Process for the synthesis of cyclic polymers using catalyst-free azide-alkene click chemistry
By employing a catalyst-free click chemistry method for the synthesis of azido-olefins, the efficient cycloaddition reaction between the norbornene ring and the azido group is utilized, overcoming the problems of metal catalyst residue and harsh reaction conditions. This method enables the synthesis of high-purity, widely applicable cyclic polymers suitable for applications in optoelectronic and biomedical materials.
Patent Information
- Application Number
- CN202611165951.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-24
AI Technical Summary
Existing methods for synthesizing cyclic polymers require the use of metal catalysts, which leads to the generation of byproducts and environmental pollution. Furthermore, the reaction conditions are harsh, making them difficult to apply in the fields of optoelectronic and biomedical materials.
Using catalyst-free azide-alkene click chemistry, cyclic polymers are synthesized by utilizing the efficient cycloaddition reaction between the tensile double bond on the norbornene ring and the azide group under metal-free and high-temperature dilution conditions. The resulting cyclic polymers are generated through intramolecular cyclization reactions, producing well-defined and high-purity cyclic polymers.
It enables the synthesis of cyclic polymers with no metal catalyst residue, high purity, and high yield. It is applicable to cyclic polymers with different chemical compositions and molecular weights, simplifies the operation process, and is suitable for large-scale production.
Smart Images

Figure CN123152018A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer synthesis technology, and in particular to a method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry. Background Technology
[0002] Cyclic polymers, due to their unique closed-ring topology and the absence of polymer chain ends, exhibit physicochemical properties distinctly different from linear polymers, such as smaller hydrodynamic volume, lower melt viscosity, higher glass transition temperature, and unique thermal decomposition behavior. They hold great promise for applications in drug delivery, nanolithography, and smart materials. Therefore, developing efficient and controllable methods for synthesizing cyclic polymers has always been a research hotspot in polymer science.
[0003] Traditional strategies for synthesizing cyclic polymers mainly include the "ring-expansion method" and the "ring-closure method." The "ring-closure method" involves first synthesizing a linear polymer precursor with reactive functional groups at the end groups, and then performing an intramolecular cyclization reaction under highly diluted conditions. This method is applicable to a wide range of monomers and offers strong polymer structure designability, making it the mainstream method for synthesizing cyclic polymers. Efficient, orthogonal click chemistry is key to achieving intramolecular ring closure.
[0004] Currently, click chemistry reactions used for the synthesis of cyclic polymers mainly focus on copper-catalyzed azido-alkynyl 1,3-dipolar cycloaddition reactions (CuAAC). For example, Laurent et al. first successfully synthesized cyclic polystyrene using this reaction (Laurent BA, Grayson S MJ Am. Chem. Soc., 2006, 128(13): 4238-4239). However, this method has the following technical drawbacks: (1) It requires the use of a copper catalyst, and the residue of the copper catalyst in the polymer is difficult to completely remove, which will affect the optical, electrical properties and biocompatibility of the polymer, and seriously limit its application in optoelectronic materials and biomedical materials; (2) To remove the copper catalyst, complex post-treatment steps such as column chromatography, multiple precipitation or dialysis are required, which increases the preparation cost and time; (3) The treatment of copper-containing waste liquid increases the environmental burden.
[0005] In addition, mercapto-alkene click chemistry has also been used for cyclization reactions, but it often requires photoinitiators or free radical initiators and is prone to side reactions (such as bimolecular coupling, chain transfer, etc.), resulting in low cyclization yields and impure products.
[0006] The 1,3-dipolar cycloaddition reaction of azide groups with ordinary carbon-carbon double bonds usually requires high temperature (>150℃) or high pressure conditions, resulting in low reaction efficiency and a tendency for thermally induced side reactions, thus limiting its application in polymer synthesis. However, when the carbon-carbon double bond is in a tensile cyclic structure (such as norbornene ring), its reactivity is significantly enhanced. Currently, studies have applied the azide-norbornene reaction to the post-modification of linear polymers or the preparation of crosslinked polymers (Zhang, X. et al. Macromol. Rapid Commun. 2016, 37(16): 1311-1317), but its use as a cyclization reaction to construct cyclic polymers has not yet been reported.
[0007] Therefore, developing a novel, mild, efficient, and convenient method for synthesizing cyclic polymers without the need for metal catalysts is of great significance for promoting the basic research and practical applications of cyclic polymers. Summary of the Invention
[0008] The purpose of this invention is to address the shortcomings of existing cyclic polymer synthesis methods, such as the need for metal catalysts and the easy generation of byproducts, by providing a catalyst-free method for synthesizing cyclic polymers using azide-ene click chemistry. This method utilizes the efficient cycloaddition reaction between the tensioned double bond on the norbornene ring and the azide group to achieve intramolecular cyclization of linear polymers under conditions of no catalyst and high-temperature dilution, synthesizing cyclic polymers with well-defined structures and high purity.
[0009] To solve the above problems, the technical solution adopted by the present invention is as follows:
[0010] A method for synthesizing cyclic polymers using catalyst-free azide-alkene click chemistry includes the following steps:
[0011] Step (1): Synthesize linear polymer precursors with norbornene end groups; details are as follows:
[0012] A living / controlled polymerization method was used to initiate the polymerization of monomers with a bifunctional initiator containing norbornene groups and halogen atoms, thereby synthesizing a linear polymer precursor with a norbornene group at one end and a halogen atom at the other end.
[0013] The bifunctional initiator containing norbornene groups and halogen atoms is 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene HO-NB-Br;
[0014] Step (2): Azide formation of linear polymer precursor;
[0015] The linear polymer precursor obtained in step (1) was reacted with sodium azide in a polar solvent to convert the terminal halogen atoms into azide groups, resulting in the azide-terminated norbornene-functionalized linear polymer HO-NB-PS-N3.
[0016] Step (3): Intramolecular cyclization reaction to prepare cyclic polymers
[0017] No metal catalyst was added during the cyclization reaction. Under the condition of no metal catalyst, the azido-terminated norbornene functionalized linear polymer obtained in step (2) was subjected to intramolecular cyclization under dilution conditions. Under heating conditions of 100–120 °C, the azido group at the end of the polymer reacted with the tensioned double bond on the norbornene ring at the other end of the same molecular chain to form an intramolecular 1,3-dipolar cycloaddition reaction, generating a structure containing a triazolinium ring, thereby closing the linear polymer chain into a cyclic structure and obtaining the cyclic polymer c-PS.
