Salicylaldimine ligands modified with oxygen substituents, pre-transition metal catalyst precursors, and preparation and use thereof
By introducing oxygen-substituent-modified salicylaldehyde imine pre-transition metal catalyst precursor into olefin polymerization catalyst, the problem of decreased activity of existing catalysts during ethylene-α-olefin copolymerization was solved, achieving efficient copolymerization reaction and comonomer insertion, and generating copolymers with different properties and mechanical properties.
Patent Information
- Application Number
- CN202510654532.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-21
- Publication Date
- 2026-11-24
AI Technical Summary
Existing olefin polymerization catalysts show a significant decrease in activity when catalyzing the copolymerization of ethylene and α-olefins, and the low comonomer insertion rate makes it difficult to adjust the topology and mechanical properties of polyethylene.
A salicylaldehyde imine pre-transition metal catalyst precursor modified with oxygen-containing substituents was designed. By introducing oxygen-containing functional groups into the catalyst to provide weak interactions, the copolymerization activity and comonomer insertion rate of the catalyst were improved. The heteroligand catalyst with asymmetric design played a synergistic role.
It improves the catalyst activity and comonomer insertion rate in the copolymerization of ethylene and α-olefins, and can catalyze the homopolymerization or copolymerization of various monomers to generate copolymers with different properties and mechanical properties.
Smart Images

Figure BDA0005411992130000021 
Figure BDA0005411992130000031 
Figure BDA0005411992130000032
Abstract
Description
Technical Field
[0001] This invention belongs to the field of olefin coordination polymerization and relates to olefin coordination polymerization catalysts. Specifically, it relates to the synthesis of a class of oxygen-substituent-modified salicylaldehyde imine pretransition metal catalyst precursors and the application of catalysts composed therefrom in catalyzing olefin polymerization. Background Technology
[0002] Polyolefins are common materials in daily life, accounting for more than half of all plastics produced annually. Industrially, polyolefins are mainly synthesized through coordination polymerization, and the development of polyolefin materials is inseparable from the continuous development and updating of catalysts. Through the study of the structure-activity relationship of olefin polymerization catalysts, scientists have summarized a series of catalyst regulation strategies, providing a reference for the design of polyolefin catalysts. Guided by these structure-activity relationships, scientists have developed a variety of olefin polymerization catalysts with different properties.
[0003] FI catalysts, using salicylaldehyde-imine as ligands and former transition metals as center metals, exhibit good activity in catalyzing olefin polymerization, and can even achieve living polymerization in ethylene and propylene polymerization. However, the probability of chain transfer during ethylene polymerization is low, resulting in polyethylene that is generally linear with fewer branches and a relatively limited topological structure.
[0004] Introducing branched chains into polyethylene can regulate the crystallinity and mechanical properties of polyolefins. However, α-olefins have greater steric hindrance than ethylene, thus significantly reducing the activity of catalysts catalyzing the copolymerization of ethylene and α-olefins. Introducing weakly interacting groups into the catalyst is an effective strategy to improve its copolymerization performance. Weakly interacting groups often contain highly electronegative atoms, which exhibit weak interactions with the metal center or the CH bonds on the polymer chain. Modifying the catalyst with weakly interacting groups can enhance its activity in ethylene polymerization; these groups can also effectively capture comonomers, improving the catalyst's activity in the copolymerization reaction and the comonomer insertion rate. Summary of the Invention
[0005] The purpose of this invention is to provide a novel oxygen-substituent-modified salicylaldehyde imine pretransition metal catalyst precursor, which utilizes the weak interactions of oxygen-containing functional groups to enhance the catalyst's activity in copolymerization and the insertion rate of comonomers, thereby modifying polyethylene.
[0006] In a first aspect of the present invention, an oxygen-substituent-modified salicylaldehyde imine catalyst ligand is provided, the structure of which is shown in Formula I:
[0007]
[0008] In Formula I, R1 is hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, or siloxy; R2 is hydrogen, straight-chain or branched alkyl, cycloalkyl, silyl, or aryl; R3, R4, R5, R6, and R7 may be the same or different, and each is independently selected from hydrogen, halogen, nitro, straight-chain or branched alkyl, halogen-substituted alkyl, cycloalkyl, or silyl.
[0009] Wherein, R1 is preferably hydroxyl, nitro, C1-C10 straight-chain or branched alkoxy, C3-C20 cycloalkyloxy, C1-C10 siloxy, phenoxy, or C1-C10 alkyl, C3-C20 cycloalkyl, or C1-C20 siloxy-substituted phenoxy; C1-C20 polyethylene glycol, C1-C20 siloxy, more preferably nitro, C1-C10 straight-chain or branched alkoxy (e.g., methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, isopropoxy, etc.). The phenoxy group may contain butoxy, tert-butoxy, etc., C3-C10 cycloalkyloxy groups (e.g., cyclopropyloxy, cyclobutyloxy, cyclopentyloxy, cyclobutyloxy, adamantyloxy, etc.), phenoxy or substituted phenoxy groups, wherein the substituted phenoxy group refers to a phenoxy group with one or more identical or different substituents, and the substituents are preferably alkyl, silyl, or cycloalkyl, such as C1-C10 alkyl-substituted phenyl, C1-C10 silyl-substituted phenyl, C3-C10 cycloalkyl-substituted phenyl, or C1-C20 polyethylene glycol group.
