A deep blue light hlct material based on symmetrical structure containing tetrafluorobenzene and application thereof
Patent Information
- Application Number
- CN202611310850.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-24
AI Technical Summary
然而,目前实现深蓝光HLCT的电子给体单元比较有限,主要为菲并咪唑、喹喔啉等具有较大共轭体系的基团
Smart Images

Figure CN123151802A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of new materials and organic electroluminescence technology, specifically relating to a deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene and its application. Background Technology
[0002] Organic light-emitting diodes (OLEDs), with their unique advantages such as self-illumination, high contrast, thinness, and flexibility, have been widely used in smartphones, tablets, televisions, wearable devices, and flexible displays, representing a core development direction for next-generation display and lighting technologies. Deep blue light, as the core foundation of the RGB three primary colors, directly determines the color gamut coverage and color reproduction of display devices. Currently, the high-end display industry has an increasingly urgent demand for deep blue light-emitting devices with wide color gamut and high color purity, particularly imposing extremely stringent standards on the luminous efficiency and color purity of organic deep blue light-emitting materials. The Ultra High Definition Display Wide Color Gamut Standard (BT.2020) established by the Radiocommunication Sector of the International Telecommunication Union in 2012 requires a CIE color coordinate y-value (CIE value) for blue light. y The value is less than 0.046. However, current commercial deep blue light emission systems generally suffer from key problems such as low exciton utilization efficiency, severe spectral redshift, excessive full width at half maximum (FWHM), and poor color purity, which seriously restrict the development of deep blue OLED devices.
[0003] Currently, commercially available OLED luminescent materials mainly fall into two categories: traditional fluorescent materials and precious metal phosphorescent materials. Traditional deep blue fluorescent materials can only utilize 25% of singlet excitons, resulting in extremely low exciton utilization and difficulty in improving device luminous efficiency. While deep blue phosphorescent materials can achieve 100% theoretical quantum efficiency, their preparation is highly dependent on rare precious metals such as iridium and platinum, leading to high raw material costs. Furthermore, deep blue phosphorescent materials have low stability, failing to meet the requirements for commercial applications. Thermally activated delayed fluorescence (TADF) deep blue materials do not require precious metals and can improve efficiency through exciton reverse transitions. However, the pure charge transfer (CT) characteristics result in severe relaxation of the excited-state structure, a broad emission spectrum, and low color purity, making it difficult to meet the high color accuracy requirements of deep blue light for high-end displays.
[0004] The proposed hybrid local charge transfer (HLCT) luminescence mechanism provides a novel technological path for the development of high-performance deep blue luminescent materials. HLCT materials combine the narrow-spectrum luminescence characteristics of locally excited (LE) states with the high exciton utilization of charge transfer (CT) states, fully utilizing high-energy triplet excitons to achieve efficient radiative transitions. This allows for the simultaneous achievement of high exciton utilization, high color purity, and low efficiency roll-off in deep blue light materials, making it an ideal luminescent system for constructing high-performance pure deep blue OLED devices. Currently reported HLCT deep blue light materials mostly employ asymmetric donor-acceptor (DA) or DA-D' structures, where the electron acceptor unit plays a decisive role in the emission color. However, the electron donor units for realizing deep blue HLCT are currently limited, mainly consisting of groups with large conjugated systems such as phenanimazole and quinoxaline. These electron acceptors result in large molecular conjugated systems and longer molecular long axis dimensions. Larger delocalized π-electron clouds reduce the molecular band gap, causing a redshift in the molecular emission spectrum, making it difficult to stably maintain deep blue light emission characteristics. Therefore, how to suppress spectral redshift while ensuring efficient HLCT process through molecular design is a technical challenge that urgently needs to be solved in this field. Summary of the Invention
[0005] This invention aims to at least solve one of the aforementioned technical problems existing in the prior art. To this end, this invention provides a symmetrical deep blue HLCT material based on tetrafluorobenzene, which uses tetrafluorobenzene as the electron acceptor unit and constructs a symmetrical deep blue HLCT material by introducing different electron donor units. This design strategy retains the design advantages of the classic DAD molecular framework, which is conducive to maintaining efficient reverse intersystem crossing processes, thereby ensuring high fluorescence quantum efficiency of the luminescent material; and by compressing the acceptor conjugation range and shortening the molecular long axis, it effectively suppresses spectral redshift and increases the proportion of locally excited components, thus achieving high efficiency in both doped and undoped processes, and maintaining high CIE color coordinates. y The high-efficiency blue light emission of less than 0.046 solves the technical problem that existing deep blue light emitting materials cannot achieve both high exciton utilization and high color purity.
[0006] The present invention also provides an organic electroluminescent device comprising the above-mentioned materials and a method for preparing the same.