[0018] The dilution condition refers to the polymer concentration in the reaction system not exceeding 0.1 mM; by controlling the polymer concentration below 0.1 mM, intermolecular coupling side reactions can be suppressed to the maximum extent, allowing intramolecular cyclization reactions to dominate.
[0019] Preferably, in step (1), the synthetic route of 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene is as follows: norbornene dianhydride is reduced by lithium aluminum hydride to obtain 2,3-dihydroxymethyl-5-norbornene; then it undergoes esterification with 2-bromoisobutyryl bromide in the presence of an acid binder to obtain HO-NB-Br.
[0020] Furthermore, the synthesis of 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene is as follows:
[0021] (a) Reduction step: Under inert gas protection, norbornadiene anhydride was dissolved in anhydrous tetrahydrofuran and then added to an anhydrous tetrahydrofuran suspension of lithium aluminum hydride, wherein the molar ratio of lithium aluminum hydride to norbornadiene anhydride was (2.8~3.2):1; after the addition was complete, the reaction was allowed to proceed to obtain 2,3-dihydroxymethyl-5-norbornene.
[0022] (b) Esterification step: Under inert gas protection, 2,3-dihydroxymethyl-5-norbornene obtained in step (a) is dissolved in anhydrous dichloromethane, triethylamine is added as an acid-binding agent, and then a dichloromethane solution of 2-bromoisobutyryl bromide is slowly added dropwise, controlling the reaction temperature below 0°C; wherein, the molar ratio of 2-bromoisobutyryl bromide to 2,3-dihydroxymethyl-5-norbornene is (0.9~1.1):1, and the amount of triethylamine used is 1.0~1.5 times the molar equivalent of 2-bromoisobutyryl bromide; after the addition is complete, the reaction is carried out at 20~30°C to obtain 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene.
[0023] Preferably, the living / controlled polymerization method is one or more of atom transfer radical polymerization, reversible addition-fragmentation chain transfer polymerization, nitrile-oxygen stable radical polymerization, or anionic polymerization.
[0024] Furthermore, when using atom transfer radical polymerization, the operation is as follows: using HO-NB-Br as an initiator and a cuprous halide / bipyridine complex as a catalyst, the polymerization of vinyl monomers is initiated to obtain the norbornene polystyrene macromolecular initiator HO-NB-PS-Br, which is a linear polymer precursor with a norbornene group at one end and a halogen atom at the other end.
[0025] Preferably, in step (2), the polar solvent is N,N-dimethylformamide; the temperature of the azidation reaction is 20℃~30℃, and the reaction time is 20 hours~28 hours; the amount of sodium azide is 10~30 times the molar equivalent of halogen atoms.
[0026] Preferably, in step (3), a high degree of dilution is achieved by slow drop-addition: the polymer obtained in step (2) is dissolved in an anhydrous solvent to prepare a dilute solution; then, using a constant pressure dropping funnel, the solution is continuously added drop-by drop at a rate of 1 drop / 10 seconds to 1 drop / 20 seconds to a reactor preheated to the reaction temperature and containing the same solvent.
[0027] Furthermore, the solvent in step (3) is anhydrous toluene; the reaction time is 12 hours to 48 hours.
[0028] Preferably, the monomers include styrene, dimethylaminoethyl methacrylate, methyl methacrylate, and ε-caprolactone.
[0029] Secondly, the present invention provides a cyclic polymer prepared by the above method;
[0030] The cyclic polymer is formed by the intramolecular 1,3-dipolar cycloaddition of polystyrene chains to connect the chain ends into a ring. The connecting points include a saturated triazolino-norbornene bridging structure formed by the cycloaddition of an azide group to a tensioned carbon-carbon double bond on a norbornene ring. The ring closure site is a fused bicyclic triazolino linker formed by the cycloaddition of an azide group to norbornene, and is confirmed by 1H NMR spectroscopy (…). 1 ¹H NMR analysis showed no characteristic signal of norbornene double bonds at δ = 6.20–6.17 ppm, while FTIR analysis showed no signal at ~2100 cm⁻¹. -1 There is no characteristic absorption of azide at this location.
[0031] The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry provided by this invention has the following technical advantages:
[0032] (1) For the first time, catalyst-free azide-norbornene click chemistry was applied to the synthesis of cyclic polymers, expanding the application scope of click chemistry in the field of polymer topology control.
[0033] (2) No metal catalyst is required, which completely avoids the problem of metal catalyst residue. The resulting cyclic polymer has high purity and does not require cumbersome metal removal post-processing steps.
[0034] (3) The reaction conditions are mild and can be carried out efficiently at atmospheric pressure and 100-120℃. There are no side reactions and the yield is high.
[0035] (4) It has good versatility and can prepare cyclic polymers with different chemical compositions and molecular weights by controlling the monomers and polymerization methods.
[0036] (5) The operation is simple, and all three steps are classic reactions, which is expected to achieve large-scale production. Attached Figure Description
[0037] Figure 1 This is a schematic diagram of a method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry.
[0038] Figure 2 This is a schematic diagram of the synthetic route for synthesizing cyclic polystyrene in Example 1 of the present invention.
[0039] Figure 3 The image shows the 1H NMR spectrum of NB-2,3-CH2OH prepared in Example 1 of this invention.
[0040] Figure 4 The image shows the ¹H NMR spectrum of HO-NB-Br prepared in Example 1 of this invention.
[0041] Figure 5Comparison of ¹H NMR spectra of (A) HO-NB-PS-Br, (B) HO-NB-PS-N3 and (C) cyclic polystyrene (c-PS) prepared in Example 1 of this invention.
[0042] Figure 6 The Fourier transform infrared (FTIR) spectra of (A) HO-NB-PS-Br, (B) HO-NB-PS-N3 and (C) cyclic polystyrene (c-PS) prepared in Example 1 of this invention are compared.
[0043] Figure 7 This is a comparison of the gel permeation chromatography (GPC) elution curves of the linear polystyrene precursor (HO-NB-PS-N3) and cyclic polystyrene (c-PS) prepared in Example 1 of this invention.
[0044] Figure 8 This is a comparison of the differential scanning calorimetry (DSC) curves of the linear polystyrene precursor and the cyclic polystyrene prepared in Example 1 of this invention.
[0045] Figure 9 This is a comparison of the 1H NMR spectra of the low molecular weight linear polystyrene precursor prepared in Example 2 of the present invention and the corresponding cyclic polystyrene.
