Method for fixing carbon dioxide by waste heterochain polymer and regenerated polymer

By using the exchange and recombination reaction of heterocyclic compounds with waste heterochain polymers, recycled copolymers are prepared, which solves the problems of low recycling rate and carbon dioxide emissions of waste heterochain polymers, realizes carbon dioxide fixation and resource utilization, and improves the performance and recycling efficiency of recycled polymers.

CN123152104APending Publication Date: 2026-11-24CHEM & CHEM ENG GUANGDONG LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611396002.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, the recycling rate of waste heterochain polymers is low, traditional treatment methods lead to carbon dioxide emissions and environmental pollution, and the performance of recycled products is downgraded, making it difficult to achieve efficient resource conversion and preservation of material value.

Method used

By exchanging and recombinating heterocyclic compounds, long-chain organics, and waste heterochain polymers under specific conditions, recycled copolymers are generated. By reacting carbon dioxide-derived heterocyclic compounds with waste polyesters, recycled polymers with controllable mechanical properties and biodegradability are prepared.

Benefits of technology

It achieves carbon dioxide fixation and resource utilization, reduces the concentration of carbon dioxide in the atmosphere, improves the performance and recycling efficiency of recycled polymers, reduces environmental pollution, and conforms to the principles of green environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152104A_ABST
    Figure CN123152104A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of polymer synthesis technology and discloses a method for fixing carbon dioxide from waste heterochain polymers and a recycled polymer. The method includes the following steps: S1, mixing a heterocyclic compound, a long-chain organic compound, and the heterochain polymer, and carrying out an exchange and recombination reaction at 150–300°C to obtain a prepolymer. The heterocyclic compound refers to a heterocyclic organic compound derived from carbon dioxide that contains a carbonyl group and at least one nitrogen or oxygen heteroatom. The long-chain organic compound includes one or both of long-chain diamines and long-chain diols. S2, reacting the prepolymer at 150–300°C and an absolute pressure of 1–1000 Pa to remove short-chain byproducts, obtaining a recycled copolymer. This invention utilizes heterocyclic compounds prepared from carbon dioxide as raw materials, reducing carbon emissions while recycling waste polyester. Furthermore, the prepared recycled polymer product possesses controllable mechanical properties and biodegradability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer material synthesis technology, specifically relating to a method for fixing carbon dioxide from waste heterochain polymers and a recycled polymer, preferably using waste polyester to fix carbon dioxide to prepare recycled copolymer products. Background Technology

[0002] With the large-scale consumption of fossil resources, global carbon dioxide emissions and atmospheric carbon dioxide concentrations continue to rise, increasing the pressure to reduce carbon emissions. Although renewable energy has developed rapidly, it is still difficult to completely replace fossil energy in the short term, and total carbon dioxide emissions remain at a high level. Carbon emissions from the production, use, and disposal of polymer materials account for a large proportion of total emissions. Reducing these emissions is an important way to achieve efficient recycling of carbon resources and promote green and low-carbon development. Heterochain polymers are a class of polymers whose main chain contains heteroatoms such as oxygen and nitrogen. Typical repeating units include esters, ethers or acetals, carbonates, amides, and urethanes. Heterochain polymers, including polyesters, polyethers, polycarbonates, polyamides, and polyurethanes, have a global annual production of hundreds of millions of tons, making them the second most important synthetic polymer material system after polyolefins. Heterochain polymers, represented by polyethylene terephthalate (PET), polyoxymethylene (POM), bisphenol A polycarbonate (BPA-PC), and nylon 66 (PA66), are widely used in textile fibers, beverage bottles, packaging films, optical devices, and automotive and electronic components.

[0003] Currently, the main methods for recycling and reusing waste heterochain polymers include physical recycling, energy recovery, and chemical recycling. Physical recycling primarily involves collecting, sorting, crushing, washing, pre-crystallizing, drying, and regranulating waste heterochain polymers to restore their processing and usability. However, this method suffers from drawbacks such as high cost, low efficiency, and performance degradation of recycled products. Energy recovery typically converts the chemical energy in waste heterochain polymers into heat or electricity through incineration, but this results in a loss of polymer material value and generates significant carbon dioxide emissions. Chemical recycling uses pyrolysis, oxidation, hydrogenation, hydrolysis, or exchange to convert waste polymers into monomers, oligomers, or other chemicals for further utilization. However, existing chemical depolymerization processes often simultaneously generate monomers, oligomers with varying degrees of polymerization, and multiple byproducts, leading to complex product compositions, increased difficulty in monomer separation and purification, and consequently, higher recycling costs and reduced overall recycling efficiency.

