A dispersion stabilizer for preparing a phenyl polysiloxane and a method for preparing a phenyl polysiloxane

By introducing a dispersant with a specific molecular structure into the diphenylsilanediol reaction system, the problem of self-polymerization of diphenylsilanediol was solved, realizing the efficient and simplified preparation of phenyl polysiloxanes, reducing costs and environmental pressures, and making it suitable for industrial production.

CN123152111APending Publication Date: 2026-11-24CHINA BLUESTAR CHENGRAND CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510670230.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the existing technology, when preparing phenyl polysiloxanes from diphenylsilanediol, self-polymerization easily occurs in the reaction system, leading to an increase in system viscosity and making it difficult to achieve industrial production. Furthermore, traditional methods require multiple reaction steps or the use of solvents, resulting in increased environmental pressure and costs.

Method used

By introducing a dispersant with a specific molecular structure into the diphenylsilanediol reaction system and controlling the amounts of the dispersant and diphenylsilanediol, a uniform and stable reaction precursor is formed, enabling one-pot reaction preparation of phenyl polysiloxanes, avoiding self-polymerization and reducing solvent usage.

Benefits of technology

It achieves an efficient and simplified preparation process, reduces costs, is suitable for industrial production, reduces environmental pressure, and has a wide range of product performance indicators, making it suitable for diverse applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

This invention discloses a dispersant and stabilizer suitable for preparing phenyl polysiloxanes and a method for preparing phenyl polysiloxanes, belonging to the field of organosilicon material technology. It is applicable to the process of preparing phenyl polysiloxanes from diphenylsilanediol as a raw material. By introducing a dispersant and stabilizer with a specific molecular structure into the reaction precursor of diphenylsilanediol, the problem of easy self-polymerization of diphenylsilanediol in the reaction system when preparing phenyl polysiloxanes with diphenyl donor is solved. By utilizing the specific molecular structure of the dispersant and stabilizer, the viscosity of the system can be controlled and a uniform and stable reaction precursor can be formed, so as to facilitate the stable control of the polymerization preparation of phenyl polysiloxanes. It can be used to prepare phenyl polysiloxanes with good transparency, covering multiple viscosity grades, wide refractive index range, multifunctional end groups, and high transparency. It achieves efficient and highly selective production, not only with simplified process and intensive equipment, but also with the potential for large-scale production, making it suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organosilicon materials technology, specifically relating to a dispersant and stabilizer suitable for preparing phenyl polysiloxanes and a method for preparing phenyl polysiloxanes. Background Technology

[0002] Phenyl polysiloxanes are organosilicon polymers with silicon-oxygen bonds as the main chain and phenyl side chains. They possess excellent high and low temperature resistance, low dielectric constant, excellent lubricity, radiation resistance, and damping properties, and are widely used in cosmetics, industrial lubrication, electronic and electrical protection, coating inks, medical, optical, and aerospace fields. According to specific types and applications, they can be divided into phenyl silicone oils, phenyl silicone rubbers, etc. At the same time, different end group types can endow phenyl polysiloxanes with different properties. For example, methyl-terminated phenyl polysiloxanes, i.e., phenyl silicone oils, have excellent chemical inertness, high hydrophobicity, and thermal stability; hydroxyl-terminated phenyl polysiloxanes are highly reactive and easily combine with polar substrates, and can be crosslinked through condensation reactions to form room temperature vulcanizing silicone rubbers; vinyl-terminated phenyl polysiloxanes can be crosslinked through addition reactions or photocuring to form highly elastic networks.

[0003] Currently, there are two main methods for preparing phenyl polysiloxanes. One is ring-opening polymerization, such as the method reported in Chinese patent CN118580495A, which uses octaphenylcyclotetrasiloxane or a diphenyl mixed cyclic form as a phenyl donor and reacts with a methyl cyclic form (such as DMC) in the presence of a catalyst to prepare methylphenyl silicone oil. Although this method can produce phenyl polysiloxanes with high refractive index, high flash point, and adjustable viscosity, it has the following problems: First, the raw material cost is high. Octaphenylcyclotetrasiloxane needs to be recrystallized multiple times to remove impurities, which prolongs the production cycle and significantly increases costs. Second, the polymerization process is heterogeneous. Octaphenylcyclotetrasiloxane is solid and forms a heterogeneous reaction system with liquid DMC. In addition, the special structure of octaphenylcyclotetrasiloxane makes it difficult for the diphenyl segments to be uniformly dispersed during the ring-opening process, directly affecting the optical transparency and performance stability of the product. This effect is even more severe when preparing products with high phenyl content. While diphenyl mixed rings can partially alleviate the above problems, as a high-temperature cracking fractionation product of dimethyldiphenylpolysiloxane, it is itself a mixture containing different phenyl contents and ring sizes. Although its liquid properties can achieve homogeneous polymerization with DMC, its high price and low phenyl content severely restrict its large-scale application.

