A compounded structure regulator and a low ethylene content solution-polymerized styrene-butadiene rubber, and a preparation method and application thereof

By adjusting the vinyl content of solution-polymerized styrene-butadiene rubber (SBR) with a compounded structure modifier, the problem of difficulty in reducing vinyl content in existing technologies has been solved, achieving efficient preparation of low-benzene, low-vinyl solution-polymerized SBR, which is suitable for high-performance tire manufacturing.

CN123152013APending Publication Date: 2026-11-24PETROCHINA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510677627.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, it is difficult to reduce the vinyl content of low-benzene and low-vinyl solution-polymerized styrene-butadiene rubber to 20% or below, resulting in an excessively low glass transition temperature that makes it unsuitable for use with medium- and high-styrene solution-polymerized styrene-butadiene rubber. Furthermore, ether and amine modifiers lead to an increase in the 1,2-vinyl content.

Method used

By employing compound structure modifiers, including ether and phosphite modifiers, and adjusting their molar ratio and dosage, the deassociation of organolithium and the formation of intermediates with double bonds in butadiene are promoted, the vinyl content is reduced, and the randomization of the molecular chain is regulated.

Benefits of technology

Successfully reducing the vinyl content in solution-polymerized styrene-butadiene rubber (SBR) and increasing the glass transition temperature to -65℃ to -85℃ makes it suitable for high-performance tire manufacturing, simplifies the preparation process, and saves on reaction reagents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152013A_ABST
    Figure CN123152013A_ABST
Patent Text Reader

Abstract

This invention provides a compound structure modifier, a solution-polymerized styrene-butadiene rubber (SBR) with low vinyl content, its preparation method, and its application. The compound structure modifier comprises an ether-based structure modifier and a phosphite-based structure modifier. The ether-based structure modifier includes a benzene ring and / or an oxygen-containing heterocycle in its structure. The phosphite-based structure modifier has a structural formula selected from (RO)3P, (R2N)3P, and (RS)3P, wherein R is a hydrocarbon group containing 1-12 carbons, and R does not react with organolithium. The molar ratio of the ether-based structure modifier to the phosphite-based structure modifier is 0.1-36:1. When applied to the preparation of solution-polymerized SBR, the compound structure modifier of this invention can significantly reduce the 1,2-vinyl content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber synthesis technology, and more specifically, to a compound structure modifier and a low vinyl content solution-polymerized styrene-butadiene rubber, its preparation method, and its application. Background Technology

[0002] Solution-polymerized styrene-butadiene rubber (SSBR) possesses excellent wet skid resistance, low rolling resistance, and wear resistance, making it a promising candidate for applications in high-performance green tires and other fields. Functional modification of SSBR to further enhance its overall performance is an important research direction in this field. SSBR is synthesized using anionic polymerization, employing active organolithium initiators in a non-polar solvent to copolymerize styrene and butadiene monomers. This allows for flexible adjustment of polymerization parameters, such as monomer ratios, types, and modifier types, enabling precise control of the molecular structure.

[0003] Solution-polymerized styrene-butadiene rubber (SBR) can be classified into low-styrene (styrene content ≤ 20%), medium-styrene (styrene content 20%-30%), and high-styrene (styrene content ≥ 30%) based on its styrene content.

[0004] In the molecular chain structure of solution-polymerized styrene-butadiene rubber (SBR), styrene microblocks refer to shorter chain segments formed by the continuous connection of multiple styrene monomer units. These microblocks consist of several to a dozen continuously linked styrene units, and their specific length is influenced by various factors such as polymerization process conditions. The rigidity of the styrene microblocks increases the hardness of the rubber but also reduces its tensile strength and elongation at break, among other mechanical properties.

[0005] Low-styrene, low-vinyl solution-polymerized styrene-butadiene rubber (SBR) has lower hardness and strength compared to medium- and high-styrene, low-vinyl solution-polymerized SBR due to the lower content of styrene and 1,2-vinyl groups in its molecular structure, and also has a lower glass transition temperature. It can be used in combination with medium- and high-styrene, low-vinyl solution-polymerized SBR in tire manufacturing. However, due to the different polymerization rates of styrene and butadiene, and the fact that the amount of butadiene added is much greater than the amount of styrene during feeding, the vinyl content in the preparation of low-styrene, low-vinyl solution-polymerized SBR is often too high, making it difficult to reduce to 20% or below. This results in a glass transition temperature that is too low for its compatibility with other SBRs. Currently, when ethers and amines are commonly used as regulators in industry, the polymerization process often leads to randomization of the polymer chain structure, resulting in an increase in the 1,2-vinyl content, making it impossible to achieve a truly low-styrene, low-vinyl content.

