A hole blocking material based on fluorane, its preparation method and electroluminescent device

By using fluorane as the parent material for hole blocking, and through the mono-substitution design of electron-withdrawing groups, the thermal stability and compatibility issues of traditional hole blocking materials in high-end display devices have been solved, achieving a highly efficient and stable hole blocking effect and improving the luminous efficiency and lifespan of the devices.

CN123151884APending Publication Date: 2026-11-24西安欧得光电材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611395927.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing hole-blocking materials suffer from poor thermal stability, easy crystallization, significant efficiency roll-off, rapid decay, and poor adaptability in high-end display devices, failing to meet the requirements for ultra-high brightness, long lifespan, and flexible displays.

Method used

Using fluorane as the parent material, a hole-blocking barrier is constructed by introducing electron-withdrawing groups into the fluorane molecule for monosubstitution, precisely controlling the HOMO energy level, and building a high hole-blocking barrier. Combined with excellent electron transport properties, a stable amorphous film is formed, which inhibits molecular crystallization and interfacial charge accumulation.

Benefits of technology

It significantly improves the luminous efficiency and lifespan of the device, reduces the driving voltage and efficiency roll-off, and enhances the device's operational stability under high brightness and high current conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123151884A_ABST
    Figure CN123151884A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of organic light-emitting materials and semiconductor technology, specifically relating to a hole-blocking material based on fluorane, its preparation method, and an electroluminescent device. The structural formula of the hole-blocking material based on fluorane is shown in Formula 1. This invention employs a molecular configuration with a single-sided electron-withdrawing group monosubstituted on the spirocycloxanthone (fluorane) matrix. As a hole-blocking material, it can reduce the efficiency roll-off and decay rate of electroluminescent devices, thereby improving adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organic light-emitting materials and semiconductor technology, specifically relating to a hole-blocking material based on fluorane, its preparation method, and an electroluminescent device. Background Technology

[0002] Novel optoelectronic materials are the core foundation for driving the iterative upgrade of display technology. Current electroluminescent devices generally employ a multi-layered functional structure, mainly including a hole injection layer, a hole transport layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a light-emitting layer. The core function of each functional layer is to balance the transport rates of electrons and holes, promote the effective recombination of charge carriers within the light-emitting layer, improve exciton utilization, and thus enhance the luminous efficiency and lifespan of the electroluminescent device.

[0003] Among the many functional layers, the hole blocking layer (HBL) is a key structure for regulating carrier behavior and optimizing the performance of electroluminescent devices. During the operation of an electroluminescent device, the hole migration rate is significantly higher than that of electrons. A large number of unrecombined holes can easily penetrate the light-emitting layer and migrate to the electron transport layer and the cathode interface. This not only leads to insufficient carrier recombination and decreased luminous efficiency, but also causes interface charge accumulation and defect generation, accelerating the aging of the electroluminescent device and severely restricting the development and application of high-performance, long-life electroluminescent devices.

[0004] Hole blocking materials, relying on their unique energy level structure, construct a hole-blocking barrier, effectively preventing holes from escaping while ensuring the smooth injection of electrons into the emitting layer, achieving a balance between electron and hole transport. They can confine the carrier recombination region within the emitting layer, reducing non-radiative recombination losses and charge leakage, while also passivating interface defects and blocking external erosion, effectively improving the device's luminescent performance and operational stability.

[0005] Currently, the hole-blocking materials commonly used in commercial and research applications are mainly traditional small organic molecules such as BCP and Bphen, which possess basic hole-blocking capabilities and film-forming properties, meeting the requirements of conventional display devices. However, with the rapid development of high-end applications such as ultra-high brightness, long lifespan, and flexible displays, the drawbacks of traditional materials are gradually becoming apparent. These small molecule materials have poor thermal stability and are prone to thin-film crystallization and morphology damage under high operating intensity, leading to the failure of their hole-blocking function. At the same time, their small energy level tunability range and poor carrier matching can easily cause significant roll-off in device efficiency and rapid decay.

[0006] In addition, traditional hole blocking materials also suffer from problems such as poor interface compatibility, insufficient mechanical properties, and weak anti-aging ability, making them unsuitable for the bending conditions of flexible devices and the industrialization needs of high-end devices.