[0007] The first aspect of the present invention provides a symmetrical deep blue HLCT material based on a tetrafluorobenzene-containing structure, the structure of which is shown in general formula (I): (I), Wherein, R is an aromatic ring or aromatic heterocyclic substituent.
[0008] The technical solution of this invention regarding a symmetrical deep blue HLCT material containing tetrafluorobenzene has at least the following beneficial effects: The material of this invention uses tetrafluorobenzene as the electron acceptor unit and constructs a symmetrical DAD structure. Compared with existing HLCT materials that use large conjugated electron acceptors such as phenanthreneimidazole and quinoxaline, the tetrafluorobenzene acceptor significantly reduces the conjugation range and long axis size of the molecule, thereby effectively suppressing the redshift of the emission spectrum. Simultaneously, the symmetrical DAD framework facilitates efficient reverse intersystem crossing, allowing the material to fully utilize triplet excitons and possess high fluorescence quantum efficiency. Therefore, the material of this invention, while maintaining the advantages of efficient exciton utilization in HLCT materials, significantly improves the purity of the emission color, meeting the BT.2020 standard for deep blue light (CIE). y The stringent requirement is <0.046).
[0009] According to some embodiments of the present invention, R is selected from any one of the following groups: , R1 and R2 are the same and are selected from H atoms, halogen atoms, methyl, tert-butyl, dimethylamine or trifluoromethyl, respectively.
[0010] According to some embodiments of the present invention, R is a carbazole group, and the structural formula of the deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene is: .
[0011] According to some embodiments of the present invention, R is a diphenylamino group, and the structural formula of the deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene is: .
[0012] A second aspect of the present invention provides an organic electroluminescent device comprising an anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a cathode layer, wherein the light-emitting layer comprises the deep blue HLCT material based on a symmetric structure containing tetrafluorobenzene provided in the first aspect of the present invention.
[0013] The technical solution of this invention concerning organic electroluminescent devices has at least the following beneficial effects: The organic electroluminescent device of the present invention utilizes the aforementioned deep blue HLCT material with high color purity and high fluorescence quantum efficiency as the emitting layer. Therefore, the device can achieve high-efficiency, high-color-purity deep blue light emission. Furthermore, because the HLCT material can fully utilize high-energy triplet excitons, the efficiency roll-off of the device is effectively suppressed. This device can meet the performance requirements of high-end displays for deep blue light sources.
[0014] According to some embodiments of the present invention, the light-emitting layer comprises a host material and a dopant material, wherein the dopant material is the aforementioned deep blue HLCT material based on a symmetric structure containing tetrafluorobenzene. The host material typically has a higher triplet energy level, which can effectively prevent energy backflow and efficiently transfer energy to the dopant material, thereby further improving the luminous efficiency of the device.
[0015] According to some embodiments of the present invention, the doping concentration of the doped material is 20wt% to 40wt%. More preferably, the doping concentration of the doped material is any value of 20wt%, 30wt%, 40wt%, or a range formed by any two of them. For example, when the doping concentration is 20wt%, 30wt%, or 40wt%, the device can obtain good energy transfer efficiency and light emission performance.
[0016] According to some embodiments of the present invention, the host material includes an electron blocking layer material or a hole blocking layer material. Using the same or similar material as the host material as adjacent functional layers helps to simplify the device structure and improve energy level matching and carrier transport between layers.
[0017] According to some embodiments of the present invention, the hole-blocking layer is made of one of the following: oxadiazole compounds, quinoxaline compounds, nitrogen-containing heterocyclic compounds, phosphoxy compounds, anthracene compounds, organoboron materials, or organosulfur materials. These materials typically have deep highest occupied molecular orbital (HOMO) energy levels and high triplet energy levels, which can effectively block holes and limit exciton recombination within the luminescent layer.
[0018] According to some embodiments of the present invention, the material of the electron blocking layer is one of carbazole compounds, aromatic triamine compounds, star-shaped triphenylamine compounds, furan compounds, or spiro compounds.
[0019] According to some embodiments of the present invention, the hole blocking layer is made of 2,8-bis(diphenylphospho)dibenzo[b,d]furan (PPF).
[0020] A third aspect of the present invention provides a method for preparing an organic electroluminescent device as described in the second aspect of the present invention, comprising the following steps: moving a substrate into a vacuum coating chamber, preparing the anode layer, hole injection layer, hole transport layer, electron blocking layer, light-emitting layer, hole blocking layer, electron transport layer, electron injection layer and cathode layer sequentially by dry method, and then encapsulating under a protective atmosphere to obtain the organic electroluminescent device.
[0021] The technical solution of the present invention regarding the fabrication method of organic electroluminescent devices has at least the following beneficial effects: The preparation method of this invention employs dry processes such as vacuum evaporation, which can precisely control the thickness and composition of each functional layer, ensuring the uniformity and stability of the device. This method is mature, simple to operate, and suitable for industrial production.