[0006] CN117567687A discloses a randomized solution-polymerized styrene-butadiene rubber (SBR) with high styrene and low vinyl content and its preparation method. The method includes: mixing butadiene and styrene in a solvent to obtain a first solution; performing a first mixing reaction of an initiator and an epoxy compound to obtain a second solution; and performing a second mixing reaction of the first solution and the second solution to obtain the solution-polymerized SBR. This method uses the product of the reaction between the epoxy compound and the initiator to initiate the polymerization of butadiene and styrene, and can prepare relatively pure solution-polymerized SBR with a completely random sequence structure and high styrene (30% to 40%) and low vinyl content (8% to 15%). Summary of the Invention

[0007] To address the problem in existing technologies where the vinyl content in low-benzene, low-vinyl solution-polymerized styrene-butadiene rubber (SBR) is difficult to reduce to 20% or below, the present invention aims to provide a compound structure modifier, low-vinyl content SBR, its preparation method, and its application. The compound structure modifier of the present invention, when applied to the preparation of SBR, can significantly reduce the 1,2-vinyl content.

[0008] To achieve the above objectives, according to a first aspect of the present invention, a compound structure modifier is provided, comprising an ether-based structure modifier and a phosphite-based structure modifier; the ether-based structure modifier comprises a benzene ring and / or an oxygen-containing heterocycle in its structure; the phosphite-based structure modifier is selected from one or more combinations of (RO)3P, (R2N)3P, and (RS)3P, wherein R is a hydrocarbon group containing 1-12 carbons, and R does not react with organolithium; the molar ratio of the ether-based structure modifier to the phosphite-based structure modifier is 0.1 to 36:1.

[0009] The compound structure modifier of this invention can be used in the preparation of solution-polymerized styrene-butadiene rubber (SBR) and can reduce styrene and vinyl content. In the preparation of solution-polymerized SBR, organolithium compounds are typically used as initiators. In the compound structure modifier of this invention, the ether-based structure modifier can promote the deassociation of organolithium compounds. Furthermore, phosphites react with Li during polymerization. + The complex forms a complex, which further forms an intermediate with the double bond in butadiene. The presence of this intermediate can effectively reduce the formation of the 1,2-butadiene structure in solution-polymerized styrene-butadiene rubber, effectively reducing the vinyl content, thereby obtaining solution-polymerized styrene-butadiene rubber with a lower glass transition temperature (-65℃ to -85℃). In addition, phosphites can regulate the randomization of the solution-polymerized styrene-butadiene rubber molecular chain.

[0010] This invention adjusts the 1,2-vinyl content on the solution-polymerized styrene-butadiene rubber molecular chain by regulating the ratio of the ether-based structure modifier and the phosphite-based structure modifier, and by adjusting the amount of the compound structure modifier used in the reaction. This achieves the effect of regulating the vinyl content and solves the problem in the prior art that it is difficult to reduce the vinyl content to 20% or below during the preparation of low-benzene, low-vinyl solution-polymerized styrene-butadiene rubber.

[0011] In some preferred embodiments of the present invention, the ether structure modifier includes one or more of the following: anisole, phenethyl ether, o-phenylenedimethyl ether, benzyl ether, 1,2,4,5-tetramethoxybenzene, 2,2-dimorpholinodiethyl ether, myristyl ether, glycidyl furfuryl ether, 2-nitrophenyl octyl ether, p-xylyl ether, and dibenzo-18-crown-6-ether.

[0012] In some preferred embodiments of the present invention, the phosphite structure modifier includes one or more of the following: tributyl phosphite, triethyl phosphite, trimethyl phosphite, triphenyl phosphite, tribenzyl phosphite, tri(2-methoxyphenyl)phosphine, tri(3-methoxyphenyl)phosphine, tri(2-methoxynaphthyl)phosphine, tri(3-methoxynaphthyl)phosphine, hexamethylphosphine, hexaethylphosphine, trimethyl trithiophosphite, and triphenyl trithiophosphite.

[0013] Controlling the structure modifier within the aforementioned preferred range, and having a molar ratio of ether-based structure modifier to phosphite-based structure modifier of 0.1 to 1:1, is more conducive to the preparation of atactic low-benzene, low-vinyl solution-polymerized styrene-butadiene rubber. If this range is exceeded, the monomer conversion rate during polymerization will decrease, or the vinyl content of the resulting product will increase.

