High-temperature-resistant polyimide material and preparation method thereof
By introducing a staged dissociation mechanism of zinc-carboxylic acid coordination structure into polyimide materials, a composite network of covalent crosslinking and hydrogen bonding crosslinking is constructed, which solves the problems of brittleness and insufficient heat resistance of traditional polyimide materials, and achieves a balance between high heat resistance and flexibility, making it suitable for large-scale production.
Patent Information
- Application Number
- CN202611669173.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing polyimide materials have shortcomings in terms of heat resistance, mechanical properties and processing flowability. In particular, traditional cross-linked networks are brittle and prone to network defects. Furthermore, the preparation process is energy-intensive and uneven, making it difficult to achieve both high heat resistance and good toughness.
By introducing zinc-coordinated diamine monomers, the zinc-carboxylic acid coordination structure is dissociated in stages during gradient heating to achieve low-temperature catalytic imidization and high-temperature crosslinking, thus constructing a composite network that is synergistically enhanced by covalent crosslinking and hydrogen bonding crosslinking, avoiding the defects of long-term high-temperature treatment and phase separation.
It significantly improves the heat resistance and mechanical properties of the material, maintains its flexibility, and reduces the energy consumption and cost of preparation, making it suitable for large-scale applications.
Smart Images

Figure CN123152108A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology and relates to a high-temperature resistant polyimide material and its preparation method. Background Technology
[0002] Currently, the main technical routes for improving the heat resistance of polyimide (PI) include introducing rigid aromatic structures, constructing chemical crosslinking networks, and introducing metal coordination crosslinking. However, each of these routes has its limitations: the introduction of rigid structures often impairs the solubility and processing fluidity of the material; the introduction of metal ions in metal coordination crosslinking is mostly carried out through physical blending or post-treatment impregnation, which makes it difficult to achieve uniform molecular-level dispersion in the matrix, easily leading to phase separation, agglomeration, and interface defects. Moreover, the metal sites are far from the polymerization reaction region, making it difficult to form an effective synergy with the polycondensation or crosslinking process.
[0003] At the preparation process level, existing technologies still have the following problems: complete thermal imidization of polyamic acid usually requires multiple stages of long-term high-temperature treatment, which is energy-intensive and easily causes thermal degradation of the main chain and yellowing of the film, resulting in deterioration of mechanical properties; the cyclization trimerization of phthalonitrile groups depends on the addition of small molecule curing agents or metal salt catalysts containing active hydrogen. Small molecule curing agents are prone to volatilization at high temperatures, resulting in incomplete crosslinking and compositional inaccuracies. Metal salt catalysts are difficult to distribute uniformly in the matrix, affecting the uniformity of performance; in addition, highly covalent single crosslinked networks lack effective stress dissipation mechanisms, the material is brittle, and micropores and network defects are easily formed during the curing process, making it difficult to achieve both high heat resistance and good toughness.
[0004] Therefore, there is an urgent need to develop a high heat-resistant polyimide material that does not require external catalysts and curing agents, can be imidized under relatively mild conditions, has a uniform and dense cross-linked network, and also has toughness and buffering capacity. Summary of the Invention
[0005] In view of the problems existing in the prior art, the present invention provides a high-temperature resistant polyimide material and its preparation method. By copolymerizing zinc-coordinated diamine monomers into the polyimide backbone, the zinc-carboxylic acid coordination structure is gradually dissociated in stages during the gradient heating process to achieve the time-sequential synergistic function of "low-temperature catalytic imidization - high-temperature catalytic cyano crosslinking - cooling to form hydrogen bond compensation". Finally, a composite network with synergistic enhancement of covalent crosslinking and hydrogen bond crosslinking is constructed, which significantly improves the heat resistance of the material while maintaining excellent mechanical flexibility and processing controllability.
[0006] To achieve the above and other objectives, the technical solution adopted by the present invention is as follows:
[0007] This invention provides a high-temperature resistant polyimide material comprising the following raw materials in parts by weight: 50-60 parts of aromatic tetracarboxylic dianhydride, 20-30 parts of a first aromatic diamine, 5-12 parts of a zinc-containing coordinated diamine monomer, and 400-570 parts of a polar aprotic solvent; wherein the ratio of the total molar amount of amino groups of the first aromatic diamine and the zinc-containing coordinated diamine monomer to the molar amount of aromatic tetracarboxylic dianhydride is 1:0.98-1.02.
[0008] Furthermore, the aromatic tetracarboxylic dianhydride is selected from one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-oxobisphthalic anhydride, and pyromellitic dianhydride, preferably 3,3',4,4'-benzophenone tetracarboxylic dianhydride.
[0009] Furthermore, the first aromatic diamine is selected from either 4,4'-diaminodiphenyl sulfone or 4,4'-diaminodiphenyl ether, preferably 4,4'-diaminodiphenyl sulfone.
