High-purity sodium diisobutyl dithiophosphate and preparation method, application thereof
Patent Information
- Application Number
- CN202611466873.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-24
AI Technical Summary
In the existing technology for the production of sodium diisobutyl dithiophosphate, hydrogen sulfide is difficult to completely remove, leading to the formation of sodium sulfide and causing safety risks and reduced sorting selectivity.
By setting up static sedimentation and negative pressure flash evaporation processes before neutralization and salt formation, free hydrogen sulfide in the liquid phase is removed, ensuring a hydrogen sulfide removal rate of 99.8%. The pH value is controlled during the alkali neutralization process to avoid the formation of sodium sulfide.
It completely eliminates the escape of hydrogen sulfide gas, eliminates safety hazards, improves the separation selectivity of polymetallic associated minerals, reduces sulfide emissions from flotation tailings, and improves concentrate grade and recovery rate.
Smart Images

Figure CN123151908A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of mineral flotation reagent synthesis technology, specifically relating to a high-purity sodium diisobutyl dithiophosphate, its preparation method, and its application. Background Technology
[0002] Dialkyl dithiophosphate, commonly known as black powder, is the second most used flotation collector for sulfide ores after xanthate. Existing alcohol black powders (such as sodium butadiene black powder) are generally prepared by reacting alcohols with phosphorus pentasulfide to generate dialkyl dithiophosphate, which is then neutralized with an alkaline reagent to form a salt. CN113680535A discloses a route for preparing dithiophosphate collectors by reacting alcohol compounds with phosphorus pentasulfide to obtain dithiophosphate, followed by neutralization with alkaline reagents such as sodium hydroxide. It also describes that the waste gas generated during the reaction is absorbed by passing it through a NaOH solution, and that vacuum distillation is used only for the separation and purification of the solid product. CN117259016A also uses anisole to prepare an intermediate by reflux with phosphorus pentasulfide, then reacts it with an alcohol solution of metallic sodium / potassium, followed by vacuum drying and desolventization to obtain solid dithiophosphate. The above-mentioned approach targets the end-of-pipe absorption of gaseous waste gas or the separation and drying of solid products. When applied to the continuous production of sodium diisobutyl dithiophosphate aqueous solution, it has the following unavoidable shortcomings: First, multi-layer alkaline absorption towers can only treat gaseous hydrogen sulfide. Some of the hydrogen sulfide generated by the phosphine reaction will dissolve and remain inside the liquid phase of crude diisobutyl dithiophosphoric acid, which cannot be removed by the tail gas treatment system. Second, when crude acid carrying dissolved hydrogen sulfide is directly neutralized with alkali, the liquid hydrogen sulfide reacts with the alkali to generate sodium sulfide, which remains stably in the finished reagent. Third, when reagents containing sodium sulfide are used in mine flotation operations, the sodium sulfide continuously decomposes to produce hydrogen sulfide gas, posing a safety risk of personnel poisoning and gas explosion in the mineral processing workshop. At the same time, sodium sulfide will act indiscriminately on all types of minerals, weakening the separation selectivity of target minerals, causing the loss of valuable metal minerals, and leading to excessive sulfide in the flotation tailwater, significantly increasing the cost of mine wastewater treatment.
[0003] Existing technologies have not recognized the causal chain of hydrogen sulfide dissolution in the liquid phase – neutralization to form sodium sulfide – release of hydrogen sulfide by flotation, nor have they proposed an effective means to eradicate the problem while preserving a mature neutralization system and modifying low-yield production lines. Summary of the Invention
[0004] To address the technical challenge of eliminating the potential hydrogen sulfide release hazard of sodium diisobutyl dithiophosphate (DIBDS) in the entire mineral flotation process while maintaining a mature alkali neutralization-endpoint pH control system and requiring minimal modifications to existing reagent production lines, this invention provides a method for preparing high-purity DIBDS, comprising the following steps: S1. Isobutanol reacts with phosphorus pentasulfide in a sulfophosphoric reaction to produce crude diisobutyl dithiophosphoric acid; S2. The crude diisobutyl dithiophosphoric acid is subjected to negative pressure flash evaporation to remove the free hydrogen sulfide dissolved in the liquid phase, thereby obtaining purified diisobutyl dithiophosphoric acid. S3. The purified diisobutyl dithiophosphate is subjected to salt formation treatment to obtain sodium diisobutyl dithiophosphate.
