Dual fluorine-modified acrylate emulsions, methods for their preparation, and coating compositions

By introducing fluorinated monomers and epoxy olefin monomers during the emulsion polymerization stage, and combining the chemical bonding reaction between epoxy groups and fluorinated aniline actives, the hydrophobicity and adhesion problems of acrylate emulsions are solved, achieving efficient dual fluorination modification, reducing costs and improving film-forming properties and stability.

CN123152033APending Publication Date: 2026-11-24ZHEJIANG QUZHOU CHENGJI PAINT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611412794.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Conventional acrylic polymer emulsions have high surface energy in their coatings, resulting in insufficient hydrophobicity and stain resistance. Furthermore, monofluoropolymer-modified acrylic emulsions suffer from poor adhesion, poor durability, easy emulsion demulsification, and the tendency for the coating to develop pinholes during application.

Method used

Fluorine-containing monomers and epoxy olefin monomers are introduced into the emulsion polymerization stage for copolymerization to prepare a monofluorinated modified acrylate emulsion containing epoxy active groups. The second fluorine source is chemically bonded to the polymer side chain through the ring-opening reaction of epoxy groups with fluorinated aniline active substances, thereby achieving dual fluorination modification.

Benefits of technology

It improves the hydrophobicity of the coating film, avoids the phase separation problem of fluorinated monomers during polymerization, reduces raw material costs, improves storage stability and film-forming properties, and forms a smooth and dense coating film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152033A_ABST
    Figure CN123152033A_ABST
Patent Text Reader

Abstract

This invention discloses a double-fluorinated modified acrylate emulsion, its preparation method, and a coating composition, comprising the following steps: S1, performing an emulsion polymerization reaction of an emulsifier, acrylate monomers, methacrylate monomers, epoxy olefin monomers, fluorinated monomers, and an initiator in deionized water to prepare a single-fluorinated modified acrylate emulsion containing epoxy groups; S2, pre-emulsifying a fluorinated aniline active material to obtain a fluorinated aniline pre-emulsion; S3, mixing the single-fluorinated modified acrylate emulsion with the fluorinated aniline pre-emulsion and reacting them. A double-fluorinated modified acrylate emulsion was obtained. The raw materials for preparing the double-fluorinated modified acrylate emulsion consisted of the following components in mass percentage: emulsifier 0.60%-1.20%, acrylate monomers 10.0%-15.0%, methacrylate monomers 10.0%-15.0%, epoxy olefin monomers 2.00%-6.00%, fluorinated monomers 1.50%-3.00%, initiator 0.20%-0.50%, fluorinated aniline active material 2.00%-6.00%, and the balance being deionized water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of waterborne polymer emulsion technology, specifically to a double-fluorinated modified acrylate emulsion, its preparation method, and a coating composition thereof. Background Technology

[0002] Acrylic polymer emulsions are widely used in coatings, adhesives, leather finishing agents, and textile finishing agents due to their excellent film-forming properties, weather resistance, and adhesion. However, conventional acrylic polymer emulsions have high surface energy, resulting in insufficient hydrophobicity and stain resistance, limiting their use in high-end applications. To address these issues, researchers have attempted to modify acrylic polymers by introducing fluorinated monomers. Fluorine atoms possess characteristics such as high electronegativity, low polarizability, and small van der Waals radius. Fluorinated segments, when enriched on the coating surface, can significantly reduce the surface energy of the coating, imparting excellent hydrophobic, oleophobic, and stain-resistant properties. However, monofluorinated modified acrylic polymer emulsions still suffer from drawbacks such as poor adhesion, poor durability, easy emulsion demulsification, easy pinhole formation during application, and poor film-forming properties. Summary of the Invention

[0003] To address the technical problems of poor adhesion, poor durability, and easy demulsification in monofluorinated modified acrylate polymer emulsions, this invention proposes a dual-fluorinated modified acrylate emulsion, its preparation method, and a coating composition. In the emulsion polymerization stage, fluorinated monomers and epoxy olefin monomers are introduced for copolymerization to prepare a monofluorinated modified acrylate emulsion containing epoxy active groups. Then, through the ring-opening reaction between the epoxy groups and the fluorinated aniline active material, a second fluorine source is chemically grafted onto the polymer side chains. This achieves dual-fluorination modification of the acrylate emulsion while avoiding the process difficulties such as large differences in the copolymerization reactivity ratios of the two fluorinated monomers and easy phase separation during polymerization.