[0046] Figure 10 The image shows a comparison of the infrared spectra of the low molecular weight linear polystyrene precursor prepared in Example 2 of this invention with the corresponding cyclic polystyrene.
[0047] Figure 11 This is a comparison of the GPC effluent curves of the low molecular weight linear polystyrene precursor prepared in Example 2 of the present invention and the corresponding cyclic polystyrene. Detailed Implementation
[0048] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are merely some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0049] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0050] Example 1
[0051] This embodiment provides a specific method for synthesizing cyclic polystyrene (c-PS) using catalyst-free azide-norbornene click chemistry, and the synthetic route is as follows: Figure 1 As shown.
[0052] (1) Synthesis of 2,3-dihydroxymethyl-5-norbornene (NB-2,3-CH2OH)
[0053] Lithium aluminum hydride (13.70 g, 0.36 mol) was added to a 250 mL three-necked flask after vacuuming and purging with argon. Anhydrous tetrahydrofuran (120 mL) was then slowly added dropwise under ice-water bath cooling. After the addition was complete, a tetrahydrofuran solution (125 mL) containing norbornene adienoic anhydride (20.00 g, 0.12 mol) was added dropwise over a period of at least 30 minutes. After the addition was complete, the reaction apparatus was transferred to a water bath and refluxed for 72 hours. After the reaction was complete, the mixture was allowed to cool naturally to room temperature under an argon atmosphere. The reaction solution was then slowly poured into 500 mL of distilled water, stirred to produce a white precipitate, and filtered under reduced pressure. The filtrate was extracted with dichloromethane, the organic phase was collected, dried over anhydrous sodium sulfate, filtered under reduced pressure, and the solvent was removed by rotary evaporation to obtain a white solid product. The product was dried under vacuum to constant weight to give 10.42 g of 2,3-dihydroxymethyl-5-norbornene, with a yield of 55.5%.
[0054] (2) Preparation of the bifunctional initiator HO-NB-Br
[0055] Take 5.88 g (38.1 mmol) of the prepared NB-2,3-CH2OH and add it to a 250 mL three-necked flask. After evacuating and purging with argon gas, inject 80 mL of anhydrous dichloromethane using a syringe under an argon atmosphere. Place the reaction flask in an ice-water bath and add 20 mL of triethylamine dropwise, followed by a slow dropwise addition of 18 mL of dichloromethane solution containing 8.76 g (38.1 mmol) of 2-bromoisobutyryl bromide, controlling the dropwise addition time to be no less than 30 minutes and maintaining the reaction temperature below 0 °C. After the addition is complete, transfer the apparatus to a constant temperature 25 °C water bath and continue the reaction for 48 hours. Monitor the reaction progress using thin-layer chromatography (developing solvent ratio: dichloromethane:methanol = 80:1), and terminate the reaction when the starting material spot completely disappears. The reaction solution was extracted with distilled water. The organic phase was dried, filtered under reduced pressure, concentrated, and then purified by silica gel column chromatography (eluent: dichloromethane: methanol = 80:1). The target product fraction was collected, the solvent was concentrated, and the product was dried under vacuum to obtain 5.80 g of the pale yellow oily product 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene (HO-NB-Br), with a yield of 60%.
[0056] (3) Synthesis of norborneol-based polystyrene macromolecular initiator (HO-NB-PS-Br)
[0057] Take a 250 mL three-necked flask, add the initiator HO-NB-Br (1.00 g, approximately 2.5 mmol), assemble the apparatus, and place it in an ice-salt bath, controlling the temperature at approximately -18℃. After three cycles of vacuuming and argon purging, add purified styrene monomer (30.00 g, 288 mmol), and vacuum again three times. Add distilled anhydrous toluene (35 mL). Weigh cuprous bromide (0.36 g, 2.5 mmol) and 2,2'-bipyridine (1.56 g, 10.0 mmol) in a glove box and add them to the reaction flask. After the system stabilizes, transfer the apparatus to a 110℃ constant temperature oil bath and stir the reaction for 11 hours. After the reaction is complete, filter the reaction solution through a neutral alumina column to remove copper salts and other metallic impurities, collect the filtrate, and concentrate it to a viscous state by rotary evaporation. Add the concentrate dropwise to methanol to precipitate a white precipitate, which is then filtered under reduced pressure. The crude product was purified three times by repeatedly dissolving in dichloromethane and precipitating in methanol. The white powder was collected by filtration and dried in a vacuum oven at 40°C to constant weight, yielding approximately 24.00 g of norbornene-based polystyrene macromolecular initiator (HO-NB-PS-Br), with a yield of approximately 80%.
[0058] (4) Azide formation of linear polystyrene (HO-NB-PS-N3)
[0059] HO-NB-PS-Br (1.00 g, approximately 0.15 mmol) was added to a 100 mL three-necked flask, and the mixture was evacuated three times. 25 mL of N,N-dimethylformamide was added, and the mixture was evacuated again until the solid was completely dissolved. Sodium azide (0.20 g, 3.0 mmol) was then added, and the mixture was evacuated again. The apparatus was then placed in a constant-temperature oil bath at 25 °C, and the reaction was allowed to proceed for 24 hours. After the reaction was complete, the liquid in the three-necked flask was poured into 100 mL of cold water, and the mixture was extracted six times with dichloromethane. The organic phase was collected, washed six times with saturated brine, and dried overnight with anhydrous magnesium sulfate. After filtration, the mixture was concentrated by rotary evaporation, and the precipitate was added dropwise to methanol. This precipitation was repeated three times, and the product was a white powder. This powder was dried in a vacuum oven at 40 °C to constant weight to obtain approximately 0.92 g of azide-terminated norbornene polystyrene (HO-NB-PS-N3), with a yield of approximately 92%.
[0060] (5) Synthesis of cyclic polystyrene (c-PS) by intramolecular cyclization reaction
[0061] Take a 1000 mL three-necked flask, quickly assemble the apparatus, and then pump it out three times. Add 500 mL of anhydrous toluene to the three-necked flask and heat to 110 °C. Separately, take a 500 mL conical flask, add 0.50 g of HO-NB-PS-N3 (approximately 0.075 mmol), and dissolve it completely in 500 mL of anhydrous toluene. Pour the polymer solution from the conical flask into a constant-pressure dropping funnel. Once the toluene in the three-necked flask reaches 110 °C, slowly add the polymer solution from the constant-pressure dropping funnel to the 1000 mL three-necked flask at a rate of 1 drop / 15 seconds (final polymer concentration <0.1 mM), without adding any metal catalyst. After the addition is complete, continue the reaction at 110 °C for 24 hours. After the reaction is complete, cool to room temperature, concentrate the reaction solution by rotary evaporation to approximately 50 mL, precipitate it by adding a large amount of methanol, filter, and dry under vacuum to obtain approximately 0.38 g of cyclic polystyrene (c-PS), with a cyclization yield of approximately 76%.