[0014] According to another aspect of the present invention, a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber is provided, comprising: mixing styrene, butadiene, an initiator, the aforementioned compounded structure modifier, and a nonpolar solvent; heating to 30-70°C (preferably 50°C; the temperature is the temperature at which the reaction is initiated, and the temperature will increase as the polymerization reaction proceeds) to carry out a polymerization reaction; then terminating the reaction; and performing post-treatment to obtain the low vinyl content solution-polymerized styrene-butadiene rubber.

[0015] The initiator includes an organolithium compound.

[0016] In some preferred embodiments of the present invention, the preparation method is carried out in a loop reactor or a batch reactor, preferably a batch reactor. Preferably, the preparation method of the present invention is carried out under an inert gas atmosphere, specifically, nitrogen, argon, etc.

[0017] In some preferred embodiments of the present invention, the terminating agent includes alcohols and / or water, etc. Alcohols include methanol and / or ethanol, etc.

[0018] In some preferred embodiments of the present invention, the post-treatment method after terminating the reaction includes: boiling the obtained adhesive solution in water to coagulate it, and then drying it. The present invention does not further limit the specific post-treatment parameters.

[0019] In some preferred embodiments of the present invention, the mass of the compound structure modifier is 0.01 to 5% of the total mass of the styrene and the butadiene, preferably 0.03 to 0.05%. Within the above range, it is more advantageous to control the styrene and vinyl content in low vinyl content solution-polymerized styrene-butadiene rubber.

[0020] In some preferred embodiments of the present invention, the preparation method includes:

[0021] S1, the compound structure modifier and the nonpolar solvent are mixed to obtain a first mixed solution;

[0022] S2, the first mixed solution is mixed with the styrene and the butadiene, and heated to 30-70°C to obtain the second mixed solution;

[0023] S3, the second mixed solution is mixed with the initiator to initiate a polymerization reaction, thereby obtaining the low vinyl content solution-polymerized styrene-butadiene rubber.

[0024] In some preferred embodiments of the present invention, the preparation method includes:

[0025] S1, the styrene, butadiene, and nonpolar solution are mixed to obtain a monomer solution;

[0026] S2, the monomer solution and the compound structure modifier are mixed and heated to 30-70°C to obtain a premixed solution;

[0027] S3, the premixed solution is mixed with the initiator to initiate a polymerization reaction, thereby obtaining the low vinyl content solution-polymerized styrene-butadiene rubber.

[0028] In some preferred embodiments of the present invention, the mass ratio of styrene to butadiene is 8:92 to 20:80.

[0029] In some preferred embodiments of the present invention, the organolithium compound includes one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, and dilithium phenylpropynate. Preferably, the organolithium compound includes n-butyllithium.

[0030] In some preferred embodiments of the present invention, the mass ratio of the initiator to the total mass of the styrene and the butadiene is 1:100 to 100000.

[0031] In some preferred embodiments of the present invention, the nonpolar solvent has 5 to 8 carbon atoms. Preferably, the nonpolar solvent includes one or more combinations of cyclopentane, cyclohexane, cycloheptane, and cyclooctane, with cyclopentane being the most preferred. In some preferred embodiments of the present invention, the amount of the nonpolar solvent relative to the sum of styrene and butadiene is 5 to 34 times by mass.

[0032] According to another aspect of the present invention, a low-vinyl-content solution-polymerized styrene-butadiene rubber prepared according to the above-described preparation method is provided, wherein the mass content of styrene groups is 6-20%, the mass content of vinyl groups is 8-20%, and the mass content of styrene microblocks does not exceed 1%. Herein, styrene microblocks refer to shorter chain segments formed by the continuous connection of multiple styrene monomer units. In this invention, unless otherwise specified, a styrene microblock refers to a short chain segment formed by the continuous connection of seven to fifteen styrene units. The rigidity of the styrene microblocks increases the hardness of the rubber, but also reduces its tensile strength and elongation at break, among other mechanical properties.

[0033] In some preferred embodiments of the present invention, the glass transition temperature of the low vinyl content solution-polymerized styrene-butadiene rubber is -65°C to -85°C.

[0034] According to another aspect of the present invention, the application of the above-mentioned low vinyl content solution-polymerized styrene-butadiene rubber as a raw material in tire manufacturing is provided.

[0035] The low-vinyl-content solution-polymerized styrene-butadiene rubber of the present invention, due to its low benzene and low vinyl content characteristics, is suitable for the manufacture of high-performance tires such as new energy vehicle tires when combined with medium- and high-benzene solution-polymerized styrene-butadiene rubbers.