[0022] According to some embodiments of the present invention, the dry preparation is achieved by one or more of the following methods: vacuum evaporation, solution spin coating, ion plating, DC sputtering, radio frequency sputtering, ion beam sputtering, ion beam assisted deposition, plasma-enhanced chemical vapor deposition, and high-density inductively coupled plasma source chemical vapor deposition. Attached Figure Description
[0023] Figure 1 These are schematic diagrams of the structures of the two devices prepared in the examples.
[0024] Figure 2 Voltage-current density-brightness and brightness-EQE plots of undoped OLED devices prepared from the product of Example 1, with the inset being the EL spectrum.
[0025] Figure 3 The figures show the voltage-current density-brightness and brightness-EQE plots of the doped OLED device prepared from the product of Example 2, with the inset being the EL spectrum. Detailed Implementation
[0026] In a first aspect, some embodiments of the present invention provide a deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene. The initial design of this material aims to address the technical problem of existing deep blue HLCT materials, which, due to the use of large conjugated electron acceptor units (such as phenanthroline and quinoxaline), result in a large molecular conjugation system and a long long axis, leading to a redshift in the emission spectrum and making it difficult to maintain deep blue light emission characteristics. The solution proposed in this invention is to use tetrafluorobenzene as the electron acceptor unit and construct a DAD symmetrical structure. As the simplest single-ring benzene skeleton, tetrafluorobenzene, through the strong electron-withdrawing inductive effect of four fluorine atoms, regulates the electron cloud distribution of the benzene ring, endowing it with electron acceptor properties, thereby fundamentally compressing the conjugated range of the acceptor and shortening the molecular long axis. Simultaneously, the DAD symmetrical structure can maintain efficient intramolecular charge transfer and reverse intersystem crossing processes. This design not only ensures the efficient utilization of triplet excitons in the HLCT material but also suppresses the spectral redshift through molecular structure optimization, thus achieving a balance between high color purity and high efficiency.
[0027] In a second aspect, some embodiments of the present invention provide an organic electroluminescent device. This device includes, as described in the first aspect, a symmetrical deep blue HLCT material containing tetrafluorobenzene as the core component of its emitting layer. This device aims to solve the problems of poor color purity, low efficiency, and severe roll-off in existing deep blue OLED devices. By employing the high-performance emitting material of the present invention, it achieves high color purity, high efficiency, and low roll-off deep blue light emission. The device, from bottom to top, comprises an anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, an emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a cathode layer.
[0028] In conjunction with the second aspect, in some embodiments of the present invention, the light-emitting layer may consist solely of the HLCT material of the present invention, thus constituting an undoped device. This undoped device has a simple structure, low fabrication cost, and avoids problems related to doping concentration control.
[0029] In conjunction with the second aspect, in some other embodiments of the present invention, the light-emitting layer can be a hybrid layer of a host material and a dopant material, wherein the dopant material is the HLCT material of the present invention, thus constituting a doped device. In a doped device, the host material typically has a higher triplet energy level, which can effectively prevent energy backflow and efficiently transfer energy to the dopant material, thereby further improving the luminous efficiency of the device.
[0030] In some embodiments of the second aspect, the hole injection layer is made of an organic conductive polymer material, poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) (PEDOT:PSS), or a metal oxide material, molybdenum trioxide (MoO3), or hexaazatriphenylhexanitrile (HATCN). For example, in specific embodiments A and B, HATCN is used as the hole injection layer material.
[0031] In some embodiments of the second aspect, the material of the hole transport layer is one of carbazole compounds, aromatic triamine compounds, star-shaped triphenylamine compounds, furan compounds, or spiro compounds. For example, carbazole compounds can be 1,3-bis(carbazole-9-yl)benzene (MCP), 9-(3-(9H-carbazole-9-yl)phenyl)-9H-carbazole-3-carboxynitrile (MCPCN), 4,4',4''-tris(carbazole-9-yl)triphenylamine (TCTA), 4,4'-bis(carbazole-9-yl)biphenyl (CBP), or 3,3-bis(9H-carbazole-9-yl)biphenyl (mCBP). Aromatic triamine compounds can be di-[4-(N,N-bitoluene-amino)-phenyl]cyclohexane (TAPC). Star-shaped triphenylamine compounds can be one of the star-shaped triphenylamine compounds containing a phenyl group (TDAB series), triphenylamine (PTDATA series), or 1,3,5-triphenylbenzene (TDAPB series) at the molecular center. For example, in specific embodiments A and B, TAPC is used as the hole transport layer material.