[0010] R2 is preferably H, a straight-chain or branched alkyl group of C1-C20, a cycloalkyl group of C3-C20, a silyl group of C1-C20, a phenyl group, a phenyl group substituted with an alkyl group of C1-C10, a phenyl group substituted with a silyl group of C1-C10, or a phenyl group substituted with a cycloalkyl group of C3-C10. More preferably, it is H, a alkyl group of C1-C6 (e.g., methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, and tert-butyl), a cycloalkyl group of C3-C10 (e.g., cyclopropyl, cyclobutyl, cyclopentyl, cyclobutyl, adamantane, etc.), a phenyl group, or a substituted phenyl group. The substituted phenyl group refers to a phenyl group with one or more identical or different substituents. The substituents are preferably alkyl, silyl, or cycloalkyl, such as a phenyl group substituted with an alkyl group of C1-C10, a phenyl group substituted with a silyl group of C1-C10, or a phenyl group substituted with a cycloalkyl group of C3-C10.
[0011] R3, R4, R5, R6, and R7 are preferably H, C1-C6 alkyl, halogen, or halogen-substituted C1-C6 alkyl, and more preferably selected from H, F, Cl, Br, I, trifluoromethyl, and C1-C4 alkyl, wherein the C1-C4 alkyl is methyl, ethyl, propyl, isopropyl, n-butyl, or tert-butyl, etc.
[0012] In a second aspect of the invention, a pre-transition metal catalyst precursor based on an oxygen-substituent-modified salicylaldehyde imine ligand as shown in Formula I is provided, the structure of which is shown in Formula II:
[0013]
[0014] In Formula II, the two salicylaldehyde imine ligands may be the same or different. R1 is hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, or siloxy; R1' is hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, siloxy, aryl, branched alkyl, or cycloalkyl; R2 and R2' may be the same or different, each independently selected from hydrogen, straight-chain or branched alkyl, cycloalkyl, silalkyl, or aryl; Ar1 and Ar1' may be the same or different, and are phenyl or phenyl with one or more substituents, wherein each substituent is independently selected from straight-chain or branched alkyl, cycloalkyl, halogen-substituted alkyl, halogen, nitro, or silalkyl.
[0015] M is a pre-transition metal, preferably one of the pre-transition metals Ti, Zr, and Hf.
[0016] L is a halogen, preferably one of Cl or Br.
[0017] In Formula II, both salicylaldehyde imine ligands can be selected from the salicylaldehyde imine ligands shown in Formula I, or only one of the salicylaldehyde imine ligands can be selected from the salicylaldehyde imine ligands shown in Formula I. For example, one salicylate imine ligand is modified with an oxygen-containing substituent, as shown in Formula I, and the other salicylate imine ligand has a sterically hindered substituent, that is, R1 and R1' in Formula II are different. R1 is an oxygen-containing substituent selected from hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, and siloxy; R1' is a sterically hindered substituent selected from aryl, branched alkyl, cycloalkyl, etc. Among them, the sterically hindered substituents are, for example, phenyl and tert-butyl.
[0018] When R1 and R1' are methoxy groups, R2 and R2' are H, Ar1 and Ar1' are pentafluorophenyl groups, and L is Cl, the compound of the above-mentioned general formula II is as shown in formula IIa:
[0019]
[0020] When R1 and R1' are ethylene glycol monomethyl ether groups, R2 and R2' are H, Ar1 and Ar1' are pentafluorophenyl groups, and L is Cl, the compound of the above general formula II is as shown in formula IIb:
[0021]
[0022] When R1 is methoxy, R1' is tert-butyl, R2 and R2' are H, Ar1 and Ar1' are pentafluorophenyl, and L is Cl, the compound of the above general formula II is as shown in formula IIc:
[0023]
[0024] When R1 is ethylene glycol monomethyl ether, R1' is tert-butyl, R2 and R2' are H, Ar1 and Ar1' are pentafluorophenyl, and L is Cl, the compound of the above general formula II is as shown in formula IId:
[0025]
[0026] In a third aspect of the present invention, a method for preparing the ligand compound shown in Formula I and the pre-transition metal catalyst precursor compound shown in Formula II is provided, comprising the following steps:
[0027]
[0028] 1) The compound shown in Formula VI is a commercially available reagent or is synthesized by a nucleophilic substitution reaction of the compound shown in Formula IV with the compound shown in Formula V.
[0029] 2) The compound shown in Formula I is synthesized by a condensation reaction of the compound shown in Formula VI and the compound shown in Formula VII under acid-catalyzed conditions.
[0030] 3) The compound shown in Formula I is deprotonated in an organic solvent and then metallized with a former transition metal source to obtain the former transition metal catalyst precursor shown in Formula II.
[0031] In step 1) above, an excess base is first added to the compound shown in formula IV for deprotonation reaction, and then a sterically hindered compound shown in formula V is added for nucleophilic substitution reaction. The base is preferably KH, NaH, or n-butyllithium. The deprotonation reaction time is generally 0.5h-8h, preferably 0.5h-2h. The solvent is preferably DMSO or DMF. After adding the compound shown in formula V, the reaction time is generally 1h-12h, preferably 2h-8h.
[0032] The condensation reaction in step 2) above uses an acid as a catalyst, preferably formic acid or p-toluenesulfonic acid, and the reaction solvent is preferably methanol or ethanol. The reaction time is generally 1h-12h, preferably 8h-12h.