[0004] Another method is the hydrolysis-condensation method, such as the one-pot process reported in Chinese patent CN117777447A, which uses diphenyldimethoxysilane, methylphenyldimethoxysilane, and methylcyclosiloxane or hydroxyl silicone oil as raw materials to prepare diphenylpolysiloxane via hydrolysis-condensation. While this method simplifies the steps of the traditional alkoxysilane hydrolysis-condensation route, reduces equipment requirements, and lowers costs to some extent, it still requires two steps: hydrolysis and condensation. Although simplified compared to traditional processes, its reaction mechanism retains the characteristics of staged operation and multi-step catalysis, making the production process relatively cumbersome.

[0005] In addition, Chinese patent CN104292464A combines the above two routes, reporting a two-step method for preparing hydroxyl-terminated phenyl polysiloxanes using a small amount of diphenylsilanediol as a raw material and methyl cyclic compounds, successively using two solvents and two catalysts. However, this method is limited by the amount of diphenylsilanediol added, resulting in a limited phenyl content in the product. It is only suitable for synthesizing phenyl silicone oils with low phenyl content, and the hydroxyl-terminated structure limits its application areas. Furthermore, the two-step process is complex, and the use of solvents such as isopropanol and toluene poses safety and environmental risks, significantly increasing post-processing costs. These factors weaken its potential for industrial application.

[0006] Chinese patent CN103819678A reports a method for preparing vinylphenylsiloxanes by heating a reaction of diphenylsilanediol and alkoxy compounds in a solvent and catalyst, followed by end-capping with a capping agent. This method utilizes the condensation of alkoxy groups provided by the alkoxy compounds with the hydroxyl groups of diphenylsilanediol, which can adjust the molecular weight and chain length of the polymer, thereby affecting the properties of the final product. Therefore, vinylphenylsiloxanes with high refractive index and high hardness can be prepared. However, this method still requires a two-step reaction, and the solvents used in the reaction can pose safety and environmental risks, hindering production cost control.

[0007] Based on the aforementioned existing technology, it is known that the hydrolysis-condensation method is rarely used in industry to prepare phenyl polysiloxanes from diphenylsilanediol without solvents. The main reason is that diphenylsilanediol is prone to self-polymerization during the reaction process (especially when the amount increases or the reaction time is prolonged), which leads to a sharp increase in the viscosity of the system, causing it to no longer participate in equilibrium copolymerization. Adding solvents can reduce the viscosity of the system and promote the diffusion of diphenylsilanediol, but the use of solvents often causes environmental pressure and increases production energy consumption. Therefore, this invention provides a new method for preparing phenyl polysiloxanes from diphenylsilanediol without solvents. Summary of the Invention

[0008] The purpose of this invention is to provide a dispersant stabilizer suitable for the preparation of phenyl polysiloxanes, which solves the problem that diphenylsilanediol is prone to self-polymerization in the reaction system when preparing phenyl polysiloxanes using diphenylsilanediol as a phenyl donor. By utilizing the specific molecular structure of the dispersant stabilizer, the viscosity of the system can be controlled and it can form a uniform and stable reaction precursor, so as to facilitate the stable control of the polymerization preparation of phenyl polysiloxanes.

[0009] Another object of the present invention is to provide a method for preparing phenyl polysiloxanes, applicable to the process of preparing phenyl polysiloxanes from diphenylsilanediol as a raw material, by introducing a dispersant with a specific molecular structure into the reaction precursor of diphenylsilanediol, which facilitates the stable control of the hydrolysis-condensation reaction.

[0010] This invention is achieved through the following technical solution: a dispersant and stabilizer suitable for preparing phenyl polysiloxanes, wherein the dispersant and stabilizer is added to a reaction system for preparing phenyl polysiloxanes using diphenylsilanediol as a raw material. The dispersion stabilizer has the structure shown in formula (1): (1) In formula (1), R1 and R2 independently represent methyl, ethyl, vinyl, phenyl, trifluoropropyl or hydrogen, respectively; R3 and R4 independently represent hydroxyl, alkoxy with 1 to 6 carbon atoms, acyloxy with 1 to 6 carbon atoms, amide with 1 to 6 carbon atoms or ketoxime with 1 to 6 carbon atoms, respectively; m is any integer between 0 and 30; n is any integer between 0 and 30; and 2≤m+n≤30.