[0004] In summary, the overall recycling rate of waste heterochain polymers remains low, and tens of millions of tons of related waste are still generated globally each year. The rigid aromatic ring structure of aromatic heterochain polymers makes them difficult to degrade in the natural environment; traditional landfill methods typically take hundreds of years or even longer to dispose of them. Incineration, on the other hand, results in the concentrated release of large amounts of carbon dioxide in a short period. While energy recovery can recover some calorific value, it essentially does not preserve the material value of the polymer, ultimately still generating carbon dioxide emissions. These traditional disposal methods not only waste existing heterochain polymer resources but may also exacerbate environmental problems such as microplastic pollution, water pollution, and the greenhouse effect.

[0005] Against this backdrop, developing novel chemical methods that can achieve efficient resource conversion of waste heterochain polymers while preserving the carbon skeleton and material value of heterochain polymers, and reduce the consumption of primary fossil raw materials and carbon dioxide emissions, has become an important requirement for reducing environmental impact and promoting the recycling of carbon resources. Summary of the Invention

[0006] To address the aforementioned technical problems, the present invention aims to provide a method for fixing carbon dioxide from waste heterochain polymers and a recycled polymer. The method utilizes heterocyclic compounds prepared from carbon dioxide as raw materials, thereby reducing carbon emissions while recycling waste polyesters. Furthermore, the recycled polymer products prepared possess controllable mechanical properties and biodegradability.

[0007] To achieve the above-mentioned objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a method for fixing carbon dioxide from waste heterochain polymers, comprising the following steps: S1. Mix heterocyclic compounds, long-chain organic compounds and heterochain polymers, and carry out an exchange and recombination reaction at 150-300℃ to obtain a prepolymer. The heterocyclic compounds refer to heterocyclic organic compounds derived from carbon dioxide that contain a carbonyl group and at least one nitrogen or oxygen heteroatom. The long-chain organic compounds have a main chain carbon number ≥ 4, including one or both of long-chain diamines and long-chain diols. S2. The prepolymer is reacted at 150–300°C and 1–1000 Pa absolute pressure to remove short-chain byproducts and obtain a recycled copolymer.

[0008] Preferably, the heterocyclic compound includes one or more of cyclic ureas, cyclic carbonates, and cyclic carbamates.

[0009] More preferably, the structure of the heterocyclic compound is as follows (I) to (II): Formula (I): ; Equation (II): ; Where X1 and X2 are respectively -N(R 11 )- or -O-; R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 and R 11 They are independent of each other and are all hydrogen or alkyl groups.

[0010] Preferably, the general structural formula of long-chain organic compounds is as follows (III): Equation (III): , where Y = -NH- or -O-, p ≥ 2.

[0011] Preferably, the heterochain polymer includes one or more of polyester, polyether, polycarbonate, polyamide and polyurethane.

[0012] More preferably, the repeating units of the heterochain polymer have the following general structural formula (IV). (VIII) or one or more: Formula (IV): ; Equation (V): ; Formula (VI): ; Equation (VII): Formula (VIII): ; Among them, R 12 R 13 R 14 R 15 R 16 R 17 R 18 R 19 R 20 and R 21 They are independent of each other and are all aromatic or aliphatic chains.

[0013] Preferably, a catalyst is used in steps S1 and S2, wherein the catalyst is one or more of an alkoxide, halide, oxide, hydroxide, or carboxylate containing antimony, tin, titanium, scandium, iron, cobalt, nickel, zinc, magnesium, manganese, and cadmium.

[0014] Preferably, in step S1, the mass of the catalyst accounts for 0.05 to 1% of the mass of the reactants to ensure a significant catalytic effect.

[0015] Preferably, in step S1, the molar ratio of the heterocyclic compound to the long-chain organic compound is 1:(0.1-10), and the molar ratio of the heterochain polymer to the heterocyclic compound is 1:(0.1-10); more preferably, the molar ratio of the heterocyclic compound to the long-chain organic compound is 1:(1-2), and the molar ratio of the heterochain polymer to the heterocyclic compound is 1:(1-2).

[0016] In a second aspect, the present invention provides a recycled polymer prepared by the method described above for fixing carbon dioxide from the waste heterochain polymer.

[0017] Beneficial effects: This invention utilizes carbon dioxide-derived heterocyclic compounds such as cyclic carbonates, cyclic ureas, and cyclic carbamates to react with waste heterochain polymers, long-chain diamines, and alcohols to obtain recycled polymers. This not only alleviates the environmental pollution caused by waste heterochain polymers but also reduces the concentration of carbon dioxide in the atmosphere, achieving rational use of resources and conforming to the principles of green environmental protection.