[0004] The technical solution adopted in this invention is as follows: A method for preparing a double-fluorinated modified acrylate emulsion, comprising the following steps: S1. An emulsion polymerization reaction is carried out in deionized water with emulsifier, acrylate monomer, methacrylate monomer, epoxy olefin monomer, fluorinated monomer and initiator to prepare a monofluorinated modified acrylate emulsion containing epoxy groups. S2. The fluoroaniline active material is pre-emulsified to obtain a fluoroaniline pre-emulsion; S3. The monofluorinated modified acrylate emulsion is mixed with the fluorinated aniline pre-emulsion and reacted to obtain the double-fluorinated modified acrylate emulsion. The raw materials for preparing the double-fluorinated modified acrylate emulsion consist of the following components in weight percentage: emulsifier 0.60%-1.20%, acrylate monomers 10.0%-15.0%, methacrylate monomers 10.0%-15.0%, epoxy olefin monomers 2.00%-6.00%, fluorinated monomers 1.50%-3.00%, initiator 0.20%-0.50%, fluorinated aniline active material 2.00%-6.00%, and the balance being deionized water.

[0005] Optionally, the emulsifier is a mixture of anionic and nonionic emulsifiers, wherein the anionic emulsifier is selected from at least one of sodium dodecylbenzenesulfonate and sodium dodecyl sulfonate, and the nonionic emulsifier is selected from at least one of nonylphenol polyoxyethylene ether and alkyl polyglycoside.

[0006] Optionally, the acrylate monomers are selected from at least one of ethyl acrylate, propyl acrylate, butyl acrylate, and isooctyl acrylate, and the methacrylate monomers are selected from at least one of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, n-octyl methacrylate, and isooctyl methacrylate.

[0007] Optionally, the epoxy olefin monomer is selected from at least one of glycidyl methacrylate and glycidyl acrylate.

[0008] Optionally, the fluorinated monomer is selected from at least one of dodecafluoroheptyl methacrylate, octafluoropentyl methacrylate, and hexafluorobutyl methacrylate, and the fluorinated aniline active material is selected from at least one of difluoroaniline and trifluoroaniline.

[0009] Optionally, the specific steps of the emulsion polymerization reaction are as follows: S11. Add part of the emulsifier and part of the deionized water to the reaction vessel, stir and heat to 75℃-80℃; S12. Add dropwise a mixture of 10%-30% of the formulated amount of acrylate monomers, methacrylate monomers, epoxy olefin monomers and fluorine-containing monomers, and 10%-30% of the formulated amount of initiator aqueous solution within 15-20 minutes, and keep warm for 15-30 minutes. S13. Add the remaining amount of initiator aqueous solution and remaining mixed monomers dropwise over 2.0-2.5 hours. After the addition is complete, raise the temperature to 90°C and continue to keep it at that temperature for 40-50 minutes. S14. Cooling and filtering yield the monofluoromodified acrylate emulsion.

[0010] Optionally, the mass fraction of fluoroaniline active ingredient in the fluoroaniline pre-emulsion is 30%-40%.

[0011] The present invention also discloses a method for preparing a double-fluorinated modified acrylate emulsion using the preparation method described above. The double-fluorinated modified acrylate emulsion forms a latex film after film formation at 80°C, and the water contact angle of the latex film is greater than 110°.

