High-temperature-resistant nylon and preparation method and application thereof
By optimizing the prepolymerization process and solid-state polymerization reaction, high-viscosity high-temperature resistant nylon was prepared, solving the problems of long prepolymerization time and unstable performance in the existing technology. This resulted in efficient production and excellent material properties, making it suitable for special spinning and bearing applications.
Patent Information
- Application Number
- CN202611318919.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
In the preparation of high-temperature resistant nylon, the existing technology results in a low relative viscosity due to the prepolymerization process, which leads to excessively long solid-phase polymerization time, high energy consumption, and low equipment utilization. Furthermore, prolonged high-temperature treatment can easily cause polymer thermal degradation or oxidative crosslinking, affecting the color and performance stability of the product.
By optimizing the prepolymerization process, using a combination of dicarboxylic acid and aliphatic diamine, controlling the reaction temperature and time, and combining solid-state polymerization under vacuum, a prepolymer with high relative viscosity is prepared, shortening the solid-state polymerization time and improving production efficiency.
The prepared high-temperature resistant nylon material has a relative viscosity of 2.0~2.4, a tensile strength exceeding 100MPa, and is pure white in color. It possesses anti-yellowing properties, high reflectivity, and good processing performance, making it suitable for special spinning and bearing applications.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature resistant nylon technology, specifically relating to a high-temperature resistant nylon, its preparation method, and its application. Background Technology
[0002] High-temperature resistant nylon refers to a special nylon material that can be used for a long time in environments above 150℃. Its melting point is generally between 290-320℃. It is a high heat-resistant resin between general engineering plastic nylon and high-temperature engineering plastic PEEK. Due to its excellent comprehensive performance, this nylon material is widely used in the electronics and electrical industry and the automotive industry.
[0003] Currently, existing domestic and international patents such as CN1012153751A, CN102477219A, CN101289535A, US4076664, US4603166, US6518341, US4762910, and US4246395 disclose methods for preparing high-temperature resistant nylon, employing a prepolymerization followed by polymerization method. The tensile strength of the pure resin is below 100 MPa. The main reason for this is that the prepolymer synthesized in existing prepolymerization processes has a relatively low viscosity (generally below 1.0), leading to a longer solid-state polymerization time (usually 4-8 hours or even longer) to allow the polymer to reach the target molecular weight. Solid-state polymerization, as the rate-limiting step in the entire process, not only results in high energy consumption, low equipment utilization, and long production cycles due to its excessively long reaction time, but also easily triggers polymer thermal degradation or oxidative crosslinking during prolonged high-temperature treatment, affecting the product's color and performance stability.
[0004] In addition, patents such as CN 119708469 A introduce phosphorus- or halogen-containing functional monomers into copolymerization to simultaneously improve the flame retardancy and mechanical strength of the material. However, such methods are essentially chemical modifications of the material, which alter the polymer backbone structure. Furthermore, the synthesis of functional monomers is costly and the process control is complex, making them unsuitable for the large-scale and efficient preparation of conventional high-temperature resistant nylon resins.
[0005] Therefore, for high-temperature resistant nylons using conventional aromatic diacids or heterocyclic diacids and aliphatic diamine monomer systems, how to obtain prepolymers with high relative viscosity without introducing special functional monomers or changing the established monomer composition, solely through optimization of the prepolymerization process itself, thereby significantly shortening the subsequent solid-state polymerization time and improving production efficiency, while ensuring that the tensile strength and other mechanical properties of the final resin meet application requirements, remains an urgent problem to be solved. Summary of the Invention
[0006] The main objective of this invention is to provide a high-temperature resistant nylon, its preparation method, and its application, so as to overcome the defects of the prior art.
[0007] To achieve the aforementioned objectives, the technical solution adopted by this invention includes: The first aspect of this invention provides a method for preparing high-temperature resistant nylon, comprising: The mixed reaction system containing reactive monomers, solvents and additives is heated to a first temperature to carry out a first reaction, then heated to a second temperature to carry out a second reaction, and then cooled to a third temperature. After post-processing, a prepolymer is obtained. In a vacuum environment, the temperature is raised to a fourth temperature to cause the prepolymer to undergo a solid-state polymerization reaction, thereby obtaining high-temperature resistant nylon; The reaction monomers include a combination of a dicarboxylic acid and an aliphatic diamine.
[0008] A second aspect of the present invention provides a high-temperature resistant nylon prepared by the aforementioned preparation method, wherein the high-temperature resistant nylon has a relative viscosity of 2.0 to 2.4.