[0036] Compared to existing technologies, this invention provides a novel compound structure modifier applied to the solution polymerization of styrene-butadiene rubber (SBR). This overcomes the problem in existing technologies where the polymerization process often leads to an increase in 1,2-vinyl content while causing randomization of the polymer chain structure, thus failing to achieve low benzene and low vinyl content. Furthermore, the compound structure modifier of this invention can accelerate the reaction process, save reaction reagents, and make the preparation process simpler and more efficient. Attached Figure Description

[0037] Figure 1 This refers to the random, low-benzene, low-vinyl content solution-polymerized styrene-butadiene rubber prepared in Example 1 of the present invention. 1 H-NMR spectrum.

[0038] Figure 2 The random solution-polymerized styrene-butadiene rubber prepared for Comparative Example 1 1 H-NMR spectrum.

[0039] Figure 3 For the solution-polymerized styrene-butadiene rubber prepared in Comparative Example 3 1 H-NMR spectrum.

[0040] Figure 4 For the solution-polymerized styrene-butadiene rubber prepared in Comparative Example 4 1 H-NMR spectrum. Detailed Implementation

[0041] In order to provide a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention will now be described in detail below, but it should not be construed as limiting the scope of implementation of the present invention.

[0042] Raw material source:

[0043] Styrene, 99% purity. Butadiene, 99% purity. Cyclopentane, 99% purity.

[0044] All other reagents are commercially available industrial products.

[0045] Analysis and testing methods:

[0046] Molecular weight determination: Molecular weight was determined using a Waters 2414 gel permeation chromatography (GPC) system (Waters, Inc., USA). A polystyrene standard was used as the calibration curve. The mobile phase was tetrahydrofuran, the column temperature was 40℃, the sample concentration was 1 mg / mL, the injection volume was 50 μL, the elution time was 40 min, and the flow rate was 1 mL / min. -1 .

[0047] Determination of styrene group content, vinyl content, and styrene block content: The components of solution-polymerized styrene-butadiene rubber were calculated using 1H NMR spectroscopy, and the test spectra were analyzed according to the calculation method for solution-polymerized styrene-butadiene rubber (SSBR) in GB / T 37388-2019.

[0048] Determination of glass transition temperature (Tg): The glass transition temperature of the product was measured using DSC. The instrument model was DSC1, manufactured by Mettler AG, Switzerland. The heating range was -80 to 80 °C, and the heating rate was 10 °C / min.

[0049] Example 1:

[0050] This embodiment provides a compound structure modifier comprising: 0.1g anisole and 0.1g tributyl phosphite, with a molar ratio of approximately 2.31:1.

[0051] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0052] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 36g of styrene, and 564g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 0.1g anisole, 0.1g tri-n-butyl phosphite, and 7.5g cyclopentane) was added. After heating to 30℃, 2.72g of the initiator, n-butyllithium, was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually decreased from 30℃. The temperature was raised to about 85°C, which took about 9 minutes. After reaching the highest temperature of 85°C, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50°C, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain a random solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 132739) with low benzene and low vinyl content. The styrene content was about 6%, the vinyl content was about 10%, and the styrene block content was about 0.6%.

[0053] Example 2:

[0054] This embodiment provides a compound structure modifier comprising: 0.1g anisole and 0.2g tributyl phosphite, with a molar ratio of approximately 1.16:1.

[0055] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0056] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 60g of styrene, and 540g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 0.1g anisole, 0.2g tri-n-butyl phosphite, and 7.5g cyclopentane) was added. After heating to 40℃, 2.4g of the initiator, n-butyllithium, was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually increased from 40℃. The reaction was carried out at a temperature of approximately 87°C for about 8 minutes. After reaching the highest temperature of 87°C, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50°C, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain a random solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 143623) with low benzene and low vinyl content. The styrene content was approximately 10%, the vinyl content was approximately 10%, and the styrene block content was approximately 0.3%.

[0057] Example 3:

[0058] This embodiment provides a compound structure modifier comprising: 0.1g anisole and 0.3g tributyl phosphite, with a molar ratio of approximately 0.76:1.