[0010] Furthermore, the polar aprotic solvent is N-methylpyrrolidone.
[0011] Further, the zinc-containing coordinating diamine monomer is a 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, which is prepared by:
[0012] (1) Intermediate synthesis: In a dry three-necked flask, 4-nitrophthalonitrile and 3,5-dinitro-4-hydroxybenzoic acid were dissolved in anhydrous N,N-dimethylformamide. Then, anhydrous potassium carbonate was added as a catalyst and acid-binding agent. The molar amount of anhydrous potassium carbonate was 2.5-3.5 times that of 3,5-dinitro-4-hydroxybenzoic acid, and the molar ratio of 4-nitrophthalonitrile to 3,5-dinitro-4-hydroxybenzoic acid was 1:1.05-1.10. The temperature was raised to 60-80℃ and the reaction was carried out for 6-8 hours. After the reaction was completed, the reaction solution was slowly poured into ice water to precipitate the precipitate. After filtration, the precipitate was washed successively with deionized water and anhydrous ethanol, and dried under vacuum to obtain the intermediate 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid, the structural formula of which is shown below: ;
[0013] (2) Reduction: The 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid intermediate obtained in step (1) is dissolved in anhydrous ethanol, and then palladium on carbon catalyst is added to it. The mass ratio of intermediate to catalyst is 1:0.05-0.1. Hydrogen gas is introduced and the flow rate of hydrogen gas is maintained at a continuous bubbling state below the liquid surface. Catalytic hydrogenation reduction is carried out at room temperature and pressure for 4-6 hours. The catalyst is removed by filtration, the solvent is removed by vacuum distillation, and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid is obtained by recrystallization with ethanol-water.
[0014] (3) Coordination reaction: Dissolve the 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid obtained in step (2) in a mixed solvent of ethanol and water with a volume ratio of 3:1 to obtain mixed solution a, and heat to 50-60℃; separately dissolve zinc acetate in an equal volume of ethanol-water mixed solvent to prepare solution b, and then slowly add solution b to mixed solution a, wherein the molar ratio of 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid to zinc acetate is 2:1, reflux reaction for 4-6 hours, after which cool, filter, wash three times with anhydrous ethanol, and vacuum dry to obtain 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, that is, zinc-containing coordinated diamine monomer.
[0015] This invention also provides a method for preparing a high-temperature resistant polyimide material, comprising the following steps:
[0016] S1. Preparation of prepolymer solution: Under nitrogen protection and drying conditions, the first aromatic diamine and the zinc-coordinated diamine monomer are dissolved in a polar aprotic solvent and cooled to 0-10℃. Aromatic tetracarboxylic dianhydride is added in three equal molar amounts, with an interval of 15 minutes between each batch. The system temperature is controlled not to exceed 10℃. After stirring for 2-4 hours, the temperature is raised to 20-30℃ and the reaction continues for another 2-4 hours to obtain a polyamic acid prepolymer solution with phthalonitrile groups in the side chain and zinc-carboxylic acid coordination structure in the molecular chain. In this step, the primary amino group of the zinc-coordinated diamine monomer undergoes a ring-opening addition reaction with the anhydride group in the aromatic tetracarboxylic dianhydride to generate amic acid bonds, so that the zinc-carboxylic acid coordination structure is chemically bonded into the polyimide molecular chain.
[0017] S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution obtained in step S1 is uniformly cast and coated onto a clean glass substrate, and dried at 80-100℃ for 1-2 hours to remove most of the solvent, thereby obtaining a polyamic acid solid gel film with self-supporting properties.
[0018] S3. Thermal imidization: The polyamic acid solid gel film obtained in step S2 is subjected to gradient heat treatment in an inert atmosphere: the temperature is raised to 140-160℃ at a heating rate of 1-3℃ / min for 1-2 hours, then raised to 220-240℃ at the same heating rate for 1 hour, and finally raised to 270-300℃ for 0.5-1 hour. During this stage, the zinc-carboxylic acid coordination structure is partially dissociated by heat, and the released zinc ions act as Lewis acid to coordinate with the carbonyl oxygen of the amic acid, enhancing the positive charge of the carbonyl carbon and promoting the intramolecular dehydration cyclization of the amic acid unit, thus completing the conversion of polyamic acid to polyimide and obtaining a polyimide film with some undissociated zinc-carboxylic acid coordination structure and phthalonitrile groups in the side chain.