[0018] This invention can achieve performance editing of regenerated copolymers by controlling the types and proportions of heterocyclic compounds, waste heterochain polymers, long-chain diamines or alcohols. For example, the final regenerated copolymer can be endowed with properties such as easy processing and biodegradability by introducing carbon dioxide units, aliphatic diamines, and alcohol units. Attached Figure Description

[0019] Figure 1 The nuclear magnetic resonance hydrogen spectrum of the prepolymer prepared in Example 1.

[0020] Figure 2 The 1H and 1C NMR spectra of the regenerated copolymer prepared in Example 1.

[0021] Figure 3 The nuclear magnetic resonance hydrogen spectrum of the prepolymer prepared in Example 2.

[0022] Figure 4 The 1H and 1C NMR spectra of the regenerated copolymer prepared in Example 2 are shown.

[0023] Figure 5 The 1H and 1C NMR spectra of the regenerated copolymer prepared for Comparative Example 1 are shown.

[0024] Figure 6 The 1H and 1C NMR spectra of the regenerated copolymer prepared for Comparative Example 2 are shown. Detailed Implementation

[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the specific implementation methods of the present invention will be described below with reference to the accompanying drawings. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings and other implementation methods can be obtained based on these drawings without any creative effort.

[0026] This invention proposes a method for fixing carbon dioxide from waste heterochain polymers, directly utilizing organic matter from which carbon dioxide originates as raw materials to recycle waste polyester. The specific steps are as follows: S1. Mix heterocyclic compounds, long-chain organic compounds and heterochain polymers, and carry out an exchange and recombination reaction at 150-300℃ to obtain a prepolymer. The heterocyclic compounds refer to heterocyclic organic compounds derived from carbon dioxide that contain a carbonyl group and at least one nitrogen or oxygen heteroatom. The long-chain organic compounds have a main chain carbon number ≥ 4, including one or both of long-chain diamines and long-chain diols. S2. The prepolymer is reacted at 150–300°C and 1–1000 Pa absolute pressure to remove short-chain byproducts, resulting in a recycled copolymer, i.e., a recycled polymer.

[0027] In steps S1 and S2, the reaction is carried out in an inert atmosphere to avoid oxidation.

[0028] In step S1, the exchange and recombination reactions between heterocyclic compounds, long-chain organics, and heterochain polymers are a collective term for cyclic acyl transfer, alcoholysis, aminolysis, heterochain bond exchange, and the resulting segment recombination reactions. Specifically, exchange and recombination reactions mainly include the following four types of reactions: First, the amino or hydroxyl groups in long-chain diamines and / or long-chain diols nucleophilically attack the carbonyl carbon in heterocyclic compounds, causing the carbonyl-oxygen bond and / or carbonyl-nitrogen bond in the ring to break, forming a ring-opening product containing urea, carbonate and / or carbamate groups, and retaining the active hydroxyl and / or amino end groups. Second, the hydroxyl, amino and / or other active hydrogen-containing groups on the end of the main chain or side chain of the waste heterochain polymer nucleophilically attack the carbonyl carbon in the heterocyclic compound, causing the heterocyclic compound to open the ring and be incorporated into the molecular chain of the waste heterochain polymer. Third, under catalytic and reaction conditions, heterocyclic compounds undergo ring-opening insertion and exchange recombination reactions with heterocyclic bonds within the waste heterochain polymer molecular chain that are capable of breaking, exchanging, or recombination. This allows the carbonyl structure and intracyclic organic segments from the heterocyclic compound to be incorporated into the waste heterochain polymer molecular chain. The reactive heterochain bonds include one or more of the following: ester bonds, carbonate bonds, urethane bonds, urea bonds, amide bonds, and activatable ether bonds that are capable of breaking, transetherification, or segment recombination under catalytic and reaction conditions. Fourth, long-chain diamines and / or long-chain diols can directly undergo aminolysis, alcoholysis, and / or exchange reactions with the aforementioned reactive heterochain bonds in the waste heterochain polymer, thereby incorporating long-chain diamine and / or long-chain diol segments into the waste heterochain polymer molecular chain and causing the original polymer segments to form new hydroxyl, amino, and / or other reactive end groups.

[0029] The hydroxyl, amino, and / or other active groups retained or newly generated in the above-mentioned ring-opening and exchange products can continue to undergo ring-opening, alcoholysis, aminolysis, interchain exchange, and / or polycondensation reactions with reactive heterochain bonds in heterocyclic compounds, long-chain diamines, long-chain diols, and / or waste heterochain polymers.

