction film stabilization. Different combinations of prefabricated structure, core-shell reactive powder composition, and infiltrator composition can create different ceramic phase enrichment characteristics in the two types of friction disks, facilitating friction pair pair design.

[0038] A third aspect of the present invention provides the application of ceramic matrix composite friction pairs as described in the second aspect of the present invention in high-energy friction braking components, aerospace braking components, vehicle braking components, clutch friction components, or wear-resistant structural components.

[0039] The beneficial effects of this invention are:

[0040] 1) This invention introduces Ti, Al and C reaction components using Ti / TiAl@carbon source core-shell reactive powder. The core-shell reactive powder consists of a Ti / TiAl mixed powder core, an inner carbon source layer and an outer carbon source layer, which can form Ti / Al / C short-range reaction units at the powder scale. This ensures that the Ti source, Al source and carbon source maintain a good contact matching relationship, which is beneficial to the in-situ generation of ceramic phases such as TiC, Ti2AlC and / or Ti3AlC2, and improves the controllability of ceramic phase distribution.

[0041] 2) This invention sets up a first reactive impregnation slurry and a second reactive impregnation slurry respectively, and controls the carbon source supply of the two types of green bodies by the difference in boron-modified phenolic resin content; the first reactive impregnation slurry has a higher boron-modified phenolic resin content, which is conducive to the formation of TiC and SiC in the friction disk A enriched by hard ceramic phase; the second reactive impregnation slurry has a relatively lower boron-modified phenolic resin content, which can promote the formation and control of Ti-Al-C system MAX phase while ensuring powder fixation and carbon source supply.

[0042] 3) This invention forms a thickness gradient structure through cross-linking curing, pyrolysis, and pressure reaction melting infiltration; the cross-linking curing and pyrolysis cycle can form a C / C-TiC-MAX pre-reaction skeleton in the pores of the porous C / C blank, and retain subsequent melting channels; during the pressure reaction melting infiltration process, the Si-rich first melting agent is conducive to the formation of SiC hard ceramic phase in friction disk A, and the TiAl-rich second melting agent is conducive to the formation of Ti2AlC and / or Ti3AlC2 and other MAX phases in friction disk B, thereby achieving ceramic phase enrichment on the friction working surface.

[0043] 4) The friction pair prepared by this invention consists of a hard ceramic phase-enriched friction disk A and a MAX phase-enriched friction disk B. Friction disk A focuses on hard load-bearing, anti-ploughing, and wear resistance, while friction disk B focuses on interlayer constraint, anti-delamination, interface stability, and friction film retention. The two types of friction disks complement each other in terms of structure, composition, and phase function, achieving synergy between load-bearing, wear resistance, and interface stability in the same friction pair. This makes it suitable for friction service scenarios such as high-energy braking, clutches, and wear-resistant structural components.

[0044] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Attached Figure Description

[0045] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0046] Figure 1 The two are the hard ceramic phase enrichment friction disk A (a) and the MAX phase enrichment friction disk B (b) of Embodiment 1 of the present invention. Detailed Implementation

[0047] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.

[0048] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0049] In this application, TiAl powder refers to titanium-aluminum powder with TiAl phase or Ti-Al intermetallic compound as the main component; sandwich-structured porous C / C preform refers to a multi-layered carbon fiber preform composed of a middle structural functional layer and two side friction functional layers, wherein the structural functional layer is a carbon cloth / mesh laminated needle-punched structure, and the friction functional layer is a carbon fiber mesh structure, the two being needle-punched together to form an integral porous structure; puncture-structured porous C / C preform refers to a three-dimensional porous C / C preform formed by puncturing multi-layered carbon fiber woven fabric with carbon fiber bundles in the thickness direction, its planar direction being reinforced by woven fabric, and its thickness... Interlayer connection and Z-axis reinforcement are achieved by puncture wire bundles in the azimuth direction; the relatively enriched region of hard ceramic phase refers to the friction working surface region where the TiC and SiC content is higher than that in the core region; the relatively enriched region of MAX phase refers to the friction working surface region where the Ti2AlC and / or Ti3AlC2 content is higher than that in the core region; the phenolic resin used is TB-1547 alcohol-soluble phenolic resin (abbreviated as TB-1547), the boron-modified phenolic resin used is TB-03 boron-modified phenolic resin (abbreviated as TB-03), and the dispersant used is polyvinylpyrrolidone-vinyl acetate copolymer (abbreviated as PVP / VA).