[0005] Furthermore, prior to the negative pressure flash evaporation treatment, the crude diisobutyl dithiophosphoric acid is subjected to a sedimentation and impurity removal treatment; or, After the negative pressure flash evaporation treatment, the purified diisobutyl dithiophosphoric acid is subjected to precipitation to remove impurities.
[0006] Furthermore, the sedimentation and impurity removal treatment includes settling and slag discharge, with the settling time being 6-8 hours.
[0007] Furthermore, in step S1, the molar ratio of isobutanol to phosphorus pentasulfide is 4~5:1, and the temperature of the phosphine reaction is 80~90℃.
[0008] Furthermore, the vacuum degree of the negative pressure flash evaporation in step S2 is -0.06 to -0.09 MPa, the operating temperature is 50 to 70°C, and the material residence time is 15 to 40 minutes.
[0009] Furthermore, the hydrogen sulfide produced by the sulfur phosphating reaction includes the escaped hydrogen sulfide and the hydrogen sulfide remaining in the crude diisobutyl dithiophosphoric acid. The released hydrogen sulfide is then subjected to alkaline absorption treatment. The molar percentage of hydrogen sulfide remaining in the crude diisobutyl dithiophosphoric acid in the total hydrogen sulfide is no higher than 5%.
[0010] Furthermore, the salt formation process includes: mixing the purified diisobutyl dithiophosphate with an alkaline agent, controlling the neutralization endpoint pH to be 10-13, to obtain sodium diisobutyl dithiophosphate; The alkaline agent includes a sodium hydroxide solution; the concentration of the alkaline agent is 10% to 30%; and the reaction temperature of the salt formation treatment is 30 to 50°C.
[0011] This invention provides a high-purity sodium diisobutyl dithiophosphate, which is prepared by the preparation method described above.
[0012] This invention also provides an application of the high-purity sodium diisobutyl dithiophosphate as described above in the processing of polymetallic minerals, comprising the following steps: The high-purity sodium diisobutyl dithiophosphate was prepared into an aqueous solution with a concentration of 5-10 wt% to obtain a flotation reagent; The flotation reagent is applied to the flotation separation treatment of the polymetallic mineral; the pH of the flotation separation treatment is 4-7.
[0013] Furthermore, the amount of flotation reagent added is 50-150g per ton of raw ore.
[0014] Compared with the prior art, the present invention has at least the following advantages: This invention incorporates a pre-desulfurization process involving static sedimentation for impurity removal and negative pressure flash evaporation before neutralization and salt formation. It also directionally removes dissolved free hydrogen sulfide from the liquid phase to a removal rate ≥99.8%, overcoming the limitation of traditional multi-layer alkaline washing which can only treat gaseous hydrogen sulfide. No free hydrogen sulfide participates in the reaction during the neutralization stage, eliminating the generation of sodium sulfide byproducts at the source. Sodium sulfide is undetectable in the finished aqueous solution, and no hydrogen sulfide gas escapes throughout the entire flotation process in the mine. This completely eliminates the risks of poisoning and explosion in the mineral processing workshop and significantly reduces fugitive emissions.