[0009] A third aspect of the invention provides the application of the high-temperature resistant nylon in the fields of specialty spinning or bearings.
[0010] Compared with the prior art, the present invention has at least the following beneficial effects: (1) This invention obtains a high relative viscosity prepolymer by optimizing the existing prepolymerization process, shortens the solid-phase polymerization reaction time in the later stage, and the viscosity of the high temperature resistant nylon material prepared is maintained at 2.0~2.4, and the tensile strength exceeds 100MPa. It can well balance the processing performance and mechanical properties of nylon and can be applied in special spinning, bearing and other fields.
[0011] (2) The prepolymer and the final product, high-temperature resistant nylon material, obtained by this invention are both pure white in color and have advantages such as anti-yellowing, high reflectivity, and colorability in practical applications. Detailed Implementation
[0012] In view of the problems existing in the above-mentioned prior art, after in-depth research, a high-temperature resistant nylon, its preparation method and application are provided.
[0013] The following will provide a further explanation of the technical solution, its implementation process, and its principles.
[0014] The first aspect of the present invention provides a method for preparing high-temperature resistant nylon, comprising: The mixed reaction system containing reactive monomers, solvents and additives is heated to a first temperature to carry out a first reaction, then heated to a second temperature to carry out a second reaction, and then cooled to a third temperature. After post-processing, a prepolymer is obtained. In a vacuum environment, the temperature is raised to a fourth temperature to cause the prepolymer to undergo a solid-state polymerization reaction, thereby obtaining high-temperature resistant nylon; The reaction monomers include a combination of a dicarboxylic acid and an aliphatic diamine.
[0015] In some embodiments, the mass ratio of the reactant monomer, solvent, and auxiliary agent is 100:15~30:0.1~3.0.
[0016] In some embodiments, the molar ratio of the dicarboxylic acid to the aliphatic diamine in the reactant monomer is 1:1.0~1.1.
[0017] In some embodiments, the preparation method specifically includes: heating the mixed reaction system to 200-220 °C (i.e., the first temperature) in a closed environment of 0.05-0.2 MPa, allowing the first reaction to occur for 1-3 hours, then heating to 270-290 °C (i.e., the second temperature), allowing the second reaction to occur for 1-2 hours, and then cooling to 200-220 °C (i.e., the third temperature), followed by post-treatment to obtain the prepolymer. The first and second reactions are both dehydration condensation reactions of nylon salts. In this invention, the staged prepolymerization at 200-220 °C and the high-temperature prepolymerization at 270-290 °C effectively increase the polymer viscosity, resulting in a prepolymer with high viscosity and high polymer content. Furthermore, since diamines easily undergo cyclization reactions during polymerization, leading to an imbalance in the amino acid ratio, the high-temperature prepolymerization at 270-290 °C allows for rapid reaction, reduces reaction time, effectively avoids the cyclization reaction of diamines, reduces amine loss, and improves reaction efficiency.
[0018] Further, the post-processing includes: mixing the reactants obtained after cooling to a third temperature with water until homogeneous, filtering or centrifuging the resulting solid-liquid mixture to obtain the prepolymer. The obtained prepolymer is a solid. In the post-processing stage, water washing removes water-soluble unpolymerized raw materials or oligomers, which further ensures the viscosity of the prepolymer.
[0019] Furthermore, the mass ratio of the reactants to water is 1:2 to 6.
[0020] Furthermore, the relative viscosity of the prepolymer is 1.4 to 1.6.
[0021] In some embodiments, the preparation method specifically includes: heating to 240-260°C (i.e., the fourth temperature) under a vacuum environment of 10-100 Pa to allow the prepolymer to undergo a solid-state polymerization reaction for 2-4 hours to obtain the high-temperature resistant nylon.
[0022] In some embodiments, the dicarboxylic acid includes one or more combinations of aromatic diacids, heterocyclic diacids, aliphatic dicarboxylic acids, and alicyclic dicarboxylic acids.
[0023] In some preferred embodiments, the aromatic diacid includes, but is not limited to, at least one of terephthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalic acid, 2,7-naphthalic acid, 1,4-naphthalic acid, 4,4'-biphenyldicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, and diphenyl sulfone-4,4'-dicarboxylic acid.
[0024] Furthermore, the aromatic diacid includes a combination of terephthalic acid and isophthalic acid.