[0050] Methods for testing the performance of the composite materials prepared according to specific embodiments: Flexural strength: Flexural strength test according to GB / T 10311-2021; Friction and wear properties: According to GB / T 40398.1-2021 standard, using an MM-3000 friction and wear testing machine, braking condition 10000 rpm, 0.50 kg·m 2 The friction coefficient, linear wear, and mass wear of the sample were measured at 0.90 MPa.

[0051] Example 1

[0052] This embodiment prepares a gradient-containing MAX phase ceramic matrix composite friction pair, consisting of a hard ceramic phase-enriched friction disk A and a MAX phase-enriched friction disk B. The specific preparation steps are as follows:

[0053] 1) Preparation of Ti / TiAl@carbon source core-shell reactive powder:

[0054] Preparation of the first Ti / TiAl@carbon source core-shell reactive powder (for hard ceramic phase enrichment friction disk A): Ti powder and TiAl powder were weighed at a mass ratio of 15:4, mixed and added with sufficient TB-1547 (phenolic resin) to fully wet and disperse the Ti powder and TiAl powder. After stirring, ball milling dispersion and filtration, the powder was cured at 110℃ for 4h; then it was pre-carbonized at 800℃ for 1h under an argon atmosphere to obtain an in-situ cured powder with an inner carbon source layer on the surface.

[0055] The pre-carbonized powder was placed in a fluidized bed reactor, and acetylene and hydrogen were introduced under an argon atmosphere. The powder was deposited at 600°C for 30 min, allowing the gaseous carbon source to continue to deposit on the powder surface to form an outer carbon source layer, thus obtaining the first Ti / TiAl@carbon source core-shell reaction powder.

[0056] Preparation of the second Ti / TiAl@carbon source core-shell reactive powder (for MAX phase enrichment friction disk B): Ti powder and TiAl powder were weighed at a mass ratio of 3:5. The remaining in-situ curing, coating, pre-carbonization and chemical vapor deposition treatment methods and conditions were the same as those for the preparation of the first Ti / TiAl@carbon source core-shell reactive powder, thus obtaining the second Ti / TiAl@carbon source core-shell reactive powder.

[0057] In the first Ti / TiAl@carbon source core-shell reactive powder, the mass ratio of Ti powder to TiAl powder is greater than that in the second Ti / TiAl@carbon source core-shell reactive powder; both types of core-shell reactive powders are composed of a Ti / TiAl mixed powder core, an inner carbon source layer, and an outer carbon source layer.

[0058] 2) Preparation of C / C-TiC-MAX green bodies:

[0059] A density of 0.8 g / cm³ was selected. 3 The T700 sandwich-structured porous C / C preform is used as the reinforcing skeleton of the friction disk A, with a density of 0.8 g / cm³. 3 The T700 puncture structure porous C / C preform serves as the reinforcing skeleton for the friction disc B;

[0060] The first Ti / TiAl@carbon source core-shell reactive powder, TB-03 (boron-modified phenolic resin), PVP / VA (polyvinylpyrrolidone-vinyl acetate copolymer), and anhydrous ethanol were mixed in a mass ratio of 5:12:1:2 and dispersed by stirring and ball milling to obtain the first reactive impregnation slurry. The sandwich-structured porous C / C preform was placed in the first reactive impregnation slurry for vacuum-pressure impregnation, so that the slurry could enter the pores of the preform.

[0061] The second Ti / TiAl@carbon source core-shell reactive powder, TB-03, PVP / VA and anhydrous ethanol were mixed in a mass ratio of 5:6:1:2 and dispersed by stirring and ball milling to obtain the second reactive impregnation slurry. The puncture-structured porous C / C preform was placed in the second reactive impregnation slurry for vacuum-pressure impregnation, so that the slurry entered the pores of the preform.

[0062] After impregnation, both types of preforms were cross-linked and cured separately to solidify TB-03 and fix the position of Ti / TiAl@carbon source core-shell reactive powder in the pores. The specific process of vacuum-pressure impregnation and cross-linking curing included: vacuum impregnation for 1 hour at a vacuum degree of -0.1 MPa and an impregnation temperature of 40°C; followed by pressure impregnation and cross-linking curing at a pressure of 3.0 MPa, an impregnation temperature of 70°C, an impregnation time of 2 hours, and cross-linking curing for 15 hours at a curing temperature of 130°C. Subsequently, a pyrolysis treatment was performed, including two stages: the first stage involved holding at 900°C for 1 hour to carbonize TB-03 into activated carbon; the second stage involved holding at 1400°C for 1.5 hours to allow the Ti / TiAl@carbon source core-shell reactive powder to react in situ with the activated carbon, generating TiC, Ti2AlC, and / or Ti3AlC2.