[0033] In step 3) above, the deprotonating agent is KH or NaH, and the metal source used in the metallization reaction is MCl4(THF)2. The molar ratio of the compound shown in Formula I, the deprotonating agent, and the metallization precursor is 1:(1-4):(0.5-2). In some embodiments of the present invention, the molar ratio of the compound shown in Formula I, NaH, and the metal source MCl4(THF)2 is 1:2:1; the reaction temperature is 0-40°C, preferably 0-25°C, and the reaction time is 3-48 h, preferably 8 h-12 h. The two salicylaldehyde imine ligands in the compound shown in Formula II may be the same or different, and coordinate with the metal source in one or two steps.
[0034] In a fourth aspect of the invention, a catalyst is provided consisting of the aforementioned pre-transition metal catalyst precursor and a co-catalyst, wherein the co-catalyst is an aluminum-containing reagent or a boron-containing reagent.
[0035] The aluminum-containing reagent is preferably an alkylaluminoxane or its modified compound, wherein the general formula of the alkylaluminoxane is:
[0036]
[0037] In Formula III, R is an alkyl group, preferably a C1-C8 alkyl group, such as methyl, ethyl, or isooctyl; n is an integer greater than 1. The polyaluminoxane can be linear, branched, or cyclic / cage-like, such as methylaluminoxane. In the embodiments of the present invention, the co-catalyst used is methylaluminoxane, and the molar ratio of the metal catalyst precursor to methylaluminoxane in the catalyst system is 1:(500-9000), preferably 1:(500-1500).
[0038] The boron-containing reagent is preferably B(C6F5)3, [Ph3C][B(C6F5)4], Na{B[C6H3(CF3)2]}4 or [HNMe2Ph][B(C6F5)4], etc.
[0039] In a fifth aspect of the invention, the application of the above-described catalyst in catalyzing olefin polymerization or copolymerization reactions is provided. The catalyst system composed of the pre-transition metal catalyst precursor based on an oxygen-substituent-modified salicylaldehyde-imine ligand synthesized in this invention and an aluminum-containing or boron-containing reagent can exhibit unique catalytic performance in olefin polymerization. In embodiments of the invention, ethylene undergoes polymerization under the action of this catalyst at a polymerization temperature range of -20 to 50°C; catalyzing the copolymerization of ethylene, propylene, and C3-C10 α-olefins, dienes, or cycloolefins, wherein the comonomers are preferably 1-pentene, 1-hexene, 1-heptene, 1-octene, 1,5-hexadiene, isoprene, norbornene, or C1-C10 alkyl-substituted norbornene.
[0040] The polymerization reaction catalyzed by the catalyst of the present invention can be carried out in an inert solvent, typically an aromatic solvent such as toluene or benzene.
[0041] Compared with the prior art, the present invention has the following technical advantages:
[0042] 1. A phenol-oxygen ortho-modified salicylaldehyde imine isoligand or heteroligand precursor for a transition metal catalyst was synthesized for the first time.
[0043] 2. In heteroligand salicylaldehyde-imine pre-transition metal catalysts, one ligand is modified with an oxygen-containing substituent, providing a weak interaction that helps capture sterically hindered monomers in the system; the other ligand is substituted with a sterically hindered group, offering some protection to the metal center. The two salicylaldehyde-imine ligands in the heteroligand catalyst, designed using an asymmetric design strategy, work synergistically, allowing for more precise catalyst control.
[0044] 3. In the copolymerization experiments of ethylene and α-olefin monomers, the oxygen-functionalized salicylaldehyde-imine pre-transition metal catalyst exhibited excellent catalytic copolymerization performance, maintaining high levels of both catalyst activity and comonomer insertion rate. By controlling the copolymerization conditions, a series of copolymers with different properties and mechanical characteristics can be obtained using the oxygen-functionalized salicylaldehyde-imine pre-transition metal catalyst.
[0045] 4. The oxygen-functionalized salicylaldehyde imine pre-transition metal catalyst is applicable to a wide range of monomers and can catalyze the homopolymerization or copolymerization with ethylene of monomers such as propylene, 1-hexene, 1,5-hexadiene, isoprene, and norbornene. Detailed Implementation
[0046] The present invention will be further described in detail below through specific embodiments:
[0047] Example 1
[0048] The preparation of the salicylaldehyde imine ligand shown in Formula I follows the reaction process described below:
[0049]
[0050] 1) Synthesis of compound 2
[0051] Vanillin 1 (0.500 g, 3.29 mmol) and pentafluoroaniline (0.602 g, 3.29 mmol) were added to a flask, dissolved in methanol, and a few drops of formic acid were added as a dehydrating agent. The reaction was carried out overnight at room temperature. After the reaction was completed, the mixture was filtered, and the solid fraction was recrystallized from methanol, filtered, and dried to give compound 2 as a yellow solid (0.530 g, 50.8%). 1HNMR (400MHz, CDCl3) δ12.59(s,1H,OH),8.86(s,1H,N=CH),7.09–7.01(m,2H,Ar-H),6.93(t,J=7.9Hz,1H,Ar-H),3.95(s,3H,OCH3).