[0015] By eliminating the indiscriminate collection interference of sodium sulfide on various minerals, the separation selectivity of polymetallic associated minerals is simultaneously improved. Under the same flotation conditions, Example 1 of this application increases the concentrate grade of polymetallic ores from 44.23% to 47.36% and the recovery rate from 78.66% to 84.71% in the traditional process (Comparative Example 1), and the sulfide in the flotation tailwater meets environmental emission requirements. At the same time, this application uses a mature neutralization system, and the flash evaporation conditions are mild and do not damage the effective components, with virtually no loss in product yield. The entire process only requires the addition of a negative pressure flash evaporation device. The reaction tail gas and flash gas are washed in the same closed-loop alkaline tower to achieve sulfur resource recovery, which is suitable for low-cost technical transformation and large-scale implementation of existing reagent production lines. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0017] Figure 1 The flowchart of the preparation process of high-purity sodium diisobutyl dithiophosphate provided in the embodiment of the present invention is shown; wherein, 1 is a synthesis vessel, 2 is a precipitation vessel, 3 is an evaporation vessel, and 4 is a sodium treatment vessel. Detailed Implementation
[0018] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0019] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.
[0020] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention, as well as the prior art known to those skilled in the art and the description of the invention, may be implemented using any prior art methods, devices, and materials similar to or equivalent to the methods, devices, and materials in the embodiments of the present invention.
[0021] This invention provides a method for preparing high-purity sodium diisobutyl dithiophosphate, comprising the following steps: S1. Isobutanol undergoes a sulfurization reaction with phosphorus pentasulfide to produce crude diisobutyl dithiophosphoric acid.
[0022] In some embodiments, the molar ratio of isobutanol to phosphorus pentasulfide is 4-5:1, and the temperature of the phosphine reaction is 80-90°C.
[0023] For example, the molar ratio of isobutanol to phosphorus pentasulfide can be 4.0:1, 4.05:1, 4.1:1, 4.15:1, 4.2:1, 4.25:1, 4.3:1, 4.4:1, 4.5:1, or any value between such a minimum and maximum, or any range of two such values; the phosphating reaction temperature can be 80℃, 82℃, 85℃, 88℃, 90℃, or any value between such a minimum and maximum, or any range of two such values.
[0024] In some embodiments, the hydrogen sulfide produced by the phosphine reaction includes the escaped hydrogen sulfide and the hydrogen sulfide remaining in the crude diisobutyl dithiophosphoric acid; The released hydrogen sulfide is then subjected to alkaline absorption treatment. In all embodiments of the present invention, the molar proportion of hydrogen sulfide remaining in the crude diisobutyl dithiophosphoric acid in the total hydrogen sulfide is not higher than 5%.
[0025] S2. The crude diisobutyl dithiophosphoric acid is subjected to negative pressure flash evaporation to remove the free hydrogen sulfide dissolved in the liquid phase, thereby obtaining purified diisobutyl dithiophosphoric acid.
[0026] In some embodiments, the crude diisobutyl dithiophosphoric acid is subjected to a sedimentation purification treatment before the negative pressure flash evaporation treatment; or, After the negative pressure flash evaporation treatment, the purified diisobutyl dithiophosphoric acid is subjected to precipitation to remove impurities.
[0027] More specifically, the sedimentation and impurity removal treatment includes settling and slag discharge, with the settling time being 6-8 hours.
[0028] In some embodiments, the vacuum degree of the negative pressure flash evaporation in step S2 is -0.06 to -0.09 MPa, the operating temperature is 50 to 70°C, and the material residence time is 15 to 40 minutes.
[0029] For example, the vacuum degree (gauge pressure) of the negative pressure flash evaporation can be -0.06MPa, -0.065MPa, -0.07MPa, -0.075MPa, -0.08MPa, -0.085MPa, -0.09MPa, and any value between such a minimum and maximum value, or any range of two such values; the operating temperature of the negative pressure flash evaporation can be 55℃, 58℃, 60℃, 62℃, 65℃, 68℃, 70℃, and any value between such a minimum and maximum value, or any range of two such values; the material residence time of the negative pressure flash evaporation can be 15min, 20min, 25min, 30min, 35min, 40min, and any value between such a minimum and maximum value, or any range of two such values.
