A photocurable modified silicone resin, and a preparation method and application thereof

By introducing specific structural side chains into the organopolysiloxane chain, the photocurable modified organosilicon resin has solved the problems of unpleasant curing conditions and insufficient comprehensive performance in the existing technology, and achieved rapid curing film formation and long-lasting anti-fouling and anti-graffiti effects.

CN123152114APending Publication Date: 2026-11-24GUANGZHOU SILOK POLYMER
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611659004.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing photocurable silicone resins have limitations in the field of protective coatings, including harsh curing conditions and insufficient overall performance, failing to meet the requirements for long-lasting stain and graffiti resistance.

Method used

By introducing specific structural side chains onto the organopolysiloxane chain, a photocurable modified organosilicon resin is prepared. It is then rapidly cured into a film under the action of a photoinitiator and ultraviolet light, forming a dense low surface energy crosslinked network.

Benefits of technology

It achieves rapid curing and film formation, forming a dense, low surface energy cross-linked network, which has excellent long-lasting anti-fouling and anti-graffiti properties, and is suitable for protection needs in multiple scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152114A_ABST
    Figure CN123152114A_ABST
Patent Text Reader

Abstract

This invention discloses a photocurable modified silicone resin, its preparation method, and its applications. The photocurable modified silicone resin has the structure shown in the following formula: This invention, through molecular structure design, introduces specific structural side chains onto the organopolysiloxane chain to achieve photocurable modification of the silicone resin. Upon photoinitiation, it can rapidly cure into a film, forming a dense, low-surface-energy cross-linked network. This network effectively resists the wetting and penetration of contaminants such as water, oil, paint, and ink, exhibiting excellent long-lasting anti-fouling and anti-graffiti properties, and can meet the protection needs of various scenarios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organosilicon material technology, specifically relating to a photocurable modified organosilicon resin, its preparation method, and its application. Background Technology

[0002] Organosilicon materials, with their excellent weather resistance, thermal stability, hydrophobicity, and flexibility, have great application prospects in high-end protective coatings such as building exteriors, public facilities, electronic components, and automotive coatings. However, traditional thermosetting organosilicon resins suffer from problems such as high curing temperatures, high energy consumption, and long curing cycles, making them difficult to apply to heat-sensitive substrates such as plastics and precision electronic components, thus limiting their application scope.

[0003] While UV curing technology offers a new, highly efficient, and energy-saving approach, existing UV curing systems often rely on high-intensity UV light sources or highly reactive monomers in pursuit of rapid curing. This leads to increased equipment and process costs and may cause problems such as poor storage stability, brittle coatings, and strong irritation from residual monomers. Furthermore, conventional UV-cured coatings often focus on basic physical properties or simple hydrophobic functions. When faced with combined oil and dust contamination, as well as stubborn graffiti such as paint and ink, their anti-fouling and easy-to-clean properties rapidly decline, failing to meet the urgent needs of modern buildings, transportation, public facilities, and electronic products for long-lasting intelligent surface protection.

[0004] In the prior art, there have been studies on using acrylate-modified organopolysiloxanes for photocuring systems. For example, Chinese patent application CN101092481A discloses an acrylate-modified organopolysiloxane, specifically through a hydrosilylation reaction of an organopolysiloxane having at least one SiH group with a compound having at least two acrylate groups in equimolar amounts at a temperature of 60-130°C in the presence of a rhodium catalyst. The rhodium catalyst induces 1,2-position addition in the addition reaction of polyacrylate and hydrosiloxane, forming a SiC-linked acrylate-modified organopolysiloxane, avoiding the aging, gelation, and peeling performance degradation caused by SiOC bonding products; Chinese patent application CN1192644 39A discloses a photocurable silicone resin, specifically obtained by hydrogenation reaction of a hydrogen-containing double-terminated resin with allyl glycidyl ether in the presence of a platinum catalyst to obtain an epoxy-based double-terminated resin. This is then followed by ring-opening esterification reaction with excess acrylic acid in the presence of a ring-opening esterification catalyst to obtain a hydroxyacryloyloxy double-terminated resin. Further esterification and dehydration reaction with excess acrylic acid in the presence of a cyclohexane dehydrating agent and an acidic catalyst yields a bisacryloyloxy double-terminated resin. Finally, a rearrangement reaction is carried out with polydimethylsiloxane in the presence of a linear phosphazene chloride catalyst to synthesize a photocurable silicone oligomer. This oligomer, combined with acrylate monomers and a free radical photoinitiator, forms a UV adhesive exhibiting excellent adhesion strength to low surface energy materials such as PE, PP, PET, and POE. The above scheme primarily focuses on the application of photocurable silicone resin in adhesives, emphasizing its bonding performance on substrate surfaces, without addressing its application in protective coatings for improving anti-fouling and anti-graffiti properties.