[0025] For example, in a typical implementation, the molar ratio of terephthalic acid to isophthalic acid is 55:45.
[0026] In some preferred embodiments, the heterocyclic dicarboxylic acid includes at least one of furanyl dicarboxylic acid, thiophene dicarboxylic acid, and pyridine dicarboxylic acid, but is not limited to it.
[0027] In some preferred embodiments, the aliphatic dicarboxylic acid includes, but is not limited to, at least one of malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, octanoic acid, azelaic acid, sebacic acid, dimethylmalonic acid, 3,3-diethylsuccinic acid, 2-methyladipic acid, and 2,2-dimethylglutaric acid.
[0028] Furthermore, the aliphatic dicarboxylic acid includes adipic acid.
[0029] In some preferred embodiments, the alicyclic dicarboxylic acid includes at least one of 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid, but is not limited thereto.
[0030] In some embodiments, the aliphatic diamine includes, but is not limited to, one or more combinations of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tetanediamine, 2-methyl-1,5-pentanediamine, 2,2,4-trimethyl-1,6-hexanediamine, and 2-methyl-1,8-octanediamine.
[0031] In some embodiments, the solvent includes, but is not limited to, at least one of water, methanol, ethanol, propanol, butanol, pentanol, hexanol, octanol, decanol, hexanediol, glycerol, DMAc, and NMP.
[0032] In some preferred embodiments, the solvent is water.
[0033] In some embodiments, the adjuvant includes sodium hypophosphite, but is not limited to this.
[0034] In some more specific embodiments, the method for preparing the high-temperature resistant nylon specifically includes the following steps: (1) Add the dicarboxylic acid, aliphatic diamine, solvent and other additives to a high temperature and high pressure reactor. After replacing the air in the reactor with nitrogen three times, purge with nitrogen to keep the pressure in the reactor at 0.05~0.2MPa. Turn on the heating and raise the temperature in the reactor to 200~220℃. Maintain the first reaction at this temperature for 1~3 h. Continue to raise the temperature to 270~290℃ and maintain the second reaction at this temperature for 1~2 h. Cool down to 200~220℃ and pass deionized water under this condition to obtain an aqueous solution of the reactants. By filtration or centrifugation, a white prepolymer is obtained with a relative viscosity controlled at 1.4~1.6.
[0035] (2) The white prepolymer is placed in a vacuum drum, the vacuum is drawn to 20 Pa, the heating is turned on, the temperature is raised to 240~260℃, and the solid-state polymerization reaction is carried out at this temperature for 2~4 h; the white polymer is obtained by cooling and discharging, and high-temperature resistant nylon is obtained.
[0036] A second aspect of the present invention provides a high-temperature resistant nylon prepared by the aforementioned preparation method, wherein the high-temperature resistant nylon has a relative viscosity of 2.0 to 2.4.
[0037] The third aspect of this invention provides the application of the high-temperature resistant nylon in the fields of special spinning or bearings. For example, the high-temperature resistant nylon of this invention has a high melting point, extremely low water absorption, and combines rigidity with melt processability. It overcomes the shortcomings of ordinary nylon, such as insufficient temperature resistance and easy moisture absorption and deformation, and can serve for a long time at high temperatures, realizing the metal replacement of high-temperature fiber spinning and maintenance-free bearings.
[0038] The technical solution of the present invention will be further described below with reference to the embodiments. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available. Other unmentioned raw materials and instruments are all conventionally selected and do not involve the core technical means of the present invention.
[0039] Example 1 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 20 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out at this condition for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.5).
[0040] Preparation of high-temperature resistant nylon: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a white polymer (relative viscosity 2.2), thus obtaining high-temperature resistant nylon.
[0041] Example 2 Preparation of the prepolymer: 100 parts of terephthalic acid, isophthalic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and isophthalic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to isophthalic acid is 55:45), 20 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out at this condition for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.55).
[0042] Preparation of high-temperature resistant nylon: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a white polymer (relative viscosity 2.3), thus obtaining high-temperature resistant nylon.
[0043] Example 3 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and pentanediamine (the molar ratio of terephthalic acid and adipic acid to pentanediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 20 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out at this temperature for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.52).
[0044] Preparation of high-temperature resistant nylon: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a white polymer (relative viscosity 2.22), thus obtaining high-temperature resistant nylon.
[0045] Example 4 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 15 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out at this condition for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.53).
[0046] Preparation of high-temperature resistant nylon: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a white polymer (relative viscosity 2.24), thus obtaining high-temperature resistant nylon.