[0052] 2) Synthesis of Compound 5
[0053] Compound 3 (0.500 g, 3.62 mmol) was added to a Schlenk flask, and the atmosphere was purged with nitrogen three times. KH (0.290 g, 7.24 mmol) was added and dissolved in redistilled THF. The mixture was stirred at room temperature for one hour. After the deprotonation reaction was complete, compound 4 (0.834 g, 3.62 mmol) was added dropwise to the Schlenk flask under nitrogen protection, and the reaction was allowed to proceed overnight at room temperature. After the reaction was complete, H2O was carefully added to quench the reaction mixture. The mixture was washed three times with CHCl3, and the aqueous phase was adjusted to pH 2 with HCl and extracted three times with CHCl3. The organic phase was dried over anhydrous calcium sulfate, filtered, and the organic solvent was removed by rotary evaporation. The crude product was purified by column chromatography using petroleum ether / ethyl acetate (10:1, v / v) as the developing solvent. Compound 5 was finally obtained as a yellow solid (0.481 g, 67.6%). 1 H NMR (400MHz, CDCl3) δ10.97(d,J=2.4Hz,1H,OH),9.94(s,1H,CHO),7.25–7.16(m,2H,Ar-H),6.94(td,J=7.9,1.9 Hz, 1H, Ar-H), 4.25–4.19 (m, 2H, OCH2CH2O), 3.79 (td, J = 5.2, 2.1Hz, 2H, OCH2CH2O), 3.46 (d, J = 2.1Hz, 3H, OCH3).
[0054] 3) Synthesis of Compound 6
[0055] Compound 5 (0.280 g, 1.43 mmol) and pentafluoroaniline (0.261 g, 1.43 mmol) were added to a flask, dissolved in methanol, and a few drops of formic acid were added as a dehydrating agent. The reaction was carried out overnight at room temperature. After the reaction was complete, the methanol was concentrated using a rotary evaporator and filtered. The filtrate was partially evaporated to dryness, recrystallized from methanol, filtered, and dried. The two solid fractions were combined to give compound 6 as a yellow solid (0.363 g, 74.3%). 1H NMR (400MHz, CDCl3) δ12.49(s,1H,OH),8.85(s,1H,N=CH),7.10(d,J=7.8Hz,2H,Ar-H),6.91(t,J =7.8Hz,1H,Ar-H),4.28–4.21(m,2H,OCH2CH2O),3.86–3.80(m,2H,OCH2CH2O),3.47(s,3H,OCH3). 13 C NMR (101MHz, CDCl3) δ170.5,152.2,147.8,125.4,119.1,71.1,69.3,69.0,59.3. HRMS(ESI,m / z):Calculated for C 16 H 13 F5NO3[(M+H) + ]:362.0810,found:362.0805.
[0056] Example 2
[0057] The reaction process for preparing the metal catalyst precursor shown in Formula II is as follows:
[0058]
[0059] 1) Synthesis of catalyst precursor OMe-Ti
[0060] In a glove box, compound 2 (0.22 g, 0.73 mmol) and KH (0.09 g, 2.18 mmol) were added to a Schlenk flask, dissolved in THF, and stirred overnight at room temperature. After complete deprotonation, the solvent was removed, and the remaining solid was dissolved in ultradry DCM. This solution was then added dropwise to a DCM solution of TiCl4(THF)2 (0.12 g, 0.36 mmol) and stirred overnight at room temperature. After the reaction was complete, the reaction solution was filtered in a glove box to remove inorganic salts, and the filtrate was dried under vacuum. The crude product was dissolved in a small amount of DCM, and then recrystallized with a large amount of n-hexane to finally obtain OMe-Ti as a red solid (0.174 g, 63.4%). 1 H NMR (400MHz, CDCl3) δ8.86(s,1H,N=CH),7.10–7.02(m,2H,Ar-H),6.94(t,J=7.9Hz,1H,Ar-H),3.95(s,3H). HRMS(ESI,m / z):Calculated forC 28 H 15 Cl2F 10 N₂O₄Ti[(M+H)] +]:750.9727,found:750.9755.
[0061] 2) Synthesis of catalyst precursor EM-Ti
[0062] In a glove box, compound 6 (0.13 g, 0.36 mmol) and KH (0.06 g, 1.08 mmol) were added to a Schlenk flask, dissolved in THF, and stirred overnight at room temperature. After complete deprotonation, the solvent was removed by vacuum, and the remaining solid was dissolved in ultradry DCM. This solution was then added dropwise to a DCM solution of TiCl4(THF)2 (0.09 g, 0.18 mmol) and stirred overnight at room temperature. After the reaction was complete, the reaction solution was filtered in a glove box to remove inorganic salts, and the filtrate was dried under vacuum. The crude product was dissolved in a small amount of DCM, and then recrystallized with a large amount of n-hexane to finally obtain EM-Ti as a red solid (0.194 g, 69.0%). 1 H NMR (400MHz, CDCl3) δ8.21(s,1H,N=CH),7.17(s,1H,Ar-H),7.03(d,J=7.3Hz,1H,Ar-H),6.93(t,J=7.9Hz,1H,Ar-H),4.25 (dd,J=9.4,4.7Hz,1H,OCH2CH2O),4.06(dd,J=8.8,4.7Hz,1H,OCH2CH2O),3.72–3.60(m,2H,OCH2CH2O),3.41(s,3H,OCH3). 13 CNMR (101MHz, CDCl3) δ171.4,153.6,145.1,127.4,124.2,122.9,121.4,70.2,69.8,58.5,30.6,21.6,13.1.