[0011] The molecular weight of the dispersion stabilizer is 300 to 3000.

[0012] The viscosity of the dispersion stabilizer is 15–300 cp.

[0013] The reaction system consists of at least diphenylsilanediol and a dispersant stabilizer, with the mass ratio of the dispersant stabilizer to diphenylsilanediol being 15–600:100.

[0014] A method for preparing phenyl polysiloxane from diphenylsilanediol as a raw material involves melting diphenylsilanediol, a dispersant stabilizer, and a capping agent to form a reaction system for preparing phenyl polysiloxane. In the presence of a catalyst, the phenyl polysiloxane is obtained through polymerization, catalyst breaking, and desaturation. The dispersant stabilizer is as described above.

[0015] By mass, the diphenylsilanediol is 100 parts, the dispersant stabilizer is 15-600 parts, and the end-capping agent is 0-140 parts.

[0016] The amount of catalyst added is 50 to 2000 ppm of the total mass of the reaction system.

[0017] The phenyl polysiloxane meets the following performance specifications: Viscosity: 100-100,000 cp; Refractive index: 1.40~1.56; Light transmittance: ≥95%.

[0018] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) This invention solves the problem that it is difficult to achieve industrial production when using low-cost diphenylsilanediol as a raw material in the existing hydrolysis condensation preparation of phenyl polysiloxane. For the first time, a dispersant with a specific molecular structure is introduced into the reaction system of diphenylsilanediol. By controlling the specific amount of dispersant and diphenylsilanediol, the diphenylsilanediol can be diluted and isolated in the reaction system to prevent local self-aggregation caused by excessive amount or increased reaction time, which would then form gelled particles and make the subsequent reaction process difficult to control.

[0019] (2) This invention achieves high-temperature stable co-condensation of diphenylsilanediol through a dispersing stabilizer, breaking through the limitations of traditional multi-step reaction or multi-catalysis. Only one pot reaction, one catalyst, and one feeding are needed to prepare phenyl polysiloxanes with good transparency, covering multiple viscosity grades, wide refractive index range, and multifunctional end groups. It achieves efficient and highly selective production, which not only has the characteristics of simplified process and intensive equipment, but also has the potential for large-scale production and is suitable for industrial production.

[0020] (3) By introducing a dispersant stabilizer, the present invention achieves the goal of not adding an extra solvent during the polymerization process, and the reaction byproducts are only a small amount of water, alcohol, acid, amide or ketoxime, which reduces environmental pressure and reduces post-processing energy consumption and equipment investment.

[0021] (4) The present invention uses low-cost diphenylsilanediol to replace expensive diphenyl cyclic compounds as raw materials. The raw materials are simple and readily available, and have significant cost advantages, which can reduce the overall raw material cost by more than 50%. Detailed Implementation

[0022] The invention's objective, technical solution, and beneficial effects will be further explained in detail below.

[0023] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the claimed invention. Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0024] The traditional process for preparing phenyl polysiloxanes by hydrolysis and condensation of diphenylsilanediol has several problems: First, the low-cost diphenylsilanediol is used in small quantities, requiring the introduction of other expensive raw materials, thus increasing costs; second, the reaction requires solvents to dissolve the raw materials, and the subsequent solvent recovery step increases environmental pressure; third, the polymerization process requires at least two reaction steps or two catalytic steps, making the process flow not simple enough; in addition, reaction control is difficult, and the performance range of the obtained phenyl polysiloxanes is narrow due to limitations imposed by raw materials or end-capping agents, which is not conducive to large-scale engineering applications. The new method provided by this invention effectively solves the above problems.

[0025] The following is a further overview of the novel method of this invention: A dispersion stabilizer having the structure shown in formula (1) is used: (1) In formula (1), R1 and R2 independently represent methyl, ethyl, vinyl, phenyl, trifluoropropyl, or hydrogen, respectively; R3 and R4 independently represent hydroxyl, alkoxy, acyloxy, amide, or ketoxime, respectively, with 1 to 6 carbon atoms; m is any integer between 0 and 30; n is any integer between 0 and 30; and 2 ≤ m + n ≤ 30. The molecular weight is 300 to 3000.

