A method for preparing an asymmetric silicone oil

The reaction of alkoxysilanes with alkali metal hydroxides to generate silanol alkali metal salts, replacing alkyl lithium initiators, solves the safety risks and high costs in the preparation of asymmetric silicone oils, and realizes low-cost and safe industrial production. The products are suitable for surface modification of thermally conductive fillers, leveling of coatings, toughening of adhesives, and modification of resins.

CN123152113APending Publication Date: 2026-11-24上海普信高分子材料有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611569701.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing asymmetric silicone oil preparation processes rely on alkyl lithium initiators, which have problems such as high safety risks, high costs, large equipment investment, and unstable product quality, making it difficult to achieve large-scale industrial production.

Method used

Asymmetric silicone oil is prepared by in-situ generation of silanol alkali metal salts through the reaction of alkoxysilanes with alkali metal hydroxides, replacing alkyl lithium initiators, and ring-opening polymerization via nucleophilic substitution reaction. The reaction is carried out under normal pressure and mild conditions, avoiding the use of hazardous chemicals and the strict requirements of anhydrous and oxygen-free environment.

Benefits of technology

It reduces raw material costs, simplifies production processes, lowers safety risks and equipment investment, and improves the stability and applicability of products, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

This invention relates to the field of organosilicon polymer preparation technology, specifically to a method for preparing asymmetric silicone oil. The method includes the following steps: mixing alkoxysilanes with alkali metal hydroxides, followed by a nucleophilic substitution reaction to obtain a silanol alkali metal salt; mixing the silanol alkali metal salt with a cyclosiloxane monomer, followed by a ring-opening polymerization reaction to obtain a siloxane intermediate; adding a capping agent to the siloxane intermediate for capping, followed by post-treatment to obtain the asymmetric silicone oil. This invention uses the reaction of alkoxysilanes with alkali metal hydroxides, replacing the expensive and flammable alkyl lithium initiators used in existing technologies. Furthermore, the raw materials are all readily available chemical products, significantly reducing procurement costs. The reaction is carried out under normal pressure and mild conditions, eliminating the need for strict anhydrous and oxygen-free low-temperature control, greatly reducing production safety risks and storage, transportation, and management costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organosilicon polymer preparation technology, specifically to a method for preparing asymmetric silicone oil. Background Technology

[0002] This invention relates to the field of organosilicon polymer preparation technology, specifically to a method for preparing asymmetric silicone oil. Asymmetric silicone oil, also known as single-terminated functionalized polydimethylsiloxane, has an inert alkyl end cap on one end of its molecular chain and a reactive functional group end cap on the other. It combines the low surface energy and weather resistance of polysiloxanes with the reactivity of its functional end groups, making it irreplaceable in applications such as surface modification of thermally conductive fillers, leveling of coatings, toughening of adhesives, and resin modification.

[0003] Currently, the mainstream process for preparing asymmetric silicone oil in the industry is the alkyl lithium-initiated ring-opening polymerization method. Chinese invention patent CN112608480B discloses a method for preparing asymmetric silicone oil, which uses alkyl lithium such as n-butyllithium as initiators to catalyze the ring-opening polymerization of cyclosiloxanes in an organic solvent system, followed by chlorosilane end-capping, water washing to remove acid, and drying to obtain the product. Although this method can yield asymmetric silicone oil with a well-defined structure, it has significant industrialization drawbacks: First, alkyl lithium raw materials are expensive and chemically extremely reactive, readily flammable and explosive in water and oxygen, resulting in extremely high costs for storage, transportation, and safety management during the reaction process, posing significant risks for large-scale production; second, the reaction must be carried out in a strictly anhydrous and oxygen-free low-temperature environment, leading to high equipment investment and energy consumption costs; third, the post-processing requires a water washing step to remove hydrogen chloride, which easily triggers the breaking and rearrangement of silicon-oxygen bonds, resulting in a wider molecular weight distribution of the product and the introduction of silanol byproducts, reducing the reactivity of functional end groups and affecting downstream applications.

[0004] In addition to the above, existing preparation routes such as hydrosilylation and hydroxyl condensation have limitations. The former requires platinum-based noble metal catalysts, resulting in high raw material costs and lengthy reaction steps; the latter requires the preparation of a single-hydroxyl-terminated silicone oil intermediate before condensation to introduce functional groups, leading to a long process path and low functionalization conversion rate. Existing schemes using alkali metal silanodes as initiators mostly require the purchase of pre-prepared silanodes, resulting in high procurement costs, and few offer a simple process for efficiently preparing single-trimethoxy-functionalized asymmetric silicone oils. Therefore, developing a method for preparing asymmetric silicone oils that does not require alkyl lithium, is simple in process, low in cost, and produces stable product quality is a pressing technical problem to be solved in this field. Summary of the Invention