[0063] 3) Synthesis of the catalyst precursor OMe-tBu-Ti: In a glove box, compound 2 (0.10 g, 0.33 mmol) and KH (0.04 g, 0.99 mmol) were added to a Schlenk flask, dissolved in THF, and stirred overnight at room temperature. After complete deprotonation, the solvent was removed by vacuum, and the remaining solid was dissolved in ultradry DCM. This solution was then added dropwise to a DCM solution of 0.19 g, 0.33 mmol, and stirred overnight at room temperature. After the reaction was complete, the reaction solution was filtered in a glove box to remove inorganic salts, and the filtrate was dried under vacuum. The crude product was dissolved in a small amount of DCM, and then recrystallized with a large amount of n-hexane to finally obtain OMe-tBu-Ti as a red solid (0.133 g, 51.9%). 1H NMR (400MHz, CDCl3) δ8.29(s,1H,N=CH),8.16(s,1H,N=CH),7.70(d,J=6.5Hz,1H,Ar-H),7.35(d,J=6.5Hz, 1H, Ar-H), 7.07–7.03 (m, 2H, Ar-H), 6.95 (d, J = 4.9Hz, 2H, Ar-H), 3.90 (s, 3H, OCH3), 1.29 (s, 9H, C (CH3) 3). 13 C NMR (101MHz, CDCl3) δ173.2,147.8,138.3,136.4,134.3,126.6,123.3,122.2,120.2,56.8,35.1,29.0,22.7. HRMS(ESI,m / z):Calculated for C 31 H 21 Cl2F 10 N₂O₃Ti[(M+H)] + ]:777.0248,found:777.0227.
[0064] 4) Synthesis of catalyst precursor EM-tBu-Ti
[0065] In a glove box, compound 6 (0.10 g, 0.28 mmol) and KH (0.03 g, 0.83 mmol) were added to a Schlenk flask, dissolved in THF, and stirred overnight at room temperature. After complete deprotonation, the solvent was removed, and the remaining solid was dissolved in ultradry DCM. This solution was then added dropwise to a DCM solution of compound 7 (0.14 g, 0.28 mmol) and stirred overnight at room temperature. After the reaction was complete, the reaction solution was filtered in a glove box to remove inorganic salts, and the filtrate was dried under vacuum. The crude product was dissolved in a small amount of DCM, and then recrystallized with a large amount of n-hexane to finally obtain EM-tBu-Ti as a red solid (0.157 g, 68.3%). 1H NMR (400MHz, CDCl3) δ8.30(s,1H,N=CH),8.18(s,1H,N=CH),7.70(d,J=7.7Hz,1H,Ar-H) ,7.35(d,J=7.6Hz,1H,Ar-H),7.19(d,J=7.1Hz,1H,Ar-H),7.09–7.05(m,1H,Ar-H),7.01 (d,J=7.7Hz,1H,Ar-H),6.94(t,J=7.8Hz,1H,Ar-H),4.44(d,J=4.2Hz,1H,OCH2CH2O),4 .20(s,1H,OCH2CH2O),4.04(s,2H,OCH2CH2O),3.52(s,3H,OCH3),1.29(s,9H,C(CH3)3). 13 C NMR (101MHz, CDCl3) δ161.0,138.0,132.3,131.7,118.9,71.2,59.2,35.0,29.3,29.0. HRMS(ESI,m / z):Calculated for C 33 H 25 Cl2F 10 N₂O₄Ti[(M+H)] + ]:821.0510,found:821.0501.
[0066] 5) Synthesis of catalyst precursor OMe-tBu-Zr
[0067] In a glove box, compound 2 (0.10 g, 0.33 mmol) and KH (0.04 g, 0.99 mmol) were added to a Schlenk flask, dissolved in THF, and stirred overnight at room temperature. After complete deprotonation, the solvent was removed, and the remaining solid was dissolved in ultradry DCM. This solution was then added dropwise to a DCM solution of 0.20 g, 0.33 mmol, and stirred overnight at room temperature. After the reaction was complete, the reaction solution was filtered in a glove box to remove inorganic salts, and the filtrate was dried under vacuum. The crude product was dissolved in a small amount of DCM, and then recrystallized with a large amount of n-hexane to finally obtain OMe-tBu-Zr as a yellow solid (0.155 g, 57.4%). 1H NMR (400MHz, CDCl3) δ8.31(s,1H,N=CH),8.22(s,1H,N=CH),7.69(dd,J=7.7,1.5Hz,1H,Ar-H),7.30(dd,J=7.8,1.5Hz,1H,Ar-H ),7.05–7.01(m,1H,Ar-H),6.93(d,J=4.9Hz,2H,Ar-H),6.84(t,J=7.9Hz,1H,Ar-H),3.85(s,3H,OCH3),1.27(s,9H,C(CH3)3). 13 CNMR (101MHz, CDCl3) δ176.6,160.9,149.5,139.8,136.9,134.8,121.1,121.0,119.8,56.4,35.0,29.1,28.9,28.7,14.1. HRMS(ESI,m / z):Calculated for C 31 H 21 Cl2F 10 N₂O₃Ti[(M+H)] + ]:820.9802,found:820.9708.