[0012] The present invention also discloses a coating composition comprising the aforementioned dual-fluorinated modified acrylate emulsion. Optionally, the mass fraction of the dual-fluorinated modified acrylate polymer emulsion in the coating composition is 30%-60%.

[0013] The beneficial effects of this invention are: (1) Only a small amount (1.50%-3.00%) of fluorinated monomers are introduced during the emulsion polymerization stage to prepare a monofluorinated modified acrylate emulsion containing epoxy active groups; then, through the ring-opening reaction between the epoxy groups and the fluorinated aniline active material, the second fluorine source is chemically bonded to the polymer side chain. This process allows the fluorinated monomers to fully participate in copolymerization during the polymerization stage, avoiding the problem in the traditional dual-fluorination modification process where some fluorinated monomers fail to effectively integrate into the polymer chain due to the large difference in the reactivity rates of the two fluorinated monomers, and significantly improving the utilization rate of the fluorinated monomers. Under the premise of achieving the same or even better hydrophobic properties of the coating film, the total fluorine addition is effectively reduced, greatly reducing the raw material cost and improving the cost-effectiveness of the product.

[0014] (2) Only a single type of fluorinated monomer is used, and the amount of fluorinated monomer is low (1.50%-3.00%), avoiding the problems of large differences in the polymerization rates of the two fluorinated monomers and severe phase separation during polymerization in the traditional dual-fluorination modification process. The system maintains a good homogeneous state throughout the polymerization process, with no obvious gelation or demulsification. The resulting emulsion has a uniform particle size distribution, does not separate or precipitate during storage, and has good storage stability. At the same time, due to the reduced amount of fluorinated monomer, the reaction heat control during polymerization is easier, further reducing the risk of demulsification in industrial production.

[0015] (3) The fluorine element is partly derived from the fluorine-containing monomers copolymerized and incorporated into the main chain during the emulsion polymerization stage, and partly from the fluorine-containing aniline groups grafted onto the side chains through chemical bonds during the later reaction stage. Due to the low amount of fluorine monomers used in the polymerization stage, the flexibility and crystallinity of the polymer main chain are not excessively affected. The latex particles can fully fuse and aggregate during the film formation process to form a continuous and complete coating film. Compared with the defects such as pinholes and cracks in the coating film caused by excessive fluorine content or uneven distribution of fluorine segments in the traditional double fluorine modification process, the emulsion prepared by this invention has excellent film-forming properties, and the coating film surface is smooth and dense. Attached Figure Description

[0016] Figure 1 The infrared spectrum of the monofluorinated modified acrylate emulsion coating film prepared in Example 1 of this invention; Figure 2The infrared spectrum of the double fluorine modified acrylate emulsion coating film prepared in Example 1 of this invention; Figure 3 This is a contact angle test diagram of the monofluoromodified acrylate emulsion coating film prepared in Example 2 of the present invention; Figure 4 This is a contact angle test diagram of the double fluorine modified acrylate emulsion coating film prepared in Example 2 of the present invention. Detailed Implementation

[0017] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.

[0018] Example 1

[0019] In a 250 mL four-necked flask equipped with a stirrer, reflux condenser, and dropping funnel, add 1.50 g of a mixed emulsifier of sodium dodecylbenzenesulfonate and nonylphenol polyoxyethylene ether (total mass of the mixed emulsifier is 2.00 g) and 38.50 g of deionized water. Stir and heat in a water bath to 80 °C. Over 15 min, add dropwise 3.00 g of a mixed monomer of methyl methacrylate, butyl acrylate, hexafluorobutyl methacrylate, and glycidyl methacrylate, along with 3.00 g of potassium persulfate aqueous solution (0.24 g potassium persulfate dissolved in 2.76 g deionized water). After the addition is complete, continue to maintain the temperature for 30 min. Then, the remaining 27.00 g of potassium persulfate aqueous solution and 27.00 g of the mixed monomers were added dropwise to a four-necked flask at a uniform rate over 2.5 h. After the addition was complete, the temperature was raised to 90 °C and maintained for 60 min. Then, the temperature was lowered to room temperature, and the mixture was filtered through 100-mesh gauze to obtain the monofluoromodified acrylate emulsion. The infrared spectrum of its coating is shown in [Figure number missing]. Figure 1 .