[0005] This invention addresses the industry pain point that existing asymmetric silicone oil preparation systems are highly dependent on alkyl lithium initiators. Starting from the underlying mechanism of reactive center construction, it achieves complete equivalent substitution of alkyl lithium initiators by generating silanol alkali metal salts in situ through a nucleophilic substitution reaction of alkoxysilanes with alkali metal hydroxides. Therefore, this invention provides a method for preparing asymmetric silicone oil, comprising the following steps: mixing alkoxysilanes with alkali metal hydroxides and undergoing a nucleophilic substitution reaction to obtain silanol alkali metal salts; mixing silanol alkali metal salts with cyclosiloxane monomers and undergoing a ring-opening polymerization reaction to obtain siloxane intermediates; adding an end-capping agent to the siloxane intermediates for end-capping reaction, and then performing post-treatment to obtain asymmetric silicone oil.

[0006] In existing mainstream processes, alkyllithium dissociates highly reactive alkyl anions to attack cyclic siloxanes, generating lithium silanolate active centers to trigger anionic ring-opening polymerization. However, alkyllithium is extremely chemically reactive, reacting violently with water or oxygen, even igniting or exploding. Raw material storage and transportation, as well as the reaction process, require a strict anhydrous, oxygen-free, low-temperature, and explosion-proof control system. Furthermore, the high cost of raw materials significantly increases the safety risks and overall costs of industrial production. This invention involves a nucleophilic substitution reaction between alkoxysilanes and alkali metal hydroxides to generate silanolate alkali metal salts with initiating activity. These silanolate alkali metal salts can dissociate to generate siloxane anion active centers, whose nucleophilic attack capability is identical to that of the siloxane anions generated in the alkyllithium system. Both can efficiently attack the central silicon atom of the cyclic siloxane monomer, triggering siloxane bond breaking and chain growth reactions. The final product is a linear polysiloxane intermediate capped with an inert alkyl group at one end and an active silanolate at the other, fully meeting the requirements for initiating the polymerization of asymmetric silicone oils. The system uses readily available, general-purpose chemical raw materials, significantly reducing procurement costs compared to alkyl lithium. These raw materials are chemically stable and can be safely stored and transported at room temperature and pressure without the need for special high-risk chemical control measures. The entire reaction can be carried out under normal pressure and mild conditions, without the need for strict anhydrous and oxygen-free environments and low-temperature control, greatly reducing equipment investment and operational barriers. Furthermore, it is highly compatible with subsequent post-processing techniques such as chlorosilane end-capping and filtration desalination, eliminating the need for water washing throughout the process. It is suitable for large-scale industrial production needs in all aspects, from raw material procurement and production operation to safety management.

[0007] The general structural formula of the alkoxysilane is shown in Formula 1. Formula 1; wherein R1, R2 and R3 are each selected from methyl, ethyl, phenyl or butyl; R4 is selected from methyl or ethyl.

[0008] The asymmetric silicone oil has a kinematic viscosity of 10-60 mmHg at 25°C. 2 / s.

[0009] The nucleophilic substitution reaction is carried out at a temperature of 70-100℃ for 3-8 hours.

[0010] The ring-opening polymerization reaction is carried out at a temperature of 60-100℃ for 4-8 hours.

[0011] The end-capping reaction is carried out at a temperature of 30-50℃ for 3-5 hours.

[0012] Optionally, the nucleophilic substitution reaction is carried out at a temperature of 80-90°C for 4-7 hours.

[0013] Optionally, the ring-opening polymerization reaction is carried out at a temperature of 70-90°C for 5-7 hours.

[0014] Optionally, the end-capping reaction is carried out at a temperature of 35-45°C for 4-5 hours.

[0015] The alkali metal hydroxide includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, and cesium hydroxide.

[0016] Optionally, the alkali metal hydroxide includes at least one of sodium hydroxide and potassium hydroxide.

[0017] The cyclosiloxane monomer includes at least one of octamethylcyclotetrasiloxane, dimethylsiloxane mixed cyclic, hexamethylcyclotrisiloxane, decamethylcyclopentasiloxane, and dodecylcyclohexasiloxane.

[0018] The end-capping agent includes alkoxy-substituted chlorosilanes.

[0019] The molar ratio of the alkoxy-substituted chlorosilane and the cyclosiloxane monomer is 1:(10-30).

[0020] The trialkoxychlorosilane includes at least one of trimethoxychlorosilane, triethoxychlorosilane, tri-n-propoxychlorosilane, triisopropoxychlorosilane, and tri-n-butoxychlorosilane.

[0021] Beneficial effects 1. This invention avoids the use of traditional alkyl lithium, and the raw materials are all readily available chemical products, which greatly reduces the procurement cost; the reaction is carried out under normal pressure and mild conditions, without the need for strict low-temperature control of anhydrous and oxygen-free conditions, which greatly reduces the production safety risks and storage, transportation and control costs.