[0019] S4. Curing and Crosslinking: The polyimide film treated in step S3 is further heated to 330-370°C in an inert atmosphere at a heating rate of 1-2°C / min and held for 1-4 hours. At this high temperature, the residual zinc-carboxylic acid coordination structure is completely dissociated, and the released zinc ions coordinate with the cyano nitrogen atom of the phthalonitrile side chain, activating the C≡N triple bond and promoting intermolecular nucleophilic addition of adjacent cyano groups. Through cyclization trimerization, a triazine ring crosslinking structure is generated, forming a covalent crosslinking network. At the same time, the exposed carboxyl groups of the side chain after the coordination bond dissociation form intermolecular hydrogen bonds with the nitrogen atom of the triazine ring and the oxygen atom of the imine carbonyl group of the main chain during the cooling process, filling the network vacancies left by the broken coordination bonds, and finally forming a composite network with synergistic reinforcement of "covalent crosslinking-hydrogen bond crosslinking". After the process is completed, it is cooled to room temperature to obtain the high-temperature resistant polyimide material.
[0020] Furthermore, the inert atmosphere is high-purity nitrogen or high-purity argon.
[0021] Compared with the prior art, the beneficial effects of the present invention are:
[0022] This invention designs a zinc-containing coordinating diamine monomer to partially replace conventional aromatic diamines in polycondensation. Utilizing the ring-opening addition reaction between the free primary amine and dianhydride, the zinc-carboxylic acid coordination structure is covalently anchored to the polyimide molecular chain, effectively avoiding phase separation and agglomeration defects that easily occur when physically mixing metal salts or crosslinking aids. Furthermore, this coordination structure exhibits controlled hierarchical dissociation behavior during gradient heating—partial dissociation during the thermal imidization stage, releasing in situ zinc ions with Lewis acid activity, thereby lowering the activation energy barrier for amide acid dehydration and cyclization through coordination. This promotes the imidization reaction to be completed under milder conditions; the residual coordination structure completely dissociates at higher temperatures, and the released zinc ions once again play a catalytic role, activating the phthalonitrile groups of the side chain to undergo cyclization trimerization and constructing a uniform covalent crosslinking network; the carboxyl groups of the side chain exposed in situ after the coordination bonds dissociate spontaneously form intermolecular hydrogen bonds with the nitrogen atoms of the triazine ring and the carbonyl oxygen atoms of the main chain during cooling, thereby filling and reconstructing the micropores and vacancies in the covalent network in situ, solving the problem that the traditional polyimide crosslinking system relies solely on the covalent bond network, is brittle, and is prone to network defects.
[0023] Thanks to the above design, the polyimide material of this invention achieves significant improvements in heat resistance, mechanical properties, and process adaptability. Firstly, regarding heat resistance, the hierarchical catalytic effect of zinc ions enables the imidization reaction to be completed efficiently at lower temperatures, avoiding the thermal degradation of the main chain caused by prolonged high-temperature treatment. The triazine ring covalent crosslinking network formed during the high-temperature stage significantly increases the glass transition temperature and thermal decomposition temperature of the material, endowing it with excellent heat resistance. Secondly, regarding mechanical properties, the hydrogen bond network significantly enhances the material's structural density by filling gaps and repairing defects in the covalent crosslinking network. Furthermore, the reversible destruction-reconstruction characteristics of hydrogen bonds effectively dissipate applied stress, giving the highly crosslinked rigid network good flexibility, overcoming the inherent brittleness of traditional highly crosslinked resins. In addition, the synthetic route of the zinc-coordinated diamine monomer of this invention uses commercially available reagents, and the reaction conditions are mild. The entire process of molding-imidization-curing is highly compatible with existing polyimide processing technologies, requiring no additional specialized equipment. The overall preparation cost is low, making it suitable for large-scale preparation and application. Attached Figure Description
[0024] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below.
[0025] Figure 1 This is a process flow diagram for preparing high-temperature resistant polyimide materials according to an embodiment of the present invention. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this application.
[0028] Unless otherwise specified, all materials used in the following examples are new materials purchased from the market. The preparation process of the high-temperature resistant polyimide material in the examples is as follows: Figure 1 As shown.
[0029] Example 1
[0030] This embodiment provides a high-temperature resistant polyimide material, prepared from the following raw materials in parts by weight: 50 parts of aromatic tetracarboxylic dianhydride, 20 parts of a first aromatic diamine, 5 parts of a zinc-containing coordinated diamine monomer, and 400 parts of a polar aprotic solvent; wherein, the aromatic tetracarboxylic dianhydride is selected from 3,3',4,4'-benzophenone tetracarboxylic dianhydride, the first aromatic diamine is selected from 4,4'-diaminodiphenyl sulfone, and the polar aprotic solvent is selected from N-methylpyrrolidone; the molar ratio of the aromatic tetracarboxylic dianhydride to the total amino molar ratio of the first aromatic diamine and the zinc-containing coordinated diamine monomer is 0.98:1.