[0020] Subsequently, 5.00 g of trifluoroaniline was pre-emulsified with an appropriate amount of mixed emulsifier, resulting in a trifluoroaniline content of 30% in the pre-emulsion. At a reaction temperature of 45°C, the above monofluoromodified acrylate emulsion was added dropwise to a reaction flask containing pre-emulsified trifluoroaniline under stirring for 4.0 h. Finally, the mixture in the flask was filtered to obtain a double-fluorinated modified acrylate emulsion. The infrared spectrum of its coating is shown in [Figure number missing]. Figure 2 .

[0021] The above-mentioned mixed monomers consist of 11.60g methyl methacrylate, 11.60g butyl acrylate, 5.00g glycidyl methacrylate and 1.80g hexafluorobutyl methacrylate; the potassium persulfate aqueous solution is prepared by dissolving 0.24g potassium persulfate in 29.76g deionized water.

[0022] contrast Figure 1 and Figure 2NC can be detected at 1614 cm. -1 The characteristic absorption peak at , C-OH at 1342 cm⁻¹ -1 Stretching vibrations at 698 cm⁻¹ and ortho-substituted benzene ring at 698 cm⁻¹ -1 The absorption peak at [location missing]. Infrared spectroscopy confirms that the double-fluorinated modified acrylate emulsion can be prepared by reacting the monofluorinated modified acrylate emulsion with a fluorinated aniline active material.

[0023] Example 2

[0024] In a 250 mL four-necked flask equipped with a stirrer, reflux condenser, and dropping funnel, add 0.40 g of sodium dodecylbenzenesulfonate, 1.20 g of alkyl polyglycoside, and 38.40 g of deionized water. Stir and heat in a water bath to 80 °C. Over 15 min, add dropwise 6.00 g of a mixture of methyl methacrylate, butyl acrylate, dodecyl fluoroheptyl methacrylate, and glycidyl acrylate monomers in a specified ratio, along with 6.00 g of an aqueous solution of ammonium persulfate (0.30 g of ammonium persulfate dissolved in 5.70 g of deionized water). After the addition is complete, continue heating for 15 min. Then, add the remaining 24.00 g of the ammonium persulfate aqueous solution and 24.00 g of the mixed monomers dropwise to the four-necked flask over 2.0 h. After the addition is complete, heat to 90 °C and maintain the temperature for 60 min. After cooling to room temperature, filter the material through 100-mesh gauze to obtain the monofluoromodified acrylate emulsion. The contact angle of its coating is shown in the figure. Figure 3 .

[0025] Subsequently, 5.00 g of difluoroaniline was pre-emulsified with a mixed emulsifier of 0.20 g sodium dodecylbenzenesulfonate and 0.20 g nonylphenol polyoxyethylene ether, resulting in a difluoroaniline content of 30% in the pre-emulsion. The monofluoromodified acrylate emulsion was then added dropwise to a reaction flask containing the pre-emulsified difluoroaniline at a reaction temperature of 45°C with stirring for 4.0 h. Finally, the mixture in the flask was filtered to obtain a double-fluorinated modified acrylate emulsion, the contact angle of which is shown in the figure. Figure 4 .

[0026] The above-mentioned mixed monomers consist of 11.50g methyl methacrylate, 11.50g butyl acrylate, 5.00g glycidyl methacrylate and 2.00g hexafluorobutyl methacrylate; the ammonium persulfate aqueous solution is prepared by dissolving 0.30g ammonium persulfate in 29.70g deionized water.