[0022] 2. The three-step reaction of the present invention is carried out continuously in the same reactor, adopting a "one-pot" process, which eliminates the need to transfer materials, add additional organic solvents, or pre-prepare silanol intermediates.

[0023] 3. The present invention has a simplified process, requires less equipment investment, has a short production cycle, can be directly adapted to existing industrial equipment for organosilicon polymerization, and is easy to scale up for production.

[0024] 4. The product of this invention has a wide adjustable viscosity range, suitable for various applications, and can be adjusted from 10-60 mm.2 The kinematic viscosity of the product can be adjusted within a range of / s. Low viscosity products are suitable for surface treatment of nanofillers, while medium viscosity products are suitable for resin modification and coating additives, which can flexibly match the performance requirements of different downstream applications.

[0025] 5. The asymmetric silicone oil prepared by this invention is suitable for the fields of surface modification of thermally conductive fillers, leveling of coatings, toughening of adhesives, and modification of resins. Detailed Implementation

[0026] Example 1 A method for preparing an asymmetric silicone oil includes the following steps: mixing alkoxysilane with potassium hydroxide, subjecting it to a nucleophilic substitution reaction (reaction at 85°C for 5.5 h), distilling off the byproduct ethanol to obtain a silanol alkali metal salt; mixing the silanol alkali metal salt with octamethylcyclotetrasiloxane, subjecting it to a ring-opening polymerization reaction (reaction at 80°C for 6 h) to obtain a siloxane intermediate; adding trimethoxychlorosilane to the siloxane intermediate for an end-capping reaction (reaction at 40°C for 4 h), and filtering to obtain the asymmetric silicone oil.

[0027] The general structural formula of the alkoxysilane is shown in Formula 1. Formula 1; wherein R1, R2 and R3 are all methyl groups, and R4 is an ethyl group.

[0028] The molar ratio of the trimethoxychlorosilane to the siloxane intermediate is 1:10.

[0029] Example 2 The specific implementation method is the same as in Example 1; the difference is that the molar ratio of the trimethoxychlorosilane and the siloxane intermediate is 1:15.

[0030] Example 3 The specific implementation method is the same as in Example 1; the difference is that the molar ratio of the trimethoxychlorosilane and the siloxane intermediate is 1:20.

[0031] Example 4 The specific implementation method is the same as in Example 1; the difference is that the molar ratio of the trimethoxychlorosilane and the siloxane intermediate is 1:25.

[0032] Example 5 The specific implementation method is the same as in Example 1; the difference is that the molar ratio of the trimethoxychlorosilane and the siloxane intermediate is 1:30.

[0033] Performance testing methods The viscosity (25°C) of the asymmetric silicone oil prepared in the examples was tested, and the test data are listed in Table 1.

[0034] Performance test data Table 1

Claims

1. A method for preparing an asymmetric silicone oil, characterized in that, Includes the following steps: Alkoxysilanes are mixed with alkali metal hydroxides and subjected to nucleophilic substitution reactions to obtain silanol alkali metal salts. A siloxane intermediate is obtained by mixing a siloxane alkali metal salt with a cyclosiloxane monomer and then performing a ring-opening polymerization reaction. An end-capping agent is added to the siloxane intermediate to perform an end-capping reaction, and the resulting product is an asymmetric silicone oil after post-treatment.

2. The preparation method according to claim 1, characterized in that, The general structural formula of the alkoxysilane is shown in Formula 1. Formula 1; wherein R1, R2 and R3 are each selected from methyl, ethyl, phenyl or butyl; R4 is selected from methyl or ethyl.

3. The preparation method according to claim 1 or 2, characterized in that, The asymmetric silicone oil has a kinematic viscosity of 10-60 mmHg at 25°C. 2 / s.

4. The preparation method according to claim 1, characterized in that, The nucleophilic substitution reaction is carried out at a temperature of 70-100℃ for 3-8 hours.

5. The preparation method according to claim 1, characterized in that, The ring-opening polymerization reaction is carried out at a temperature of 60-100℃ for 4-8 hours.

6. The preparation method according to claim 1, characterized in that, The end-capping reaction is carried out at a temperature of 30-50℃ for 3-5 hours.

7. The preparation method according to claim 1 or 4, characterized in that, The alkali metal hydroxide includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, and cesium hydroxide.

8. The preparation method according to claim 7, characterized in that, The alkali metal hydroxide includes at least one of sodium hydroxide and potassium hydroxide.

9. The preparation method according to claim 1 or 5, characterized in that, The cyclosiloxane monomer includes at least one of octamethylcyclotetrasiloxane, dimethylsiloxane mixed cyclic, hexamethylcyclotrisiloxane, decamethylcyclopentasiloxane, and dodecylcyclohexasiloxane.

10. The preparation method according to claim 1 or 6, characterized in that, The end-capping agent includes trialkoxychlorosilane.

Citation Information

Patent Citations

  • An asymmetric silicone oil, its preparation method and application

    CN112608480B