[0007] Therefore, developing novel hole-blocking materials with high stability, high efficiency, and strong adaptability has become an urgent problem to be solved in the field of electroluminescence. Summary of the Invention

[0008] To address the technical problems of existing hole-blocking materials causing significant efficiency roll-off, rapid decay, and poor adaptability in devices, this invention provides a hole-blocking material based on fluorane, its preparation method, and an electroluminescent device.

[0009] This invention is achieved through the following technical solution: In a first aspect, the present invention provides a hole-blocking material based on fluorane, wherein the structural formula of the hole-blocking material based on fluorane is shown in Formula 1:

[0010] In the formula: A is selected from C6~C 20 aryl, C3~C 20 heteroaryl groups; R1 to R5 are each independently selected from hydrogen, substituted or unsubstituted C6 to C6. 30 aryl, substituted or unsubstituted C3~C 30 The heteroaryl group, and R1 to R5 cannot all be H at the same time; R1 to R5 can be bonded to each other or not bonded; Group It is an electron-withdrawing group.

[0011] Preferably, A is selected from phenyl, naphthyl, dibenzofuranyl, triazineyl, pyrimidinyl, pyridinyl, and quinoxalyl.

[0012] The substituted or unsubstituted C6~C 30 The aryl group refers to the aryl group that can be substituted by other substituents or can remain unsubstituted. When substituted, the substituents can be selected from triazine, phenyl, cyano, trifluoromethyl, and deuterium.

[0013] The substituted or unsubstituted C3~C 30 The term "heteroaryl" refers to a heteroaryl group that can be substituted by other substituents or not. When substituted, the substituents can be selected from phenyl, naphthyl, benzonitrile, trifluorophenyl, and deuterated phenyl.

[0014] Preferably, the group in Formula 1 Selected from the following groups: .

[0015] Preferably, the hole-blocking material based on fluorane is selected from one of the following compounds: .

[0016] A second aspect of the present invention provides a method for preparing a hole-blocking material based on fluorane:

[0017] Among them, reactant l is (X is Br or Cl) structure; S1: Reactant p and A ring-closing reaction occurs to obtain intermediate Mn-1; S2: Intermediate Mn-1 undergoes a nucleophilic substitution reaction with phosphorus tribromide (PBr3) to give intermediate Mn-2; S3: Intermediate Mn-2 and pinacol diboronic acid ester The Miyaura borylation reaction occurs to give intermediate Mn; S4: Intermediate Mn and reactant l The Suzuki-Miyaura reaction occurs to obtain the hole-blocking material based on fluorane as described in this invention.

[0018] Preferably, S1 specifically uses toluene as the reaction solvent, methanesulfonic acid as the catalyst, and reactant p and A closed-loop reaction occurs, yielding intermediate Mn-1. At this point, toluene can further shift the equilibrium to the right through azeotropic water separation.

[0019] Preferably, S2 specifically involves using toluene as the reaction solvent and DMF as the catalyst. Intermediate Mn-1 undergoes a nucleophilic substitution reaction with phosphorus tribromide (PBr3) to obtain intermediate Mn-2. Toluene is used as an azeotropic solvent, which can adjust the boiling point of the system, remove the H3PO3 byproduct and trace amounts of water generated in the reaction, and promote the forward shift of the equilibrium.

[0020] Preferably, S3 is specifically: using 1,4-dioxane as solvent, Pd(dppf)Cl2 as catalyst, and KOAc as base, intermediate Mn-2 undergoes a Miyaura borylation reaction with pinacol diboronic acid to obtain intermediate Mn.

[0021] Preferably, S4 specifically comprises: using THF / H2O as solvent, Pd(PPh3)4 as catalyst, and K2CO3 as base, with intermediate Mn reacting with reactant l The Suzuki-Miyaura reaction occurs to obtain the hole-blocking material based on fluorane as described in this invention.

[0022] A third aspect of the present invention provides an electroluminescent device, comprising a cathode layer, an anode layer, and an organic layer located between the cathode layer and the anode layer. The organic layer comprises a hole injection layer (HIL), a hole transport layer, an electron blocking layer (EBL), an emission material layer (EML), a hole blocking layer (HBL), an electron transport layer, and an electron injection layer (EIL). The hole blocking layer is located between the electron transport layer and the emission layer, and the material of the hole blocking layer comprises the hole blocking material based on fluorane.