[0027] Compare Figure 3 and Figure 4It is known that the contact angle of the double-fluorinated modified acrylic emulsion coating (114.8°) is higher than that of the single-fluorinated modified acrylic emulsion coating (63.1°). After the double-fluorinated modified acrylic emulsion forms a film, the surface energy of the latex film is further reduced due to the distribution of more fluorinated groups at the interface between the latex film and the air, making it less susceptible to water wetting and enhancing its water resistance. The surface migration mechanism of fluorinated segments during film formation is as follows: based on the minimization of interfacial free energy and the thermodynamic incompatibility between fluorinated segments and hydrocarbon chains, during water evaporation, latex particle fusion, and chain relaxation, the highly mobile perfluoroalkyl chains spontaneously migrate and accumulate towards the air interface of the coating film, forming a fluorine element gradient distribution along the film thickness.

[0028] Example 3

[0029] In a 250 mL four-necked flask equipped with a stirrer, reflux condenser, and dropping funnel, add 0.20 g of sodium dodecyl sulfonate, 1.40 g of nonylphenol polyoxyethylene ether, and 38.40 g of deionized water. Stir and heat in a water bath to 80 °C. Over 30 min, add dropwise 7.50 g of a mixture of methyl methacrylate, butyl acrylate, hexafluorobutyl methacrylate, and glycidyl acrylate monomers in a specified ratio, along with 7.50 g of potassium persulfate aqueous solution (0.30 g potassium persulfate dissolved in 7.20 g deionized water). After the addition is complete, continue heating for 15 min. Then, add the remaining 22.50 g of the mixed monomers and 22.50 g of potassium persulfate aqueous solution dropwise to the four-necked flask over 2.0 h. After the addition is complete, heat to 90 °C and maintain this temperature for 60 min. Cool to room temperature and filter through 100-mesh gauze to obtain the monofluoromodified acrylate emulsion.

[0030] Subsequently, 5.50 g of trifluoroaniline was pre-emulsified with a mixed emulsifier of 0.20 g sodium dodecylbenzenesulfonate and 0.20 g nonylphenol polyoxyethylene ether, resulting in a trifluoroaniline content of 35% in the pre-emulsion. The monofluoromodified acrylate emulsion was then added dropwise to a reaction flask containing the pre-emulsified trifluoroaniline at a reaction temperature of 45°C with stirring for 4.0 h. Finally, the mixture in the flask was filtered to obtain a doubly fluorinated modified acrylate emulsion.

[0031] The above-mentioned mixed monomers consist of 10.50g butyl acrylate, 10.50g methyl methacrylate, 2.50g hexafluorobutyl methacrylate and 6.50g glycidyl methacrylate; the potassium persulfate aqueous solution is prepared by dissolving 0.30g potassium persulfate in 29.70g deionized water.

[0032] Example 4

[0033] In a 250 mL four-necked flask equipped with a stirrer, reflux condenser, and dropping funnel, add 0.60 g of sodium dodecyl sulfonate, 0.45 g of nonylphenol polyoxyethylene ether, 0.45 g of alkyl polyglycoside, and 38.50 g of deionized water. Stir and heat in a water bath to 80 °C. Over 20 min, add dropwise 9.00 g of a mixture of methyl methacrylate, butyl acrylate, glycidyl acrylate, and dodecyl fluoroheptyl methacrylate monomers in a specified ratio, along with 9.00 g of an aqueous solution of ammonium persulfate (0.20 g of ammonium persulfate dissolved in 8.80 g of deionized water). After the addition is complete, continue heating for 15 min. Then, add the remaining 21.00 g of the ammonium persulfate aqueous solution and 21.00 g of the mixed monomers dropwise to the four-necked flask over 2.0 h. After the addition is complete, heat to 90 °C and maintain the temperature for 60 min. After cooling to room temperature, filter the material through 100-mesh gauze to obtain the monofluorinated modified acrylate emulsion.