[0047] Example 5 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 30 parts of deionized water, and 1 part of additives were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out at this condition for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.48).
[0048] Preparation of high-temperature resistant nylon: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a white polymer (relative viscosity 2.19), thus obtaining high-temperature resistant nylon.
[0049] Example 6 The difference between this embodiment and Embodiment 1 is that adipic acid is replaced with furanyl dicarboxylic acid.
[0050] Example 7 The difference between this embodiment and Embodiment 1 is that adipic acid is replaced with 1,4-cyclohexanedicarboxylic acid.
[0051] Example 8 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and 1,4-butanediamine (the molar ratio of terephthalic acid and adipic acid to 1,4-butanediamine is 1:1.05, and the molar ratio of terephthalic acid and adipic acid is 55:45), 20 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.20 MPa. Heating and stirring were turned on, and the temperature of the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 270℃, and the reaction was carried out at this temperature for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.45).
[0052] Preparation of high-temperature resistant nylon: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a white polymer (relative viscosity 2.35), thus obtaining high-temperature resistant nylon.
[0053] Example 9 The difference between this embodiment and Example 1 is that hexamethylenediamine is replaced with 2-methylpentanediamine.
[0054] Comparative Example 1 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 20 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. 300 parts of deionized water were introduced, and the material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.05).
[0055] Preparation of nylon material: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 10 h; the material is discharged after cooling to obtain a white polymer (relative viscosity 1.8), thus obtaining nylon material.
[0056] Comparative Example 2 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 10 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out under this condition for 1.5 hours. The material solidified and could not be discharged normally.
[0057] Comparative Example 3 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 35 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 210℃. The reaction was carried out at this temperature for 2 hours. The temperature inside the reactor was further raised to 280℃, and the reaction was carried out at this condition for 1.5 hours. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a white prepolymer (relative viscosity 1.3).
[0058] Preparation of nylon material: White prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 4 hours; the material is discharged after cooling to obtain a white polymer (relative viscosity 2.0), thus obtaining nylon material.
[0059] Comparative Example 4 Preparation of the prepolymer: 100 parts of terephthalic acid, adipic acid, and hexamethylenediamine (the molar ratio of terephthalic acid and adipic acid to hexamethylenediamine is 1:1, and the molar ratio of terephthalic acid to adipic acid is 55:45), 20 parts of deionized water, and 1 part of sodium hypophosphite were added to a high-temperature and high-pressure reactor. The air was replaced with nitrogen three times, and a certain amount of nitrogen was introduced. The initial pressure inside the reactor was 0.15 MPa. Heating and stirring were started, and the temperature inside the reactor was raised to 280℃. The reaction was carried out for 1.5 h under these conditions. The temperature was then lowered to 210℃, and 300 parts of deionized water were introduced. The material was filtered or centrifuged to obtain a yellow prepolymer (relative viscosity 1.12).
[0060] Preparation of high-temperature resistant nylon: Yellow prepolymer is added to a vacuum drum, and the pressure inside the drum is maintained at 20 Pa; the temperature is raised to 250℃, and the reaction is carried out at this temperature for 3 hours; the material is cooled and discharged to obtain a yellow polymer (relative viscosity 2.13), thus obtaining high-temperature resistant nylon.
[0061] In this comparative example, because no staged prepolymerization was performed, the resulting prepolymer was yellow, and consequently, the high-temperature resistant nylon also turned yellow.
[0062] Performance testing The viscosity and mechanical properties of the nylon resins obtained in each embodiment and comparative example were tested. The specific test methods are as follows: (1) Relative viscosity [η] The prepolymer and polymer nylon were dissolved in concentrated sulfuric acid to obtain a concentration of 1 g / dl. The relative viscosity (η) of the solution was measured at 25 ºC. r ):η r =t1 / t0; Where t0 represents the time (s) for solvent outflow, t1 represents the time (s) for sample solution outflow, and η r This indicates relative viscosity.
[0063] (2) Mechanical properties The prepared nylon injection-molded test specimens were tested for tensile strength according to GB / T1040.2 standard, flexural strength and flexural modulus according to GB / T9341-2008 standard, and simply supported beam impact strength according to GB / T1043.1 standard.
[0064] The test results are shown in Tables 1 and 2.
[0065] Table 1: Properties of the high-temperature resistant nylon resin obtained in the examples
[0066] Table 2. Properties of the high-temperature resistant nylon resin obtained in the comparative example
[0067] In addition, the present invention has also conducted experiments with other raw materials, process operations and process conditions described in this specification, with reference to the foregoing embodiments, and has obtained relatively ideal results.