[0030] In step S1, the carbon dioxide-derived heterocyclic compound refers to a heterocyclic compound in which the carbonyl carbon is derived from carbon dioxide. That is, the heterocyclic compound required by this invention can be synthesized using carbon dioxide. Preferably, the heterocyclic compound includes one or more of cyclic ureas, cyclic carbonates, and cyclic carbamates; that is, in cyclic ureas, cyclic carbonates, and cyclic carbamates, the carbonyl carbon in the corresponding urea group, carbonate group, or carbamate group is derived from carbon dioxide.

[0031] Furthermore, cyclic ureas can be prepared by carbonylation cyclization of carbon dioxide with a diamine having a suitable ring-forming distance. The diamine is preferably one or more of 1,2-diamine, 1,3-diamine, and their derivatives. Cyclic carbonates can be prepared by cycloaddition of carbon dioxide with epoxides, oxetanes, and their derivatives, or by dehydration cyclization of carbon dioxide with vicinal diols, 1,3-diols, and their derivatives. Cyclic carbamates can be prepared by cycloaddition of carbon dioxide with aziridines and their derivatives, or by carboxylation cyclization of carbon dioxide with amino alcohols, amino epoxides, propargylamines, or alkenylamines and their derivatives. The above preparation methods include, but are not limited to, the methods described above.

[0032] Furthermore, based on the fact that five- and six-membered rings have low ring strain and relatively stable and readily available structures, heterocyclic compounds are preferably five- or six-membered heterocyclic organic compounds, that is, heterocyclic compounds include one or more of five- or six-membered cyclic ureas, cyclic carbonates, and cyclic carbamates.

[0033] V. The structures of six-membered cyclic ureas, cyclic carbonates, and cyclic carbamates are one or two of the following formulas (I) to (II): Formula (I): ; Equation (II): ; Where X (i.e., X1 and X2) is -N(R) 11 )- or -O-, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 and R 11They are independent of each other and are all hydrogen or alkyl groups.

[0034] Furthermore, the heterocyclic compounds include one or more of 2-imidazolidineone, 1,3-dimethyl-2-imidazolidineone, N,N-dimethylpropenylurea, ethylene carbonate, propylene carbonate, trimethylene carbonate, A-methyltrimethylene carbonate, 2-oxazolidineone, 4-methyl-2-azolidineone, 5-methyl-1,3-oxazolidine-2-one, and 1,3-oxazolidinyl-2-one.

[0035] Taking five-membered cyclic urea, five-membered cyclic carbonate and / or five-membered cyclic carbamate as examples, the general formulas of the four types of exchange recombination reactions that occur in step S1 mentioned above are shown in reaction formula (i), reaction formula (ii a), reaction formula (ii b) and reaction formula (iii), respectively.

[0036] Formula (i): ; Formula (ii a): ; Equation (ii b): ; Equation (iii): .

[0037] In the above reaction formula, R1, R2, R3, R4 and R 11 Each segment is independent of the others and is either hydrogen or alkyl; P represents a discarded heterochain polymer segment, and P, P1, and P2 each independently represent the same or different discarded heterochain polymer segments, and X (i.e., X1 to X3) is -N(R 11 - or -O-, in the structural formula of long-chain organic compounds, the subscript p indicates the number of repeating structures in the chain segment, preferably p≥2. Reaction formulas (i), (ii a), (ii b) and (iii) are used to represent the net structural changes that may occur during the reaction process, and do not constitute a limitation on the specific reaction mechanism, the order of reactions, the structure of intermediates, the location of heterochain bond breakage, or the ring-opening direction of cyclic compounds.

[0038] Through the continuous occurrence of the above reactions, covalent bonding, segment exchange, and sequence recombination occur between carbon dioxide-derived carbonyl structures, long-chain diamines and / or long-chain diol segments, and waste heterochain polymer segments, forming a prepolymer containing hydroxyl, amino, and / or other reactive end groups. The prepolymer further undergoes interchain exchange, end-group condensation, and / or exchange condensation reactions under the high temperature and reduced pressure conditions of step S2. If low-molecular-weight byproducts are generated, the reaction equilibrium is shifted towards chain growth by removing short-chain diols, short-chain diamines, amino alcohols, and / or other low-molecular-weight byproducts, yielding a regenerated copolymer.

[0039] In step S1, the general structural formula of the long-chain organic compound is shown in formula (III) below: Equation (III): , where Y = -NH- or -O-, p ≥ 2.

[0040] Preferably, the long-chain diamine includes one or more of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine.

[0041] Preferably, the long-chain diols include one or more of 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol.