[0023] Preferably, the electroluminescent device comprises, in sequence from the anode layer to the cathode layer, a substrate, an anode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer and an electron injection layer, a cathode layer and a high-refractive-index covering protection layer (CPL).

[0024] As a substrate, it needs to have high mechanical strength, excellent thermal stability, excellent water resistance and excellent transparency; polyethylene terephthalate (PET) plastic is preferred.

[0025] As the anode layer, the anode layer material is preferably a material with a high work function in order to facilitate the injection of holes into the organic layer. Specific examples of anode layer materials that can be used in this invention include metals such as vanadium, chromium, copper, and zinc, or their alloys; oxides such as zinc oxide, aluminum oxide, or tin dioxide; and conductive polymers such as polypyrrole and polyaniline.

[0026] The materials used in the hole injection layer, hole transport layer, electron blocking layer, light emission layer, electron transport layer, and electron injection layer of this invention are selected from corresponding materials with excellent cost performance in the industry. The compatibility between each layer needs to be determined through a series of tests and screening processes.

[0027] Preferably, the material of the hole injection layer of the present invention is MoO3.

[0028] Preferably, the material of the hole transport layer of the present invention is selected from one of the following materials:

[0029] .

[0030] Preferably, the material of the electron blocking layer of the present invention is selected from one of the following materials: .

[0031] Preferably, the material of the light-emitting layer of the present invention includes a host light-emitting material and a guest light-emitting material, wherein the host light-emitting material includes a first host light-emitting material and a second host light-emitting material; wherein the first host light-emitting material is selected from... and The second main luminescent material is The mass ratio of the first and second primary luminescent materials is 30:70 to 60:40, and the accompanying guest luminescent material is... The mass fraction of the luminescent material in the luminescent layer is 2%.

[0032] Preferably, the material of the electron transport layer in this invention is selected from one of the following materials: .

[0033] Preferably, the material of the electron injection layer of the present invention is LiF.

[0034] As a cathode layer, the cathode layer material is preferably a material with a low work function in order to facilitate the injection of electrons into the functional organic layer. Specific examples of cathode layer materials that can be used in this invention include metals such as magnesium, calcium, sodium, potassium, titanium, indium, yttrium, lithium, gadolinium, aluminum, silver, tin, and lead, or their alloys, such as Mg-Al and Mg-Ag.

[0035] The high-refractive-index capping layer used in this invention can improve the refractive index of the cathode layer surface and increase the light extraction efficiency; the capping layer material is preferably made of... .

[0036] In a fourth aspect, the present invention provides a method for fabricating the above-mentioned electroluminescent device, wherein an anode layer is adhered to a substrate after pretreatment and cleaning, and then a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, and an electron injection layer of predetermined thickness are sequentially vapor-deposited under low-temperature conditions. A cathode layer and a protective coating are then sputtered at low temperature, and finally the device is packaged using conventional device packaging methods to obtain the electroluminescent device.

[0037] A fifth aspect of the present invention provides a display panel comprising the electroluminescent device as described above.

[0038] Compared with the prior art, the present invention has the following beneficial effects: The present invention adopts a molecular configuration of spirocycloxanthone (fluorane) with a single electron-withdrawing group monosubstituted on one side, which has the following technical advantages: (1) The present invention uses fluorane as the parent body and performs single substitution of electron-withdrawing groups on the parent structure of fluorane, which can accurately lower the molecular HOMO energy level, increase the energy level difference with the light-emitting layer to build a high hole blocking barrier, effectively prevent the holes of the light-emitting layer from leaking outward, and confine the exciton recombination region inside the light-emitting layer, greatly reduce the non-radiative exciton quenching at the interface, and significantly alleviate the efficiency roll-off problem of the device under high brightness. (2) The monosubstituted structure of the present invention breaks the central symmetry of the fluorane molecule, weakens the π-π stacking effect between molecules, inhibits the crystallization and aggregation of the film, maintains the stable amorphous film morphology, and improves the thermal stability of the film; at the same time, the electron-withdrawing group (e.g., triazine) can effectively guide the accumulated charge at the dispersion interface, reduce the generation of charge trapping defects, reduce the film aging rate, and extend the device lifespan; (3) The electron-withdrawing group (e.g., triazine) of the present invention has excellent electron transport characteristics. The monosubstituted design will not over-enhance the hole transport capability. While realizing the hole blocking function, it gives the molecule a balanced electron conduction performance, so that the electron and hole recombination ratio inside the light-emitting layer is matched, avoids the accumulation of excess charge carriers at the interface, and further improves the long-term working stability of the device under high current and high brightness conditions. It overcomes the inherent defects of existing hole blocking materials with obvious efficiency roll-off and fast device decay from the three dimensions of energy level, film morphology and charge carrier transport.