[0062] (6) Characterization results
[0063] 1H NMR spectrum ( 1 H NMR) such as Figure 3 As shown: The 1H NMR spectrum of NB-2,3-CH2OH obtained in step (1) was tested. The peak at δ=6.09 ppm was attributed to the two proton peaks of the double bond on the norbornene ring, the peak at δ=3.67 ppm was attributed to the two proton peaks of the two hydroxyl groups, the peak at δ=3.50 ppm was attributed to the proton peak of the methylene group connected to the hydroxyl group, and the peak at δ=2.58-2.73 ppm was attributed to the proton peaks of the bridgehead tertiary carbons. This indicates that 2,3-dihydroxymethyl-5-norbornene was successfully synthesized.
[0064] The HO-NB-Br obtained in step (2) was subjected to 1H NMR spectroscopy (NMR spectroscopy). 1 H NMR) test, such as Figure 4 The peaks at δ=6.09 ppm belong to the two proton peaks of the double bond on the norbornene ring, the peaks at δ=1.98 ppm belong to the six proton peaks of the two methyl groups on the 2-bromoisobutyryl group, and the peaks at δ=3.50 ppm and δ=4.00 ppm belong to the methylene proton peaks connected to the hydroxyl group and the ester group, respectively. The area ratio of each peak is consistent with the hydrogen distribution on each carbon of HO-NB-Br, indicating that the bifunctional initiator HO-NB-Br has been successfully synthesized.
[0065] 1H NMR spectrum ( 1 H NMR) such as Figure 5As shown: In spectrum A of the linear precursor HO-NB-PS-Br, a characteristic peak of a methylene proton (-CH2Br) bonded to a bromine atom appears at δ=4.5 ppm; in spectrum B of the azidated HO-NB-PS-N3, this peak shifts to δ=4.0 ppm (-CH2N3); in spectrum C of the cyclized c-PS, the characteristic peak of the norbornene double bond at δ=6.20-6.17 ppm completely disappears, and the -CH2N3 peak at δ=4.0 ppm also disappears.
[0066] Fourier transform infrared spectroscopy (FTIR) such as Figure 6 As shown: In spectrum B of HO-NB-PS-N3 after azidation, at approximately 2100 cm⁻¹ -1 A strong characteristic absorption peak of the azide group (-N3) appeared at the position; in the c-PS spectrum C after cyclization, this absorption peak completely disappeared.
[0067] Gel permeation chromatography (GPC) such as Figure 7 As shown, compared with the linear precursor HO-NB-PS-N3 (Mn, GPC=6628, PDI=1.18), the cyclized product c-PS (Mn, GPC=6196, PDI=1.14) has a longer retention time and a smaller apparent molecular weight.
[0068] Differential scanning calorimetry (DSC) such as Figure 8 As shown, the glass transition temperature (Tg≈102℃) of cyclic polystyrene c-PS is higher than that of the linear precursor HO-NB-PS-N3 (Tg≈96℃).
[0069] Example 2
[0070] This embodiment provides a method for synthesizing cyclic polystyrene (c-PS) of different molecular weights to verify the universality of the method of the present invention in the cyclization of polymers of different molecular weights.
[0071] (1) Synthesis of norborneol-based polystyrene macromolecular initiator (HO-NB-PS-Br)
[0072] Referring to step (3) of Example 1, the amount of styrene monomer was reduced to 10.40 g (100 mmol) by adjusting the feed ratio of styrene monomer to initiator HO-NB-Br. Other conditions were the same as in Example 1, and a HO-NB-PS-Br precursor with a lower molecular weight was synthesized.
[0073] (2) Azide formation (HO-NB-PS-N3) and intramolecular cyclization of linear polystyrene
[0074] The azidation and cyclization reactions were carried out in the same manner as in Example 1, following steps (4) and (5).
[0075] (3) Characterization results
[0076] The linear polystyrene precursor HO-NB-PS-N3 prepared in this embodiment has a number-average molecular weight (Mn, GPC) of approximately 4614 and a molecular weight distribution (PDI) of approximately 1.22. The cyclic polystyrene c-PS obtained after cyclization has a number-average molecular weight (Mn, GPC) of approximately 4417 and a molecular weight distribution (PDI) of approximately 1.33.
[0077] 1H NMR spectrum ( 1 H NMR) Figure 9 Analysis showed that in the linear precursor HO-NB-PS-N3, there was a characteristic peak of norbornene double bond at δ=6.20-6.17ppm and a characteristic peak of -CH2N3 at δ=4.0ppm; after the cyclization reaction, both sets of characteristic peaks disappeared completely, proving that the cyclization reaction was successful.
[0078] Fourier transform infrared spectroscopy (FTIR) Figure 10 Analysis showed that the linear precursor HO-NB-PS-N3 had a characteristic absorption peak of the azide group (-N3) at about 2100 cm⁻¹; after the cyclization reaction, the absorption peak disappeared completely, indicating that the azide group was completely consumed.
[0079] Gel permeation chromatography (GPC) analysis showed that compared with the linear precursor HO-NB-PS-N3, the cyclized product c-PS had a longer retention time and a smaller apparent molecular weight, consistent with the characteristics of reduced hydrodynamic volume of cyclic polymers. These results are consistent with those of Example 1, demonstrating the universality of the method of this invention for polymers of different molecular weights.
[0080] Characterization results as follows Figure 9 , Figure 10 , Figure 11 As shown in Example 1, this demonstrates that the method of the present invention is universally applicable to polymers of different molecular weights.
[0081] Example 3
[0082] This embodiment provides a specific method for synthesizing cyclic poly(dimethylaminoethyl methacrylate) (c-PDMAEMA) using catalyst-free azide-norbornene click chemistry.