[0059] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0060] First, the 10L high-pressure reactor is purged with nitrogen three times. Then, 3800g of cyclopentane, 60g of styrene, and 540g of butadiene are added. While stirring uniformly at 300rpm, a compound structure modifier (a mixture of 0.1g anisole, 0.3g tri-n-butyl phosphite, and 7.5g cyclopentane) is added. After heating to 50℃, 3.2g of the initiator, n-butyllithium, is added. Stirring continues under nitrogen protection, during which the temperature inside the high-pressure reactor gradually increases from 50℃ to 89℃. The reaction was carried out at approximately 0.5℃ for about 9 minutes; after reaching the highest temperature of 89.5℃, the reaction continued for another 10 minutes, and then 2g of ethanol was added to the high-pressure reactor to terminate the reaction; after the solution in the high-pressure reactor cooled to below 50℃, it was released, and the resulting solution was boiled in water to coagulate and dried to obtain a random low-benzene and low-vinyl content solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 174923), in which the styrene group content was about 10%, the vinyl content was about 20%, and the styrene block content was about 0.4%.

[0061] Example 4:

[0062] This embodiment provides a compound structure modifier comprising: 0.1g of dimethyl phthalate and 0.1g of triethyl phosphite, with a molar ratio of approximately 1.2:1.

[0063] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0064] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 100g of styrene, and 500g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 0.1g of dimethyl phthalate, 0.1g of triethyl phosphite, and 7.5g of cyclopentane) was added. After heating to 50℃, 2.72g of the initiator n-butyllithium was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually decreased from 50℃. The temperature was raised to approximately 86°C, taking about 10 minutes. After reaching the highest temperature of 86°C, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50°C, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain a random solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 194637) with low benzene and low vinyl content. The styrene content was approximately 17%, the vinyl content was approximately 14%, and the styrene block content was approximately 0.5%.

[0065] Example 5:

[0066] This embodiment provides a compound structure modifier comprising: 0.2g of dimethyl phthalate and 0.2g of trimethyl phosphite, with a molar ratio of approximately 0.9:1.

[0067] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0068] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 120g of styrene, and 480g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 0.2g of dimethyl phthalate, 0.2g of trimethyl phosphite, and 7.5g of cyclopentane) was added. The temperature was raised to 60℃, and then 2.72g of the initiator, n-butyllithium, was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually decreased from 60℃. The temperature was raised to approximately 81°C, taking about 12 minutes. After reaching the highest temperature of 81°C, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50°C, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain a random solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 216405) with low benzene and low vinyl content. The styrene content was approximately 20%, the vinyl content was approximately 20%, and the styrene block content was approximately 0.4%.

[0069] Example 6:

[0070] This embodiment provides a compound structure modifier comprising: 29g of 2-nitrophenyl octyl ether and 1.0g of triphenyl phosphite, with a molar ratio of approximately 36:1.

[0071] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0072] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 100g of styrene, and 500g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 29g of 2-nitrobenzeneoctyl ether, 1.0g of triphenyl phosphite, and 7.5g of cyclopentane) was added. After heating to 60℃, 2.72g of the initiator n-butyllithium was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually decreased from 60℃. The temperature was raised to approximately 76°C, taking about 12 minutes. After reaching the highest temperature of 76°C, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50°C, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain a random solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 174235) with low benzene and low vinyl content. The styrene content was approximately 17%, the vinyl content was approximately 15%, and the styrene block content was approximately 0.2%.

[0073] Example 7:

[0074] This embodiment provides a compound structure modifier comprising: 0.36g of dibenzo-18-crown-6-ether and 25.0g of tri-n-butyl phosphite, with a molar ratio of approximately 0.1:1.

[0075] This embodiment provides a method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, including:

[0076] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 100g of styrene, and 500g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 0.36g dibenzo-18-crown-6-ether, 25.0g tri-n-butyl phosphite, and 7.5g cyclopentane) was added. After heating to 50℃, 2.72g of the initiator n-butyllithium was added. Stirring continued under nitrogen protection. During this process, the temperature inside the high-pressure reactor would rise from 50℃. The temperature was gradually increased to about 96.3℃, which took about 9 minutes. After reaching the highest temperature of 96.3℃, the reaction continued for 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50℃, it was released. The resulting solution was boiled in water to coagulate and dried to obtain a random solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 194739) with low benzene and low vinyl content. The styrene content was about 18%, the vinyl content was about 15%, and the styrene block content was about 0.4%.

[0077] Comparative Example 1:

[0078] This comparative example provides a compound structure modifier comprising 3.0 g tetrahydrofuran and 1.0 g ethyl tetrahydrofurfuryl ether, with a molar ratio of approximately 5.42:1.