[0068] 6) Synthesis of catalyst precursor EM-tBu-Zr
[0069] In a glove box, compound 6 (0.10 g, 0.28 mmol) and KH (0.03 g, 0.83 mmol) were added to a Schlenk flask, dissolved in THF, and stirred overnight at room temperature. After complete deprotonation, the solvent was removed, and the remaining solid was dissolved in ultradry DCM. This solution was then added dropwise to a DCM solution of compound 8 (0.20 g, 0.28 mmol) and stirred overnight at room temperature. After the reaction was complete, the reaction solution was filtered in a glove box to remove inorganic salts, and the filtrate was dried under vacuum. The crude product was dissolved in a small amount of DCM, and then recrystallized with a large amount of n-hexane to finally obtain EM-tBu-Zr as a yellow solid (0.128 g, 52.7%). 1H NMR (400MHz, CDCl3) δ8.32(s,1H,N=CH),8.23(s,1H,N=CH),7.69(d,J=6.7Hz,1H,Ar-H) ,7.31(d,J=6.8Hz,1H,Ar-H),7.17(d,J=6.8Hz,1H,Ar-H),7.04(d,J=7.7Hz,1H,Ar-H),7 .01–6.97(m,1H,Ar-H),6.92(t,J=7.8Hz,1H,Ar-H),4.26(s,1H,OCH2CH2O),4.11(s,1H ,OCH2CH2O),3.82(d,J=6.2Hz,2H,OCH2CH2O),3.54(s,3H,OCH3),1.27(s,9H,C(CH3)3). HRMS(ESI,m / z):Calculated for C 33 H 25 Cl2F 10 N₂O₄Ti[(M+H)] + ]:865.0064,found:865.0063.
[0070] Example 3
[0071] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of methylaluminoxane (MAO) (1.5 M), 1-hexene (0.2 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-Ti was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.662 g of polymer with an activity of 132 kg / (mol·h). The melting point of the copolymer was determined to be 129 °C by DSC.
[0072] Example 4
[0073] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (0.2 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor EM-Ti was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.360 g of polymer with an activity of 72.0 kg / (mol·h). The melting point of the copolymer was determined to be 129 °C by DSC.
[0074] Example 5
[0075] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last vacuum purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (0.2 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the ethylene in the toluene. A toluene solution of the catalyst precursor OMe-tBu-Ti was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction solution was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.466 g of polymer with an activity of 93.2 kg / (mol·h). The melting point of the copolymer was determined to be 124 °C by DSC. The tensile test showed that the elongation at break of the copolymer was 122%.
[0076] Example 6
[0077] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last vacuum purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (0.2 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the ethylene in the toluene. A toluene solution of the catalyst precursor EM-tBu-Ti was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction solution was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.435 g of polymer with an activity of 87.0 kg / (mol·h). The melting point of the copolymer was measured to be 123℃ by DSC, and the elongation at break of the copolymer was measured to be 124% by tensile test.
[0078] Example 7
[0079] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (1.0 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v), stirred overnight, filtered, and the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 1.366 g of polymer with an activity of 273.2 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w 13.1×10 4 g / mol, The value was 3.89, the 1-hexene insertion rate was 5.47% as measured by high-temperature NMR, the melting point of the copolymer was 109℃ as measured by DSC, and the elongation at break of the copolymer was 210% as measured by tensile test.
[0080] Example 8
[0081] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (1.0 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor EM-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v), stirred overnight, filtered, and the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.955 g of polymer with an activity of 191.0 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w It is 11.7 × 10 4 g / mol, The 1-hexene insertion rate was 3.21, the high-temperature NMR measured the 1-hexene insertion rate to be 3.26%, the DSC measured the melting point of the copolymer to be 113℃, and the tensile test measured the elongation at break of the copolymer to be 432%.
[0082] Example 9
[0083] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (2.0 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v), stirred overnight, filtered, and the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 1.338 g of polymer with an activity of 267.6 kg / (mol·h). High-temperature GPC measured the polymer M... w It is 8.14×10 4 g / mol, The value was 2.73, the 1-hexene insertion rate was 6.13% as measured by high-temperature NMR, the melting point of the copolymer was 106℃ as measured by DSC, and the elongation at break of the copolymer was 908% as measured by tensile test.
[0084] Example 10
[0085] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-hexene (2.0 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor EM-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v), stirred overnight, filtered, and the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 1.965 g of polymer with an activity of 393.0 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w It is 6.86×10 4 g / mol, The value was 3.17, the 1-hexene insertion rate was 5.25% as measured by high-temperature NMR, the melting point of the copolymer was 106℃ as measured by DSC, and the elongation at break of the copolymer was 745% as measured by tensile test.
[0086] Example 11
[0087] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last vacuum purging, ethylene was introduced. A toluene solution of MAO (1.5 M) and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After 1 min of reaction, 1-hexene (3.0 M) was added to initiate copolymerization. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.548 g of polymer with an activity of 109.6 kg / (mol·h). High-temperature GPC measured the polymer M... w It is 8.98×10 4 g / mol, The value was 3.17, the 1-hexene insertion rate was 4.62% as measured by high-temperature NMR, and the melting point of the copolymer was 128.5℃ as measured by DSC.
[0088] Example 12
[0089] Synthesis of ethylene-1-hexene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M) and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor EM-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After 1 min of reaction, 1-hexene (3.0 M) was added to initiate copolymerization. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.553 g of polymer with an activity of 110.6 kg / (mol·h). High-temperature GPC measured the polymer M... w It is 8.04×10 4 g / mol, The value was 3.09, the 1-hexene insertion rate was 3.68% as measured by high-temperature NMR, and the melting points of the copolymer were 125.5℃ and 128.7℃ as measured by DSC.