[0083] (1) Synthesis of norbornene-based poly(dimethylaminoethyl methacrylate) macromolecular initiator (HO-NB-PDMAEMA-Br)
[0084] Take a 250 mL three-necked flask, add the initiator HO-NB-Br (1.00 g, 2.50 mmol), assemble the apparatus and place it in an ice-salt bath, controlling the temperature at approximately -18℃. After three cycles of vacuuming and purging with argon, add purified dimethylaminoethyl methacrylate monomer (DMAEMA, 39.30 g, 250 mmol), and vacuum again three times. Add 40 mL of distilled anhydrous toluene. Weigh cuprous bromide (0.36 g, 2.50 mmol) and 2,2'-bipyridine (1.56 g, 10.0 mmol) in a glove box and add them to the reaction flask. After the system stabilizes, transfer the apparatus to a 70℃ constant temperature oil bath and stir the reaction for 8 hours. After the reaction is complete, filter the reaction solution through a neutral alumina column to remove copper salts and other metallic impurities, collect the filtrate, and concentrate it to a viscous state by rotary evaporation. Add the concentrate dropwise to n-hexane to precipitate a white precipitate, which is then filtered under reduced pressure. The crude product was purified three times by repeatedly dissolving in dichloromethane and precipitating in n-hexane. The white powder was collected by filtration and dried in a vacuum oven at 40°C to constant weight, yielding 32.5 g of norbornene-based poly(dimethylaminoethyl methacrylate) macromolecular initiator (HO-NB-PDMAEMA-Br), with a yield of approximately 82%.
[0085] (2) Azide formation of linear poly(dimethylaminoethyl methacrylate) (HO-NB-PDMAEMA-N3)
[0086] HO-NB-PDMAEMA-Br (1.00 g, 0.12 mmol) was added to a 100 mL three-necked flask, and the mixture was evacuated three times. 25 mL of N,N-dimethylformamide was added, and the mixture was evacuated again until the solid was completely dissolved. Sodium azide (0.16 g, 2.40 mmol) was then added, and the mixture was evacuated again. The apparatus was placed in a constant-temperature oil bath at 25 °C, and the reaction was allowed to proceed for 24 hours. After the reaction was complete, the liquid in the three-necked flask was poured into 100 mL of cold water and extracted six times with dichloromethane. The organic phase was collected, washed six times with saturated brine, and dried overnight with anhydrous magnesium sulfate. After filtration, the mixture was concentrated by rotary evaporation, and the precipitate was added dropwise into n-hexane. This precipitation was repeated three times, and the product was a white powder. This powder was dried in a vacuum oven at 40 °C to constant weight to obtain 0.88 g of azide-terminated norbornene-based dimethylaminoethyl methacrylate (HO-NB-PDMAEMA-N3), with a yield of approximately 88%.
[0087] (3) Synthesis of cyclic poly(dimethylaminoethyl methacrylate) (c-PDMAEMA) by intramolecular cyclization reaction
[0088] Take a 1000 mL three-necked flask, add 500 mL of anhydrous toluene, and quickly assemble the apparatus, then pump it out three times. Separately, take a 500 mL Erlenmeyer flask, add 0.50 g of HO-NB-PDMAEMA-N3 (0.06 mmol), and dissolve it completely in 500 mL of anhydrous toluene. Pour the polymer solution from the Erlenmeyer flask into a constant-pressure dropping funnel. Transfer the apparatus to a constant-temperature oil bath at 110 °C. Once the toluene in the three-necked flask reaches 110 °C, slowly add the polymer solution from the constant-pressure dropping funnel to the 1000 mL three-necked flask at a rate of 1 drop / 15 seconds (final polymer concentration <0.1 mM). After the addition is complete, continue the reaction at 110 °C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, and the reaction solution was concentrated by rotary evaporation to about 50 mL. The solution was then added dropwise into a large amount of n-hexane to precipitate the precipitate. The precipitate was filtered and dried under vacuum to obtain 0.36 g of cyclic poly(dimethylaminoethyl methacrylate) (c-PDMAEMA), with a cyclization yield of about 72%.
[0089] (4) Characterization results
[0090] 1H NMR spectrum ( 1 ¹H NMR analysis showed that in the linear precursor HO-NB-PDMAEMA-Br, a characteristic peak of a methylene proton (-CH₂Br) bonded to a bromine atom appeared at δ=4.5 ppm, and a characteristic peak of a norbornene double bond existed at δ=6.20-6.17 ppm. After azidation, in HO-NB-PDMAEMA-N₃, the characteristic peak at δ=4.5 ppm shifted to δ=4.0 ppm (-CH₂N₃). After cyclization, in c-PDMAEMA, the characteristic peak of the norbornene double bond at δ=6.20-6.17 ppm completely disappeared, and the -CH₂N₃ peak at δ=4.0 ppm also disappeared. Meanwhile, the characteristic peaks of the methylene proton (δ=2.6 ppm) and methyl proton (δ=2.3 ppm) adjacent to the nitrogen atom in the poly(dimethylaminoethyl methacrylate) segment remained stable before and after cyclization, indicating that the polymer chain structure was not destroyed.
[0091] Fourier transform infrared (FTIR) spectroscopy analysis showed that the linear precursor HO-NB-PDMAEMA-Br was at approximately 2100 cm⁻¹ -1 No absorption peak was observed at approximately 2100 cm⁻¹; after azidation, a strong characteristic absorption peak of the azide group (-N3) appeared in HO-NB-PDMAEMA-N3 at approximately 2100 cm⁻¹; this absorption peak completely disappeared in c-PDMAEMA after cyclization. Furthermore, the characteristic absorption peak of the ester carbonyl group in the poly(dimethylaminoethyl methacrylate) segment (approximately 1730 cm⁻¹) was observed. -1 It remains stable before and after cyclization.
[0092] Gel permeation chromatography (GPC) analysis showed that the linear precursor HO-NB-PDMAEMA-N3 had a number-average molecular weight (Mn, GPC) of approximately 8300 and a molecular weight distribution (PDI) of approximately 1.21; while the cyclized product c-PDMAEMA had a number-average molecular weight (Mn, GPC) of approximately 7700 and a molecular weight distribution (PDI) of approximately 1.18. The cyclized product exhibited a longer retention time, a smaller apparent molecular weight, and a narrower molecular weight distribution compared to the linear precursor, consistent with typical GPC characteristics of cyclic polymers.
[0093] The above results show that the method of the present invention is also applicable to methacrylate monomers containing functional groups, and cyclic poly(dimethylaminoethyl methacrylate) was successfully synthesized.