[0042] In step S1, the heterochain polymer includes one or more of polyester, polyether, polycarbonate, polyamide, and polyurethane. The general structural formula of the heterochain polymer includes the following formula (IV). One or more of (VIII).

[0043] Formula (IV): ; Equation (V): ; Formula (VI): ; Equation (VII): Formula (VIII): ; Among them, R 12 R 13 R 14 R 15 R 16 R 17 R 18 R 19 R 20 and R 21 They are independent of each other and are all aromatic or aliphatic chain segments. It should be noted that R in this invention...12 ~R 21 The alkyl group is an aromatic or aliphatic segment, and there is no particular limitation on the number of carbon atoms in the aromatic or aliphatic segment. Preferably, the number of carbon atoms in the alkyl group is ≤10.

[0044] Preferably, the heterochain polymer includes one or more of polyethylene terephthalate, polyethylene terephthalate, polyethylene butylene terephthalate, polyethylene 2,5-furandicarboxylate, bisphenol A type polycarbonate, polypropylene carbonate, polyethylene carbonate, polyoxymethylene, polyethylene glycol, poly(1,2-propanediol), polyhexamethylene adipamide, polyhexamethylene sebacamide, and thermoplastic polyurethane elastomer.

[0045] In steps S1 and S2, it is determined whether a catalyst needs to be added based on the reactivity of the reactants. When the reactivity of the reactants is high, the reaction can proceed normally without the addition of a catalyst. When the reactivity of the reactants is relatively low, a catalyst is added to promote the reaction.

[0046] When a catalyst is added, the catalyst in steps S1 and S2 is the same; that is, the catalyst in step S1 is retained for use in step S2. Preferably, the catalyst is one or more of alkoxides, halides, oxides, hydroxides, and carboxylates containing antimony, tin, titanium, scandium, iron, cobalt, nickel, zinc, magnesium, manganese, and cadmium.

[0047] More preferably, the catalyst includes one or more of tin oxide, tin hydroxide, stannous chloride, stannous octoate, tetrabutyl titanate, zinc chloride, zinc oxide, zinc hydroxide, zinc acetate, magnesium chloride, magnesium oxide, magnesium hydroxide, magnesium methoxide, antimony glycolate, antimony trioxide, antimony acetate, antimony chloride, manganese oxide, manganese acetate, manganese chloride, cadmium oxide, cadmium acetate, and cadmium chloride.

[0048] Preferably, in step S1, the mass of the catalyst accounts for 0.05% to 1% of the mass of the reactants to ensure a significant catalytic effect. Here, the mass of the reactants refers to the total mass of the heterocyclic compound, long-chain organic compound, and heterochain polymer.

[0049] Preferably, in step S1, the molar ratio of heterocyclic compound to long-chain organic compound is 1:(0.1-10), and the molar ratio of heterochain polymer to heterocyclic compound is 1:(0.1-10), which is beneficial for the complete conversion of cyclic urea, cyclic carbonate and cyclic carbamate into long-unit urea, carbonate and carbamate segments, and their incorporation into the heterochain polymer segments through exchange reaction.

[0050] More preferably, the molar ratio of the heterocyclic compound to the long-chain organic compound is 1:(1-2).

[0051] More preferably, the molar ratio of the heterochain polymer to the heterocyclic compound is 1:(1-2).

[0052] It should be noted that in step S2, when the number of carbon atoms in the carbon chains of the diamine and alcohol units contained in the waste heterochain polymer (for example, the aromatic or aliphatic segments in the polymer formula can be diamines, alcohols, acids, etc.) is less than 2, the waste heterochain polymer and heterocyclic polymers (such as cyclic urea, cyclic carbonates, and cyclic carbamates) can undergo exchange reactions with long-chain diamines and alcohols. After the exchange, long-chain diamines and alcohols are more likely to remain in the chain than short-chain diamines and alcohols. In this case, in step 1, additional long-chain diamines and alcohols need to be added to promote the normal progress of the reaction. Preferably, when additional long-chain organic matter is added, the molar ratio of the repeating units of the waste heterochain polymer to the additionally added long-chain diamines or alcohols is 1:(1-2). It should be noted that when no additional long-chain organic matter is added, the molar ratio of the repeating units of the heterochain polymer to the total long-chain organic matter is 1:(1-4); when additional long-chain organic matter is added, the molar ratio of the repeating units of the heterochain polymer to the total long-chain organic matter is 1:(2-6). That is, the molar ratio of the repeating units of the heterochain polymer to the total long-chain organic matter is 1:(1-6).