[0039] The electroluminescent device of the present invention uses the hole-blocking material based on fluorane as a high-efficiency hole-blocking material in the hole-blocking layer, which effectively reduces the driving voltage and efficiency roll-off, improves the luminous efficiency, and extends the service life. Attached Figure Description

[0040] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0041] Figure 1 This is a cross-sectional view of the electroluminescent device of the present invention; Figure 2 The NMR spectrum of compound 1 of the present invention is shown below. Figure 3 The NMR spectrum of compound 20 of the present invention; Figure 4 The NMR spectrum of compound 61 of the present invention; Figure 5 The figure shows the NMR spectrum of compound 67 of the present invention.

[0042] Explanation of reference numerals in the attached figures: 1-Substrate, 2-Anode layer, 3-Hole injection layer, 4-Hole transport layer, 5-Electron blocking layer, 6-Light emitting layer, 7-Hole blocking layer, 8-Electron transport layer, 9-Electron injection layer, 10-Cathode layer, 11-Cover layer. Detailed Implementation

[0043] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0044] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. Process equipment or apparatus not specifically specified in the following examples are all conventional equipment or apparatus in the art. All raw materials used in the following examples are conventional commercially available products with specifications in the art, unless otherwise stated.

[0045] In addition, those skilled in the art can refer to the following specific embodiments to prepare compounds 1 to 72.

[0046] The key reactants involved in this invention are:

[0047] .

[0048] Compound preparation example 1 (synthesis of compound 1)

[0049] Step 1: Procedure: Under nitrogen protection, reactant p1 (77.5 g, 0.3 mol), phenol (33.9 g, 0.36 mol), methanesulfonic acid (0.3 L), and toluene (0.6 L) were added sequentially to a 2.0 L three-necked flask. The mixture was heated to 65°C and stirred for 1.5 hours until the reaction was complete. The reaction solution was cooled to room temperature, and the reactants were poured into 1.0 L of ice water and stirred for 20 minutes, followed by filtration. The resulting mixture was extracted multiple times with ethyl acetate, and the organic phases were combined. The organic phase was dried over anhydrous magnesium sulfate, filtered, and concentrated. The residue was purified by silica gel column chromatography (ethyl acetate / petroleum ether = 1:3) to obtain intermediate M1-1, weighing 42.8 g, with a yield of 45.1% and an HPLC purity of 97.8%.

[0050] Step Two: Procedure: Under nitrogen protection, intermediate M1-1 (63.3 g, 0.2 mol), DMF (7.3 g, 0.1 mol), and 0.8 L of toluene were added sequentially to a 2.0 L three-necked flask. Stirring was started, and PBr3 (65 g, 0.24 mol) was slowly added dropwise. After the addition was complete, the reaction system was heated to 100 °C and reacted for 2 h until the reaction was complete. After the reaction was complete, the reaction system was cooled to room temperature, and 1.0 L of saturated sodium acetate solution was added to the reaction solution and stirred for 20 min to obtain a mixed solution. The mixed solution was extracted multiple times with ethyl acetate, and the organic phases were combined. The organic phase was dried over anhydrous magnesium sulfate, filtered, and concentrated. The residue was purified by silica gel column chromatography (ethyl acetate / petroleum ether = 1:6) to obtain intermediate M1-2, weighing 63.9 g, with a yield of 84.3% and an HPLC purity of 98.1%.