[0031] The zinc-containing coordinated diamine monomer is a 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, and its preparation method is as follows:
[0032] (1) Synthesis of intermediate: In a dry three-necked flask, 4-nitrophthalonitrile and 3,5-dinitro-4-hydroxybenzoic acid were dissolved in anhydrous N,N-dimethylformamide. Then anhydrous potassium carbonate was added as a catalyst and acid-binding agent. The molar amount of anhydrous potassium carbonate was 2.5 times that of 3,5-dinitro-4-hydroxybenzoic acid. The molar ratio of 4-nitrophthalonitrile to 3,5-dinitro-4-hydroxybenzoic acid was 1:1.05. The temperature was raised to 60℃ and the reaction was carried out for 6 hours. After the reaction was completed, the reaction solution was slowly poured into ice water to precipitate the precipitate. After filtration, the precipitate was washed with deionized water and anhydrous ethanol in sequence and dried under vacuum to obtain 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid intermediate.
[0033] (2) Reduction: The 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid intermediate obtained in step (1) was dissolved in anhydrous ethanol, and then palladium on carbon catalyst was added to it. The mass ratio of intermediate to catalyst was 1:0.05. Hydrogen gas was introduced and the flow rate of hydrogen gas was maintained at a continuous bubbling state below the liquid surface. Catalytic hydrogenation reduction was carried out at room temperature and pressure for 4 hours. The catalyst was removed by filtration, the solvent was removed by vacuum distillation, and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid was obtained by recrystallization with ethanol-water.
[0034] (3) Coordination reaction: Dissolve the 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid obtained in step (2) in a mixed solvent of ethanol and water with a volume ratio of 3:1 to obtain mixed solution a, and heat to 50°C; separately dissolve zinc acetate in an equal volume of ethanol-water mixed solvent to prepare solution b, and then slowly add solution b to mixed solution a, wherein the molar ratio of 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid to zinc acetate is 2:1, reflux reaction for 4 hours, after which cool, filter, wash three times with anhydrous ethanol, and vacuum dry to obtain 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, that is, zinc-containing coordinated diamine monomer.
[0035] This embodiment also provides a method for preparing a high-temperature resistant polyimide material, including the following steps:
[0036] S1. Preparation of prepolymer solution: Under nitrogen protection and drying conditions, the 4,4'-diaminodiphenyl sulfone and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex were dissolved in N-methylpyrrolidone and cooled to 0°C. 3,3',4,4'-benzophenone tetracarboxylic dianhydride was added in three equal molar amounts, with an interval of 15 minutes between each batch. The system temperature was controlled to not exceed 10°C. After stirring for 2 hours, the temperature was raised to 20°C and the reaction was continued for another 2 hours to obtain a polyamic acid prepolymer solution with phthalonitrile groups in the side chain and zinc-carboxylic acid coordination structure in the molecular chain.
[0037] S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution obtained in step S1 is uniformly cast and coated onto a clean glass substrate, and dried at 80°C for 1 hour to remove most of the solvent, resulting in a polyamic acid solid gel film with self-supporting properties.
[0038] S3. Thermal imidization: The polyamic acid solid gel film obtained in step S2 is subjected to gradient heat treatment in a high-purity nitrogen atmosphere (≥99.999%): the temperature is increased to 140℃ at a heating rate of 1℃ / min for 1 hour, then increased to 220℃ at the same heating rate for 1 hour, and finally increased to 270℃ for 0.5 hours to obtain a polyimide film with some undissociated zinc-carboxylic acid coordination structure and phthalonitrile groups in the side chain;
[0039] S4. Curing and crosslinking: The polyimide film treated in step S3 is further heated to 330°C in a high-purity nitrogen atmosphere at a heating rate of 1°C / min, held at that temperature for 1 hour, and then cooled to room temperature to obtain the high-temperature resistant polyimide material.
[0040] Example 2
[0041] This embodiment provides a high-temperature resistant polyimide material, prepared from the following raw materials in parts by weight: 55 parts of aromatic tetracarboxylic dianhydride, 25 parts of a first aromatic diamine, 8 parts of a zinc-containing coordinated diamine monomer, and 500 parts of a polar aprotic solvent; wherein, the aromatic tetracarboxylic dianhydride is selected from 3,3',4,4'-benzophenone tetracarboxylic dianhydride, the first aromatic diamine is selected from 4,4'-diaminodiphenyl ether, and the polar aprotic solvent is selected from N-methylpyrrolidone; the molar ratio of the aromatic tetracarboxylic dianhydride to the total amino molar ratio of the first aromatic diamine and the zinc-containing coordinated diamine monomer is 1:1.
[0042] The preparation method of the zinc-containing coordinated diamine monomer is the same as that in Example 1, except that: in step (1), the molar amount of anhydrous potassium carbonate is 3.0 times that of 3,5-dinitro-4-hydroxybenzoic acid, the molar ratio of 4-nitrophthalonitrile to 3,5-dinitro-4-hydroxybenzoic acid is 1:1.075, and the temperature is raised to 70°C and reacted for 7 hours; in step (2), the mass ratio of intermediate to catalyst is 1:0.075, and the catalytic hydrogenation reduction is carried out for 5 hours; in step (3), the mixed solution a is heated to 55°C and refluxed for 5 hours.