[0053] In step S1, the reaction conditions are determined according to the reactants. Preferably, the reaction temperature is 150–300°C and the reaction time is 0.5–12 h. More preferably, the reaction temperature is 200–280°C and the reaction time is 1–3 h.

[0054] In step S2, the reaction conditions are determined according to the reactants. Preferably, the reaction temperature is 150–300°C and the reaction time is 0.5–48 h. More preferably, the reaction temperature is 200–280°C and the reaction time is 3–8 h.

[0055] The technical solution of the present invention will be described in detail below with specific embodiments.

[0056] Unless otherwise specified, all raw materials used in the following examples are commercially available. Furthermore, the waste heterochain polymers and the resulting recycled polymers used in the following examples were analyzed and detected using nuclear magnetic resonance spectroscopy and molecular weight analysis instruments. The nuclear magnetic resonance spectroscopy and molecular weight analysis were performed in the following manner.

[0057] MRI test procedure: 1 H, 13 C10 NMR spectroscopy was performed on a Bruker AVANCE NEO 600 MHz spectrometer. Deuterated chloroform was typically used as the solvent. For samples insoluble in chloroform, such as polyethylene terephthalate, a mixture of deuterated chloroform and trifluoroacetic acid (v / v, 2:1) was used as the solvent.

[0058] Molecular weight testing procedure: Number average molecular weight was measured using a PL-GPC 220 instrument. For polyester raw materials and their recycled products, hexafluoroisopropanol was used as the mobile phase at a flow rate of 1.0 mL / min and a test temperature of 40℃. The sample was calibrated using a monodisperse polymethyl methacrylate standard. For the recycled copolymer, chloroform was used as the solvent at a flow rate of 1.0 mL / min and a test temperature of 25℃. The sample was calibrated using a monodisperse polystyrene standard.

[0059] Example 1 S1. 18.00 g of polyethylene terephthalate (PET), 19.12 g of propylene carbonate (PC), and 43.54 g of 1,6-hexanediamine (HMDA) were added to a 250 mL reactor. The molar ratio of repeating units of HMDA, PC, and PET was 1:2:4. An inert argon gas flow was introduced for oxidation protection, and the mixture was heated to 260 °C under normal pressure and stirring for a chain exchange reaction for 3 h to obtain the prepolymer. The number average molecular weight of this precursor was determined to be 7.4 kDa.

[0060] S2. The prepolymer obtained in step S1 is vacuumed and depressurized to 100 Pa in a reactor, and polycondensation reaction is carried out under the conditions of 280℃ and 120 r / min to remove low-boiling-point small molecules. The reaction is carried out for 4 h to obtain the regenerated copolymer.

[0061] Testing revealed that the number-average molecular weight of the obtained recycled polymer was 21.3 kDa, compared to the raw materials HMDA, PET, and PC, and the prepolymer ( Figure 1 The test solvent was deuterated trifluoroacetic acid) and the product ( Figure 2 The 1H NMR spectrum of the product (using deuterated trifluoroacetic acid as the test solvent) showed a significant disappearance of the NMR peaks at the ethylene glycol unit (4.82 ppm) in the original PET and the propylene glycol unit (4.88, 4.58, 4.04 ppm) in the PC. Meanwhile, the chemical shift values ​​of HMDA fixed by the terephthalic acid unit and carbonate unit showed a significant shift (3.81 ppm, 3.70 ppm, 3.40 ppm, 3.32 ppm). The 1C NMR spectrum of the product showed a distinct urea peak at 159.09 ppm, successfully demonstrating the chain exchange reaction and the fixation of carbon dioxide.

[0062] Example 2 S1. In a 250 mL reactor, 16.26 g of polyethylene terephthalate (PET), 17.29 g of propylene carbonate (PC), and 40 g of 1,6-hexanediol (HDO) were added, with the molar ratio of repeating units of HDO, PC, and PET being 1:2:4. Then, 0.036 g of antimony glycol was added, and an inert argon gas flow was introduced for oxidation protection. The mixture was heated to 260 °C under normal pressure and stirring for a chain exchange reaction for 3 hours to obtain the prepolymer. The number average molecular weight of this precursor was determined to be 5.2 kDa.

[0063] S2. The prepolymer obtained in step S1 is vacuumed and depressurized to 100 Pa in a reactor, and polycondensation reaction is carried out at a temperature of 240℃ and a rotation speed of 120 r / min to remove low-boiling-point small molecules. The reaction lasts for 4 hours to obtain a regenerated copolymer.