[0063] The above-mentioned impregnation, cross-linking curing, and pyrolysis cycles were performed three times, resulting in a porosity of 16.2% and a density of 1.48 g / cm³. 3 The first C / C-TiC-MAX preform has a porosity of 26.4% and a density of 1.40 g / cm³. 3 The second C / C-TiC-MAX billet.

[0064] 3) Pressure-induced melting and infiltration:

[0065] The first C / C-TiC-MAX green body was subjected to pressure reaction infiltration using a first infiltration agent: the mass ratio of Si powder to TiAl powder in the first infiltration agent was 8:1; the first C / C-TiC-MAX green body was embedded in the first infiltration agent, and the preset friction working surface side was made to be in full contact with the infiltration agent; the temperature was raised to 1650℃ and held for 2 hours; in the last hour of holding, the pressure was increased to 12MPa at a rate of 0.25MPa / min, and after reaching the target pressure, the temperature was lowered under the pressure holding state, and the residual infiltration agent on the surface was removed after cooling to obtain a hard ceramic phase enriched friction disk A;

[0066] The second C / C-TiC-MAX billet was subjected to pressure reaction melting infiltration using a second melting agent: the mass ratio of Si powder to TiAl powder in the second melting agent was 13:4; the second C / C-TiC-MAX billet was embedded in the second melting agent, and the preset friction working surface side was made to be in full contact with the melting agent; the temperature was raised to 1600℃ and held for 2 hours; in the last hour of holding, the pressure was increased to 10MPa at a rate of 0.25MPa / min, and after reaching the target pressure, the temperature was lowered under pressure, and the residual melting agent on the surface was removed after cooling to obtain the MAX phase enriched friction disk B;

[0067] In this process, the mass ratio of Si powder to TiAl powder in the first infiltrator is greater than that in the second infiltrator; the first infiltrator is used to promote the formation of SiC hard ceramic phase in friction disk A, and the second infiltrator is used to increase the tendency of Ti-Al-C MAX phase formation in friction disk B.

[0068] 4) Friction pair pairing:

[0069] Pairing hard ceramic phase-enriched friction disk A with MAX phase-enriched friction disk B yields a gradient MAX phase-containing ceramic matrix composite friction pair (e.g., Figure 1 (As shown).

[0070] The friction pair prepared in this embodiment was tested against the reference standard. The test results are as follows: the bending strength of friction disk B in this embodiment is 298 MPa; the average friction coefficient of the friction pair composed of friction disk A and friction disk B is 0.34, the linear wear is 2.15 μm / cycle, and the mass loss is 10.14 mg / cycle.

[0071] In this friction pair, friction disk A focuses on hard load-bearing, anti-ploughing, and wear resistance; friction disk B focuses on interlayer constraint, anti-delamination, interface stability, and friction film retention.

[0072] Example 2

[0073] This embodiment prepares a gradient ceramic matrix composite friction pair containing MAX phase. This embodiment is basically the same as Example 1, except that some raw material mass ratios are adjusted; the remaining methods and process parameters are consistent with Example 1.

[0074] In step 1) of this embodiment, the mass ratio of Ti powder to TiAl powder in the first Ti / TiAl@carbon source core-shell reaction powder is 4:1; the mass ratio of Ti powder to TiAl powder in the second Ti / TiAl@carbon source core-shell reaction powder is 1:2.

[0075] In step 2) of this embodiment, the mass ratio of the first Ti / TiAl@carbon source core-shell reactive powder, TB-03, PVP / VA and anhydrous ethanol in the first reactive impregnation slurry is 5:14:1:2; the mass ratio of the second Ti / TiAl@carbon source core-shell reactive powder, TB-03, PVP / VA and anhydrous ethanol in the second reactive impregnation slurry is 5:7:1:2.

[0076] In step 3) of this embodiment, the mass ratio of Si powder to TiAl powder in the first infiltration agent is 17:2, and the mass ratio of Si powder to TiAl powder in the second infiltration agent is 12:5.