[0005] Currently, there is a lack of modified silicone materials for protective coatings that can simultaneously achieve mild curing conditions, excellent overall performance, and meet the requirements for long-lasting anti-fouling and anti-graffiti. Therefore, developing new photocurable silicone resins that can meet the protection needs of multiple scenarios has important practical application value. Summary of the Invention

[0006] To overcome the shortcomings of the existing technology, the present invention aims to provide a photocurable modified silicone resin that can be rapidly cured into a film under the action of a photoinitiator and ultraviolet light, forming a cross-linked network with low surface energy and dense structure, exhibiting excellent long-lasting anti-fouling and anti-graffiti properties.

[0007] The objective of this invention is achieved through the following technical solution: In a first aspect, the present invention provides a photocurable modified silicone resin having the structure shown in formula (1): Equation (1); Wherein, R1 is a C8-C12 alkyl group, or ; R2 is an alkylene group. or ; R3 is an alkyl group; R4 is a carbon-carbon single bond, an alkylene group, or... ; R5, R 13 It is -H or alkyl; R6, R7, R8, R9, R 10 R 11 R 12 Each is independently an alkylene group; * indicates a substitution site; a, b, and c are each an independent natural number from 1 to 100; m, n, j, and k are each independent natural numbers from 0 to 20. m and n are not both 0 at the same time, and j and k are not both 0 at the same time.

[0008] Preferably, R1 is .

[0009] Preferably, R2 is .

[0010] Preferably, R3 is a C1-C12 alkyl group; more preferably, it is a C1-C6 straight-chain alkyl group or a branched alkyl group.

[0011] Preferably, R6, R7, R8, R9, R 10 R 11 R 12 Each is independently a C1 to C22 alkylene group (e.g., it can be C1, C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C19, C20, C21, C22); more preferably, it is a C1 to C8 alkylene group.

[0012] Preferably, a is a natural number from 1 to 30; b is a natural number from 1 to 48; and c is a natural number from 1 to 50.

[0013] Preferably, the kinematic viscosity of the photocurable modified silicone resin is 40-300 cSt. The viscosity is measured according to standard ASTM D445-26 at a test temperature of 25°C.

[0014] Secondly, the method for preparing the photocurable modified organosilicon resin of the present invention includes the following steps: S1. Hydrosilylation reaction of hydrogen-containing polysiloxane, hydroxyl-containing olefinic unsaturated compound, and non-hydroxyl olefinic unsaturated compound under the action of a catalyst is carried out to obtain modified polyhydroxyl polysiloxane; S2. The modified polyhydroxy polysiloxane is reacted with an olefinic unsaturated carboxylic acid under the action of a dehydrating agent and an esterification catalyst to prepare a photocurable modified organosilicon resin.

[0015] Preferably, in step S1, the number average molecular weight of the hydrogen-containing polysiloxane is 1200~20000 g / mol, and the active hydrogen content is 0.05~1.2 wt%.

[0016] Preferably, in step S1, the hydroxyl-containing olefinic unsaturated compound is selected from any one of allyl alcohol, hydroxyethyl methacrylate, hydroxyethyl acrylate, 4-penten-1-ol, 5-hexen-1-ol, 7-octen-1-ol, 10-undecen-1-ol, 3-buten-2-ol, and allyl alcohol polyoxyethylene ether.

[0017] Preferably, in step S1, the non-hydroxyl olefin unsaturated compound is selected from any one of aliphatic olefins, aromatic olefins, and olefin unsaturated polyethers.

[0018] Furthermore, the aliphatic olefin is selected from any one of octene, nonene, decene, undecene, and dodecene; the aromatic olefin is selected from any one of styrene and α-methylstyrene; and the olefinic unsaturated polyether is selected from any one of allyl polyoxyethylene ether, allyl polyoxypropylene ether, allyl polyoxyethylene polyoxypropylene random polyether, allyl polyoxyethylene polyoxypropylene block polyether, and allyl polyoxybutylene ether.