[0043] This embodiment also provides a method for preparing a high-temperature resistant polyimide material, including the following steps:
[0044] S1. Preparation of prepolymer solution: Under nitrogen protection and drying conditions, 4,4'-diaminodiphenyl ether and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex were dissolved in N-methylpyrrolidone and cooled to 5°C. 3,3',4,4'-benzophenone tetracarboxylic dianhydride was added in three equal molar amounts, with an interval of 15 minutes between each batch. The system temperature was controlled to not exceed 10°C. After stirring for 3 hours, the temperature was raised to 25°C and the reaction was continued for another 3 hours to obtain a polyamic acid prepolymer solution with phthalonitrile groups in the side chain and zinc-carboxylic acid coordination structure in the molecular chain.
[0045] S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution obtained in step S1 is uniformly cast and coated onto a clean glass substrate, and dried at 90°C for 1.5 hours to remove most of the solvent, thereby obtaining a polyamic acid solid gel film with self-supporting properties.
[0046] S3. Thermal imidization: The polyamic acid solid gel film obtained in step S2 is subjected to gradient heat treatment in a high-purity nitrogen atmosphere: the temperature is raised to 150℃ at a heating rate of 2℃ / min for 1.5 hours, then raised to 230℃ at the same heating rate for 1 hour, and finally raised to 285℃ for 0.75 hours to obtain a polyimide film with some undissociated zinc-carboxylic acid coordination structure and phthalonitrile groups in the side chain;
[0047] S4. Curing and crosslinking: The polyimide film treated in step S3 is further heated to 350°C in a high-purity nitrogen atmosphere at a heating rate of 1.5°C / min, and held at that temperature for 2.5 hours. After the process is completed, it is cooled to room temperature to obtain the high-temperature resistant polyimide material.
[0048] Example 3
[0049] This embodiment provides a high-temperature resistant polyimide material, prepared from the following raw materials in parts by weight: 60 parts of aromatic tetracarboxylic dianhydride, 30 parts of a first aromatic diamine, 12 parts of a zinc-containing coordinated diamine monomer, and 570 parts of a polar aprotic solvent; wherein, the aromatic tetracarboxylic dianhydride is selected from 3,3',4,4'-benzophenone tetracarboxylic dianhydride, the first aromatic diamine is selected from 4,4'-diaminodiphenyl sulfone, and the polar aprotic solvent is selected from N-methylpyrrolidone; the molar ratio of the aromatic tetracarboxylic dianhydride to the total amino molar ratio of the first aromatic diamine and the zinc-containing coordinated diamine monomer is 1.02:1.
[0050] The preparation method of the zinc-containing coordinated diamine monomer is the same as that in Example 1, except that: in step (1), the molar amount of anhydrous potassium carbonate is 3.5 times that of 3,5-dinitro-4-hydroxybenzoic acid, the molar ratio of 4-nitrophthalonitrile to 3,5-dinitro-4-hydroxybenzoic acid is 1:1.10, and the temperature is raised to 80°C and the reaction is carried out for 8 hours; in step (2), the mass ratio of intermediate to catalyst is 1:0.1, and the catalytic hydrogenation reduction is carried out for 6 hours; in step (3), the mixed solution a is heated to 60°C and refluxed for 6 hours.
[0051] This embodiment also provides a method for preparing a high-temperature resistant polyimide material, including the following steps:
[0052] S1. Preparation of prepolymer solution: Under nitrogen protection and drying conditions, the 4,4'-diaminodiphenyl sulfone and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex were dissolved in N-methylpyrrolidone and cooled to 10°C. 3,3',4,4'-benzophenone tetracarboxylic dianhydride was added in three equal molar amounts, with an interval of 15 minutes between each batch. The system temperature was controlled to not exceed 10°C. After stirring for 4 hours, the temperature was raised to 30°C and the reaction was continued for another 4 hours to obtain a polyamic acid prepolymer solution with phthalonitrile groups in the side chain and zinc-carboxylic acid coordination structure in the molecular chain.
[0053] S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution obtained in step S1 is uniformly cast and coated onto a clean glass substrate, and dried at 100°C for 2 hours to remove most of the solvent, resulting in a polyamic acid solid gel film with self-supporting properties.
[0054] S3. Thermal imidization: The polyamic acid solid gel film obtained in step S2 is subjected to gradient heat treatment in a high-purity nitrogen atmosphere: the temperature is raised to 160℃ at a heating rate of 3℃ / min for 2 hours, then raised to 240℃ at the same heating rate for 1 hour, and finally raised to 300℃ for 1 hour to obtain a polyimide film with some undissociated zinc-carboxylic acid coordination structure and phthalonitrile groups in the side chain;
[0055] S4. Curing and crosslinking: The polyimide film treated in step S3 is further heated to 370°C in a high-purity nitrogen atmosphere at a heating rate of 2°C / min, and held at that temperature for 4 hours. After the process is completed, it is cooled to room temperature to obtain the high-temperature resistant polyimide material.