[0026] When R3 / R4 represents an alkoxy group having 1 to 6 carbon atoms, the selectable groups include, but are not limited to, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, isobutoxy, tert-butoxy, n-pentoxy, isopentoxy, tert-pentoxy, n-hexyloxy, cyclohexyloxy, and 2-methylpentoxy.

[0027] When R3 / R4 represents an acyloxy group with 1 to 6 carbon atoms, the selectable groups include, but are not limited to, formyloxy, acetoxy, propionyloxy, n-butyryloxy, isobutyryloxy, n-valeryloxy, isovaleryloxy, and n-hexanoyloxy.

[0028] When R3 / R4 represents an amide group with 1 to 6 carbon atoms, the selectable groups include, but are not limited to, formamido, acetamido, n-propionamido, n-butamido, isobutamido, n-pentamido, n-hexamido, N-methylacetamido, N-ethylpropionamido, N,N-dimethylformamido, and N,N-diethylacetamido.

[0029] When R3 / R4 represents a ketoxime group with 1 to 6 carbon atoms, the selectable groups include, but are not limited to, acetone oxime, methyl ethyl ketoxime, 2-pentanone oxime, 2-hexanone oxime, cyclohexanone oxime, and unsaturated ketoxime.

[0030] In some specific implementation cases, the dispersant stabilizer can be selected from the following: methoxy-terminated polydimethylsiloxane, hydrogen-containing polydimethylsiloxane on the ethoxy-terminated side, hydroxyl-terminated polydimethylsiloxane, phenyl-terminated polydimethylsiloxane on the hydroxyl-terminated side, acetoxy-terminated polydimethylsiloxane, hydrogen-containing polydimethylsiloxane on the acetoxy-terminated side, trifluoropropyl polydimethylsiloxane on the acetamide-terminated side, ethyl polydimethylsiloxane on the acetamide-terminated side, hydrogen-containing polydimethylsiloxane on the methyl ethyl ketone oxime-terminated side, vinyl polydimethylsiloxane on the methyl ethyl ketone oxime-terminated side, etc.

[0031] The aforementioned dispersant and stabilizer is added to a reaction system for preparing phenyl polysiloxanes using diphenylsilanediol as a raw material, and melted to form a homogeneous and stable reaction precursor. This reaction system consists at least of diphenylsilanediol and the dispersant and stabilizer, or, depending on the polymerization requirements, may also include a catalyst, a capping agent, or other possible auxiliaries.

[0032] This dispersion stabilizer has a specific chain segment structure and end groups, such as −(O−Si(CH3)2). m -or −(O−SiR1R2) n - Terminal groups such as hydroxyl, alkoxy, acyloxy, amide, or ketoxime groups can form a homogeneous system with diphenylsilanediol in the reaction system through steric hindrance and interfacial interactions. This allows for dilution and isolation of diphenylsilanediol without the need for additional solvents, thus solving the problem of easy self-condensation formation of diphenylsilanediol (due to the electron-withdrawing effect of phenyl groups). Simultaneously, for −(O−SiR1R2) n The synergistic regulation of substituents R1 and R2, end-capping agents, and degree of polymerization (m, n) of the chain segment can also endow phenyl polysiloxanes with high light transmittance and a wide range of selectivity in terms of viscosity and refractive index. The viscosity and refractive index of phenyl polysiloxanes can be significantly adjusted, making them suitable for a variety of applications.

[0033] It should be noted that the dispersant stabilizer used in this invention can be purchased externally or prepared in-house. When prepared in-house, taking the hydroxyl-terminated type as an example, it can be prepared by ring-opening polymerization or hydrolysis condensation. For example, methyl cyclic and / or phenyl cyclic are used as raw materials, potassium hydroxide is used as a catalyst, and water is used as a capping agent and molecular weight regulator. After ring-opening equilibrium polymerization under heating, it is neutralized with acids such as acetic acid or silicone phosphate to obtain hydroxyl-terminated polydimethylsiloxane or hydroxyl-terminated polydimethylsiloxane containing phenyl groups.

[0034] In this invention, the ratio of dispersant stabilizer to diphenylsilanediol is controlled at 15-600:100, and more preferably 20-450:100. An appropriate amount of dispersant stabilizer can effectively control the uniformity and stability of the reaction system. If the ratio is lower than the above range, it may lead to an increase in the probability of intermolecular contact of diphenylsilanediol, triggering a local self-polymerization reaction and forming gelled particles. This will not only reduce the transparency of phenyl polysiloxane, but also affect its key performance indicators such as refractive index and thermal stability.