[0064] Testing revealed that the number-average molecular weight of the obtained recycled polymer was 18.1 kDa. This was compared to the raw materials HDO, PET, and PC, and the prepolymer (…). Figure 3 The test solvent was deuterated chloroform) and the product ( Figure 4 The 1H NMR spectrum of the product (using deuterated chloroform as the test solvent) showed that the NMR peaks at the ethylene glycol unit (4.82 ppm) in the original PET and the propylene glycol unit (4.88, 4.58, 4.04 ppm) in the PC were significantly lost, while the chemical shift of HDO fixed by the terephthalic acid unit and carbonate unit was significantly shifted and multiple peaks appeared (4.37 ppm, 4.15 ppm, 3.77 ppm, 3.66 ppm, 3.54 ppm, 3.48 ppm). The 1C NMR spectrum of the product showed a distinct carbonate peak at 155.35 ppm, successfully proving that the chain exchange reaction took place and carbon dioxide was fixed.

[0065] Example 3 S1. In a 250 mL reactor, 24.44 g of polybutylene terephthalate (PBT), 22.66 g of propylene carbonate (PC), and 40 g of 1,4-butanediol (BDO) were added, with the molar ratio of repeating units of BDO, PBT, and PC being 1:2:4. Then, 0.036 g of antimony glycol was added, and an inert argon gas flow was introduced for oxidation protection. The mixture was heated to 240 °C under normal pressure and stirring for a chain exchange reaction for 3 hours to obtain the prepolymer. The number average molecular weight of this precursor was determined to be 6.6 kDa.

[0066] S2. The prepolymer obtained in step S1 is subjected to vacuum decompression to 100 Pa in a reactor, and a polycondensation reaction is carried out at a temperature of 240℃ and a rotation speed of 120 r / min to remove low-boiling-point small molecules. This reaction lasts for 4 hours to obtain a regenerated copolymer. The number average molecular weight of the obtained regenerated polymer is 19.8 kDa.

[0067] Example 4 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 1, except that 2-imidazolidineone is used instead of propylene carbonate in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 31.8 kDa.

[0068] Example 5 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that ethylene carbonate is used instead of propylene carbonate in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 26.3 kDa.

[0069] Example 6 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 1, except that 2-oxazolidinone is used instead of propylene carbonate in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 27.9 kDa.

[0070] Example 7 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that 1,8-octanediamine is used instead of 1,6-hexanediamine in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 34.6 kDa.

[0071] Example 8 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that 1,8-octanediol is used instead of 1,6-hexanediol in Example 2. The number-average molecular weight of the obtained recycled polymer was measured to be 27.2 kDa.

[0072] Example 9 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that 1,10-decanediol is used instead of 1,6-hexanediol in Example 2. The number-average molecular weight of the obtained recycled polymer was measured to be 19.5 kDa.

[0073] Example 10 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that polypropylene terephthalate (PTT) is used instead of polypropylene terephthalate (PET) in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 23.5 kDa.

[0074] Example 11 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that: in this embodiment, copolyoxymethylene (CPOM) is used instead of polypropylene terephthalate (PET) in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 25.3 kDa.

[0075] Example 12 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that bisphenol A polycarbonate (BPA-PC) is used instead of polypropylene terephthalate (PET) in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 17.4 kDa.

[0076] Example 13 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that polyamide 66 (PA66) is used instead of polypropylene terephthalate (PET) in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 29.1 kDa.

[0077] Example 14 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that thermoplastic polyurethane elastomer (TPU) is used instead of polypropylene terephthalate (PET) in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 19.6 kDa.

[0078] Example 15 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that stannous chloride is used instead of antimony glycolate in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 24.9 kDa.

[0079] Example 16 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this embodiment is basically the same as that in Example 2, except that tetrabutyl titanate is used instead of antimony glycolate in Example 1. The number-average molecular weight of the obtained recycled polymer was measured to be 22.4 kDa.

[0080] Comparative Example 1 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this comparative example is basically the same as that in Example 1, except that: in this example, flowing carbon dioxide is used to replace propylene carbonate (PC) in Example 1.

[0081] The number-average molecular weight of the obtained recycled polymer was found to be 6.9 kDa. Due to the inert structure of carbon dioxide, it is difficult for it to undergo exchange reactions with waste heterochain polymers, long-chain diamines, and alcohols. (Comparative Example 1) Figure 2 ), carbon NMR spectrum of the product ( Figure 5 The absence of a peak for urea-carbon in approximately 159.09 ppm indicates that direct introduction of carbon dioxide cannot effectively fix it, and it must be converted into more reactive cyclic urea, cyclic carbonate, or cyclic carbamate. In addition, excess long-chain diamines that cannot react with carbon dioxide cannot be effectively removed from the reaction system, thus hindering the increase in molecular weight and causing a significant decrease in the molecular weight of the waste heterochain polymer.