[0019] Preferably, in step S1, the catalyst is selected from platinum catalysts; the platinum catalyst is selected from at least one of Karstedt catalysts or MOF-modified Karstedt catalysts.

[0020] Preferably, the amount of platinum catalyst used is 1 to 10 ppm.

[0021] Preferably, in step S2, the olefinic unsaturated carboxylic acid is selected from acrylic acid, 3-butenoic acid, 4-pentenoic acid, 11-undecenoic acid, and allyloxyacetic acid.

[0022] Preferably, in step S2, the dehydrating agent is selected from carbodiimide dehydrating agents. The carbodiimide dehydrating agents include, but are not limited to, N,N-dicyclohexylcarbodiimide.

[0023] Preferably, in step S2, the esterification catalyst is selected from 4-dimethylaminopyridine.

[0024] Preferably, the amount of the esterification catalyst is 100~1000 ppm.

[0025] Preferably, the molar ratio of the hydrogen-containing polysiloxane, the hydroxyl-containing olefinic unsaturated compound, and the non-hydroxyl olefinic unsaturated compound is 1:(1~30):(1~40).

[0026] Preferably, the molar ratio between the hydroxyl-containing olefinic unsaturated compound, the olefinic unsaturated carboxylic acid, and the dehydrating agent is 1:(1~1.2):(1~1.2).

[0027] Preferably, in step S1, the reaction temperature of the hydrosilylation reaction is 60~130℃, and the reaction time is 1~24h; Preferably, in step S2, the esterification reaction is carried out at a temperature of 30-80°C for 2-24 hours.

[0028] Thirdly, the present invention provides the application of the aforementioned photocurable modified silicone resin in photocurable coatings.

[0029] Fourthly, the present invention provides a stain-resistant and graffiti-resistant photocurable coating, comprising a base resin and a photoinitiator; the base resin comprises the photocurable modified silicone resin described in the first aspect.

[0030] Preferably, based on a weight percentage of 100 wt% for the anti-fouling and anti-graffiti UV-curable coating, the amount of photoinitiator added is 1 wt% to 10 wt%.

[0031] Compared with the prior art, the present invention has the following beneficial effects: This invention introduces specific structural side chains into the organopolysiloxane chain through molecular structure design, thereby achieving photocuring modification of organosilicon resin. It can be rapidly cured into a film by photoinitiation, forming a dense low surface energy cross-linked network that can effectively resist the wetting and penetration of pollutants such as water, oil, paint, and ink. It exhibits excellent long-lasting anti-fouling and anti-graffiti performance and can meet the protection needs of multiple scenarios. Attached Figure Description

[0032] Figure 1 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR1 in Example 1 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified organosilicon resin AR1.

[0033] Figure 2 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR2 in Example 2 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified organosilicon resin AR2.

[0034] Figure 3The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR3 in Example 3 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified organosilicon resin AR3.

[0035] Figure 4 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR4 in Example 4 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified organosilicon resin AR4.

[0036] Figure 5 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR5 of Example 5 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified silicone resin AR5.

[0037] Figure 6 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR6 of Example 6 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified silicone resin AR6.

[0038] Figure 7 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR7 of Example 7 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified organosilicon resin AR7.

[0039] Figure 8 The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR8 of Example 8 are shown, where a is the modified polyhydroxy polysiloxane intermediate and b is the photocurable modified organosilicon resin AR8.

[0040] Figure 9 Photos taken for anti-graffiti performance testing. Detailed Implementation

[0041] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0042] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0043] Unless otherwise specified, room temperature or normal temperature in the embodiments of the present invention refers to 25±1℃.

[0044] Example 1

[0045] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.5 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=2000 g / mol, hydrogen content 0.3%), 2.5 mol of allyl alcohol, 0.5 mol of 1-octene, 3 ppm of Karstedt catalyst, 2.6 mol of acrylic acid, 2.6 mol of N,N-dicyclohexylcarbodiimide, and 200 ppm of 4-dimethylaminopyridine.

[0046] The preparation method is as follows: A measured amount of hydrogen-containing polysiloxane, allyl alcohol, and 1-octene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 75°C and slowly increased. When the temperature reached 40°C, the Karstedt catalyst was added all at once. After the temperature stabilized at 75°C, the reaction continued for 2 h. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 40°C. After stirring for 4 h, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified silicone resin AR1 with a viscosity of 45 cSt.