[0079] This comparative example provides a method for preparing random solution-polymerized styrene-butadiene rubber, specifically including:

[0080] First, the 10L high-pressure reactor is purged with nitrogen three times. Then, 3800g of cyclopentane, 100g of styrene, and 500g of butadiene are added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 3.0g tetrahydrofuran, 1.0g ethyl tetrahydrofurfuryl ether, and 7.5g cyclopentane) is added. After heating to 50℃, 2.72g of the initiator n-butyllithium is added. Stirring continues under nitrogen protection, during which the temperature inside the high-pressure reactor gradually increases from 50℃. The temperature was raised to approximately 93.5℃, and the reaction took about 9 minutes. After reaching the highest temperature of 90.5℃, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50℃, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 172346) with low benzene and low vinyl content. The styrene content was approximately 17%, the vinyl content was approximately 30%, and the styrene block content was approximately 0.4%.

[0081] As can be seen from Comparative Example 1, using a modifier not of this invention, the styrene block content can be reduced to below 1% due to the use of ethyl tetrahydrofurfuryl ether and a higher amount of tetrahydrofuran, but the 1,2-vinyl content cannot reach ≤20%.

[0082] Comparative Example 2:

[0083] This comparative example provides a method for preparing solution-polymerized styrene-butadiene rubber, specifically including:

[0084] First, the reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 120g of styrene, and 480g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a structure modifier (a mixture of 2.0g ethyl tetrahydrofurfuryl ether and 7.5g cyclopentane) was added. The temperature was raised to 45℃, and then 2.72g of the initiator n-butyllithium was added. Stirring continued under nitrogen protection, during which the temperature inside the reactor gradually increased from 45℃ to 96.8℃. The reaction was carried out at approximately ℃ for about 11 minutes; after reaching the highest temperature of 96.8℃, the reaction continued for another 10 minutes, and then 2g of ethanol was added to the high-pressure reactor to terminate the reaction; after the solution in the high-pressure reactor cooled to below 50℃, it was released, and the resulting solution was boiled in water to coagulate and dried to obtain solution-polymerized styrene-butadiene rubber with low benzene and high vinyl content (number average molecular weight Mn is 192376), of which the styrene content was about 20%, the vinyl content was about 48%, and the styrene block content was about 2.3%.

[0085] As can be seen from Comparative Example 2, when using a modifier not of this invention, due to the use of ethyl tetrahydrofurfuryl ether, the 1,2-vinyl content cannot reach ≤20%, and the block content reaches 2.3%, so the microstructure cannot be randomized.

[0086] Comparative Example 3:

[0087] This comparative example provides a method for preparing solution-polymerized styrene-butadiene rubber, specifically including:

[0088] First, the 10L high-pressure reactor is purged with nitrogen three times. Then, 3800g of cyclopentane, 120g of styrene, and 480g of butadiene are added. While stirring uniformly at 300rpm, a solution containing a structure modifier (a mixture of 1.0g of 2,2-tetrahydrofuranylpropane and 7.5g of cyclopentane) is added. After heating to 50℃, 2.72g of the initiator n-butyllithium is added. Stirring continues under nitrogen protection, during which the temperature inside the high-pressure reactor gradually increases from 50℃ to 92℃. The reaction was carried out at approximately 0.6℃ for about 10 minutes; after reaching the highest temperature of 92.6℃, the reaction continued for another 10 minutes, and then 2g of ethanol was added to the high-pressure reactor to terminate the reaction; after the solution in the high-pressure reactor cooled to below 50℃, it was released, and the resulting solution was boiled in water to coagulate and dried to obtain solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 164427) with low benzene and low vinyl content, of which the styrene content was about 20%, the vinyl content was about 35%, and the styrene block content was about 4.6%.

[0089] As can be seen from Comparative Example 3, when using a modifier not of this invention, due to the use of 2,2-tetrahydrofuranylpropane, the 1,2-vinyl content cannot reach ≤20%, and the styrene block content reaches 4.6%, so the microstructure cannot be randomized.

[0090] Comparative Example 4:

[0091] This comparative example provides a method for preparing solution-polymerized styrene-butadiene rubber, specifically including:

[0092] First, nitrogen was purged three times in a 10L high-pressure reactor. Then, 3800g of cyclopentane, 90g of styrene, and 510g of butadiene were added. A solution containing a structure modifier (a mixture of 0.2g of tributyl phosphite and 7.5g of cyclopentane) was added while stirring uniformly at 300rpm. The temperature was raised to 50℃, and then 2.72g of initiator n-butyllithium was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually increased from 50℃ to approximately 72.1℃, taking about 120 minutes. After reaching the highest temperature of 72.1℃, the reaction continued for another 40 minutes. Then, 2g of ethanol was added as a terminator to terminate the reaction. The solution was cooled to below 50℃ and then discharged. The resulting solution was then boiled, coagulated, and dried to obtain a solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 173647) with low benzene and low vinyl content. The styrene content was approximately 15%, the vinyl content approximately 17%, and the styrene block content approximately 5.1%.