[0030] S3. The purified diisobutyl dithiophosphate is subjected to salt formation treatment to obtain sodium diisobutyl dithiophosphate.
[0031] In some embodiments, the salt formation process includes: mixing the purified diisobutyl dithiophosphate with an alkaline agent, controlling the neutralization endpoint pH to be 10-13, to obtain sodium diisobutyl dithiophosphate; The alkaline agent includes a sodium hydroxide solution; the concentration of the alkaline agent is 10% to 30%; and the reaction temperature of the salt formation treatment is 30 to 50°C.
[0032] For example, the neutralization endpoint pH can be 10, 10.5, 11, 11.5, 12, 12.5, 13, or any value between such a minimum and maximum value, or a range of any two values; the neutralization reaction temperature can be 30°C, 35°C, 40°C, 45°C, 50°C, or any value between such a minimum and maximum value, or a range of any two values.
[0033] like Figure 1 As shown, isobutanol and phosphorus pentasulfide are fed into synthesis reactor 1 via feed pipelines. Under stirring and temperature control conditions, a phosphosulfurization reaction is carried out to produce crude diisobutyl dithiophosphoric acid. The hydrogen sulfide tail gas released from the reaction is led out through the gas phase pipeline at the top of synthesis reactor 1 and merged into the tail gas main pipe. After multi-stage absorption by liquid alkali, it is sent to the tail gas treatment. The crude diisobutyl dithiophosphoric acid at the bottom of synthesis reactor 1 is sent to precipitation reactor 2 via a first transfer pump. In precipitation reactor 2, it is allowed to settle and separate into layers for slag removal. The lower layer of solid waste is discharged for disposal, while the upper layer of clear liquid is sent to evaporation reactor 3 via a second transfer pump.
[0034] Evaporator 3, acting as a negative pressure flash evaporation device, performs negative pressure flash evaporation on the clarified liquid phase under conditions of vacuum degree -0.06~-0.09MPa, temperature 55~70℃, and material residence time 15~40min. This directionally removes dissolved free hydrogen sulfide from the liquid phase, achieving a removal rate ≥99.8%. The hydrogen sulfide-containing gas phase released during flash evaporation is led out through the gas phase pipeline at the top of evaporator 3 and merged into the same tail gas main. Together with the tail gas from synthesis reactor 1, it undergoes multi-stage absorption by liquid alkali before being sent to the tail gas treatment, achieving closed-loop recovery of sulfur resources. The purified diisobutyl dithiophosphate after hydrogen sulfide removal by negative pressure flash evaporation is sent from the bottom of evaporator 3 to sodium treatment reactor 4 via a third transfer pump. Liquid alkali is introduced into sodium treatment reactor 4 for salt formation, controlling the final pH of neutralization to 10~13, and pure water is added for adjustment to obtain a finished sodium diisobutyl dithiophosphate aqueous solution, which is discharged and packaged from the bottom of sodium treatment reactor 4.
[0035] The present invention also provides a high-purity sodium diisobutyl dithiophosphate, which is prepared by the preparation method described above.
[0036] This invention also provides an application of the high-purity sodium diisobutyl dithiophosphate as described above in the processing of polymetallic minerals, comprising the following steps: The high-purity sodium diisobutyl dithiophosphate was prepared into an aqueous solution with a concentration of 5-10 wt% to obtain a flotation reagent; The flotation reagent is applied to the flotation separation treatment of the polymetallic mineral; the pH of the flotation separation treatment is 4-7.
[0037] In some embodiments, the amount of flotation reagent added is 50-150g per ton of raw ore.
[0038] For example, the dosage of the reagent can be 50g / t, 60g / t, 80g / t, 100g / t, 120g / t, 150g / t of raw ore, as well as each value between such minimum and maximum values, or a range of any two values.
[0039] In some embodiments, the polymetallic mineral includes at least one of chalcopyrite (CuFeS2), galena (PbS), sphalerite / ferro-zinc sphalerite ((Zn,Fe)S), and pyrite (FeS2).