[0032] In some embodiments of the second aspect, the electron blocking layer is made of one of carbazole compounds, aromatic triamine compounds, star-shaped triphenylamine compounds, furan compounds, or spiro compounds. For example, carbazole compounds can be 1,3-bis(carbazole-9-yl)benzene (MCP), 9-(3-(9H-carbazole-9-yl)phenyl)-9H-carbazole-3-carboxynitrile (MCPCN), 4,4',4''-tris(carbazole-9-yl)triphenylamine (TCTA), 4,4'-bis(carbazole-9-yl)biphenyl (CBP), or 3,3-bis(9H-carbazole-9-yl)biphenyl (mCBP). Aromatic triamine compounds can be di-[4-(N,N-bitoluene-amino)-phenyl]cyclohexane (TAPC). Star-shaped triphenylamine compounds can be one of the star-shaped triphenylamine compounds containing a phenyl group (TDAB series), triphenylamine (PTDATA series), or 1,3,5-triphenylbenzene (TDAPB series) at the molecular center. For example, in specific embodiments A and B, mCBP is used as the electron blocking layer material.
[0033] In some embodiments of the second aspect, the hole-blocking layer is made of one of the following: oxadiazole compounds, quinoxaline compounds, nitrogen-containing heterocyclic compounds, phosphooxy compounds, anthracene compounds, organoboron materials, or organosulfur materials. For example: oxadiazole compounds include 2-(4-diphenyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (PBD) or 1,3-bis[2-(4-tert-butylphenyl)-1,3,4-oxadiazole-5-yl]benzene (OXD-7); nitrogen-containing heterocyclic compounds include 1,3,5-(triN-phenyl-2-benzimidazole-2)benzene (TPBi), 1,3,5-tris(3-pyridyl-m-phenyl)benzene (TmPyPB), 4,7-bidiphenyl-1,10-o-diazaphenanthrene (Bphen), 2,9-dimethyl-4,7-bidiphenyl-1,10-o-diazaphenanthrene (BCP), 3-(4-diphenyl)-4-benzene-5-tert-butylphenyl-1,2,4-benztriazole (TAZ), 3,5,3'',5''-tetra-3- Pyridine-[1,1';3',1'']terphenyl (B3PyPB), 3-(diphenylphosphochloro)-9-benzyl-9H-carbazole (PPO1) or 3,6-bis(diphenylphosphochloro)-9-benzyl-9H-carbazole (PPO2); phosphonooxy compounds are 2,8-bis(diphenylphosphoyl)dibenzo[b,d]furan (PPF), di(2-(diphenylphospho)phenyl)ether oxide (DPEPO) or 2,8-bis(xylphospho)thiofluorene (PO15); anthracene compounds are 9,10-di-(2-naphthyl)anthracene (AND); organoboron materials are tris(2,4,6-trimethyl-3-(pyridine-3-yl)phenyl)borane (3TPYMB); organosulfur materials are 2,8-bis(xylphospho)thiofluorene (PO15). For example, in devices A and B of the specific embodiments, PPF is used as the hole blocking layer material. PPF is a phosphonooxy compound with a deep HOMO level and a high triplet level, which can effectively block holes.
[0034] In some embodiments of the second aspect, the material of the electron transport layer is one of a metal complex, an oxadiazole compound, a quinoxaline compound, a nitrogen-containing heterocyclic compound, a phosphoxy compound, an anthracene compound, an organoboron material, or an organosulfur material. For example, the metal complex is aluminum 8-hydroxyquinoline (Alq~3~), bis(2-methyl-8-hydroxyquinoline)(p-phenylphenol)aluminum (BAlq), bis(10-hydroxybenzo[h]quinoline)beryllium (Bebq~2~), or bis[2-(2-hydroxyphenyl-1)-pyridine]beryllium (Bepp~2~); the oxadiazole compound is 2-(4-diphenyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (PBD) or 1,3 -Bis[2-(4-tert-butylbenzene)-1,3,4-oxadiazole-5-yl]benzene (OXD-7); nitrogen-containing heterocyclic compounds include 1,3,5-(trisN-phenyl-2-benzimidazole-2)benzene (TPBi), 1,3,5-tris(3-pyridyl-m-phenyl)benzene (TmPyPB), 4,7-biphenyl-1,10-o-diazaphenanthrene (Bphen), and 2,9-dimethyl-4,7-biphenyl-1,10-o-diazaphenanthrene (BC). P), 3-(4-diphenyl)-4-benzene-5-tert-butylbenzene-1,2,4-benztriazole (TAZ), 3,5,3'',5''-tetra-3-pyridine-[1,1';3',1'']terphenyl (B3PyPB), 3-(diphenylphosphochlorophosphate)-9-benzene-9H-carbazole (PPO1) or 3,6-bis(diphenylphosphochlorophosphate)-9-benzene-9H-carbazole (PPO2); the phosphonooxy compound is 2,8-bis(diphenylphosphoyl) The electron transport layer material can be 2,8-dibenzo[b,d]furan (PPF), di(2-(diphenylphosphino)phenyl)ether oxide (DPEPO), or 2,8-di(xylylphosphonic acid)thiofluorene (PO15); the anthracene compound is 9,10-di-(2-naphthyl)anthracene (AND); the organoboron material is tris(2,4,6-trimethyl-3-(pyridin-3-yl)phenyl)borane (3TPYMB); and the organosulfur material is 2,8-di(xylylphosphonic acid)thiofluorene (PO15). For example, in specific embodiments A and B, TmPyPB is used as the electron transport layer material.