[0035] The reaction system of this invention further includes a catalyst and a capping agent. By adding diphenylsilanediol, a dispersant stabilizer, a catalyst, and a capping agent to a reaction vessel, the target product, phenyl polysiloxane, can be prepared in one step. The catalyst can be one of the following: acid catalysts, basic catalysts, organotin catalysts, or titanate catalysts. Specific examples include hydrochloric acid, sulfuric acid, phosphoric acid, p-toluenesulfonic acid, trifluoroacetic acid, etc.; tetramethylammonium hydroxide, tetrabutylphosphine hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, etc.; dibutyltin dilaurate, stannous octoate, di(dodecyl sulfide)dibutyltin, dibutyltin diacetate, etc.; tetraisopropyl titanate or tetrabutyl titanate, etc. The amount of catalyst used is 50–2000 ppm of the total mass of the reaction system, preferably 100–1000 ppm. Optional end-capping agents include methyl silicone oil, vinyl silicone oil, hydroxyl silicone oil, water, or one of the following: dimethylethoxysiloxane, trimethylethoxysilane, vinyldimethylmethoxysilane, etc. The ratio of end-capping agent to diphenylsilanediol is 0–140:100, with a preferred ratio of 1–100:100.

[0036] The novel method of this invention has the potential for industrial production, and the preparation process can be summarized as follows: (a) Hot melt According to the aforementioned proportions, diphenylsilanediol, dispersant stabilizer, and end-capping agent are added to the reactor in one step. The mixture is heated to melt, forming a liquefied homogeneous system that maintains stable dispersion of the diphenylsilanediol and prevents solid precipitation. The melting temperature can be controlled between 130 and 200°C, preferably 140 to 160°C, and the melting time can be controlled between 30 and 360 minutes, preferably 120 to 240 minutes.

[0037] (ii) Aggregation The homogeneous system obtained by melting is cooled to 130-160°C, an appropriate amount of catalyst is added, and the mixture is stirred and the reaction begins. The condensation byproducts of the system are removed, and no diphenylsilanediol self-agglomerates during the reaction. The equilibrium reaction proceeds towards the product. The polymerization temperature is 130-160°C, and the reaction time is 3-12 hours, preferably 4-10 hours.

[0038] (iii) Breaking the match For catalyst deactivation, selectable deactivation methods include acid-base neutralization, high-temperature catalyst destruction, and adsorption elimination.

[0039] (iv) Lowering Low-boiling-point substances in the reaction system are removed by vacuum distillation. The pressure of vacuum distillation is less than 200 Pa, the material temperature is 180-250 °C, and the removal time is 4-12 h. The common low-boiling-point substances are mainly one or more of dimethylcyclosiloxane, methylphenylcyclosiloxane, and oligomeric methylphenylpolysiloxane. Depending on the different end groups in formula (1), a small amount of water, alcohol, acid, amide or ketoxime will also be collected.

[0040] After the reaction, a colorless and transparent phenyl polysiloxane is obtained, whose viscosity, refractive index and transmittance can be customized over a wide range. Specifically, the viscosity is 100 to 100,000 cp, the refractive index is 1.40 to 1.56 and the transmittance is ≥95%. Further preferred, the viscosity can be controlled to be 300 to 50,000 cp, the refractive index is 1.42 to 1.52 and the transmittance is ≥97%.

[0041] The present invention will be further described in detail below with reference to embodiments, but the implementation of the present invention is not limited thereto.

[0042] Example 1: 100 kg of diphenylsilanediol, 60 kg of methoxy-terminated polydimethylsiloxane with a viscosity of 40 cp, and 45 kg of methyl silicone oil with a viscosity of 10 cp were added to a reactor in one batch. The reactor was heated to 150°C, and the molten material was heated for 3 hours to liquefy and form a homogeneous system. The reactor was then cooled to 130°C, and 1000 ppm of sulfuric acid was added. The reactor pressure was controlled at -0.02 MPa, and the temperature was raised to 140°C. After equilibration for another 8 hours, sodium bicarbonate was used for neutralization and inactivation. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 180°C for 8 hours to remove low-boiling-point substances. In addition to the usual low-boiling-point substances, a small amount of methanol was also removed. After filtration, a colorless and transparent methyl-terminated phenyl polysiloxane was finally obtained.