[0047] The synthesis route of the photocurable modified silicone resin AR1 in Example 1 is shown below: .

[0048] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR1 in Example 1 are shown below. Figure 1 As shown.

[0049] Example 2

[0050] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.5 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=2000 g / mol, hydrogen content 0.3%), 2.5 mol of allyl alcohol, 0.5 mol of styrene, 3 ppm of Karstedt catalyst, 2.6 mol of acrylic acid, 2.6 mol of N,N-dicyclohexylcarbodiimide, and 200 ppm of 4-dimethylaminopyridine.

[0051] The preparation method is as follows: A measured amount of hydrogen-containing polysiloxane, allyl alcohol, and styrene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 75°C and slowly increased. When the temperature reached 40°C, the Karstedt catalyst was added all at once. After the temperature stabilized at 75°C, the reaction continued for 2 hours. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 40°C. After stirring for 4 hours, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified silicone resin AR2 with a viscosity of 42 cSt.

[0052] The synthesis route of the photocurable modified silicone resin AR2 in Example 2 is shown below: .

[0053] Example 2: Fourier transform infrared spectra of modified polyhydroxy polysiloxane intermediate and photocurable modified silicone resin AR2 are shown below. Figure 2 As shown.

[0054] Example 3

[0055] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.5 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=2000 g / mol, hydrogen content 0.3%), 2.5 mol of allyl alcohol polyoxyethylene ether (300 g / mol), 0.5 mol of styrene, 3 ppm of Karstedt catalyst, 2.6 mol of acrylic acid, 2.6 mol of N,N-dicyclohexylcarbodiimide, and 200 ppm of 4-dimethylaminopyridine.

[0056] The preparation method is as follows: A measured amount of hydrogen-containing polysiloxane, allyl alcohol polyoxyethylene ether, and styrene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 75°C and slowly increased. When the temperature reached 40°C, the Karstedt catalyst was added all at once. After the temperature stabilized at 75°C, the reaction continued for 2 hours. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 40°C. After stirring for 4 hours, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified organosilicon resin AR3 with a viscosity of 64 cSt.

[0057] The synthesis route of the photocurable modified silicone resin AR3 in Example 3 is shown below: .

[0058] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR3 in Example 3 are shown below. Figure 3 As shown.

[0059] Example 4

[0060] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.5 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=2000 g / mol, hydrogen content 0.3%), 2.5 mol of hydroxyethyl methacrylate, 0.5 mol of styrene, 3 ppm of Karstedt catalyst, 2.6 mol of acrylic acid, 2.6 mol of N,N-dicyclohexylcarbodiimide, and 200 ppm of 4-dimethylaminopyridine.

[0061] The preparation method is as follows: A measured amount of hydrogen-containing polysiloxane, hydroxyethyl methacrylate, and styrene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 75°C and slowly increased. When the temperature reached 40°C, the Karstedt catalyst was added all at once. After the temperature stabilized at 75°C, the reaction continued for 2 hours. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 40°C. After stirring for 4 hours, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified silicone resin AR4 with a viscosity of 47 cSt.

[0062] The synthesis route of the photocurable modified silicone resin AR4 in Example 4 is shown below: .

[0063] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified organosilicon resin AR4 in Example 4 are shown below. Figure 4 As shown.

[0064] Example 5

[0065] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.25 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=4000 g / mol, hydrogen content 0.6%), 4 mol of allyl alcohol, 2 mol of 1-octene, 5 ppm of Karstedt catalyst, 4.1 mol of acrylic acid, 4.1 mol of N,N-dicyclohexylcarbodiimide, and 300 ppm of 4-dimethylaminopyridine.

[0066] The preparation method is as follows: A measured amount of hydrogen-containing polysiloxane, allyl alcohol, and 1-octene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 100 °C and slowly increased. When the temperature reached 40 °C, the Karstedt catalyst was added all at once. After the temperature stabilized at 100 °C, the reaction continued for 2 h. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 45 °C. After stirring for 6 h, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified silicone resin AR5 with a viscosity of 92 cSt.

[0067] The synthesis route of the photocurable modified silicone resin AR5 in Example 5 is shown below: .