[0035] In some embodiments of the second aspect, the electron injection layer is a very thin buffer insulating layer, such as lithium fluoride (LiF) or lithium 8-hydroxyquinoline (LiQ). For example, in specific embodiments A and B, LiQ is used as the electron injection layer material.
[0036] In some embodiments of the second aspect, the cathode layer is a low work function metal material such as lithium, magnesium, calcium, strontium, aluminum, indium, or an alloy thereof with copper, gold, or silver. For example, in specific embodiments A and B, metal Al is used as the cathode layer material.
[0037] In a third aspect, some embodiments of the present invention provide a method for fabricating the aforementioned organic electroluminescent device. This method aims to fabricate a high-performance deep blue light-emitting device using a controllable and efficient process. The method mainly includes: moving a substrate into a vacuum deposition chamber, and sequentially fabricating an anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a cathode layer using a dry deposition process, followed by encapsulation under a protective atmosphere.
[0038] In conjunction with the third aspect, in a specific embodiment of the present invention, a method for fabricating device A and device B is provided, comprising the following steps: First, the transparent conductive ITO glass substrate was ultrasonically cleaned using detergent, deionized water, acetone, and ethanol solutions, respectively, and then dried in an oven. The ITO film on the glass substrate serves as the anode layer of the device, with a sheet resistance of 8 Ω / sq and a film thickness of 120 nm. The dried substrate was then transferred to an oxygen plasma treatment chamber and subjected to oxygen plasma treatment for 15 minutes in a vacuum chamber at a pressure of 1 Pa.
[0039] Then, the processed transparent substrate is transferred to a high-vacuum organic evaporation chamber, and the chamber is evacuated to a pressure below 4 × 10⁻³ Pa. The organic functional layers are then deposited sequentially from bottom to top. The evaporation rate for the hole injection layer and electron injection layer is 0.02-0.05 nm / s; the evaporation rate for the hole transport layer, electron blocking layer, hole blocking layer, and electron transport layer is 0.5-0.8 nm / s. For the light-emitting layer of device A, only 4F-Ph-Cz is deposited at a rate of 0.05-0.08 nm / s. For the light-emitting layer of device B, both the host material PPF and the dopant material 4F-Ph-Cz are co-deposited, with the PPF deposition rate at 0.5-0.8 nm / s and the 4F-Ph-Cz deposition rate at 0.05-0.08 nm / s. A doping concentration of 40 wt% is achieved by controlling the ratio of their deposition rates. The deposition rate for aluminum (cathode) is 1-5 nm / s. The deposition rate and thickness are monitored by a film thickness gauge installed near the substrate.
[0040] Finally, the prepared device is transferred to a nitrogen-filled glove box for encapsulation, thus obtaining the organic electroluminescent device.
[0041] In other embodiments of the preparation method of the present invention, each functional layer can also be formed by solution spin coating, ion plating, DC sputtering coating, radio frequency sputtering coating, ion beam sputtering coating, ion beam assisted deposition, plasma-enhanced chemical vapor deposition, high-density inductively coupled plasma source chemical vapor deposition, etc.
[0042] The following will clearly and completely describe the concept and technical effects of the present invention with reference to specific embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.
[0043] In the description of this invention, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0044] Unless otherwise specified, "room temperature" in this invention means 25℃±5℃.
[0045] Unless otherwise specified, "about" in this invention means that the allowable error is within ±2%.
[0046] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0047] Example 1 The present invention provides a symmetrical deep blue HLCT material containing tetrafluorobenzene, wherein the R group is a carbazole group, and the resulting target product is named 4F-Ph-Cz, with the following structure:
[0048] Synthesis steps of 4F-Ph-Cz: 1,4-Dibromotetrafluorobenzene (0.50 g, 1.62 mmol) and 4-(9H-carbazolyl)phenylboronic acid (1.12 g, 3.9 mmol) were added to a 250 mL reaction flask, followed by 2M potassium carbonate aqueous solution (2.9 mL), ethanol (3 mL), and toluene (20 mL). The mixture was bubbled with argon for 30 min to remove oxygen, then Pd(PPh3)4 was added, and argon was continued for another 20 min. The mixture was refluxed at 105 °C for 12 h. After cooling, the mixture was extracted three times with dichloromethane-water, and the organic phase was concentrated by rotary evaporation. The crude product was mixed with 300-mesh silica gel and purified by column chromatography (DCM / petroleum ether = 1:4, v / v). The collected liquid was evaporated to dryness and then vacuum dried for 24 h to obtain the product 4F-Ph-Cz.