[0043] Example 2: 100 kg of diphenylsilanediol, 360 kg of ethoxylated polydimethylsiloxane with a viscosity of 250 cp, and 40 kg of hydroxyl silicone oil with a viscosity of 20 cp were added to a reactor in one batch. The reactor was heated to 140°C, and the molten material was heated for 3 hours to liquefy and form a homogeneous system. The reactor was then cooled to 130°C, and 1000 ppm of p-toluenesulfonic acid was added. The reactor pressure was controlled at -0.01 MPa, and the temperature was raised to 140°C. After equilibration for another 6 hours, sodium carbonate was used for neutralization and inactivation. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 220°C for 10 hours to remove low-boiling-point substances. In addition to the usual low-boiling-point substances, a small amount of ethanol was also removed. After filtration, a colorless and transparent hydroxyl-terminated phenyl polysiloxane was finally obtained.

[0044] Example 3: 100 kg of diphenylsilanediol, 200 kg of 20 cp hydroxyl-terminated polymethylsiloxane, and 35 kg of 100 cp vinyl silicone oil were added to a reactor in one batch. The reactor was heated to 160°C, and the molten material was heated for 4 hours to liquefy and form a homogeneous system. The reactor was then cooled to 140°C, and 800 ppm of sodium hydroxide was added. The reactor pressure was controlled at -0.02 MPa, and the temperature was raised to 160°C. After equilibration for another 6 hours, the material was neutralized and inactivated using silanized phosphate ester. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 200°C for 6 hours to remove low-boiling-point substances, as well as a small amount of water, ultimately yielding a colorless and transparent hydroxyl-terminated polymethylsiloxane.

[0045] Example 4: 100 kg of diphenylsilanediol, 120 kg of acetoxy-terminated polymethylsiloxane with a viscosity of 150 cp, and 10 kg of dimethylethoxysiloxane were added to a reactor in one step. The reactor was heated to 150°C, and the molten material was heated for 4 hours to liquefy and form a homogeneous system. The reactor was then cooled to 140°C, and 100 ppm of dibutyltin dilaurate was added. The reactor pressure was controlled at -0.01 MPa, and the temperature was raised to 150°C. After equilibration for another 8 hours, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 190°C for 6 hours to remove impurities. In addition to the usual low-boiling substances, a small amount of acetic acid and ethanol were also removed. After adsorption and filtration by activated carbon, a colorless and transparent hydrogen-terminated phenyl polysiloxane was finally obtained.

[0046] Example 5: 100 kg of diphenylsilanediol, 30 kg of acetamide-terminated polymethylsiloxane with a viscosity of 200 cp, and 20 kg of trimethylethoxysilane were added to a reactor in one step. The reactor was heated to a material temperature of 140°C and molten for 3 hours, after which the material liquefied to form a homogeneous system. The reactor was then cooled to 130°C, and 80 ppm of stannous octoate was added. The reactor pressure was controlled at -0.01 MPa, and the temperature was raised to a material temperature of 150°C. After equilibration for another 8 hours, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 200°C for 12 hours to remove acetamide and ethanol, in addition to the usual low-boiling substances. After activated carbon adsorption and filtration, a colorless and transparent methyl-terminated polymethylsiloxane was finally obtained.

[0047] Example 6: 100 kg of diphenylsilanediol, 80 kg of 300 cp methyl-terminated ketone oxime-based polymethylsiloxane, and 30 kg of vinyldimethylmethoxysilane were added to a reactor in one step. The reactor was heated to 150°C, and the molten material was heated for 2 hours to liquefy and form a homogeneous system. The reactor was then cooled to 140°C, and 50 ppm of tetraisopropyl titanate was added. The reactor pressure was controlled at -0.02 MPa, and the temperature was raised to 150°C. After equilibration for 5 hours, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 240°C for 6 hours to remove impurities. In addition to the usual low-boiling substances, a small amount of methyl ethyl ketone oxime and methanol were also removed. After activated carbon adsorption and filtration, a colorless and transparent methyl-terminated phenyl polysiloxane was finally obtained.

[0048] Comparative Example 1: The difference between this comparative example and the embodiment is that no dispersing stabilizer was used. The rest of the preparation method is exactly the same as the method of the present invention, except that the specific process parameters and conditions are slightly adjusted.

[0049] 100 kg of diphenylsilanediol and 45 kg of methyl silicone oil with a viscosity of 10 cp were added to a reactor in one step. The reactor was heated to 150°C, and the molten material was heated for 3 hours to liquefy and form a homogeneous system. The reactor was then cooled to 130°C, and 1000 ppm of sulfuric acid was added. Diphenylsilanediol began to self-polymerize and precipitate. The reactor pressure was controlled at -0.02 MPa, and the temperature was raised to 140°C. After equilibration for another 8 hours, sodium bicarbonate was used to neutralize and inactivate it. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 180°C for 8 hours to remove conventional low-boiling substances and a small amount of water. After filtration, a milky white terminal methylphenyl polysiloxane was finally obtained.