[0077] After melting and infiltration, hard ceramic phase enriched friction disk A and MAX phase enriched friction disk B were obtained, and the two were paired to form a gradient ceramic matrix composite friction pair containing MAX phase.

[0078] The performance of the friction pair prepared in this embodiment was tested according to the reference standard. The test results are as follows: the bending strength of the MAX phase enriched friction disk B prepared in this embodiment is 342 MPa; the average friction coefficient of the friction pair composed of friction disk A and friction disk B is 0.38, the linear wear is 2.64 μm / cycle, and the mass loss is 12.15 mg / cycle.

[0079] The experimental and test results of this embodiment show that, within the scope of the present invention, after adjusting the Ti / TiAl ratio, the resin carbon source ratio, and the composition of the infiltrator, friction disk A and friction disk B with differentiated phase functions can still be obtained.

[0080] Comparative Example 1

[0081] This comparative example prepares a ceramic matrix composite friction pair to investigate the role of Ti / TiAl@carbon source core-shell reactive powder. The difference between this comparative example and Example 1 is that, instead of preparing a first and a second Ti / TiAl@carbon source core-shell reactive powder, Ti powder, TiAl powder, TB-O3, PVP / VA, and anhydrous ethanol are directly mixed to prepare a common mixed powder reactive impregnation slurry. The remaining steps are the same as in Example 1.

[0082] Specifically, in this comparative example, the mass ratio of Ti powder to TiAl powder used in friction disc A is 15:4, and the mass ratio of Ti powder to TiAl powder used in friction disc B is 3:5. The corresponding proportions of Ti powder and TiAl powder were directly added to TB-03, and after stirring and ball milling dispersion, PVP / VA and anhydrous ethanol were added to obtain a common mixed powder reactive impregnation slurry. This comparative example did not undergo in-situ curing coating, pre-carbonization, or fluidized bed chemical vapor deposition treatment.

[0083] Subsequently, following the impregnation, cross-linking curing, pyrolysis, and pressure reaction melting process in Example 1, comparative friction disk A and comparative friction disk B were prepared respectively, and the two were paired to form a comparative friction pair.

[0084] The performance of the friction pair prepared in this comparative example was tested according to the reference standard. The test results are as follows: the bending strength of the comparative MAX phase friction disk B prepared in this comparative example is 261 MPa; the average friction coefficient of the friction pair composed of comparative friction disk A and comparative friction disk B is 0.26, the linear wear is 4.15 μm / cycle, and the mass loss is 18.45 mg / cycle.

[0085] In this comparative example, the Ti source, Al source, and carbon source mainly rely on ordinary mechanical mixing and contact, lacking an inner carbon source layer and an outer carbon source layer at the powder scale, making it difficult to stably construct the Ti / Al / C short-range reaction unit. The experimental and test results of this comparative example demonstrate the influence of the core-shell reaction powder of the present invention on the contact matching of reaction components, in-situ generation of ceramic phase, and stability of friction pair performance.

[0086] Comparative Example 2

[0087] This comparative example prepares ceramic matrix composite friction pairs to investigate the effect of differentiated component design between hard ceramic phase-enriched friction disk A and MAX phase-enriched friction disk B. The difference between this comparative example and Example 1 is that, although sandwich-structured porous C / C preforms and puncture-structured porous C / C preforms are still used respectively, both friction disks use Ti / TiAl@carbon source core-shell reactive powder with the same Ti / TiAl ratio, the same reactive impregnation slurry composition, and the same melt infiltration agent composition. The remaining steps are the same as in Example 1.

[0088] Specifically, in this comparative example, both friction disc A and control friction disc B use the same Ti / TiAl@carbon source core-shell reactive powder, with a Ti powder to TiAl powder mass ratio of 11:5. In the reactive impregnation slurry used on both friction discs, the mass ratio of Ti / TiAl@carbon source core-shell reactive powder, TB-03, PVP / VA, and anhydrous ethanol is 5:9:1:2. The mass ratio of Si powder to TiAl powder in the infiltration agent used on both friction discs is 11:2.

[0089] Subsequently, following the impregnation, cross-linking curing, pyrolysis, and pressure reaction melting process in Example 1, comparative friction disk A and comparative friction disk B were prepared respectively, and the two were paired to form a comparative friction pair.