[0049] Undoped organic electroluminescent devices were fabricated using 4F-Ph-Cz as the emitting layer. The structure of the device is as follows: Figure 1 As shown in (a), the hole injection layer in the device structure is HATCN, the hole transport layer is TAPC, the electron blocking layer is mCBP, the hole blocking layer is PPF, the electron transport layer is TmPyPB, the electron injection layer is LiQ, and the cathode layer is Al. The entire device structure is as follows: Glass substrate / ITO / HATCN (5nm) / TAPC (30nm) / mCBP (5nm) / 4F-Ph-Cz (15nm) / PPF (5nm) / TmPyPB (40nm) / LiQ (1nm) / Al (100nm), where the values in parentheses are the thicknesses of each layer of the device and are labeled as device A.
[0050] The fabrication methods of undoped and doped organic electroluminescent devices in this embodiment include the following steps: ① The transparent conductive substrate ITO glass was ultrasonically cleaned with detergent, deionized water, acetone and ethanol solutions respectively, and then dried in an oven. The ITO film on the glass substrate serves as the anode layer 2 of the device. The sheet resistance of the ITO film is 8Ω / sq and the film thickness is 120nm. ② The dried substrate is moved into the oxygen plasma treatment chamber and treated with oxygen plasma for 15 minutes in a vacuum chamber with a pressure of 1 Pa. ③ Transfer the treated transparent substrate into a high-vacuum organic evaporation chamber and evacuate it until the pressure reaches 4×10⁻⁶. -3 Below Pa, organic functional layers are deposited sequentially from bottom to top, including a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a cathode layer. The deposition rate of the hole injection layer and the electron injection layer is 0.02-0.05 nm / s; the deposition rate of the hole transport layer, the electron blocking layer, the hole blocking layer, and the electron transport layer is 0.5-0.8 nm / s; the deposition rate of 4F-Ph-Cz in the light-emitting layer is 0.05-0.08 nm / s; and the deposition rate of aluminum is 1-5 nm / s. The deposition rate and thickness are monitored by a film thickness gauge installed near the substrate. ④ The prepared device is transferred to a nitrogen-filled glove box for packaging, thus obtaining the organic electroluminescent device.
[0051] The photoelectric properties and electroluminescence spectrum of the organic electroluminescent device were tested, and the results are shown in Table 1 and... Figure 2 As shown in Table 1, the photoelectric performance parameters of device A in Example 1 are presented.
[0052] Table 1 Summary of OLED device performance data prepared from the products of Example 1
[0053] As can be seen from the results in Tables 1 and 2, when the deep blue HLCT luminescent material 4F-Ph-Cz described in this invention is used to prepare undoped organic electroluminescent devices, it achieves a maximum external quantum efficiency (EQE) of 6.2%, a half-wavelength of 50 nm, and a CIE y-value of 0.035, which meets the requirements of high-definition displays for deep blue light (CIE y-value < 0.046).
[0054] Example 2 The present invention provides a symmetrical deep blue HLCT material containing tetrafluorobenzene, wherein the R group is a carbazole group, and the target product obtained is named 4F-Ph-Cz.
[0055] 4F-Ph-Cz was used as the light-emitting layer to fabricate a doped organic electroluminescent device. The structure of the device is as follows: Figure 1 As shown in (b), the hole injection layer in the device structure is HATCN, the hole transport layer is TAPC, the electron blocking layer is mCBP, the host material is PPF, the weight doping ratio of the luminescent material 4F-Ph-Cz is 40%, the hole blocking layer is PPF, the electron transport layer is TmPyPB, the electron injection layer is LiQ, and the cathode layer is Al. The entire device structure is as follows: Glass substrate / ITO / HATCN (5nm) / TAPC (30nm) / mCBP (5nm) / PPF:40wt%4F-Ph-Cz (15nm) / PPF (5nm) / TmPyPB (40nm) / LiQ (1nm) / Al (100nm), where the values in parentheses are the thicknesses of each layer of the device and are marked as device B.