[0094] Example 4
[0095] This embodiment provides a specific method for synthesizing cyclic polymethyl methacrylate-b-polycaprolactone block copolymer (c-(PMMA-b-PCL)) using catalyst-free azide-norbornene click chemistry.
[0096] (1) Synthesis of norbornene-based polymethyl methacrylate macromolecular initiator (HO-NB-PMMA-Br)
[0097] Take a 250 mL three-necked flask, add the initiator HO-NB-Br (1.00 g, 2.50 mmol), assemble the apparatus and place it in an ice-salt bath, controlling the temperature at approximately -18℃. After three cycles of vacuuming and argon purging, add purified methyl methacrylate monomer (MMA, 25.00 g, 250 mmol), and vacuum again three times. Add 35 mL of distilled anhydrous toluene. Weigh cuprous bromide (0.36 g, 2.50 mmol) and 2,2'-bipyridine (1.56 g, 10.0 mmol) in a glove box and add them to the reaction flask. After the system stabilizes, transfer the apparatus to an 80℃ constant temperature oil bath and stir the reaction for 6 hours. After the reaction is complete, filter the reaction solution through a neutral alumina column to remove copper salts and other metallic impurities, collect the filtrate, and concentrate it to a viscous state by rotary evaporation. Add the concentrate dropwise to methanol to precipitate a white precipitate, which is then filtered under reduced pressure. The crude product was purified three times by a cycle of dissolving in dichloromethane and precipitating in methanol. The white powder was collected by filtration and dried in a vacuum oven at 40°C to constant weight, yielding 20.8 g of norbornene-based polymethyl methacrylate macromolecular initiator (HO-NB-PMMA-Br), with a yield of approximately 83%.
[0098] (2) Synthesis of norbornene-based polymethyl methacrylate-b-polycaprolactone block copolymer (HO-NB-PMMA-b-PCL-Br)
[0099] Take a 250 mL three-necked flask, add the above-prepared HO-NB-PMMA-Br (5.00 g, 0.50 mmol), and after three cycles of vacuum purging and argon purging, add distilled anhydrous toluene (50 mL), heat to 80 °C and stir until the polymer is completely dissolved. Add the dried ε-caprolactone monomer (ε-CL, 5.70 g, 50 mmol) and the catalyst stannous octoate (Sn(Oct)2, 10.1 mg, 0.025 mmol). Transfer the reaction apparatus to a constant temperature oil bath at 110 °C and stir for 24 hours. After the reaction is complete, cool to room temperature, concentrate the reaction solution by rotary evaporation to a viscous state, precipitate in methanol, a white precipitate forms, and filter under reduced pressure. The crude product was purified three times by a cycle of dissolving in dichloromethane and precipitating in methanol. The white powder was collected by filtration and dried in a vacuum oven at 40°C to constant weight, yielding 8.2 g of norbornene-based polymethyl methacrylate-b-polycaprolactone block copolymer (HO-NB-PMMA-b-PCL-Br), with a yield of approximately 78%.
[0100] (3) Azide formation of linear block copolymers (HO-NB-PMMA-b-PCL-N3)
[0101] HO-NB-PMMA-b-PCL-Br (1.00 g, 0.05 mmol) was added to a 100 mL three-necked flask, and the mixture was evacuated three times. 25 mL of N,N-dimethylformamide was added, and the mixture was evacuated again until the solid was completely dissolved. Sodium azide (0.07 g, 1.00 mmol) was then added, and the mixture was evacuated again. The apparatus was placed in a constant-temperature oil bath at 25 °C, and the reaction was allowed to proceed for 24 hours. After the reaction was complete, the liquid in the three-necked flask was poured into 100 mL of cold water and extracted six times with dichloromethane. The organic phase was collected, washed six times with saturated brine, and dried overnight with anhydrous magnesium sulfate. After filtration, the mixture was concentrated by rotary evaporation, and the precipitate was added dropwise into methanol. This precipitation was repeated three times, and the product was a white powder. This powder was dried in a vacuum oven at 40 °C to constant weight to obtain 0.86 g of azide-terminated norbornene-based polymethyl methacrylate-b-polycaprolactone block copolymer (HO-NB-PMMA-b-PCL-N3), with a yield of approximately 86%.
[0102] (4) Intramolecular cyclization reaction to synthesize cyclic block copolymers (c-(PMMA-b-PCL))
[0103] Take a 1000 mL three-necked flask, add 500 mL of anhydrous toluene, and quickly assemble the apparatus, then pump it out three times. Separately, take a 500 mL Erlenmeyer flask, add 0.50 g of HO-NB-PMMA-b-PCL-N3 (0.025 mmol), and dissolve it completely in 500 mL of anhydrous toluene. Pour the polymer solution from the Erlenmeyer flask into a constant-pressure dropping funnel. Transfer the apparatus to a constant-temperature oil bath at 110 °C. Once the toluene in the three-necked flask reaches 110 °C, slowly add the polymer solution from the constant-pressure dropping funnel to the 1000 mL three-necked flask at a rate of 1 drop / 15 seconds (final polymer concentration <0.1 mM). After the addition is complete, continue the reaction at 110 °C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, and the reaction solution was concentrated by rotary evaporation to about 50 mL. The solution was then added dropwise to a large amount of methanol to precipitate the precipitate. The precipitate was filtered and dried under vacuum to obtain 0.36 g of cyclic polymethyl methacrylate-b-polycaprolactone block copolymer (c-(PMMA-b-PCL)), with a cyclization yield of about 72%.
[0104] (5) Characterization results
[0105] 1H NMR spectrum ( 1 ¹H NMR analysis showed that in the linear precursor HO-NB-PMMA-Br, a characteristic peak of a methylene proton (-CH₂Br) bonded to a bromine atom appeared at δ=4.5 ppm, and a characteristic peak of a norbornene double bond appeared at δ=6.20-6.17 ppm. After ROP chain extension, in HO-NB-PMMA-b-PCL-Br, a methylene proton (-COO-CH₂Br) bonded to the ester oxygen in the polycaprolactone segment appeared at δ=4.1 ppm. 2- The characteristic peak of ) appeared at δ=2.3 ppm, showing the presence of a methylene proton (-CH) adjacent to the carbonyl group in the polycaprolactone segment. 2- The characteristic peaks of COO- were observed, and the characteristic peaks of methylene protons in the polycaprolactone segment appeared at δ=1.6 ppm and δ=1.4 ppm, indicating the successful synthesis of the block copolymer. After azidation, the characteristic peak at δ=4.5 ppm in HO-NB-PMMA-b-PCL-N3 shifted to δ=4.0 ppm (-CH2N3). After cyclization, the characteristic peaks of the norbornene double bond at δ=6.20-6.17 ppm in c-(PMMA-b-PCL) completely disappeared, and the -CH2N3 peak at δ=4.0 ppm also disappeared. The characteristic peaks of methoxy protons in the polymethyl methacrylate segment (δ=3.6 ppm) and the characteristic peaks of the polycaprolactone segment remained stable before and after cyclization, indicating that the chemical structure of the block copolymer was not destroyed.