[0056] Example 4
[0057] This embodiment provides a high-temperature resistant polyimide material, prepared from the following raw materials in parts by weight: 52 parts of aromatic tetracarboxylic dianhydride, 22 parts of a first aromatic diamine, 6 parts of a zinc-containing coordinated diamine monomer, and 450 parts of a polar aprotic solvent; wherein, the aromatic tetracarboxylic dianhydride is selected from 3,3',4,4'-biphenyltetracarboxylic dianhydride, the first aromatic diamine is selected from 4,4'-diaminodiphenyl sulfone, and the polar aprotic solvent is selected from N-methylpyrrolidone; the molar ratio of the aromatic tetracarboxylic dianhydride to the total amino molar ratio of the first aromatic diamine and the zinc-containing coordinated diamine monomer is 0.99:1.
[0058] The zinc-containing coordinated diamine monomer is a 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, and its preparation method is the same as in Example 1.
[0059] This embodiment also provides a method for preparing a high-temperature resistant polyimide material, including the following steps:
[0060] S1. Preparation of prepolymer solution: Under nitrogen protection and drying conditions, the 4,4'-diaminodiphenyl sulfone and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex were dissolved in N-methylpyrrolidone and cooled to 3°C. 3,3',4,4'-biphenyltetracarboxylic dianhydride was added in three equal molar amounts, with an interval of 15 minutes between each batch. The system temperature was controlled to not exceed 10°C. After stirring for 2.5 hours, the temperature was raised to 22°C and the reaction was continued for 3 hours to obtain a polyamic acid prepolymer solution with phthalonitrile groups in the side chain and zinc-carboxylic acid coordination structure in the molecular chain.
[0061] S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution obtained in step S1 is uniformly cast and coated onto a clean glass substrate, and dried at 85°C for 1.2 hours to remove most of the solvent, thereby obtaining a polyamic acid solid gel film with self-supporting properties.
[0062] S3. Thermal imidization: The polyamic acid solid gel film obtained in step S2 is subjected to gradient heat treatment in a high-purity nitrogen atmosphere: the temperature is increased to 145℃ at a heating rate of 1.5℃ / min for 1.2 hours, then increased to 225℃ at the same heating rate for 1 hour, and finally increased to 280℃ for 0.6 hours to obtain a polyimide film with some undissociated zinc-carboxylic acid coordination structure and phthalonitrile groups in the side chain;
[0063] S4. Curing and crosslinking: The polyimide film treated in step S3 is further heated to 340°C in a high-purity nitrogen atmosphere at a heating rate of 1.5°C / min, and held at that temperature for 1.5 hours. After the process is completed, it is cooled to room temperature to obtain the high-temperature resistant polyimide material.
[0064] Example 5
[0065] This embodiment provides a high-temperature resistant polyimide material, prepared from the following raw materials in parts by weight: 58 parts of aromatic tetracarboxylic dianhydride, 28 parts of a first aromatic diamine, 10 parts of a zinc-containing coordinated diamine monomer, and 530 parts of a polar aprotic solvent; wherein, the aromatic tetracarboxylic dianhydride is selected from pyromellitic dianhydride, the first aromatic diamine is selected from 4,4'-diaminodiphenyl ether, and the polar aprotic solvent is selected from N-methylpyrrolidone; the molar ratio of the aromatic tetracarboxylic dianhydride to the total amino molar ratio of the first aromatic diamine and the zinc-containing coordinated diamine monomer is 1.01:1.
[0066] The zinc-containing coordinated diamine monomer is a 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, and its preparation method is the same as in Example 1.
[0067] This embodiment also provides a method for preparing a high-temperature resistant polyimide material, including the following steps:
[0068] S1. Preparation of prepolymer solution: Under nitrogen protection and drying conditions, 4,4'-diaminodiphenyl ether and 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex were dissolved in N-methylpyrrolidone and cooled to 8°C. Pyromellitic dianhydride was added in three equal molar amounts, with an interval of 15 minutes between each batch. The system temperature was controlled to not exceed 10°C. After stirring and reacting for 3.5 hours, the temperature was raised to 28°C and the reaction was continued for another 3.5 hours to obtain a polyamic acid prepolymer solution with phthalonitrile groups in the side chain and zinc-carboxylic acid coordination structure in the molecular chain.
[0069] S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution obtained in step S1 is uniformly cast and coated onto a clean glass substrate, and dried at 95°C for 1.8 hours to remove most of the solvent, thereby obtaining a polyamic acid solid gel film with self-supporting properties.