[0051] Step 3: Procedure: Under nitrogen protection, intermediate M1-2 (37.9 g, 0.1 mol), pinacol diboronic acid ester (25.4 g, 0.1 mol), potassium acetate (KOAc) (19.6 g, 0.2 mol), and 1,4-dioxane 0.5 L were added sequentially to a 1.0 L three-necked flask. Stirring was started, and the system was heated to 60 °C. Pd(dppf)Cl2 (1.46 g, 2 mmol) was then added. The temperature was then raised to 100 °C, and the reaction was continued for 8 h until intermediate M1-2 was completely reacted. After the reaction was completed, the reaction solution was directly filtered, the filtrate was collected, the filtrate was concentrated to dryness under reduced pressure, dissolved in 0.5 L of toluene and washed with water, the organic phase was dried and concentrated, and the residue was purified and separated by silica gel column chromatography (ethyl acetate / petroleum ether = 8:1). The column chromatography was concentrated under reduced pressure until solid precipitated and then stopped. After crystallization at 15 °C, the mixture was filtered and dried to obtain intermediate M1, weighing 34.2 g, with a yield of 80.3% and an HPLC purity of 98.6%.

[0052] Step Four: Procedure: Under nitrogen protection, intermediate M1 (4.3 g, 0.01 mol), compound l1 (3.9 g, 0.01 mol), 20 mL of THF, 5 mL of H2O, and K2CO3 (2.8 g, 0.02 mol) were added sequentially to a 50 mL three-necked flask. The mixture was stirred and heated to 40 °C. After the solution became clear, Pd(PPh3)4 (0.23 g, 0.2 mmol) was added, and the temperature was raised to 70 °C and the reaction was continued for 12 h. The reaction solution was cooled to room temperature, extracted with ethyl acetate, and the organic phases were combined. The organic phase was dried over anhydrous magnesium sulfate, filtered, and concentrated. The residue was purified by silica gel column chromatography (ethyl acetate / petroleum ether = 1:5) to obtain compound 1, weighing 4.6 g, with a yield of 75.3% and an HPLC purity of 99%. LC-MS (Liquid Chromatograph-Mass Spectrometer) showed a molecular weight of 607.7. The NMR spectrum of compound 1 is shown below. Figure 2 As shown.

[0053] 1H NMR data for compound 1: 1 H NMR (500 MHz, CD3OD ) δ 8.36 (s, 4H), 7.96 (s, 2H), 7.87 (s, 1H), 7.57 – 7.34 (m, 12H), 7.30 (d, J = 5.0 Hz, 3H), 7.21 (s, 2H), 7.04 (s, 1H).

[0054] Compound preparation example 2 (synthesis of compound 20)

[0055] Procedure: The synthesis of compound 20 is performed following the synthesis process from intermediate M1 to compound 1 in Compound Preparation Example 1, using reactant l 20 Replacing reactant l1 (3.9 g, 0.01 mol) with (5.1 g, 0.01 mol) yielded compound 20, weighing 5.6 g, with a yield of 76.6%, an HPLC purity of 99.3%, and an LC-MS molecular weight of 733.9. The NMR spectrum of compound 20 is shown below. Figure 3 As shown.

[0056] 1H NMR data for compound 20: 1H NMR (500 MHz, CD3OD) δ 8.95 (s, 1H), 8.47 (d, 1H) J = 28.3 Hz, 2H), 8.37 (d, J = 5.7 Hz, 5H), 8.22 (s, 1H), 7.88 (d, J = 10.0 Hz, 2H), 7.77 (d, J = 5.0 Hz, 2H), 7.57 – 7.26 (m, 16H), 7.21 (s, 1H), 7.04 (s, 1H).

[0057] Compound preparation example 3 (synthesis of compound 61)

[0058] Step 1: Procedure: The synthesis of intermediate M2-1 was performed by referring to the synthesis of intermediate M1-1 from reactant p1 in Compound Preparation Example 1. Reactant p1 (77.5 g, 0.3 mol) was replaced with reactant p2 (77.5 g, 0.3 mol) to obtain compound M2-1, weighing 40.9 g, with a yield of 43.1% and an HPLC purity of 97.1%.

[0059] Step Two: Procedure: The synthesis of intermediate M2-2 was carried out by referring to the synthesis process of intermediate M1-1 to intermediate M1-2 in Compound Preparation Example 1. Intermediate M2-2 was obtained by replacing intermediate M1-1 (63.3g, 0.2mol) with intermediate M2-1 (63.3g, 0.2mol), with a weight of 62.9g, yield of 82.9%, and HPLC purity of 98.2%.

[0060] Step 3: Procedure: The synthesis of intermediate M2 was performed by referring to the synthesis of intermediate M1-2 to intermediate M1 in Compound Preparation Example 1. Intermediate M1-2 (37.9g, 0.1mol) was replaced with intermediate M2-2 (37.9g, 0.1mol) to obtain intermediate M2, weighing 33.9g, with a yield of 79.6% and an HPLC purity of 98.5%.