[0068] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR5 in Example 5 are shown below. Figure 5 As shown.

[0069] Example 6

[0070] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.25 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=4000 g / mol, hydrogen content 0.6%), 5 mol of allyl alcohol, 1 mol of 1-octene, 5 ppm of Karstedt catalyst, 5.1 mol of acrylic acid, 5.1 mol of N,N-dicyclohexylcarbodiimide, and 300 ppm of 4-dimethylaminopyridine.

[0071] The preparation method is the same as in Example 5, and the photocurable modified silicone resin AR6 with a viscosity of 103 cSt is obtained.

[0072] The synthesis route of the photocurable modified silicone resin AR6 in Example 6 is shown below: .

[0073] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR6 in Example 6 are shown below. Figure 6 As shown.

[0074] Example 7

[0075] This embodiment provides a photocurable modified organosilicon resin, which comprises the following raw materials: 0.2 mol of hydrogen-containing polysiloxane (Sloco New Materials, Mn=6000 g / mol, hydrogen content 0.5%), 4 mol of allyl alcohol polyoxyethylene ether (300 g / mol), 2 mol of styrene, 5 ppm of Karstedt catalyst, 4.1 mol of allyloxyacetic acid, 4.1 mol of N,N-dicyclohexylcarbodiimide, and 300 ppm of 4-dimethylaminopyridine.

[0076] A measured amount of hydrogen-containing polysiloxane, allyl alcohol polyoxyethylene ether, and styrene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 110 °C and slowly increased. When the temperature reached 40 °C, the Karstedt catalyst was added all at once. After the temperature stabilized at 110 °C, the reaction continued for 3 h. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, allyloxyacetic acid was added, and the temperature was raised to 50 °C. After stirring for 4 h, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified organosilicon resin AR7 with a viscosity of 135 cSt.

[0077] The synthesis route of the photocurable modified silicone resin AR7 in Example 7 is shown below: .

[0078] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR7 in Example 7 are shown below. Figure 7 As shown.

[0079] Example 8

[0080] This embodiment provides a photocurable modified silicone resin, which comprises the following raw materials: 0.1 mol of side-containing hydrogen polysiloxane (Sloco New Materials, Mn=9000 g / mol, hydrogen content 0.4%), 3 mol of allyl alcohol, 0.8 mol of styrene, 6 ppm of MOF-modified Karstedt catalyst (prepared according to the method of Example 1 in patent CN202510943166.5), 3.1 mol of acrylic acid, 3.1 mol of N,N-dicyclohexylcarbodiimide, and 500 ppm of 4-dimethylaminopyridine.

[0081] A measured amount of hydrogen-containing polysiloxane, allyl alcohol, and styrene were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 110 °C and slowly increased. When the temperature reached 40 °C, the MOF-modified Karstedt catalyst was added all at once. After the temperature stabilized at 110 °C, the reaction continued for 3 h. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 60 °C. After stirring for 4 h, the mixture was filtered, and the filtrate was collected to obtain a photocurable modified silicone resin AR8 with a viscosity of 223 cSt.

[0082] The synthesis route of the photocurable modified silicone resin AR8 in Example 8 is shown below: .

[0083] The Fourier transform infrared spectra of the modified polyhydroxy polysiloxane intermediate and the photocurable modified silicone resin AR8 in Example 8 are shown below. Figure 8 As shown.

[0084] Comparative Example 1 This comparative example provides a modified organosilicon resin comprising the following raw materials: 0.5 mol of a hydrogen-containing polysiloxane (Sloco New Materials, Mn=2000 g / mol, hydrogen content 0.3%), 3 mol of allyl alcohol, 3 ppm of Karstedt catalyst, 3.1 mol of acrylic acid, 3.1 mol of N,N-dicyclohexylcarbodiimide, and 200 ppm of 4-dimethylaminopyridine.

[0085] The preparation method is as follows: A measured amount of hydrogen-containing polysiloxane and allyl alcohol were added to a 3000 mL four-necked flask equipped with a thermometer, a stirrer, and a condenser. After stirring until homogeneous, the temperature was set to 75°C and slowly increased. When the temperature reached 40°C, the Karstedt catalyst was added all at once. After the temperature stabilized at 75°C, the reaction continued for 2 h. After naturally cooling to room temperature, a modified polyhydroxy polysiloxane intermediate was obtained. Subsequently, measured amounts of N,N-dicyclohexylcarbodiimide and 4-dimethylaminopyridine were added to the obtained modified polyhydroxy polysiloxane intermediate in sequence. After stirring until homogeneous, acrylic acid was added, and the temperature was raised to 40°C. After stirring for 4 h, the mixture was filtered, and the filtrate was collected to obtain modified organosilicon resin B1.