[0090] Example 13
[0091] Synthesis of propylene-1-hexene copolymer: A 350 mL Andrew glass polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was placed in a glove box and evacuated to room temperature. In the glove box, a 1.5 M toluene solution of MAO, 1.0 M 1-hexene, and an appropriate amount of toluene were added to the polymerization flask. The polymerization apparatus was connected and removed from the glove box. The polymerization apparatus was then connected to propylene, the gas was purged three times, the temperature was set to the required polymerization temperature (temperature change ≤ 1 °C), the propylene pressure was adjusted to 50 psi, and equilibration was allowed for 10 minutes. A 3 mL toluene solution containing the catalyst precursor OMe-tBu-Zr was added to initiate polymerization; the total volume of toluene in the system was 25 mL. After the reaction time was reached, a methanol solution of hydrochloric acid was added to terminate the reaction. The reaction solution was then poured into 300 mL of methanol and stirred for half an hour. After filtration, the resulting polymer was dried under vacuum at 65 °C for 12 hours, yielding 0.122 g of polymer with an activity of 12.2 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w 3.50×10 4 g / mol, It is 1.60.
[0092] Example 14
[0093] Synthesis of propylene-1-hexene copolymer: A 350 mL Andrew glass polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was placed in a glove box and evacuated to room temperature. In the glove box, a 1.5 M toluene solution of MAO, 1.0 M 1-hexene, and an appropriate amount of toluene were added to the polymerization flask. The polymerization apparatus was connected and removed from the glove box. The polymerization apparatus was then connected to propylene, the gas was purged three times, the temperature was set to the required polymerization temperature (temperature change ≤ 1 °C), the propylene pressure was adjusted to 50 psi, and equilibration was allowed for 10 minutes. A 3 mL toluene solution containing the catalyst precursor EM-tBu-Zr was added to initiate polymerization; the total volume of toluene in the system was 25 mL. After the reaction time was reached, a methanol solution of hydrochloric acid was added to terminate the reaction. The reaction solution was then poured into 300 mL of methanol and stirred for half an hour. After filtration, the resulting polymer was dried under vacuum at 65 °C for 12 hours, yielding 0.098 g of polymer with an activity of 9.8 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w 4.01×10 4 g / mol, It is 1.43.
[0094] Example 15
[0095] Synthesis of poly(1-hexene): A 100 mL Schlenk flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was placed in a glove box and cooled to room temperature under vacuum. In the glove box, appropriate amounts of MAO toluene solution (1.5 M), catalyst precursor OMe-tBu-Zr, and 1-hexene monomer (5.0 M) were added, with toluene as the solvent. Polymerization was carried out under ambient temperature and pressure conditions in the glove box. After the reaction time was reached, the flask was removed from the glove box, and the reaction was terminated by adding a methanol solution of hydrochloric acid. The reaction solution was then poured into 300 mL of methanol and stirred for half an hour. After filtration, the obtained polymer was dried under vacuum at 65 °C for 12 hours, yielding 0.068 g of polymer with an activity of 0.28 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w It is 1.73×10 4 g / mol, It is 1.56.
[0096] Example 16
[0097] Synthesis of ethylene-1-octene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-octene (2.0 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v), stirred overnight, filtered, and the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 3.264 g of polymer with an activity of 652.8 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w 3.20×10 4 g / mol, The value was 3.06, the 1-octene insertion rate was 12.1% as measured by high-temperature NMR, and the melting point of the copolymer was 102℃ as measured by DSC.
[0098] Example 17
[0099] Synthesis of ethylene-1-octene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven. A magnetic stir bar was added, and the flask was then cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1-octene (2.0 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor EM-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of a methanol solution acidified with hydrochloric acid (5%, v / v), stirred overnight, filtered, and the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 2.367 g of polymer with an activity of 473.4 kg / (mol·h). High-temperature GPC analysis showed that the polymer M... w 4.35×10 4 g / mol, The value was 3.00, the 1-octene insertion rate was 13.1% as measured by high-temperature NMR, and the melting point of the copolymer was 101℃ as measured by DSC.
[0100] Example 18
[0101] Synthesis of ethylene-1,5-hexadiene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), 1,5-hexadiene (1.5 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of hydrochloric acid-acidified methanol solution (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 1.643 g of polymer with an activity of 328.6 kg / (mol·h). High-temperature GPC measured the polymer M... w It is 5.43 × 10 4 g / mol, The value was 2.73, and the melting points of the copolymer were measured by DSC to be 113℃ and 96℃.
[0102] Example 19
[0103] Synthesis of ethylene-norbornene copolymer: A 250 mL three-necked polymerization flask was dried overnight at 120 °C in an oven, a magnetic stir bar was added, and then the flask was cooled under vacuum. Nitrogen gas was purged three times, and after the last purging, ethylene was introduced. A toluene solution of MAO (1.5 M), norbornene (1.5 M), and anhydrous and oxygen-free toluene were added sequentially. The system was equilibrated at a preset temperature for 5 min to saturate the toluene with ethylene. A toluene solution of the catalyst precursor OMe-tBu-Zr was added to initiate polymerization, with a total toluene volume of 25 mL. After the reaction started, the gas pressure was maintained at 1 atm. After the reaction time was reached, an ethanol solution of hydrochloric acid was added to terminate the reaction. The reaction mixture was poured into 300 mL of hydrochloric acid-acidified methanol solution (5%, v / v) and stirred overnight. After filtration, the resulting copolymer was dried under vacuum at 65 °C for 12 h to obtain 0.149 g of polymer with an activity of 29.8 kg / (mol·h). High-temperature GPC measured the polymer M... w 0.22×10 4 g / mol, The value was 2.16, and the melting point of the copolymer was 132℃ as measured by DSC.