[0056] The method for fabricating the doped organic electroluminescent device in this embodiment includes the following steps: ① The transparent conductive substrate ITO glass was ultrasonically cleaned with detergent, deionized water, acetone and ethanol solutions respectively, and then dried in an oven. The ITO film on the glass substrate serves as the anode layer 2 of the device. The sheet resistance of the ITO film is 8Ω / sq and the film thickness is 120nm. ② The dried substrate is moved into the oxygen plasma treatment chamber and treated with oxygen plasma for 15 minutes in a vacuum chamber with a pressure of 1 Pa. ③ Transfer the treated transparent substrate into a high-vacuum organic evaporation chamber and evacuate it until the pressure reaches 4×10⁻⁶. -3Below Pa, organic functional layers are deposited sequentially from bottom to top, including a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a cathode layer. The deposition rate of the hole injection layer and the electron injection layer is 0.02-0.05 nm / s; the deposition rate of the hole transport layer, the electron blocking layer, the hole blocking layer, and the electron transport layer is 0.5-0.8 nm / s; in the light-emitting layer, the deposition rate of the host material PPF is 0.5-0.8 nm / s, the deposition rate of the light-emitting material 4F-Ph-Cz is 0.05-0.08 nm / s; the deposition rate of aluminum is 1-5 nm / s. The deposition rate and thickness are monitored by a film thickness gauge installed near the substrate. ④ The prepared device is transferred to a nitrogen-filled glove box for packaging, thus obtaining the organic electroluminescent device.
[0057] The photoelectric properties and electroluminescence spectra of the organic electroluminescent device were tested, and the results are shown in Table 2. Figure 3 As shown in Table 2, the photoelectric performance parameters of device B in Example 2 are presented.
[0058] Table 2 Summary of OLED device performance data prepared from the products of Example 2
[0059] From Table 2 and Figure 3 The results show that when the deep blue HLCT luminescent material 4F-Ph-Cz described in this invention is used to prepare doped organic electroluminescent devices, it achieves a maximum EQE of 8.2%, a half-wavelength of 50 nm, and a CIE y-value of 0.031, which meets the requirements of high-definition displays for deep blue light (CIE y-value < 0.046).
[0060] Example 3 The present invention provides a symmetrical deep blue HLCT material containing tetrafluorobenzene, wherein the R group is a carbazole group, and the target product obtained is named 4F-Ph-Cz.
[0061] Undoped organic electroluminescent devices were fabricated using 4F-Ph-Cz as the emitting layer. The structure of the device is as follows: Figure 1 As shown in (a), the hole injection layer in the device structure is HATCN, the hole transport layer is TAPC, the electron blocking layer is mCBP, the hole blocking layer is PPF, the electron transport layer is TmPyPB, the electron injection layer is LiQ, and the cathode layer is Al. The entire device structure is as follows: Glass substrate / ITO / HATCN (5nm) / TAPC (60nm) / mCBP (5nm) / 4F-Ph-Cz (15nm) / PPF (5nm) / TmPyPB (80nm) / LiQ (1nm) / Al (100nm), where the values in parentheses are the thicknesses of each layer of the device.
[0062] The undoped organic electroluminescent device of this embodiment was prepared using the preparation method of Example 1. However, the thicknesses of the hole transport layer and electron transport layer in the light-emitting unit of this embodiment are different from those in Example 1.
[0063] Example 4 The present invention provides a symmetrical deep blue HLCT material containing tetrafluorobenzene, wherein the R group is a carbazole group, and the target product obtained is named 4F-Ph-Cz.
[0064] 4F-Ph-Cz was used as the light-emitting layer to fabricate a doped organic electroluminescent device. The structure of the device is as follows: Figure 1 As shown in (b), the hole injection layer in the device structure is HATCN, the hole transport layer is TAPC, the electron blocking layer is mCBP, the host material is PPF, the weight doping ratio of the luminescent material 4F-Ph-Cz is 40%, the hole blocking layer is PPF, the electron transport layer is TmPyPB, the electron injection layer is LiQ, and the cathode layer is Al. The entire device structure is as follows: Glass substrate / ITO / HATCN (5nm) / TAPC (30nm) / mCBP (5nm) / PPF:20wt%4F-Ph-Cz (15nm) / PPF (5nm) / TmPyPB (40nm) / LiQ (1nm) / Al (100nm), where the values in parentheses are the thicknesses of each layer of the device.
[0065] The doped organic electroluminescent device of this embodiment was prepared using the preparation method of Example 2, wherein the doping concentration of the luminescent material in the luminescent unit of this embodiment is different from that in Example 2.
[0066] Example 5 The present invention provides a symmetrical deep blue HLCT material containing tetrafluorobenzene, wherein the R group is a diphenylamine group, and the resulting target product is named 4F-Ph-TPA. The structural formula is as follows: .
[0067] The synthesis steps of 4F-Ph-TPA were as follows: 1,4-Dibromotetrafluorobenzene (0.50 g, 1.62 mmol) and 4-(diphenylamino)phenylboronic acid (1.12 g, 3.9 mmol) were placed in a 250 mL reaction flask, and 2.9 mL of 2MK2CO3 aqueous solution, 3 mL of ethanol, and 20 mL of toluene were added. After purging with argon gas for 30 min to remove oxygen, Pd(PPh3)4 was added, and argon gas was continued for 20 min. The mixture was then refluxed at 105 °C for 12 h. After cooling, the mixture was extracted three times with dichloromethane-water, and the organic phase was concentrated by rotary evaporation. The crude product was purified by column chromatography (DCM / petroleum ether = 1:4, v / v) by mixing with 300 mesh silica gel. The collected fraction was evaporated to dryness and then dried under vacuum for 24 h to obtain the product 4F-Ph-TPA.