[0090] The performance of the friction pair prepared in this comparative example was tested according to the reference standard. The test results are as follows: the bending strength of the comparative MAX phase friction disk B prepared in this comparative example is 241 MPa; the average friction coefficient of the friction pair composed of comparative friction disk A and comparative friction disk B is 0.24, the linear wear is 3.74 μm / cycle, and the mass loss is 15.33 mg / cycle.

[0091] Although this comparative example retains the combination of sandwich-structured porous C / C preforms and puncture-structured porous C / C preforms, it does not configure different Ti / TiAl ratios, different resin carbon source ratios, and different melt infiltration agent compositions according to the structural characteristics of the two types of preforms. This makes it difficult to form a functional division of labor that emphasizes hard load-bearing and wear resistance on one side and MAX phase interface adjustment and anti-delamination stability on the other side.

[0092] Comparative analysis of the results of the examples and comparative examples:

[0093] As shown in Example 1 and Comparative Example 1, under the same Ti / TiAl ratio, preform structure, and pressure reaction infiltration conditions, the bending strength of the MAX phase-enriched friction disk B increased from 261 MPa to 298 MPa after using Ti / TiAl@carbon source core-shell reactive powder; the average friction coefficient of the friction pair increased from 0.26 to 0.34; the linear wear decreased from 4.15 μm / cycle to 2.15 μm / cycle; and the mass loss decreased from 18.45 mg / cycle to 10.14 mg / cycle. These comparative results indicate that core-shell reactive powder can improve the contact matching degree of the Ti source, Al source, and carbon source, which is beneficial to the in-situ generation of the TiC and Ti-Al-C MAX phases, thereby improving the load-bearing capacity and tribological performance of the friction pair.

[0094] As shown in Example 1 and Comparative Example 2, when both use Ti / TiAl@carbon source core-shell reactive powder, Example 1, through matching different preform structures, different slurry compositions, and different infiltrating agent compositions, increased the flexural strength of the MAX phase-enriched friction disk B from 241 MPa to 298 MPa; the average friction coefficient of the friction pair increased from 0.24 to 0.34; the linear wear decreased from 3.74 μm / cycle to 2.15 μm / cycle; and the mass loss decreased from 15.33 mg / cycle to 10.14 mg / cycle. These results indicate that the differentiated component design of the hard ceramic phase-enriched friction disk A and the MAX phase-enriched friction disk B is beneficial for forming a friction pair structure that combines load-bearing wear resistance with interface stability.

[0095] In Example 2, after adjusting the Ti / TiAl ratio, the content of TB-03 boron-modified phenolic resin, and the composition of the infiltrator within the limits defined by this invention, the flexural strength of the MAX phase-enriched friction disk B reached 342 MPa, the average friction coefficient of the friction pair was 0.38, the linear wear was 2.64 μm / cycle, and the mass loss was 12.15 mg / cycle. Compared with Example 1, Example 2 has higher flexural strength and friction coefficient, but the wear is slightly increased, indicating that this invention can adjust the strength, friction level, and wear resistance of the friction pair by adjusting the component ratio.

[0096] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.

Claims

1. A method for preparing a ceramic matrix composite friction pair, characterized in that, Includes the following steps: S1. The first Ti / TiAl@carbon source core-shell reactive powder is introduced into the sandwich structure porous C / C preform, and the second Ti / TiAl@carbon source core-shell reactive powder is introduced into the puncture structure porous C / C preform. After cross-linking curing and pyrolysis-reaction treatment, the first C / C-TiC-MAX preform and the second C / C-TiC-MAX preform are obtained. S2. The first C / C-TiC-MAX preform is subjected to pressure reaction melting treatment using the first melting agent to obtain a hard ceramic phase enriched friction disk A. The second C / C-TiC-MAX preform was subjected to pressure reactive melting treatment using a second melting agent to obtain a MAX phase-enriched friction disk B. S3. Pair the hard ceramic phase enriched friction disk A and the MAX phase enriched friction disk B to obtain the ceramic matrix composite friction pair. Wherein, the mass ratio of Ti powder to TiAl powder in the first Ti / TiAl@carbon source core-shell reaction powder is greater than the mass ratio of Ti powder to TiAl powder in the second Ti / TiAl@carbon source core-shell reaction powder; Both the first and second infiltrating agents include Si powder and TiAl powder, and the mass ratio of Si powder to TiAl powder in the first infiltrating agent is greater than the mass ratio of Si powder to TiAl powder in the second infiltrating agent.