[0061] Step Four: Procedure: The synthesis of compound 61 followed the synthesis process from intermediate M1 to compound 1 in Compound Preparation Example 1. Intermediate M1 (4.3 g, 0.01 mol) was replaced with intermediate M2 (4.3 g, 0.01 mol) to obtain compound 61, weighing 4.4 g, with a yield of 73.1%, HPLC purity of 99.5%, and LC-MS showing a molecular weight of 607.7. The NMR spectrum of compound 61 is shown below. Figure 4 As shown.

[0062] 1H NMR data for compound 61: 500 MHz, CD3OD 1 H NMR (500 MHz, Chloroform) δ 8.36 (s, 4H), 8.00 – 7.84 (m, 4H), 7.57 – 7.35 (m, 11H), 7.33 – 7.18 (m, 5H), 7.04 (s, 1H).

[0063] Compound preparation example 4 (synthesis of compound 67)

[0064] Step 1: Procedure: The synthesis of intermediate M3-1 was performed by referring to the synthesis of intermediate M1-1 from reactant p1 in Compound Preparation Example 1. Reactant p1 (77.5 g, 0.3 mol) was replaced with reactant p3 (77.5 g, 0.3 mol) to obtain intermediate M3-1, weighing 43.8 g, with a yield of 46.2% and an HPLC purity of 97.4%.

[0065] Step Two: Procedure: The synthesis of intermediate M3-2 was carried out by referring to the synthesis process of intermediate M1-1 to intermediate M1-2 in Compound Preparation Example 1. Intermediate M3-2 was obtained by replacing intermediate M1-1 (63.3g, 0.2mol) with intermediate M3-1 (63.3g, 0.2mol), with a weight of 64.2g, yield of 84.6%, and HPLC purity of 98.2%.

[0066] Step 3: Procedure: The synthesis of intermediate M3 was performed by referring to the synthesis of intermediate M1-2 to intermediate M1 in Compound Preparation Example 1. Intermediate M1-2 (37.9 g, 0.1 mol) was replaced with intermediate M3-2 (37.9 g, 0.1 mol) to obtain intermediate M3, weighing 35.0 g, with a yield of 82.1% and an HPLC purity of 98.7%.

[0067] Step Four: Procedure: The synthesis of compound 67 followed the synthesis process from intermediate M1 to compound 1 in Compound Preparation Example 1. Intermediate M1 (4.3 g, 0.01 mol) was replaced with intermediate M3 (4.3 g, 0.01 mol), and reactant l4 (3.9 g, 0.01 mol) was replaced with reactant l1 (3.9 g, 0.01 mol) to obtain compound 67, weighing 4.7 g, with a yield of 77.2%, HPLC purity of 99.4%, and LC-MS showing a molecular weight of 607.7. The NMR spectrum of compound 67 is shown below. Figure 5 As shown.

[0068] 1H NMR data for compound 67: 1H NMR (500 MHz, CDOD3) δ 8.37 (d, J = 10.0 Hz,5H), 8.27 (s, 1H), 7.87 (d, J = 5.0 Hz, 2H), 7.74 – 7.58 (m, 3H), 7.57 – 7.34(m, 10H), 7.30 (s, 1H), 7.20 (d, J = 10.0 Hz, 2H), 7.04 (s, 1H).

[0069] The synthesis of other compounds was carried out using the same methods as compounds 1, 20, 61, and 67, with the corresponding reactants (l1~l) selected for the synthesis process. 60 The reactants p (p1~p3) are sufficient. The reactant compositions of some compounds in this invention are shown in Table 1: Table 1. Reactant composition of some compounds in this invention

[0070] Schematic diagrams of the electroluminescent devices in the various embodiments and comparative examples of this invention are shown below. Figure 1 As shown, it includes a substrate 1, an anode layer 2, a hole injection layer 3, a hole transport layer 4, an electron blocking layer 5, a light-emitting layer 6, a hole blocking layer 7, an electron transport layer 8, an electron injection layer 9, a cathode layer 10, and a capping layer 11.

[0071] Electroluminescent devices of Examples 2-26 and Comparative Examples 1-4 were prepared according to the electroluminescent device preparation method of Example 1.