[0082] Comparative Example 2 The method for fixing carbon dioxide using waste heterochain polymers disclosed in this comparative example is basically the same as that in Example 2, except that the molar ratio of repeating units of PET, PC, and HDO in this example is 1:4:2 instead of 1:2:4 in Example 2.

[0083] The number-average molecular weight of the obtained recycled polymer was tested to be 18.4 kDa, which is consistent with that of Example 2 ( Figure 4 Similarly, the HDO chemical shift values ​​fixed by terephthalic acid units and carbonate units showed significant shifts and multiple peaks (4.55 ppm, 4.17 ppm, 4.15 ppm, 3.68 ppm, 3.55 ppm); the product's carbon NMR spectrum showed a distinct carbonate peak at 161.25 ppm, successfully proving the chain exchange reaction and fixing carbon dioxide. However, due to the insufficient content of long-chain diols, it was difficult for them to fully exchange with cyclic carbonates, resulting in a significant decrease in the carbon dioxide content fixed by the product. Figure 6 ).

[0084] Based on the above embodiments and comparative examples, it can be seen that the recycling method of the present invention, compared with the traditional recycling methods for waste heterochain polymers, achieves synergistic carbon dioxide fixation and upgraded recycling of waste heterochain polymers. Furthermore, the recycled polymer products prepared by the present invention possess certain advantages. Overall, compared with the prior art, the recycling method of the present invention has the following advantages: synergistic carbon dioxide fixation; chemically selective recycling of different types of polymers; overcoming the environmental and product degradation problems caused by traditional physical and chemical recycling methods; adjusting the performance of the final product by controlling the types of reactions; and the method is simple, controllable, and conforms to the principles of green chemistry.

[0085] The embodiments provided by the present invention have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of the present invention, and the descriptions of the embodiments above are only for the purpose of helping to understand the core ideas of the present invention. It should be noted that those skilled in the art can make several improvements and modifications to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

Claims

1. A method for fixing carbon dioxide from waste heterochain polymers, characterized in that, Includes the following steps: S1. Mix heterocyclic compounds, long-chain organic compounds and heterochain polymers, and carry out an exchange and recombination reaction at 150-300℃ to obtain a prepolymer. The heterocyclic compounds refer to heterocyclic organic compounds derived from carbon dioxide that contain a carbonyl group and at least one nitrogen or oxygen heteroatom. The long-chain organic compounds have a main chain carbon number ≥ 4, including one or both of long-chain diamines and long-chain diols. S2. The prepolymer is reacted at 150–300°C and 1–1000 Pa absolute pressure to remove short-chain byproducts and obtain a recycled copolymer.

2. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, Heterocyclic compounds include one or more of cyclic ureas, cyclic carbonates, and cyclic carbamates.

3. The method for fixing carbon dioxide from waste heterochain polymers according to claim 2, characterized in that, The structures of heterocyclic compounds are shown in formulas (I) to (II): Equation (I): ; Equation (II): ; Where X1 and X2 are respectively -N(R 11 - or -O-; R1~R 11 They are independent of each other and are all hydrogen or alkyl groups.

4. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, The general structural formula of long-chain organic compounds is as follows (III): Equation (III): , where Y = -NH- or -O-, p ≥ 2.

5. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, Heterochain polymers include one or more of polyesters, polyethers, polycarbonates, polyamides, and polyurethanes.

6. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, The general formula for repeating unit structures of heterochain polymers includes the following formula (IV). (VIII) or one or more: Formula (IV): ; Equation (V): ; Formula (VI): ; Equation (VII): Formula (VIII): ; Among them, R 12 ~R 21 They are independent of each other and are all aromatic or aliphatic chains.

7. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, A catalyst is used in steps S1 and S2, wherein the catalyst is one or more of an alkoxide, halide, oxide, hydroxide, or carboxylate containing antimony, tin, titanium, scandium, iron, cobalt, nickel, zinc, magnesium, manganese, and cadmium.

8. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, In step S1, the mass of the catalyst accounts for 0.05 to 1% of the mass of the reactants.

9. The method for fixing carbon dioxide from waste heterochain polymers according to claim 1, characterized in that, In step S1, the molar ratio of heterocyclic compound to long-chain organic compound is 1:(0.1-10), and the molar ratio of heterochain polymer to heterocyclic compound is 1:(0.1-10).

10. A recycled polymer, characterized in that, It is prepared by the method for fixing carbon dioxide using waste heterochain polymers as described in any one of claims 1-9.