[0086] The synthesis route of the modified organosilicon resin B1 in Comparative Example 1 is shown below: .

[0087] Comparative Example 2 The only difference between this comparative example and Example 1 is that acrylic acid is replaced with an equimolar amount of cinnamic acid. Everything else is the same as in Example 1, and modified organosilicon resin B2 is prepared.

[0088] The synthetic route of the modified organosilicon resin B2 in Comparative Example 2 is shown below: .

[0089] Application Example 1 95 wt% of the photocurable modified silicone resin AR1 prepared in Example 1 was mixed with 5 wt% of the photoinitiator TPO to obtain a photocurable coating. The photocurable coating was applied to a rigid PC board and allowed to level naturally. Then, it was cured by irradiation with a mercury lamp (200-450 nm broad spectrum, main peak 365 nm; 120-140 W / cm) to obtain a cured paint film.

[0090] Application Examples 2-8 The only difference between Application Examples 2-8 and Application Example 1 is that the matrix resin used in Application Examples 2-8 is the photocurable modified silicone resin (AR2-AR8) prepared in Examples 2-8.

[0091] Comparative Application Examples 1-2 The difference between Comparative Application Example 1-2 and Application Example 1 is that the matrix resin used in Comparative Application Example 1-2 is the modified organosilicon resin (B1~B2) prepared in Comparative Example 1-2.

[0092] Performance testing: The paint films obtained in Application Examples 1 to 8 and Comparative Application Examples 1 to 2 were tested according to the following method.

[0093] (1) Gloss: The gloss of the coating surface was tested in accordance with GB / T 9754-2025 standard.

[0094] (2) Contact angle test: The static water contact angle was measured using the seated drop method, referring to the ISO 19403 series of standards. In an environment with a temperature of 23±2°C and a relative humidity of 50±5%, a 3.0 μL droplet of ultrapure water was gently deposited onto the coating surface using a contact angle measuring instrument. After it stabilized, the contact angle was calculated by fitting the Young-Laplace equation. At least 5 different locations were randomly measured for each sample, and the results were taken as the arithmetic mean.

[0095] (3) Anti-graffiti performance test: Using an oil-based marker, draw a straight line about 10 cm long on the cured paint film surface with uniform force, and let it sit at room temperature for 5 minutes. Then, place a 500 g weight on the slider wrapped with a dry paper towel, so that the wiping surface bears the weight equivalent to 500 g. Wipe back and forth along the graffiti line 10 times. If there is no visible residue on the surface, it is recorded as one effective erasure. Repeat the graffiti-erasure process in the same position until there are indelible residue marks on the surface. Record the total number of erasures to evaluate the anti-graffiti performance. Test 3 different positions for each sample and take the arithmetic mean. The higher the total number of erasures, the better the anti-graffiti performance.

[0096] (4) Durability: The cured paint film was placed in a 60℃ oven for 30 min for heat treatment, and after being taken out and cooled to room temperature, its anti-graffiti performance was tested.

[0097] Table 1 Performance test results of Application Examples 1-8 and Comparative Application Examples 1-2

[0098] The results show that the present invention introduces a specific structural side chain on the organopolysiloxane chain to achieve photocuring modification of organosilicon resin. It can be rapidly cured into a film by photoinitiation, forming a dense low surface energy cross-linked network. The resulting paint film has high gloss and high hydrophobicity (gloss of paint film ≥94Gs, static contact angle ≥125°), and can effectively resist the wetting and penetration of contaminants such as ink, exhibiting excellent long-lasting anti-fouling and anti-graffiti performance.

[0099] The above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A photocured modified silicone resin, characterized by, It has the structure shown in equation (1): Formula (1); wherein R1is a C8-C12 alkyl group, or ; R2is alkylene, or ; R3 is an alkyl group; R4is a carbon-carbon single bond, alkylene or ; R5, R 13 is -H or alkyl; R6, R7, R8, R9, R 10 , R 11 , R 12 each independently is alkylene; * indicates a substitution site; a, b, and c are each an independent natural number from 1 to 100; m, n, j, and k are each an independent natural number from 0 to 20. m and n are not both 0 at the same time, and j and k are both 0 at the same time.