[0093] As can be seen from Comparative Example 4, when phosphite structure modifiers are used alone, the polymerization reaction proceeds slowly and the styrene block content is relatively high, reaching 5.1%.

[0094] Comparative Example 5:

[0095] This comparative example provides a compound structure modifier comprising: 0.1 g tetrahydrofuran and 0.1 g ethyl tetrahydrofurfuryl ether, with a molar ratio of approximately 1.80:1.

[0096] This comparative example provides a method for preparing random solution-polymerized styrene-butadiene rubber, specifically including:

[0097] First, the 10L high-pressure reactor was purged with nitrogen three times. Then, 3800g of cyclopentane, 100g of styrene, and 500g of butadiene were added. While stirring uniformly at 300rpm, a solution containing a complex structure modifier (a mixture of 0.1g tetrahydrofuran, 0.1g ethyl tetrahydrofurfuryl ether, and 7.5g cyclopentane) was added. After heating to 50℃, 2.72g of the initiator n-butyllithium was added. Stirring continued under nitrogen protection, during which the temperature inside the high-pressure reactor gradually increased from 50℃. The reaction temperature was raised to approximately 93.5℃, taking about 43 minutes. After reaching the highest temperature of 76.5℃, the reaction continued for another 10 minutes. Then, 2g of ethanol was added to the high-pressure reactor to terminate the reaction. After the solution in the high-pressure reactor cooled to below 50℃, it was released. The resulting solution was then boiled in water to coagulate and dried to obtain solution-polymerized styrene-butadiene rubber (number average molecular weight Mn of 162966) with low benzene and low vinyl content. The styrene content was approximately 17%, the vinyl content was approximately 30%, and the styrene block content was approximately 0.4%.

[0098] Comparative Example 5 used a regulator not of this invention, and the amount used was similar to that of this invention. However, due to the use of ethyl tetrahydrofurfuryl ether, the 1,2-vinyl content in the product could not reach ≤20%, and because the amount of ethyl tetrahydrofurfuryl ether added was low, the time required to reach the highest temperature was longer.

[0099] Figure 1 This refers to the random, low-benzene, low-vinyl content solution-polymerized styrene-butadiene rubber prepared in Example 1 of the present invention. 1 H-NMR spectrum. Figure 1 Integrating the 1H NMR spectrum revealed a styrene content of 6% and a vinyl content of 10%, with a randomized microstructure (no peaks in the chemical shift range of 6.2-6.75 indicate randomization). Testing showed that the low-benzene, low-vinyl-content solution-polymerized styrene-butadiene rubber prepared in Example 1 had a glass transition temperature of approximately -80°C.

[0100] Figure 2 The random solution-polymerized styrene-butadiene rubber prepared for Comparative Example 1 1 1H-NMR spectrum. Integration of the 1H NMR spectrum reveals a styrene content of 17% and a vinyl content of 30%, with a randomized microstructure (no peaks in the chemical shift range of 6.2-6.75 indicate randomization). Because Comparative Example 1 did not use compounding with phosphite, the 1,2-vinyl content in the styrene-butadiene rubber increased, resulting in a glass transition temperature of approximately -62°C. This increased glass transition temperature reduces its flexibility in tire formulations, affecting its compatibility with other rubber types. Simultaneously, the increased 1,2-vinyl content increases the rubber's hardness, making processing and mixing more difficult and reducing its processing performance.

[0101] Figure 3 The solution-polymerized styrene-butadiene rubber with low vinyl content in benzene prepared for Comparative Example 3 1 H-NMR spectrum. Figure 3 Integrating the 1H NMR spectrum revealed a styrene content of 20% and a vinyl content of 35%, with a block structure (peaks at chemical shifts of 6.2–6.75 indicate block structure), and a block content of approximately 4.6%. Testing showed that the glass transition temperature of the low-vinyl-content solution-polymerized styrene-butadiene rubber prepared in Comparative Example 3 was approximately -54°C.

