Preparation method and application of water-based fluorine-free hand mark-free water-repellent finishing agent
A water-based fluorine-free water-repellent finishing agent was prepared by constructing an amino-containing polysiloxane adduct through a mercapto-olefin addition reaction. This solved the problems of stiff hand feel and easy scratching of water-repellent agents in the prior art, and achieved softness, washability and water repellency of the fabric.
Patent Information
- Application Number
- CN202611514733.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing fluorine-free water-repellent finishing agents struggle to balance water repellency, washability, and a soft hand feel, and are prone to scratches.
A amino-containing polysiloxane adduct was constructed by thiol-olefin addition reaction to prepare a water-based, fluorine-free, scratch-resistant, water-repellent finishing agent. Combined with organic acid and emulsifier, it forms an aqueous emulsion for application in fabric finishing.
This technology enables fabrics to possess excellent water repellency and washability while also having a soft hand feel and not leaving scratch marks after being gripped, thus improving the overall performance of water repellency, washability, and hand feel.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of finishing agent technology, specifically to a method for preparing and applying a water-based, fluorine-free, scratch-resistant, water-repellent finishing agent. Background Technology
[0002] Fluorinated water-repellent agents have long dominated the textile functional finishing market due to their excellent water and oil repellency. However, their production and use generate persistent pollutants such as perfluorooctanoic acid (PFOA) and perfluorooctane sulfonic acid (PFOS), which have been gradually restricted by domestic and international regulations. Developing fluorine-free water-repellent finishing agents has become an industry consensus. Existing fluorine-free water-repellent finishing agents mainly include acrylates, polyurethanes, and silicones. Acrylates have lower costs and better water-repellent effects, but their resin films are hard and brittle, and long-chain alkyl side chains are prone to crystallization, resulting in stiff fabrics after finishing. The film layer breaks after being scratched or rubbed and cannot recover, easily producing noticeable scratch marks. Furthermore, to achieve water repellency requirements, large quantities are often used, further exacerbating these defects. Polyurethanes have a relatively good hand feel, but are more expensive and have poor moisture permeability. Silicones have a soft hand feel, but when used alone, their water repellency is low and their wash resistance is poor. While compounding or copolymerizing silicones with acrylates can improve the hand feel to some extent, it is still difficult to simultaneously meet the comprehensive requirements of water repellency, wash resistance, and no scratch marks. Therefore, developing a water-based, fluorine-free water-repellent finishing agent that combines water repellency, washability, soft feel, and no scratches is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0003] The purpose of this disclosure is to provide a method for preparing and applying a water-based, fluorine-free, scratch-resistant, water-repellent finishing agent to address the shortcomings in related technologies.
[0004] According to a first aspect of the present disclosure, a method for preparing a water-based, fluorine-free, scratch-resistant, water-repellent finishing agent is provided, the preparation method comprising: Step 1: Prepare an amino-containing silane compound; the amino-containing silane compound has the structure represented by the following formula IA:
[0005] Wherein, n1 is selected from 6-20; R 11 R 12 R 15 R 16 Each is independently selected from hydrogen, substituted or unsubstituted C1-C30 alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted 3-30 membered heterocyclic, or substituted or unsubstituted 5-30 membered heteroaryl; R 13 R 14Each is independently selected from substituted or unsubstituted C1-C30 alkyl groups, or substituted or unsubstituted C1-C30 alkoxy groups; R 17 R 18 Each is independently selected from substituted or unsubstituted C1-C10 alkylene groups or substituted or unsubstituted C1-C30 alkene groups; Step 2: Mix the amino-containing silane compound obtained in Step 1 with the polythiol compound, and carry out a mercapto-olefin addition reaction in the presence of a free radical initiator to obtain the amino-containing polysiloxane adduct. Step 3: The amino-containing polysiloxane adduct obtained in Step 2 is mixed with organic acid and water, and then sheared and emulsified to obtain the water-based fluorine-free, scratch-resistant, water-repellent finishing agent.
[0006] In one aspect of the embodiments of this disclosure, the polythiol compound is a compound containing two or more thiol groups, selected from one or more of C2-C18 alkylene dithiols and polythiols containing ester bonds; The C2-C18 alkylene dithiols are selected from one or more of 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, and 1,12-dodecanedithiol; the polythiols containing ester bonds are selected from one or more of ethylene glycol bis(3-mercaptopropionate), 1,4-butanediol bis(3-mercaptopropionate), 1,6-hexanediol bis(3-mercaptopropionate), neopentyl glycol bis(3-mercaptopropionate), ethylene glycol bis(mercaptoacetate), trimethylolpropane tri(3-mercaptopropionate), and pentaerythritol tetra(3-mercaptopropionate).
[0007] In one aspect of this disclosure, in step 2, the free radical initiator is selected from thermal initiators and / or photoinitiators; the thermal initiator is selected from one or more of azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobiscyanopentanoic acid, azobisisobutyramidazoline hydrochloride, benzoyl peroxide, and di-tert-butyl peroxide; the photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and benzophenone; the amount of the free radical initiator is 0.1%-2% of the total mass of the amino-containing silane compound and the polythiol compound.