[0070] S3. Thermal imidization: The polyamic acid solid gel film obtained in step S2 is subjected to gradient heat treatment in a high-purity nitrogen atmosphere: the temperature is raised to 155℃ at a heating rate of 2.5℃ / min for 1.8 hours, then raised to 235℃ at the same heating rate for 1 hour, and finally raised to 295℃ for 0.9 hours to obtain a polyimide film with some undissociated zinc-carboxylic acid coordination structure and phthalonitrile groups in the side chain;
[0071] S4. Curing and crosslinking: The polyimide film treated in step S3 is further heated to 360°C in a high-purity nitrogen atmosphere at a heating rate of 1.8°C / min, and held at that temperature for 3 hours. After the heating is completed, it is cooled to room temperature to obtain the high-temperature resistant polyimide material.
[0072] Comparative Example 1
[0073] The difference between this comparative example and Example 2 is that the raw materials do not contain zinc-coordinated diamine monomers, but are replaced with an equimolar amount of 4,4'-diaminodiphenyl sulfone, so that the system is obtained by polymerizing 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 4,4'-diaminodiphenyl sulfone to obtain conventional polyimide, without phthalonitrile side groups and zinc-carboxylic acid coordination structures; the remaining raw material ratios and preparation methods are the same as in Example 2.
[0074] Comparative Example 2
[0075] The difference between this comparative example and Example 2 is that the zinc-coordinated diamine monomer is replaced with 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid (i.e., it does not contain zinc coordination, but only retains the phthalonitrile side group and carboxyl group); the remaining raw material ratios and preparation methods are the same as in Example 2.
[0076] Comparative Example 3
[0077] The difference between this comparative example and Example 2 is that the thermal imidization treatment in step S3 is carried out without an inert atmosphere (i.e., heat treatment is carried out in an air atmosphere); the remaining raw material ratios and methods are the same as in Example 2.
[0078] Comparative Example 4
[0079] The difference between this comparative example and Example 2 is that the gradient heat treatment in step S3 is omitted, and the polyamic acid solid gel film is placed in a high-temperature environment of 350°C for 3 hours to directly complete imidization and curing crosslinking, skipping the segmented heating of 140–160°C, 220–240°C, and 270–300°C, so that the zinc-carboxylic acid coordination bond cannot be dissociated in stages and catalyze imidization and trimerization reactions respectively; the remaining raw material ratios and preparation methods are the same as in Example 2.
[0080] To verify the performance of the composite material of the present invention, the high-temperature resistant polyimide materials prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to the following tests:
[0081] Thermal stability test: A thermogravimetric analyzer was used under a nitrogen atmosphere (flow rate 100 mL / min) to raise the temperature from 30℃ to 800℃ at a rate of 10℃ / min. The mass change curve of the sample as a function of temperature was recorded. Test parameters included: 5% weight loss temperature (T0). 5% ), 10% weight loss temperature (T) 10%), 50% weight loss temperature (T) 50% The carbon residue at 800℃ was also measured. Each sample was tested in triplicate, and the average value was taken.
[0082] Differential scanning calorimetry (DSC): A DSC was used under a nitrogen atmosphere (flow rate 50 mL / min) to heat the sample from -50℃ to 420℃ at a rate of 10℃ / min. The second heating curve was used for data analysis. The glass transition temperature (Tg) was taken as the midpoint of the specific heat capacity jump in the heating curve. Each sample was tested in triplicate, and the average value was taken.
[0083] Mechanical property testing: Using a universal testing machine, according to ASTM D882 standard, a thin film sample with a thickness of about 20 μm was used, and the tensile rate was 5 mm / min to determine the tensile strength and elongation at break.
[0084] Dielectric performance testing: The dielectric constant and dielectric loss of the thin film were measured using an impedance analyzer (Agilent E4991A) at a frequency of 1MHz.
[0085] The test results are shown below:
[0086] Table 1 Thermal stability test results
[0087]
[0088] Table 2. Test results of glass transition temperature, mechanical properties and dielectric properties
[0089]
[0090] As shown in Table 1, the 5% thermogravimetric temperature (Tg) of Examples 1-3 all reached above 545℃, and the char residue at 800℃ all reached above 62%, significantly better than the comparative examples. This proves that the present invention, by introducing a zinc-carboxylic acid coordination structure and phthalonitrile side groups into the polyimide molecular chain, can form a highly cross-linked triazine ring network structure after gradient heat treatment. Simultaneously, zinc ions play a Lewis acid catalytic role in the thermal imidization stage, increasing the degree of imidization. The synergistic effect of these two factors significantly improves the heat resistance of the material. As shown in Table 2, the Tg of Examples 1-3 all reached above 358℃, significantly higher than the comparative examples, with Example 3 having the highest Tg (382℃). Furthermore, the tensile strength of Examples 1-3 all reached above 155 MPa, significantly better than the comparative examples; Comparative Example 4, due to the omission of gradient heat treatment, resulted in insufficient cross-linking reaction and network structure defects, leading to significantly lower mechanical properties than the example groups.