[0068] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.
Claims
1. A method for preparing high-temperature resistant nylon, characterized in that, include: The mixed reaction system containing reactive monomers, solvents and additives is heated to a first temperature to carry out a first reaction, then heated to a second temperature to carry out a second reaction, and then cooled to a third temperature. After post-processing, a prepolymer is obtained. In a vacuum environment, the temperature is raised to a fourth temperature to cause the prepolymer to undergo a solid-state polymerization reaction, thereby obtaining high-temperature resistant nylon; The reaction monomers include a combination of a dicarboxylic acid and an aliphatic diamine.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the reactant monomer, solvent, and auxiliary agent is 100:15~30:0.1~3.0; And / or, the molar ratio of the dicarboxylic acid to the aliphatic diamine in the reactant monomer is 1:1.0~1.
1.
3. The preparation method according to claim 1, characterized in that, Specifically, it includes: In a closed environment of 0.05-0.2 MPa, the mixed reaction system is heated to 200-220 °C and the first reaction occurs for 1-3 h. Then the temperature is raised to 270-290 °C and the second reaction occurs for 1-2 h. The temperature is then lowered to 200-220 °C and after post-processing, the prepolymer is obtained.
4. The preparation method according to claim 3, characterized in that, The post-processing includes: mixing the reactants obtained after cooling to a third temperature with water until homogeneous, filtering or centrifuging the resulting solid-liquid mixture to obtain the prepolymer.
5. The preparation method according to claim 4, characterized in that: The mass ratio of the reactant to water is 1:2~6; And / or, the relative viscosity of the prepolymer is 1.4 to 1.
6.
6. The preparation method according to claim 1, characterized in that, Specifically, it includes: Under a vacuum environment of 10~100Pa, the temperature is raised to 240~260℃ to allow the prepolymer to undergo the solid-phase polymerization reaction for 2~4 hours, thereby obtaining the high-temperature resistant nylon.
7. The preparation method according to any one of claims 1-5, characterized in that: The dicarboxylic acid includes one or more combinations of aromatic dicarboxylic acids, heterocyclic dicarboxylic acids, aliphatic dicarboxylic acids, and alicyclic dicarboxylic acids; And / or, the aliphatic diamine includes one or more combinations of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 2-methyl-1,5-pentanediamine, 2,2,4-trimethyl-1,6-hexanediamine, and 2-methyl-1,8-octanediamine; And / or, the solvent includes one of water, methanol, ethanol, propanol, butanol, pentanol, hexanol, octanol, decanol, hexanediol, glycerol, DMAc, and NMP, preferably water; And / or, the adjuvant includes sodium hypophosphite.
8. The preparation method according to claim 7, characterized in that: The aromatic diacids include at least one of terephthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalic acid, 2,7-naphthalic acid, 1,4-naphthalic acid, 4,4'-biphenyldicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, and diphenyl sulfone-4,4'-dicarboxylic acid; And / or, the aromatic diacid includes a combination of terephthalic acid and isophthalic acid; And / or, the heterocyclic dicarboxylic acid includes at least one of furanyl dicarboxylic acid, thiophene dicarboxylic acid, and pyridine dicarboxylic acid; And / or, the aliphatic dicarboxylic acid includes at least one of malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, octanoic acid, azelaic acid, sebacic acid, dimethylmalonic acid, 3,3-diethylsuccinic acid, 2-methyladipic acid, and 2,2-dimethylglutaric acid; Preferably, the aliphatic dicarboxylic acid includes adipic acid; And / or, the alicyclic dicarboxylic acid includes at least one of 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid.
9. The high-temperature resistant nylon prepared by any one of claims 1-8, characterized in that: The relative viscosity of the high-temperature resistant nylon is 2.0~2.
4.
10. The application of the high-temperature resistant nylon according to claim 9 in the fields of special spinning or bearings.
Citation Information
Patent Citations
Long carbon chain condensed ring semi-aromatic nylon and synthetic process thereof
CN101289535A
High-temperature resistant semi-aromatic nylon and its preparation method
CN102477219A
612 OR 610 / 6I or 6T / 636 Polyamide terpolymer
US4076664A
6T / 6I Terpolyamide
US4246395A
Crystalline polyamide composition from dicarboxylic acid mixture and diamine
US4603166A