[0106] Fourier transform infrared (FTIR) spectroscopy analysis showed that the linear precursor HO-NB-PMMA-Br was at approximately 2100 cm⁻¹-1 No absorption peak was observed at approximately 2100 cm⁻¹; after azide formation, HO-NB-PMMA-b-PCL-N₃ showed an absorption peak at approximately 2100 cm⁻¹. -1 A strong characteristic absorption peak of the azide group (-N3) appeared at [location]; this absorption peak completely disappeared in c-(PMMA-b-PCL) after cyclization. In addition, the characteristic absorption peak of the ester carbonyl group in the polymethyl methacrylate segment (approximately 1730 cm⁻¹) was observed. -1 The characteristic absorption peak of the ester carbonyl group in the polycaprolactone segment (approximately 1735 cm⁻¹) and the characteristic absorption peak of the ester carbonyl group in the polycaprolactone segment. -1 It remains stable before and after cyclization, and the two overlap.
[0107] Gel permeation chromatography (GPC) analysis showed that the linear precursor HO-NB-PMMA-b-PCL-N3 had a number-average molecular weight (Mn, GPC) of approximately 15800 and a molecular weight distribution (PDI) of approximately 1.24; the cyclized product c-(PMMA-b-PCL) had a number-average molecular weight (Mn, GPC) of approximately 14200 and a molecular weight distribution (PDI) of approximately 1.21. The cyclized product exhibited a longer retention time, a smaller apparent molecular weight, and a narrower molecular weight distribution compared to the linear precursor, consistent with typical GPC characteristics of cyclic polymers.
[0108] The above results show that the method of the present invention is also applicable to the cyclization of block copolymers, and cyclic polymethyl methacrylate-b-polycaprolactone block copolymers were successfully synthesized.
[0109] Comparative Example 1
[0110] This comparative example aims to verify the crucial role of the tensioned double bond on the norbornene ring in achieving catalyst-free cycloaddition reactions.
[0111] A linear polystyrene precursor (PS-CH=CH2-N3) with ordinary carbon-carbon double bonds replacing the strained double bonds on the norbornene ring was synthesized. The specific synthetic steps are as follows:
[0112] (1) Polystyrene (CH2=CH-PS-Cl) with double bonds at the ends and chlorine atoms at the ends was synthesized by atom transfer radical polymerization using 4-vinylbenzyl chloride as an initiator. The polymerization conditions were the same as in step (3) of Example 1: 4-vinylbenzyl chloride (0.38 g, 2.50 mmol), styrene monomer (26.00 g, 250 mmol), cuprous bromide (0.36 g, 2.50 mmol), 2,2'-bipyridine (1.56 g, 10.0 mmol) and anhydrous toluene (35 mL) were reacted at 110 °C for 11 hours. After purification, CH2=CH-PS-Cl was obtained with a yield of about 85%.
[0113] (2) CH2=CH-PS-Cl (1.00 g, 0.15 mmol) was reacted with sodium azide (0.20 g, 3.00 mmol) in 25 mL of DMF at 25 °C for 24 hours to convert it into CH2=CH-PS-N3. The yield after purification was about 90%.
[0114] CH2=CH-PS-N3 (Mn≈6500) was cyclized under the same conditions as step (5) in Example 1: 1000 mL of three-necked flask was taken and anhydrous toluene (500 mL) was added. CH2=CH-PS-N3 (0.50 g, 0.077 mmol) was dissolved in 500 mL of anhydrous toluene and added dropwise at a rate of 1 drop / 15 seconds to anhydrous toluene at 110 °C (final polymer concentration <0.1 mM). The reaction was carried out for 24 hours.
[0115] Gel permeation chromatography (GPC) analysis showed that the GPC elution curves of the polymer before and after the reaction almost completely overlapped, with no significant change in number-average molecular weight (Mn,GPC≈6300, PDI≈1.18 before reaction; Mn,GPC≈6280, PDI≈1.19 after reaction). ¹H NMR analysis showed that the characteristic peaks of the terminal double bonds in the δ=5.8-5.0 ppm range did not significantly decrease, and the -CH₂N₃ peak in the δ=3.8-4.0 ppm range did not disappear. Fourier transform infrared spectroscopy (FTIR) analysis showed that at approximately 2100 cm⁻¹... -1 The characteristic absorption peak of the azide group at the reaction site still exists after the reaction and does not decrease significantly.
[0116] The above results indicate that ordinary carbon-carbon double bonds cannot undergo effective cycloaddition reactions with azide groups under catalyst-free conditions (110°C, 24 hours). This is because ordinary double bonds lack the ring strain of the norbornene ring and therefore lack the thermodynamic driving force required for the reaction. This comparative example demonstrates that the strained double bond on the norbornene ring is a key structural feature for achieving the catalyst-free cycloaddition reaction of this invention.
[0117] Comparative Example 2
[0118] This comparative example aims to verify the crucial role of highly diluted conditions (polymer concentration <0.1 mM) in achieving intramolecular cyclization rather than intermolecular coupling.
[0119] The same azide-terminated norbornene polystyrene precursor (HO-NB-PS-N3, Mn≈6600) as in Example 1 was used, but the polymer concentration in the cyclization reaction was changed.
[0120] HO-NB-PS-N3 (0.50 g, 0.075 mmol) was dissolved in 50 mL of anhydrous toluene (polymer concentration approximately 1.5 mM), instead of being dissolved in 500 mL of toluene (concentration approximately 0.075 mM) as in Example 1. A 250 mL three-necked flask was filled with 50 mL of anhydrous toluene, and the polymer solution was added dropwise to anhydrous toluene at 1 drop / 15 seconds (final polymer concentration approximately 0.75 mM). The reaction was allowed to proceed for 24 hours.