[0072] Example 1: Electroluminescent device containing compound 1 From the anode layer to the cathode layer, the layers are sequentially: PET substrate, indium tin oxide (ITO), MoO3, HT-1, EB-1, light-emitting layer 6, hole-blocking layer 7, E1, LiF, Al-Mg, and CPL; the CPL is made of the following material: ; In the luminescent layer 6, CBP and BCP are used as the main luminescent materials, and BD-1 is used as the guest luminescent material, with a mass ratio of 49:49:2.

[0073] The method for preparing the electroluminescent device containing compound 1 includes the following steps: 1. Using a 1.5mm PET substrate as substrate 1 and a 0.15mm ITO material as anode layer 2, the substrate is washed in sequence by alkaline washing, pure water washing, drying, and then ultraviolet-ozone washing to remove organic residues from the surface of the PET substrate and ITO material.

[0074] 2. A layer of ITO material is adhered to a PET substrate. Using a vacuum evaporation apparatus, a 20nm thick MoO3 film is deposited as a hole injection layer 3. Then, an 80nm thick HT-1 film is deposited as a hole transport layer 4. Subsequently, a 30nm thick EB-1 film is deposited as an electron blocking layer 5. On the EB-1, a 60nm thick light-emitting layer 6 is formed by CBP, BCP and BD-1 with a mass ratio of 49:49:2 is deposited. On the light-emitting layer 6, a 10nm thick compound 1 film is deposited as a hole blocking layer 7. Then, a 30nm thick E1 film is deposited as an electron transport layer 8. On the electron transport layer 8, a 16nm thick LiF film is deposited as an electron injection layer 9. After the electron injection layer 9 is deposited, a 10nm thick Al-Mg (Al:Mg=9:1) alloy film is sputtered at low temperature as a cathode layer 10. Finally, a 40nm thick CPL film is deposited on the cathode layer 10 as a high refractive index capping layer 11.

[0075] 3. Vacuum encapsulation of MoO3, HT-1, EB-1, light-emitting layer 6, hole-blocking layer 7, E1, and LiF is performed to prepare an electroluminescent device.

[0076] Examples 2 to 62 The difference from Example 1 is that in Examples 2 to 62, compounds 2 to 60 (Examples 2 to 60), compound 61 (Example 61), and compound 67 (Example 67) were selected as hole blocking layer materials to prepare hole blocking layer 7, respectively.

[0077] Comparative Example 1 The difference from Example 1 is that compound 2a is used. Hole blocking layer 7 was prepared as a hole blocking layer material.

[0078] The structure of the electroluminescent device is as follows: PET substrate / ITO / MoO3 (20nm) / HT-1 (80nm) / EB-1 (30nm) / CBP:BCP:BD-1=49:49:2 (60nm) / 2a (10nm) / E1 (30nm) / LiF (16nm) / Al:Mg= 9:1 (10nm) / CPL (40nm).

[0079] Comparative Example 2 The difference from Example 1 is that compound S-5 was used. Hole blocking layer 7 was prepared as a hole blocking layer material.

[0080] The structure of the electroluminescent device is as follows: PET substrate / ITO / MoO3 (20nm) / HT-1 (80nm) / EB-1 (30nm) / CBP:BCP:BD-1=49:49:2 (60nm) / S-5 (10nm) / E1 (30nm) / LiF (16nm) / Al:Mg= 9:1 (10nm) / CPL (40nm).

[0081] Comparative Example 3 The difference from Example 1 is that the compound S-1 is used. Hole blocking layer 7 was prepared as a hole blocking layer material.

[0082] The structure of the electroluminescent device is as follows: PET substrate / ITO / MoO3 (20nm) / HT-1 (80nm) / EB-1 (30nm) / CBP:BCP:BD-1=49:49:2 (60nm) / S-1 (10nm) / E1 (30nm) / LiF (16nm) / Al:Mg= 9:1 (10nm) / CPL (40nm).

[0083] The electroluminescent devices from the above embodiments and comparative examples were fabricated into 30mm × 30mm samples. The anode and cathode layers were then connected using an industry-known driving circuit to characterize the luminous performance of the electroluminescent devices. Specifically, the driving voltage and luminous efficiency of the electroluminescent devices were measured at a current density of 10mA / cm, and the time required for the brightness of the electroluminescent device to reach 50% of its initial brightness was measured at a current density of 50mA / cm (LT). 50 (i.e., lifespan). The test results are shown in Table 2.