[0034] Subsequently, 5.50 g of trifluoroaniline was pre-emulsified with a mixed emulsifier of 0.25 g sodium dodecylbenzenesulfonate and 0.25 g nonylphenol polyoxyethylene ether, resulting in a trifluoroaniline content of 35% in the pre-emulsion. The monofluoro-modified acrylate emulsion was then added dropwise to a reaction flask containing the pre-emulsified trifluoroaniline at a reaction temperature of 45°C with stirring for 4.0 h. Finally, the mixture in the flask was filtered to obtain a doubly fluorinated modified acrylate emulsion.

[0035] The above-mentioned mixed monomers consist of 10.75g methyl methacrylate, 10.75g butyl acrylate, 6.00g glycidyl methacrylate and 2.50g dodecafluoroheptyl methacrylate; the ammonium persulfate aqueous solution is prepared by dissolving 0.20g ammonium persulfate in 29.80g deionized water.

[0036] Example 5

[0037] The double-fluorinated modified acrylic emulsion is applied to the preparation of coatings. The specific preparation method is as follows: 15.00g titanium dioxide, 5.00g mica powder, 15.00g talc powder, 1.00g ethylene glycol, 0.50g hydroxyethyl cellulose, 1.00g sodium tripolyphosphate, and 0.60g polydimethylsiloxane were added to an SDF400 grinding and dispersing machine, followed by 30.00g deionized water. The mixture was mechanically stirred at 1200 rpm for 1.5 hours to ensure uniform dispersion. Then, 80.00g of the double-fluorinated modified acrylic emulsion prepared in Example 1 and 1.20g defoamer were added, and the mixture was mechanically stirred at 600 rpm for 2.0 hours to ensure uniform dispersion. The resulting product was the double-fluorinated modified acrylic latex coating.

[0038] Examples 1-5 above show that the present invention prepares a monofluorinated modified acrylate emulsion containing epoxy groups by first introducing fluorinated monomers and epoxy olefin monomers in the emulsion polymerization stage, and then introducing fluorinated aniline active material in the post-reaction stage, using the ring-opening reaction between epoxy groups and aniline groups to chemically bond a second fluorine source to the polymer chain, thereby achieving dual fluorination modification of the acrylate emulsion.

[0039] The polymerization reaction formula for the monofluoromodified acrylate emulsion is as follows:

[0040] The copolymer side chain of the monofluorinated modified acrylic emulsion contains an epoxy functional group introduced by glycidyl methacrylate. This epoxy group undergoes a ring-opening addition reaction with pre-emulsified trifluoroaniline, grafting a trifluoromethyl-containing aromatic fluorine structure onto the polymer chain to obtain a double-fluorinated modified acrylic emulsion. The reaction formula is as follows:

[0041] Examples 1 to 4 verified that, under different types of fluorinated monomers (hexafluorobutyl methacrylate, dodecafluoroheptyl methacrylate), different types of fluorinated aniline actives (trifluoroaniline, difluoroaniline), different types of initiators (potassium persulfate, ammonium persulfate), and different emulsifier systems (anionic / nonionic binary composite, anionic / nonionic ternary composite), double-fluorinated modified acrylate emulsions could be successfully prepared. Furthermore, after film formation at 80°C, the water contact angle of the resulting emulsions was significantly higher than that of the corresponding single-fluorinated modified acrylate emulsion films (Example 2). Figure 3 , Figure 4 This demonstrates that the technical solution of the present invention has broad raw material adaptability and process universality. Example 5 further confirms that the double-fluorinated modified acrylate emulsion prepared by the present invention can be directly applied to water-based coating formulations, possessing good compatibility and practical application value.

[0042] As can be seen from the above embodiments, the preparation method provided by the present invention has stable process, flexible raw material selection, and excellent hydrophobic properties, and is applicable to multiple fields such as architectural coatings, plastic coatings, adhesives, textile and leather finishing agents.