[0040] More specifically, when the polymetallic mineral includes chalcopyrite, its material composition by mass percentage is: 0.5%~2% copper, 1%~5% sulfur, 1%~5% iron, with the balance being gangue.
[0041] More specifically, when the polymetallic mineral includes galena, its material composition by mass percentage is: lead 0.5%~2%, sulfur 1%~4%, and the balance being gangue.
[0042] More specifically, when the polymetallic mineral includes sphalerite / iron sphalerite, its material composition by mass percentage is: zinc 0.5%~3%, iron 1%~5%, sulfur 1%~5%, with the balance being gangue.
[0043] More specifically, when the polymetallic mineral includes pyrite, its material composition by mass percentage is: 1%~10% iron, 1%~12% sulfur, and the balance being gangue; optionally, at least one of the target metals copper, lead, and zinc may also be present, totaling 0.1%~2%.
[0044] It should be noted that the typical mineral composition of polymetallic associated sulfide ores, in addition to chalcopyrite (CuFeS2), galena (PbS), sphalerite / iron sphalerite ((Zn,Fe)S), pyrite (FeS2), and pyrrhotite, often includes associated gold and silver, and the gangue is mainly composed of quartz, silicates, and carbonates. The essence of its flotation separation is the synergy of selective collection and selective inhibition. Diisobutyl dithiophosphate has a strong affinity for soft / interfacial acid metal sites such as copper and lead, and can form a stable disulfide coordination chelate hydrophobic film, while it has a weak affinity for zinc and iron. This is the natural selectivity of black powder to strongly capture copper and lead and weakly capture zinc and iron. The establishment of this selectivity is highly dependent on the slurry pH, redox potential Eh, and the surface chemical window created by the modifier not being destroyed.
[0045] Sodium sulfide causes interference because it is not an inert impurity in the pulp, but rather a potent sulfiding agent / activator / reducing agent, which worsens the selectivity window. Firstly, strong hydrolysis of Na2S releases HS-H2S. - / S 2-And raise the pH (Na2S + H2O ⇌ NaHS + NaOH), HS - / S 2- It can cause sulfidation activation on the surface of pyrite, sphalerite, and even semi-oxidized copper-lead minerals that need to be suppressed, generating floatable metal sulfide sites in situ; secondly, HS - / S 2- Like diisobutyl dithiophosphate, it belongs to the sulfur-containing soft base ligand family. It competes with collectors for adsorption on mineral surfaces and desorbs existing collector films, while also reacting with Cu in solution. 2+ / Pb 2+ It forms metal sulfides with extremely low solubility (approximately 10 μL of CuS). -36 PbS approximately 10 -28 (on a certain scale), preemptively consuming the effective collector and altering surface properties, leading to fluctuations in recovery rate; thirdly, S 2- With Ca in the slurry 2+ Heavy metal ions generate CaS / metal sulfide colloidal precipitates, which non-selectively cover the surface of gangue and target minerals and aggravate foam entrainment, thus lowering the concentrate grade. Furthermore, the continuous hydrolysis of Na2S during flotation dilution and pulp conditioning releases H2S (which is both toxic and has a further sulfidation and activation effect), simultaneously worsening selectivity, recovery rate, and safety and environmental impact.
[0046] The mechanism by which sodium sulfide is eliminated is to preserve intrinsic selectivity: only diisobutyl dithiophosphate, a sulfur-containing ligand, remains in the reagent, and HS-containing compounds are no longer present. - / S 2- Indiscriminate sulfidation activation keeps pyrite and sphalerite hydrophilic and prevents them from floating; Eh returns to the appropriate window, pyrite remains suppressed, while hydrophobic metal-dithiophosphate chelate films can be successfully formed on the surface of copper and lead minerals, resulting in fast flotation rate and stable loading; the collector is no longer consumed by competitive adsorption, desorption or precipitation, the effective concentration is stable, and the target mineral is collected more fully; and there is no CaS / metal sulfide colloidal capping, gangue inclusions are reduced, and concentrate grade is improved.