[0104] Example 20
[0105] Performance of ethylene-1-octene copolymer as an adhesive: The ethylene-1-octene copolymer obtained in Example 17 was added to the joint of two overlapping glass plates. Heating with an infrared lamp was used until the copolymer was completely melted into a liquid state. The bonding area was controlled to be 2.5 cm × 1 cm. After cooling, the two glass plates were bonded together. A universal tensile testing machine was used to pull the two glass plates apart at the fastest possible tensile speed, and the stress-strain curves during this process were recorded. The maximum force that the adhesive could withstand was found to be 258.9 N.
[0106] The results of the above examples show that, in the copolymerization experiments of ethylene with comonomers such as α-olefins, catalysts modified with oxygen-containing substituents, especially heteroligand catalysts, exhibit excellent performance, high activity, and high comonomer insertion rates. By controlling the copolymerization conditions, a series of copolymers with different properties and mechanical properties can be obtained using catalysts modified with oxygen-containing substituents. The catalysts are applicable to a wide range of monomers and can catalyze the homopolymerization or copolymerization of various monomers such as propylene, 1-hexene, 1,5-hexadiene, isoprene, and norbornene.
[0107] The above detailed embodiments describe the oxygen-substituent-modified salicylaldehyde imine catalyst precursor and the catalyst composed therefrom for catalyzing ethylene polymerization or ethylene (co)polymerization provided by the present invention. Those skilled in the art should understand that certain changes or modifications can be made to the present invention without departing from the spirit of the present invention, and are not limited to the contents disclosed in the embodiments.
Claims
1. The application of an oxygen-substituent-modified salicylaldehyde-imine ligand in catalytic olefin polymerization or copolymerization reactions, characterized in that, The salicylaldehyde imine ligand, used as a ligand in the pre-transition metal catalyst precursor, has the structure shown in Formula I: In Formula I, R1 is hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, or siloxy; R2 is hydrogen, straight-chain or branched alkyl, cycloalkyl, silyl, or aryl; R3, R4, R5, R6, and R7 may be the same or different, and each is independently selected from hydrogen, halogen, nitro, straight-chain or branched alkyl, halogen-substituted alkyl, cycloalkyl, or silyl.
2. A pre-transition metal catalyst precursor, the structure of which is shown in Formula II: In Formula II, R1 is hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, or siloxy; R1' is hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, siloxy, aryl, branched alkyl, or cycloalkyl; R2 and R2' may be the same or different, each independently selected from hydrogen, straight-chain or branched alkyl, cycloalkyl, silalkyl, or aryl; Ar1 and Ar1' may be the same or different, and are phenyl or phenyl with one or more substituents, wherein each substituent is independently selected from straight-chain or branched alkyl, cycloalkyl, halogen-substituted alkyl, halogen, nitro, or silalkyl; M is a pre-transition metal element; L is a halogen.
3. The pre-transition metal catalyst precursor as described in claim 2, characterized in that, M represents Ti, Zr, or Hf; L represents Cl or Br.
4. The pre-transition metal catalyst precursor as described in claim 2, characterized in that, R1 is an oxygen-containing substituent selected from hydroxyl, nitro, straight-chain or branched alkoxy, cycloalkyloxy, aryloxy, polyethylene glycol, and siloxy; R1' is a sterically hindered substituent selected from aryl, branched alkyl, and cycloalkyl.
5. The pre-transition metal catalyst precursor as described in claim 2, characterized in that, The pre-transition metal catalyst precursor is selected from compounds represented by the following formulas IIa, IIb, IIc, and IId:
6. A method for preparing the pre-transition metal catalyst precursor according to any one of claims 2 to 5, comprising the following steps: 1) Prepare the compound shown in Formula VI: either commercially available or synthesized by nucleophilic substitution reaction of the compound shown in Formula IV with the compound shown in Formula V; 2) The compound shown in formula I was synthesized by condensation reaction of the compound shown in formula VI and the compound shown in formula VII under acid-catalyzed conditions. 3) The compound shown in Formula I is deprotonated in an organic solvent and then metallized with a former transition metal source to obtain the former transition metal catalyst precursor shown in Formula II.
7. The preparation method according to claim 6, characterized in that, In step 1), an excess base is first added to deprotonate the compound shown in formula IV, followed by the addition of a sterically hindered compound shown in formula V for affinity substitution. In step 2), the condensation reaction is carried out in methanol solvent using formic acid or p-toluenesulfonic acid as an acid catalyst. In step 3), the deprotonating agent is potassium hydride or sodium hydride, and the metal source is MCl4(THF)2. The two salicylaldehyde imine ligands in the compound shown in formula II may be the same or different, and coordinate with the metal source in one or two steps.
8. A catalyst comprising a pre-transition metal catalyst precursor as described in any one of claims 2 to 5 and a co-catalyst, wherein the co-catalyst is an aluminum-containing reagent or a boron-containing reagent.
9. The catalyst as claimed in claim 8, characterized in that, The aluminum-containing reagent is an alkylaluminoxane or a modified compound thereof, and the general formula of the alkylaluminoxane is: Where R is an alkyl group from C1 to C8, and n is an integer greater than 1; the boron-containing reagent is B(C6F5)3, [Ph3C][B(C6F5)4], Na{B[C6H3(CF3)2]}4 or [HNMe2Ph][B(C6F5)4].
10. The application of the catalyst of claim 8 in catalyzing olefin polymerization or copolymerization reactions.