[0084] Table 2 Performance test results of electroluminescent devices

[0085] As can be seen from the test data in Table 2, compared with the electroluminescent devices prepared using compounds 2a, S-5, and S-1 in Comparative Examples 1-3, the electroluminescent devices prepared using the hole-blocking material based on fluorane of this invention have significant advantages in overall luminous efficiency. Specifically, the driving voltage is significantly reduced, the roll-off efficiency is significantly decreased, the current efficiency is increased by more than 2 times, the brightness is increased by about 65%, and the service life is extended by about 30%.

[0086] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of this invention.

Claims

1. A hole-blocking material based on fluorane, characterized in that, Its structural formula is shown in Equation 1: In the formula: A is selected from C6~C 20 aryl, C3~C 20 heteroaryl groups; R1 to R5 are each independently selected from hydrogen, C6 to C6. 30 aryl, C3~C 30 The heteroaryl group, and R1 to R5 cannot all be H at the same time; R1 to R5 can be bonded to each other or not bonded; Group It is an electron-withdrawing group.

2. The hole-blocking material based on fluorane according to claim 1, characterized in that, A is selected from phenyl, naphthyl, dibenzofuranyl, triazineyl, pyrimidinyl, pyridinyl, and quinoxalyl.

3. The hole-blocking material based on fluorane according to claim 1, characterized in that, Group in Formula 1 Selected from the following groups: 。 4. The hole-blocking material based on fluorane according to claim 1, characterized in that, The hole-blocking material based on fluorane is selected from one of the following compounds: 。 5. The method for preparing the hole-blocking material based on fluorane according to any one of claims 1 to 4, characterized in that, include: S1: Reactant p undergoes a ring-closing reaction with phenol to obtain intermediate Mn-1; S2: The intermediate Mn-1 undergoes a nucleophilic substitution reaction with phosphorus tribromide to obtain the intermediate Mn-2; S3: Intermediate Mn-2 undergoes a Miyaura borylation reaction with pinacol diboronic acid ester to obtain intermediate Mn; S4: The intermediate Mn undergoes a Suzuki-Miyaura reaction with reactant l to obtain the hole-blocking material based on fluorane; The structural formula of reactant p is as follows: The structural formula of intermediate Mn-1 is The structural formula of intermediate Mn-2 is The structural formula of intermediate Mn is The structural formula of reactant l is X is Br or Cl.

6. The method for preparing the hole-blocking material based on fluorane according to claim 5, characterized in that, S1 specifically involves using toluene as the reaction solvent and methanesulfonic acid as the catalyst to cause reactant p to undergo a ring-closing reaction with phenol to obtain intermediate Mn-1. S2 specifically involves using toluene as the reaction solvent and DMF as the catalyst to induce a nucleophilic substitution reaction between intermediate Mn-1 and phosphorus tribromide to obtain intermediate Mn-2. S3 is specifically: using 1,4-dioxane as solvent, Pd(dppf)Cl2 as catalyst, and KOAc as base, intermediate Mn-2 undergoes a Miyaura borylation reaction with pinacol diboronic acid ester to obtain intermediate Mn; S4 specifically involves using THF / H2O as a solvent, Pd(PPh3)4 as a catalyst, and K2CO3 as a base to induce a Suzuki-Miyaura reaction between intermediate Mn and reactant l, thereby obtaining the hole-blocking material based on fluorane.

7. An electroluminescent device, characterized in that, It includes a cathode layer, an anode layer, and an organic layer located between the cathode layer and the anode layer. The organic layer includes, in sequence from the anode layer to the cathode layer, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, and an electron injection layer. The material of the hole blocking layer includes the hole blocking material based on fluorane as described in any one of claims 1 to 4.

8. The electroluminescent device according to claim 7, characterized in that, The material of the light-emitting layer includes a host light-emitting material and a guest light-emitting material; the host light-emitting material includes a first host light-emitting material and a second host light-emitting material, wherein the first host light-emitting material is selected from... and The second main luminescent material is .

9. The electroluminescent device according to claim 8, characterized in that, The object luminescent material is .

10. The electroluminescent device according to claim 7, characterized in that, The material of the hole transport layer is selected from one of the following materials: 。