[0050] Comparative Example 2: The difference between this comparative example and the embodiment is that the amount of dispersant stabilizer added is reduced to only 1 / 10 of the mass of diphenylsilanediol. The rest of the preparation method is exactly the same as that of the present invention, except that the specific process parameters and conditions are slightly adjusted.

[0051] 100 kg of diphenylsilanediol, 10 kg of methoxy-terminated polydimethylsiloxane with a viscosity of 40 cp, and 45 kg of methyl silicone oil with a viscosity of 10 cp were added to a reactor in one batch. The reactor was heated to 150°C, and the molten material was heated for 3 hours to liquefy and form a homogeneous system. The reactor was then cooled to 130°C, and 1000 ppm of sulfuric acid was added. A small amount of colloidal particles precipitated. The reactor pressure was controlled at -0.02 MPa, and the temperature was raised to 140°C. After equilibration for another 8 hours, sodium bicarbonate was used for neutralization and inactivation. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 180°C for 8 hours to remove low-boiling-point substances. In addition to the usual low-boiling-point substances, a small amount of methanol was also removed. After filtration, a translucent methyl-terminated phenyl polysiloxane was finally obtained.

[0052] Comparative Example 3: The difference between this comparative example and the embodiment is that no dispersing stabilizer was used, but diphenyldiethoxysilane was added to the reaction system. The rest of the preparation method is exactly the same as the method of the present invention, with slight adjustments to the specific process parameters.

[0053] 100 kg of diphenylsilanediol, 40 kg of diphenyldiethoxysilane, and 35 kg of vinyl silicone oil with a viscosity of 100 cp were added to a reactor in one step. The reactor was heated to 140°C, and the material was melted for 4 hours, liquefying to form a homogeneous system. Then, 800 ppm of sodium hydroxide was added, and the system turned white with the precipitation of byproducts such as phenyl rings. The reactor pressure was controlled at -0.02 MPa, and the material temperature was maintained at 140°C. After equilibration for another 6 hours, silanol-based phosphate was used to neutralize and inactivate the material. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 200°C for 6 hours to remove low-boiling-point substances. In addition to the usual low-boiling-point substances, a large amount of ethanol and a small amount of water were also removed, finally yielding a translucent terminal vinylphenyl polysiloxane.

[0054] Comparative Example 4: The difference between this comparative example and the embodiment is that no dispersant stabilizer was used, but diphenyldiethoxysilane and xylene (solvent) were added to the reaction system. The rest of the preparation method is exactly the same as the method of the present invention, with slight adjustments to the specific process parameters.

[0055] 100 kg of diphenylsilanediol, 40 kg of diphenyldiethoxysilane, 35 kg of vinyl silicone oil with a viscosity of 100 cp, and 200 kg of xylene were added to a reactor in one batch. The reactor was heated to 140°C, and the material was melted for 4 hours, liquefying to form a homogeneous system. Then, 800 ppm of sodium hydroxide was added, and the reactor pressure was controlled at -0.02 MPa. The material temperature was maintained at 140°C, and after equilibration for another 6 hours, it was neutralized and inactivated using silanized phosphate ester. Then, the reactor pressure was controlled below 200 Pa, and the temperature was maintained at 200°C for 6 hours to remove low-boiling-point substances, as well as the solvent xylene, a large amount of ethanol, and a small amount of water, ultimately yielding a transparent terminal vinylphenyl polysiloxane.

[0056] The homogeneous systems and phenyl polysiloxanes obtained in the above examples and comparative examples were compared and tested as follows: Viscosity measurement method: rheometer (shear rate 0.9s) -1 (temperature 25℃) Method for determining refractive index: Abbe refractometer (20℃); Transmittance measurement method: Ultraviolet spectrophotometer (wavelength range 500-600 nm, using methyl cyclohexane as reference).

[0057] Table 1 As shown in Table 1 above, in Examples 1 to 6 of the present invention, phenyl polysiloxane products with different end groups, viscosities and refractive indices can be prepared by selecting different dispersing stabilizers and end capping agents, and all of them have high light transmittance.