[0102] Figure 4 The solution-polymerized styrene-butadiene rubber with low benzene and low vinyl content prepared for Comparative Example 4 1 H-NMR spectrum. Figure 3Integrating the 1H NMR spectrum revealed a styrene content of 15% and a vinyl content of 17%, with a block structure (peaks at chemical shifts of 6.2–6.75 indicate block structure), and a block content of approximately 5.1%. Testing showed that the glass transition temperature of the low-vinyl-content solution-polymerized styrene-butadiene rubber prepared in Comparative Example 4 was approximately -73°C.

[0103] The comparison shows that the solution-polymerized styrene-butadiene rubber obtained by the embodiments of the present invention has a lower glass transition temperature.

Claims

1. A compound structure modifier, wherein, Including ether-based structure modifiers and phosphite-based structure modifiers; The structure of the ether-based structure modifier includes a benzene ring and / or an oxygen-containing heterocycle. The phosphite structure modifier is selected from one or more combinations of (RO)3P, (R2N)3P and (RS)3P, wherein R is a hydrocarbon group containing 1-12 carbons, and R does not react with organolithium. The molar ratio of the ether-based structure modifier to the phosphite-based structure modifier is 0.1–36:

1.

2. The compound structure modifier according to claim 1, wherein, The ether structure modifiers include one or more of the following: anisole, phenethyl ether, o-phenylenedimethyl ether, benzyl ether, 1,2,4,5-tetramethoxybenzene, 2,2-dimorpholinodiethyl ether, myristyl ether, glycidyl furfural ether, 2-nitrophenyl octyl ether, p-xylyl ether, and dibenzo-18-crown-6-ether.

3. The compound structure modifier according to claim 1, wherein, The phosphite structure modifiers include one or more of the following: tributyl phosphite, triethyl phosphite, trimethyl phosphite, triphenyl phosphite, tribenzyl phosphite, tri(2-methoxyphenyl)phosphine, tri(3-methoxyphenyl)phosphine, tri(2-methoxynaphthyl)phosphine, tri(3-methoxynaphthyl)phosphine, hexamethylphosphine, hexaethylphosphine, trimethyl trithiophosphite, and triphenyl trithiophosphite.

4. The compound structure modifier according to claim 1, wherein, The molar ratio of the ether-based structure modifier to the phosphite-based structure modifier is 0.1 to 1:

1.

5. A method for preparing low vinyl content solution-polymerized styrene-butadiene rubber, wherein, include: Styrene, butadiene, initiator, compound structure modifier according to any one of claims 1 to 4, and non-polar solvent are mixed, heated to 30-70°C, and a polymerization reaction is carried out. Then the reaction is terminated and post-treatment is performed to obtain the solution-polymerized styrene-butadiene rubber with low vinyl content. The initiator includes an organolithium compound.

6. The method for preparing low vinyl content solution-polymerized styrene-butadiene rubber according to claim 5, wherein, The mass of the compound structure modifier is 0.01 to 5% of the total mass of the styrene and the butadiene.

7. The method for preparing low vinyl content solution-polymerized styrene-butadiene rubber according to claim 5, wherein, The mass ratio of styrene to butadiene is 8:92 to 20:

80.

8. The method for preparing low vinyl content solution-polymerized styrene-butadiene rubber according to claim 5, wherein, The mass ratio of the initiator to the total mass of the styrene and butadiene is 1:100 to 100000.

9. The method for preparing low vinyl content solution-polymerized styrene-butadiene rubber according to claim 5, wherein, The nonpolar solvent has 5 to 8 carbon atoms.

10. A low vinyl content solution-polymerized styrene-butadiene rubber, wherein, The low-vinyl content solution-polymerized styrene-butadiene rubber is prepared by the method for preparing low-vinyl content solution-polymerized styrene-butadiene rubber according to any one of claims 5 to 9, wherein the mass content of styrene groups is 6-20%, the mass content of vinyl groups is 8-20%, and the mass content of styrene microblocks does not exceed 1%.

11. The application of a low-vinyl-content solution-polymerized styrene-butadiene rubber as a raw material in tire manufacturing, wherein, The low vinyl content solution-polymerized styrene-butadiene rubber is the low vinyl content solution-polymerized styrene-butadiene rubber according to claim 10, or the low vinyl content solution-polymerized styrene-butadiene rubber prepared by the method for preparing low vinyl content solution-polymerized styrene-butadiene rubber according to any one of claims 5 to 9.

Citation Information

Patent Citations

  • High-styrene low-vinyl-content random solution polymerized styrene-butadiene rubber and preparation method thereof

    CN117567687A