[0091] The dielectric performance test data show that the dielectric constant and dielectric loss of Examples 1-3 are all at relatively low levels. The dielectric constant and dielectric loss of Comparative Example 1 are higher than those of the Examples, which is related to the greater degree of freedom of molecular chain movement under its uncrosslinked structure. The dielectric constant and dielectric loss of Comparative Example 3 are the highest, because zinc ions in the air are oxidized into ZnO particles and dispersed in the matrix. The high dielectric constant of ZnO itself increases the overall dielectric constant of the composite system. At the same time, the polar end groups generated by thermal oxidation degradation increase the dipole relaxation loss, further deteriorating the dielectric performance.
[0092] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
[0093] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention. The actual application is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar methods and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.
Claims
1. A high-temperature resistant polyimide material, characterized in that, The raw materials include the following parts by weight: 50-60 parts of aromatic tetracarboxylic dianhydride, 20-30 parts of a first aromatic diamine, 5-12 parts of a zinc-containing coordinated diamine monomer, and 400-570 parts of a polar aprotic solvent; the ratio of the total molar amount of amino groups in the first aromatic diamine and the zinc-containing coordinated diamine monomer to the molar amount of aromatic tetracarboxylic dianhydride is 1:0.98-1.02; the preparation method of the polyimide material includes the following steps: S1. Preparation of prepolymer solution: Dissolve the first aromatic diamine and the zinc-containing coordinated diamine monomer in a polar aprotic solvent, cool, and then add aromatic tetracarboxylic dianhydride in batches. Stir the reaction and then heat up to continue the reaction to obtain a polyamic acid prepolymer solution. S2. Molding: After vacuum degassing, the polyamic acid prepolymer solution is uniformly cast and coated onto a glass substrate, and after drying, a polyamic acid solid gel film is obtained. S3. Thermal imidization: The polyamic acid solid gel film is subjected to gradient heat treatment to obtain a polyimide film; S4. Curing and crosslinking: The treated polyimide film is cured at high temperature and then cooled to room temperature to obtain the high-temperature resistant polyimide material.
2. The high-temperature resistant polyimide material according to claim 1, characterized in that, The aromatic tetracarboxylic dianhydride is selected from one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-oxobisphthalic anhydride, and pyromellitic dianhydride.
3. The high-temperature resistant polyimide material according to claim 1, characterized in that, The first aromatic diamine is selected from either 4,4'-diaminodiphenyl sulfone or 4,4'-diaminodiphenyl ether.
4. The high-temperature resistant polyimide material according to claim 1, characterized in that, The polar aprotic solvent is N-methylpyrrolidone.
5. The high-temperature resistant polyimide material according to claim 1, characterized in that, The zinc-containing coordinated diamine monomer is a 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, and its preparation method is as follows: (1) Synthesis of intermediate: 4-nitrophthalonitrile and 3,5-dinitro-4-hydroxybenzoic acid were dissolved in anhydrous N,N-dimethylformamide, and then anhydrous potassium carbonate was added to the solution for heating reaction. After the reaction was completed, a precipitate was formed, filtered, washed and dried to obtain 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid intermediate; (2) Reduction: The intermediate of 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid was dissolved in anhydrous ethanol, and then palladium on carbon catalyst was added to carry out catalytic hydrogenation reduction. After the reduction was completed, the mixture was filtered, distilled under reduced pressure, and recrystallized to obtain 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid. (3) Coordination reaction: Dissolve 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid in a mixed solvent of ethanol and water to obtain a mixed solution a and heat it; separately dissolve zinc acetate in a mixed solvent of ethanol and water to prepare solution b, and then slowly add solution b dropwise to mixed solution a for reflux reaction. After the reaction is completed, cool, filter, wash and dry to obtain 3,5-diamino-4-(3,4-dicyanophenoxy)benzoic acid-zinc complex, i.e. zinc-containing coordinated diamine monomer.
6. The high-temperature resistant polyimide material according to claim 5, characterized in that, The molar amount of anhydrous potassium carbonate is 2.5-3.5 times that of 3,5-dinitro-4-hydroxybenzoic acid; the molar ratio of 4-nitrophthalonitrile to 3,5-dinitro-4-hydroxybenzoic acid is 1:1.05-1.
10.
7. The high-temperature resistant polyimide material according to claim 5, characterized in that, The mass ratio of the 3,5-dinitro-4-(3,4-dicyanophenoxy)benzoic acid intermediate to the palladium on carbon catalyst is 1:0.05-0.
1.
8. The high-temperature resistant polyimide material according to claim 1, characterized in that, The gradient heat treatment in step S3 is as follows: first, heat to 140-160℃ for 1-2 hours, then heat to 220-240℃ for 1 hour, and finally heat to 270-300℃ for 0.5-1 hour.