2. The photocurable modified silicone resin according to claim 1, characterized in that, R1is ; R2is ; a is a natural number from 1 to 30; b is a natural number from 1 to 48; c is a natural number from 1 to 50.

3. The method for producing a photocured modified silicone resin according to any one of claims 1 to 2, characterized by, Includes the following steps: S1. Hydrosilylation reaction of hydrogen-containing polysiloxane, hydroxyl-containing olefinic unsaturated compound, and non-hydroxyl olefinic unsaturated compound under the action of a catalyst is carried out to obtain modified polyhydroxyl polysiloxane; S2. The modified polyhydroxy polysiloxane is reacted with an olefinic unsaturated carboxylic acid under the action of a dehydrating agent and an esterification catalyst to prepare a photocurable modified organosilicon resin.

4. The method for preparing the photocurable modified organosilicon resin according to claim 3, characterized in that, In step S1, The hydrogen-containing polysiloxane has a number-average molecular weight of 1200~20000 g / mol and an active hydrogen content of 0.05~1.2 wt%. The hydroxyl-containing olefinic unsaturated compound is selected from any one of allyl alcohol, hydroxyethyl methacrylate, hydroxyethyl acrylate, 4-penten-1-ol, 5-hexen-1-ol, 7-octen-1-ol, 10-undecen-1-ol, 3-buten-2-ol, and allyl alcohol polyoxyethylene ether. The non-hydroxyl-containing olefinic unsaturated compound is selected from any one of aliphatic olefins, aromatic olefins, and olefinic unsaturated polyethers; the aliphatic olefin is selected from any one of octene, nonene, decene, undecene, and dodecene; the aromatic olefin is selected from any one of styrene and α-methylstyrene; the olefinic unsaturated polyether is selected from any one of allyl polyoxyethylene ether, allyl polyoxypropylene ether, allyl polyoxyethylene polyoxypropylene random polyether, allyl polyoxyethylene polyoxypropylene block polyether, and allyl polyoxybutylene ether. The catalyst is selected from platinum catalysts.

5. The method for preparing the photocurable modified organosilicon resin according to claim 3, characterized in that, In step S2, The olefinic unsaturated carboxylic acid is selected from acrylic acid, 3-butenoic acid, 4-pentenoic acid, 11-undecenoic acid, and allyloxyacetic acid; The dehydrating agent is selected from carbodiimide dehydrating agents; The esterification catalyst is selected from 4-dimethylaminopyridine.

6. The method for preparing the photocurable modified organosilicon resin according to claim 3, characterized in that, The molar ratio of the hydrogen-containing polysiloxane, the hydroxyl-containing olefinic unsaturated compound, and the non-hydroxyl olefinic unsaturated compound is 1:(1~30):(1~40). The molar ratio between the hydroxyl-containing olefinic unsaturated compound, the olefinic unsaturated carboxylic acid, and the dehydrating agent is 1:(1~1.2):(1~1.2).

7. The method for preparing the photocurable modified organosilicon resin according to claim 3, characterized in that, In step S1, the reaction temperature of the hydrosilylation reaction is 60~130℃, and the reaction time is 1~24 h; In step S2, the esterification reaction is carried out at a temperature of 30-80°C for 2-24 hours.

8. The application of the photocurable modified silicone resin according to any one of claims 1 to 2 in photocurable coatings.

9. A stain-resistant and graffiti-resistant UV-curable coating, characterized in that, It includes a matrix resin and a photoinitiator; the matrix resin includes the photocurable modified silicone resin according to any one of claims 1 to 2.

10. The anti-fouling and anti-graffiti UV-curable coating according to claim 9, characterized in that, Based on a weight percentage of 100 wt% for the anti-fouling and anti-graffiti UV-curable coating, the amount of photoinitiator added is 1 wt% to 10 wt%.

Citation Information

Patent Citations

  • Acrylate group modified organic silicone when existence of rhodium catalyst

    CN101092481A

  • Photo-curing organic silicon and UV (ultraviolet) adhesive composition for difficult-to-adhere materials

    CN119264439A

  • MOF modified metal catalyst as well as preparation method and application thereof

    CN120438063A