[0068] Undoped organic electroluminescent devices were fabricated using 4F-Ph-TPA as the emitting layer. The device structure is as follows: Figure 1 As shown in (a), the hole injection layer in the device structure is HATCN, the hole transport layer is TAPC, the electron blocking layer is mCBP, the hole blocking layer is PPF, the electron transport layer is TmPyPB, the electron injection layer is LiQ, and the cathode layer is Al. The entire device structure is as follows: Glass substrate / ITO / HATCN (5nm) / TAPC (60nm) / mCBP (5nm) / 4F-Ph-TPA (15nm) / PPF (5nm) / TmPyPB (80nm) / LiQ (1nm) / Al (100nm), where the values in parentheses are the thicknesses of each layer of the device.
[0069] The undoped organic electroluminescent device of this embodiment was prepared using the preparation method of Example 1.
[0070] Example 6 The present invention provides a symmetrical deep blue HLCT material containing tetrafluorobenzene, wherein the R group is a carbazole group and a diphenylamine group, and the target product obtained is named 4F-Ph-TPA.
[0071] 4F-Ph-TPA was used as the light-emitting layer to fabricate a doped organic electroluminescent device. The structure of the device is as follows: Figure 1 As shown in (b), the hole injection layer in the device structure is HATCN, the hole transport layer is TAPC, the electron blocking layer is mCBP, the host material is PPF, the luminescent material 4F-Ph-TPA has a weight doping ratio of 40%, the hole blocking layer is PPF, the electron transport layer is TmPyPB, the electron injection layer is LiQ, and the cathode layer is Al. The entire device structure is as follows: Glass substrate / ITO / HATCN (5nm) / TAPC (30nm) / mCBP (5nm) / PPF:20wt%4F-Ph-TPA (15nm) / PPF (5nm) / TmPyPB (40nm) / LiQ (1nm) / Al (100nm), where the values in parentheses are the thicknesses of each layer of the device.
[0072] The doped organic electroluminescent device of this embodiment was prepared using the preparation method of Example 2.
[0073] The present invention has been described in detail above with reference to the embodiments. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A deep blue HLCT material based on a symmetric structure containing tetrafluorobenzene, characterized in that, The structure is shown in general formula (I): (I), Wherein, R is an aromatic ring or aromatic heterocyclic substituent.
2. The deep blue HLCT material based on a symmetric structure containing tetrafluorobenzene according to claim 1, characterized in that, R is selected from any of the following groups: , R1 and R2 are the same and are selected from H atoms, halogen atoms, methyl, tert-butyl, dimethylamine or trifluoromethyl, respectively.
3. The deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene according to claim 1, characterized in that, R is a carbazole group, and the structural formula of the deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene is: 。 4. The deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene according to claim 1, characterized in that, R is a diphenylamine group, and the structural formula of the deep blue HLCT material based on a symmetrical structure containing tetrafluorobenzene is: 。 5. An organic electroluminescent device, characterized in that, It includes an anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a cathode layer, wherein the light-emitting layer comprises a deep blue HLCT material based on a symmetric structure containing tetrafluorobenzene as described in any one of claims 1-4.
6. The organic electroluminescent device according to claim 5, characterized in that, The light-emitting layer comprises a host material and a doped material, wherein the doped material is any one of the symmetrical deep blue HLCT materials containing tetrafluorobenzene according to claims 1-4.
7. The organic electroluminescent device according to claim 6, characterized in that, The doping concentration of the doped material is 20wt%~40wt%.
8. The organic electroluminescent device according to claim 6, characterized in that, The main material includes an electron blocking layer material or a hole blocking layer material.
9. The organic electroluminescent device according to claim 8, characterized in that, The hole-blocking layer is made of one of the following: oxadiazole compounds, quinoxaline compounds, nitrogen-containing heterocyclic compounds, phosphooxy compounds, anthracene compounds, organoboron materials, or organosulfur materials; and / or, the electron-blocking layer is made of one of the following: carbazole compounds, aromatic triamine compounds, astral triphenylamine compounds, furan compounds, or spiro compounds.
10. A method for preparing an organic electroluminescent device as described in any one of claims 5-9, characterized in that, Includes the following steps: The substrate is moved into a vacuum coating chamber, and the anode layer, hole injection layer, hole transport layer, electron blocking layer, light-emitting layer, hole blocking layer, electron transport layer, electron injection layer and cathode layer are prepared sequentially by dry process. Then, the substrate is encapsulated under a protective atmosphere to obtain the organic electroluminescent device.