Claims

1. A method for preparing a double-fluorinated modified acrylate emulsion, characterized in that, Includes the following steps: S1. An emulsion polymerization reaction is carried out in deionized water with emulsifier, acrylate monomer, methacrylate monomer, epoxy olefin monomer, fluorinated monomer and initiator to prepare a monofluorinated modified acrylate emulsion containing epoxy groups. S2. The fluoroaniline active material is pre-emulsified to obtain a fluoroaniline pre-emulsion; S3. The monofluorinated modified acrylate emulsion is mixed with the fluorinated aniline pre-emulsion and reacted to obtain the double-fluorinated modified acrylate emulsion. The raw materials for preparing the double-fluorinated modified acrylate emulsion consist of the following components in weight percentage: emulsifier 0.60%-1.20%, acrylate monomers 10.0%-15.0%, methacrylate monomers 10.0%-15.0%, epoxy olefin monomers 2.00%-6.00%, fluorinated monomers 1.50%-3.00%, initiator 0.20%-0.50%, fluorinated aniline active material 2.00%-6.00%, and the balance being deionized water.

2. The method for preparing the double-fluorinated modified acrylate emulsion according to claim 1, characterized in that, The emulsifier is a mixture of anionic and nonionic emulsifiers. The anionic emulsifier is selected from at least one of sodium dodecylbenzenesulfonate and sodium dodecyl sulfonate, and the nonionic emulsifier is selected from at least one of nonylphenol polyoxyethylene ether and alkyl polyglycoside.

3. The method for preparing the double-fluorinated modified acrylate emulsion according to claim 1, characterized in that, The acrylate monomers are selected from at least one of ethyl acrylate, propyl acrylate, butyl acrylate, and isooctyl acrylate, and the methacrylate monomers are selected from at least one of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, n-octyl methacrylate, and isooctyl methacrylate.

4. The method for preparing the double-fluorinated modified acrylate emulsion according to claim 1, characterized in that, The epoxy olefin monomer is selected from at least one of glycidyl methacrylate and glycidyl acrylate.

5. The method for preparing the double-fluorinated modified acrylate emulsion according to claim 1, characterized in that, The fluorinated monomer is selected from at least one of dodecafluoroheptyl methacrylate, octafluoropentyl methacrylate, and hexafluorobutyl methacrylate, and the fluorinated aniline active material is selected from at least one of difluoroaniline and trifluoroaniline.

6. The method for preparing the double-fluorinated modified acrylate emulsion according to claim 1, characterized in that, The specific steps of the emulsion polymerization reaction are as follows: S11. Add part of the emulsifier and part of the deionized water to the reaction vessel, stir and heat to 75℃-80℃; S12. Add dropwise a mixture of 10%-30% of the formulated amount of acrylate monomers, methacrylate monomers, epoxy olefin monomers and fluorine-containing monomers, and 10%-30% of the formulated amount of initiator aqueous solution within 15-20 minutes, and keep warm for 15-30 minutes. S13. Add the remaining amount of initiator aqueous solution and remaining mixed monomers dropwise over 2.0-2.5 hours. After the addition is complete, raise the temperature to 90°C and continue to keep it warm for 40-50 minutes. S14. Cooling and filtering yield the monofluoromodified acrylate emulsion.

7. The method for preparing the double-fluorinated modified acrylate emulsion according to claim 1, characterized in that, The mass fraction of fluoroaniline active ingredient in the fluoroaniline pre-emulsion is 30%-40%.

8. A double-fluorinated modified acrylate emulsion prepared by the preparation method according to any one of claims 1 to 7, characterized in that, The double-fluorinated modified acrylate emulsion forms a latex film after being filmed at 80°C, and the water contact angle of the resulting latex film is greater than 110°.

9. A coating composition, characterized in that, It comprises the dual-fluorinated modified acrylate emulsion as described in claim 8.

10. The coating composition according to claim 9, characterized in that, The mass fraction of the dual-fluorinated modified acrylate polymer emulsion in the coating composition is 30%-60%.