[0047] To facilitate a further understanding of the present invention by those skilled in the art, the following examples are provided: Example 1 A method for preparing sodium diisobutyl dithiophosphate includes the following steps: S1. Add 7 kg of isobutanol to the reactor, add 5.1 kg of phosphorus pentasulfide in batches, control the temperature at 85℃ and react fully for 4 hours to generate crude diisobutyl dithiophosphoric acid; the hydrogen sulfide tail gas released by the reaction is continuously passed into the alkaline washing tower to absorb the gaseous hydrogen sulfide. S2. Crude acid settling and impurity removal: Crude diisobutyl dithiophosphoric acid is transferred to a closed settling tank and settling for 7 hours. The lower layer of solid waste is discharged and disposed of, and the upper layer of clear liquid phase is transported to a flash evaporator. Negative pressure flash liquid phase deep desulfurization of hydrogen sulfide: the vacuum degree of the flash tank is controlled at -0.07MPa, the liquid temperature is raised to 62℃, the material stays for 25min, and the hydrogen sulfide gas and liquid alkali at the top of the flash tower are absorbed and treated. S3. Preparation of finished product by alkaline neutralization: After clarification and desulfurization, diisobutyl dithiophosphate is introduced into a neutralization vessel. 20% mass concentration liquid alkali is added dropwise at a uniform rate. The stirring speed is 90 r / min, the neutralization temperature is 40℃, and the final pH is stabilized at 11.5. The reaction is stirred for 1 hour, and then pure water is added to adjust the concentration to 50% to obtain sodium diisobutyl dithiophosphate solution.
[0048] Example 2 A method for preparing sodium diisobutyl dithiophosphate, the steps are the same as in Example 1, the only difference being that the flash evaporation parameters in step S2 are adjusted to a vacuum degree of -0.09 MPa, a temperature of 55°C, and a residence time of 40 min.
[0049] Example 3 A method for preparing sodium diisobutyl dithiophosphate, the steps are the same as in Example 1, the only difference being that the flash evaporation parameters in step S2 are adjusted to a vacuum degree of -0.06 MPa, a temperature of 70°C, and a residence time of 15 min.
[0050] Comparative Example 1 The traditional process for preparing sodium diisobutyl dithiophosphate does not include the S2 negative pressure flash evaporation step. The crude diisobutyl dithiophosphate is directly neutralized with 20% liquid alkali, with an endpoint pH of 11.5. The remaining raw material ratios and reaction temperatures are completely consistent with those in Example 1.
[0051] Comparative Example 2 A method for preparing sodium diisobutyl dithiophosphate, the steps are the same as in Example 1, the only difference being that the vacuum degree of negative pressure flash evaporation is only -0.04MPa (lower than the lower limit of the present invention), the temperature is 62℃, and the residence time is 25min.
[0052] Comparative Example 3 A method for preparing sodium diisobutyl dithiophosphate, the steps are the same as in Example 1, the only difference being that the vacuum degree of negative pressure flash evaporation is -0.07MPa, the operating temperature is 45℃ (lower than the lower limit of the present invention), and the residence time is 25min.
[0053] Comparative Example 4 A method for preparing sodium diisobutyl dithiophosphate, with the same steps as in Example 1, except that the vacuum degree of negative pressure flash evaporation is -0.07MPa, the operating temperature is 62℃, and the material residence time is 8min (shorter than the minimum residence time of this invention).