[0058] Compared to Comparative Example 1 (no dispersant stabilizer added), Comparative Example 2 (reduced amount of dispersant stabilizer), and Comparative Example 3 (no dispersant stabilizer added, but diphenyldiethoxysilane added), the reaction precursors formed by the molten addition of the catalyst exhibited by-product precipitation such as self-polymerization of diphenylsilanediol, precipitation of a small amount of colloidal particles, and precipitation of phenyl cyclic compounds, resulting in reduced transparency and consequently lower efficiency and poor light transmittance in subsequent reactions. This demonstrates that, in Examples 1 to 6 of the present invention, by adding an appropriate amount of dispersant stabilizer, a uniform and stable reaction precursor can be obtained, and subsequent reaction efficiency and light transmittance can be improved.

[0059] Compared to Comparative Example 4 (without dispersant stabilizer, but with diphenyldiethoxysilane and xylene), the addition of xylene solvent can dissolve raw materials such as diphenylsilanediol, ensuring the uniformity and stability of the reaction precursors and guaranteeing the product's transmittance. However, the preparation process requires an additional solvent removal post-processing step, posing environmental pressure. Furthermore, the product may contain a solvent odor that is difficult to remove, affecting product quality. Examples 1 to 6 of this invention, because no solvent is added and the byproducts from the addition of dispersant stabilizer are small or water-based, exhibit significant environmentally friendly characteristics. For example, in Example 2, the ethoxylated polydimethylsiloxane used has an ethanol byproduct ratio of approximately 7 wt% of the dispersant stabilizer; in Comparative Example 4, the diphenyldiethoxysilane used has an ethanol byproduct ratio of over 30 wt% of the dispersant stabilizer; and in Example 3, the hydroxyl-terminated polymethylsiloxane used has a water byproduct, demonstrating excellent environmental compatibility.

[0060] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications or equivalent changes made to the above embodiments based on the technical essence of the present invention shall fall within the protection scope of the present invention.

Claims

1. A dispersant and stabilizer suitable for preparing phenyl polysiloxanes, characterized in that: The dispersant stabilizer is added to the reaction system for preparing phenyl polysiloxane using diphenylsilanediol as a raw material. The dispersion stabilizer has the structure shown in formula (1): (1) In formula (1), R1 and R2 independently represent methyl, ethyl, vinyl, phenyl, trifluoropropyl or hydrogen, respectively; R3 and R4 independently represent hydroxyl, alkoxy with 1 to 6 carbon atoms, acyloxy with 1 to 6 carbon atoms, amide with 1 to 6 carbon atoms or ketoxime with 1 to 6 carbon atoms, respectively; m is any integer between 0 and 30; n is any integer between 0 and 30; and 2≤m+n≤30.

2. The dispersant stabilizer according to claim 1, characterized in that: The molecular weight of the dispersion stabilizer is 300 to 3000.

3. The dispersant stabilizer according to claim 1, characterized in that: The viscosity of the dispersion stabilizer is 15–300 cp.

4. The dispersion stabilizer according to claim 1, characterized in that: The reaction system consists of at least diphenylsilanediol and a dispersant stabilizer, with the mass ratio of the dispersant stabilizer to diphenylsilanediol being 15–600:

100.

5. A method for preparing phenyl polysiloxane from diphenylsilanediol, characterized in that: A reaction system for preparing phenyl polysiloxane is formed by melting diphenylsilanediol, a dispersant stabilizer and a capping agent. In the presence of a catalyst, the phenyl polysiloxane is obtained by polymerization, catalyst breaking and de-capping, wherein the dispersant stabilizer is as described in any one of claims 1 to 3.

6. The method according to claim 5, characterized in that: By mass, the diphenylsilanediol is 100 parts, the dispersant stabilizer is 15-600 parts, and the end-capping agent is 0-140 parts.

7. The method according to claim 5, characterized in that: The amount of catalyst added is 50 to 2000 ppm of the total mass of the reaction system.

8. The method according to claim 5, characterized in that: The phenyl polysiloxane meets the following performance specifications: Viscosity: 100-100,000 cp; Refractive index: 1.40~1.56; Light transmittance: ≥95%.

Citation Information

Patent Citations

  • Vinylphenylpolysiloxane, preparation method and application

    CN103819678A

  • Preparation method of phenyl hydroxyl silicone oil

    CN104292464A

  • Method for preparing methyl phenyl silicone oil by one-kettle method

    CN117777447A

  • Phenyl dimethyl-terminated or triphenyl-terminated methyl phenyl silicone oil and preparation method thereof

    CN118580495A