2. The preparation method according to claim 1, characterized in that, Both the first Ti / TiAl@carbon source core-shell reactive powder and the second Ti / TiAl@carbon source core-shell reactive powder include a Ti / TiAl mixed powder core, an inner carbon source layer formed by in-situ curing and coating, and an outer carbon source layer formed by chemical vapor deposition.

3. The preparation method according to claim 2, characterized in that, The preparation methods of the first Ti / TiAl@carbon source core-shell reactive powder and the second Ti / TiAl@carbon source core-shell reactive powder include the following steps: Ti powder and TiAl powder are mixed and added to phenolic resin. After ball milling and dispersion, the mixture is filtered and then subjected to in-situ curing and coating treatment at 90~220℃. The mixture is then pre-carbonized at 600~900℃ to form an inner carbon source layer on the surface of the powder. Subsequently, an outer carbon source layer is formed by fluidized bed chemical vapor deposition at 500~700℃, resulting in Ti / TiAl@carbon source core-shell reactive powder.

4. The preparation method according to any one of claims 1 to 3, characterized in that, The mass ratio of Ti powder to TiAl powder in the first Ti / TiAl@carbon source core-shell reaction powder is (10~20):(1~8); the mass ratio of Ti powder to TiAl powder in the second Ti / TiAl@carbon source core-shell reaction powder is (2~5):(2~7).

5. The preparation method according to claim 1, characterized in that, In step S1, the method of introducing Ti / TiAl@carbon source core-shell reactive powder into the porous C / C preform is as follows: the Ti / TiAl@carbon source core-shell reactive powder is mixed with boron-modified phenolic resin, dispersant and solvent to obtain reactive impregnation slurry, and the porous C / C preform is placed in the reactive impregnation slurry and impregnated under vacuum-pressure. The first Ti / TiAl@ carbon source core-shell reactive powder is mixed with boron-modified phenolic resin, dispersant and solvent in a mass ratio of 5: (9~14): (1~2): (1~3) to obtain the first reactive impregnation slurry, which is used to impregnate sandwich structure porous C / C preforms. The second Ti / TiAl@ carbon source core-shell reactive powder is mixed with boron-modified phenolic resin, dispersant and solvent in a mass ratio of 5:(4~8):(1~2):(1~3) to obtain a second reactive impregnation slurry, which is used to impregnate porous C / C preforms with puncture structure.

6. The preparation method according to claim 5, characterized in that, In step S1, the pyrolysis-reaction treatment includes two stages: the first stage involves pyrolysis at 800~1000℃ for 0.5~2h, and the second stage involves reaction at 1200~1500℃ for 1~2h. The impregnation, cross-linking curing, and pyrolysis treatments are repeated 2 to 4 times; the densities of both the first C / C-TiC-MAX preform and the second C / C-TiC-MAX preform are 1.20–1.60 g / cm³. 3 The open area ratio is 15% to 40%.

7. The preparation method according to claim 1, characterized in that, In step S2, the mass ratio of Si powder to TiAl powder in the first infiltration agent is (14~17):(1~3); the mass ratio of Si powder to TiAl powder in the second infiltration agent is (12~14):(3~6).

8. The preparation method according to claim 1, characterized in that, In step S2, the temperature of the pressure reaction melting treatment is 1450-1750℃, the holding time is 1-2.5h, and in the last hour of holding, the pressure is increased to 5-15MPa at a pressurization rate of 0.15-0.4MPa / min, and then the pressure is maintained until the end of the holding time. Finally, the temperature is reduced while maintaining the pressure.

9. A ceramic matrix composite friction pair, characterized in that, Includes a hard ceramic phase enrichment friction disk A and a MAX phase enrichment friction disk B prepared by the preparation method according to any one of claims 1 to 8, which are paired with each other; The hard ceramic phase enriched friction disk A uses a sandwich-structured porous C / C preform as a reinforcing skeleton, and its friction working surface is a relative enrichment area of ​​TiC and SiC hard ceramic phases. The MAX phase-enriched friction disk B uses a puncture-structured porous C / C blank as a reinforcing skeleton, and its friction working surface is a Ti2AlC and / or Ti3AlC2 relatively enriched region.

10. The application of the ceramic matrix composite friction pair as described in claim 9 in high-energy friction braking components, aerospace braking components, vehicle braking components, clutch friction components, or wear-resistant structural components.

Citation Information

Patent Citations

  • A ceramic matrix composite material with high matrix toughness and preparation method thereof

    CN118206384B