[0054] Analysis example 1 Performance Testing: The flotation reagents prepared in each embodiment and comparative example were used for flotation separation tests of polymetallic ores. The raw material used was pyrite ore from a certain location (including pyrite; by mass percentage, the material composition of the pyrite ore was: iron 3.6%, sulfur 4.2%, with the balance being gangue). The target metal was iron, and the grade of the target metal in the raw ore was 3.6%. The flotation operation conditions were uniform: the raw ore was ground to a particle size of -0.074 mm or more (70%), the pulp was adjusted to a pulp mass concentration of 30%, the finished aqueous solution was diluted to 10 wt% reagent, the diluted reagent was added at a rate of 100 g / t of raw ore, the pH was adjusted to 5, and the concentrate was obtained after conventional closed-circuit flotation processes of roughing, scavenging, and cleaning. The test results are shown in Table 1.
[0055] Table 1. Results of flotation separation experiments in the examples and comparative examples. The above technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made under the technical concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for preparing high-purity sodium diisobutyl dithiophosphate, characterized in that, Includes the following steps: S1. Isobutanol reacts with phosphorus pentasulfide in a sulfophosphoric reaction to produce crude diisobutyl dithiophosphoric acid; S2. The crude diisobutyl dithiophosphoric acid is subjected to negative pressure flash evaporation to remove the free hydrogen sulfide dissolved in the liquid phase, thereby obtaining purified diisobutyl dithiophosphoric acid. S3. The purified diisobutyl dithiophosphate is subjected to salt formation treatment to obtain sodium diisobutyl dithiophosphate.
2. The preparation method according to claim 1, characterized in that, Prior to the negative pressure flash evaporation treatment, the crude diisobutyl dithiophosphoric acid is subjected to a sedimentation purification treatment; or, After the negative pressure flash evaporation treatment, the purified diisobutyl dithiophosphoric acid is subjected to precipitation to remove impurities.
3. The preparation method according to claim 2, characterized in that, The sedimentation and impurity removal process includes settling and slag discharge, with the settling time being 6-8 hours.
4. The preparation method according to claim 1, characterized in that, In step S1, the molar ratio of isobutanol to phosphorus pentasulfide is 4~5:1, and the temperature of the phosphine reaction is 80~90℃.
5. The preparation method according to claim 1, characterized in that, The vacuum degree of the negative pressure flash evaporation in step S2 is -0.06~-0.09MPa, the operating temperature is 50~70℃, and the material residence time is 15~40min.
6. The preparation method according to claim 1, characterized in that, The hydrogen sulfide produced by the sulfur phosphating reaction includes the escaped hydrogen sulfide and the hydrogen sulfide remaining in the crude diisobutyl dithiophosphoric acid. The released hydrogen sulfide is then subjected to alkaline absorption treatment. The molar percentage of hydrogen sulfide remaining in the crude diisobutyl dithiophosphoric acid in the total hydrogen sulfide is no higher than 5%.
7. The preparation method according to claim 1, characterized in that, The salt formation process includes: mixing the purified diisobutyl dithiophosphate with an alkaline agent, controlling the neutralization endpoint pH to be 10-13, to obtain sodium diisobutyl dithiophosphate. The alkaline agent includes a sodium hydroxide solution; the concentration of the alkaline agent is 10% to 30%; and the reaction temperature of the salt formation treatment is 30 to 50°C.
8. A high-purity sodium diisobutyl dithiophosphate, characterized in that, It is prepared by the preparation method according to any one of claims 1-7.
9. The application of the high-purity sodium diisobutyl dithiophosphate as described in claim 8 in the processing of polymetallic minerals, characterized in that, Including the following steps: The high-purity sodium diisobutyl dithiophosphate was prepared into an aqueous solution with a concentration of 5-10 wt% to obtain a flotation reagent; The flotation reagent is applied to the flotation separation process of the polymetallic mineral; The pH of the flotation separation process is 4-7.
10. The application of high-purity sodium diisobutyl dithiophosphate according to claim 9 in the processing of polymetallic minerals, characterized in that, The amount of flotation reagent added is 50-150g per ton of raw ore.
Citation Information
Patent Citations
Alkyl ether dithiophosphate collecting agent and preparation method and application thereof
CN113680535A
Flotation collecting agent, preparation method of flotation collecting agent, combined flotation reagent and application of combined flotation reagent