[0121] Gel permeation chromatography (GPC) analysis showed a distinct bimodal distribution in the GPC curve of the reaction product, with a significant high molecular weight shoulder peak (Mn, GPC≈35000) appearing at the shorter retention time, indicating severe intermolecular coupling side reactions. The retention time of the main peak was slightly longer than that of the linear precursor, but the molecular weight distribution was significantly broadened (PDI≈1.45). (1H NMR spectroscopy...) 1 ¹H NMR analysis showed that the characteristic peak of the norbornene double bond at δ=6.20-6.17 ppm still had some residue (about 30%), indicating that the cyclization reaction was incomplete. Calculations using GPC peak area integration showed that the yield of the cyclized product was only 35%, far lower than the 76% in Example 1.
[0122] This comparative example demonstrates that when the polymer concentration is above 0.1 mM, intermolecular coupling side reactions dominate, making it impossible to efficiently obtain cyclic polymers. Only under conditions of high dilution (polymer concentration <0.1 mM) can intermolecular reactions be effectively suppressed, allowing intramolecular cyclization reactions to occur preferentially. Therefore, controlling the polymer concentration in the reaction system below 0.1 mM is a key process condition for achieving the efficient cyclization reaction of this invention.
[0123] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry, characterized in that, Includes the following steps: Step (1) Synthesis of linear polymer precursors with norbornene end groups: A living / controlled polymerization method was used to initiate the polymerization of monomers with a bifunctional initiator containing norbornene groups and halogen atoms, thereby synthesizing a linear polymer precursor with a norbornene group at one end and a halogen atom at the other end. The bifunctional initiator containing norbornene groups and halogen atoms is 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene HO-NB-Br; Step (2) Azide formation of linear polymer precursor: The linear polymer precursor obtained in step (1) was reacted with sodium azide in a polar solvent to convert the terminal halogen atoms into azide groups, resulting in the azide-terminated norbornene-functionalized linear polymer HO-NB-PS-N3. Step (3) Intramolecular cyclization reaction to prepare cyclic polymers: The azide-terminated norbornene-functionalized linear polymer obtained in step (2) was subjected to an intramolecular cyclization reaction under dilution conditions; the reaction was carried out under heating conditions of 100–120℃ to obtain the cyclic polymer c-PS; The dilution condition refers to the concentration of the polymer in the reaction system not exceeding 0.1 mM.
2. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 1, characterized in that, In step (1), the synthetic route of 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene is as follows: norbornene dianhydride is reduced by lithium aluminum hydride to obtain 2,3-dihydroxymethyl-5-norbornene; then it undergoes esterification with 2-bromoisobutyryl bromide in the presence of an acid binder to obtain HO-NB-Br.
3. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 2, characterized in that, The synthesis method of the 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene is as follows: (a) Reduction step: Under inert gas protection, norbornadiene anhydride was dissolved in anhydrous tetrahydrofuran and then added to an anhydrous tetrahydrofuran suspension of lithium aluminum hydride, wherein the molar ratio of lithium aluminum hydride to norbornadiene anhydride was (2.8~3.2):1; after the addition was complete, the reaction was allowed to proceed to obtain 2,3-dihydroxymethyl-5-norbornene. (b) Esterification step: Under inert gas protection, 2,3-dihydroxymethyl-5-norbornene obtained in step (a) is dissolved in anhydrous dichloromethane, triethylamine is added as an acid-binding agent, and then a dichloromethane solution of 2-bromoisobutyryl bromide is slowly added dropwise, controlling the reaction temperature below 0°C; wherein, the molar ratio of 2-bromoisobutyryl bromide to 2,3-dihydroxymethyl-5-norbornene is (0.9~1.1):1, and the amount of triethylamine used is 1.0~1.5 times the molar equivalent of 2-bromoisobutyryl bromide; after the addition is complete, the reaction is carried out at 20~30°C to obtain 2-hydroxymethyl-3-(2-bromoisobutyrylethyl)-5-norbornene.
4. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 1, characterized in that, The living / controlled polymerization method is one or more of the following: atom transfer radical polymerization, reversible addition-fragmentation chain transfer polymerization, nitrile-oxygen stable radical polymerization, or anionic polymerization.
5. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 4, characterized in that, When using atom transfer radical polymerization, the operation is as follows: using HO-NB-Br as an initiator and a cuprous halide / bipyridine complex as a catalyst, the polymerization of vinyl monomers is initiated to obtain the norbornene polystyrene macromolecular initiator HO-NB-PS-Br, which is a linear polymer precursor with a norbornene group at one end and a halogen atom at the other end.
6. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 1, characterized in that, In step (2), the polar solvent is N,N-dimethylformamide; the temperature of the azidation reaction is 20℃~30℃, and the reaction time is 20 hours~28 hours; the amount of sodium azide is 10~30 times the molar equivalent of halogen atoms.
7. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 1, characterized in that, In step (3), a high degree of dilution is achieved by slow drop-addition: the polymer obtained in step (2) is dissolved in an anhydrous solvent to prepare a dilute solution; then, using a constant pressure dropping funnel, the solution is continuously added drop-by drop at a rate of 1 drop / 10 seconds to 1 drop / 20 seconds to a reactor preheated to the reaction temperature and containing the same solvent.
8. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 1, characterized in that, The solvent in step (3) is anhydrous toluene; the reaction time is 12 hours to 48 hours.
9. The method for synthesizing cyclic polymers using catalyst-free azide-ene click chemistry according to claim 1, characterized in that, The monomers include styrene, dimethylaminoethyl methacrylate, methyl methacrylate, and ε-caprolactone.
10. A cyclic polymer prepared by the method of any one of claims 1 to 9; the cyclic polymer is formed by connecting the ends of a polystyrene chain into a ring via intramolecular 1,3-dipolar cycloaddition, wherein the connection point comprises a saturated triazolino-norbornene bridging structure formed by the cycloaddition of an azide group to a tensioned carbon-carbon double bond on a norbornene ring; its ring closure site is a fused bicyclic triazolino linker formed by the cycloaddition of an azide group to norbornene, and is confirmed by proton nuclear magnetic resonance spectroscopy (1H NMR spectroscopy). 1 ¹H NMR analysis showed no characteristic signal of norbornene double bonds at δ = 6.20–6.17 ppm, while FTIR analysis showed no signal at ~2100 cm⁻¹. -1 There is no characteristic absorption of azide at this location.