[0008] In one aspect of the embodiments of this disclosure, in step 3, the organic acid is selected from one or more of formic acid, acetic acid, propionic acid, lactic acid, glycolic acid, and citric acid.
[0009] In one aspect of this disclosure, the amino-containing silane compound has a structure represented by the formula II-A:
[0010] Wherein, n1 is selected from 6-20; R 17 R 18 Each is independently selected from C1-C5 alkylene groups; R 19 R 20 Each is independently selected from C1-C5 alkyl groups.
[0011] In one aspect of the embodiments of this disclosure, the polythiol compound is selected from trimethylolpropane tris(3-mercaptopropionate) or pentaerythritol tetra(3-mercaptopropionate); The amino-containing polysiloxane adduct obtained in step 2 has the structure represented by formula I-B1 or formula I-B2:
[0012]
[0013] Wherein, n1 is selected from 6-20; R 17 R 18 R 19 R 20 Each is independently selected from C1-C5 alkylene groups.
[0014] In one aspect of this disclosure, the amino-containing silane compound has a structure represented by the following formula III-A:
[0015] The amino-containing silane compound having the structure represented by Formula III-A is prepared by the following steps: Step 1-1: Mix N,N-dimethylformamide, deionized water, and acetic acid. Slowly add 1,3-divinyl-1,1,3,3-tetramethyldisilazane dropwise while stirring at room temperature. After the addition is complete, purge with nitrogen gas for 0.5-2 hours to remove the ammonia gas generated in the reaction. Then dry with a drying agent to obtain a vinyl dimethylsilanol N,N-dimethylformamide solution. The mass ratio of 1,3-divinyl-1,1,3,3-tetramethyldisilazane to deionized water is 1:(0.15-0.25), and the amount of acetic acid used is 0.5%-1.5% of the mass of 1,3-divinyl-1,1,3,3-tetramethyldisilazane. Step 1-2: Under nitrogen protection, the N,N-dimethylformamide solution of vinyl dimethylsilanol obtained in Step 1-1, hexamethylcyclotrisiloxane, and toluene are mixed, and 1,8-diazabicycloundec-7-ene is added as a catalyst. The ring-opening polymerization reaction is carried out at room temperature for 3-8 hours. Then, acetic acid is added to neutralize and terminate the reaction. After washing with water, drying, and removing toluene and N,N-dimethylformamide under reduced pressure, α-vinyl-ω-hydroxy polydimethylsiloxane is obtained. The molar ratio of vinyl dimethylsilanol to hexamethylcyclotrisiloxane is 1:(2-15), and the amount of 1,8-diazabicycloundec-7-ene is 2%-3% of the mass of hexamethylcyclotrisiloxane. The α-vinyl-ω-hydroxy polydimethylsiloxane has the following structural formula:
[0016] Steps 1-3: Under nitrogen protection, the α-vinyl-ω-hydroxy polydimethylsiloxane obtained in step 1-2 is mixed with aminoethylaminopropyltrialkoxysilane, and 1,8-diazabicycloundec-7-ene is added as a catalyst. The mixture is reacted at 60-75°C for 2-4 hours. Then, unreacted aminoethylaminopropyltrialkoxysilane is removed at 140-160°C and -0.095 MPa to obtain the amino-containing silane compound shown in Formula III-A.
[0017] In one aspect of the embodiments of this disclosure, the amino-containing polysiloxane adduct obtained in step 2 has a structure represented by formula II-B1 or formula II-B2:
[0018]
[0019] In one aspect of this disclosure, step 2 includes: Under nitrogen protection, the amino-containing silane compound obtained in step 1 is mixed with trimethylolpropane tris(3-mercaptopropionate) or pentaerythritol tetra(3-mercaptopropionate), a free radical thermal initiator is added, and after stirring evenly, the mixture is heated to 60-80°C to carry out a mercapto-olefin addition reaction for 3-5 hours. After the reaction is completed, the low-boiling-point substances are removed under reduced pressure to obtain an amino-containing polysiloxane adduct; the free radical thermal initiator is azobisisobutyronitrile and / or azobisisoheptanenitrile. In one aspect of this disclosure, step 3 includes: The amino-containing polysiloxane adduct obtained in step 2 is mixed with an emulsifier, stirred evenly, and then acetic acid is added. Stirring is continued for 10-30 minutes. Then, deionized water is added in portions under shear conditions of 2500-5000 r / min. Shear emulsification is carried out for 1-3 hours to obtain the water-based fluorine-free, scratch-free, water-repellent finishing agent. The emulsifier is a nonionic emulsifier selected from one or more of fatty alcohol polyoxyethylene ether and isomeric fatty alcohol polyoxyethylene ether, and the amount of the emulsifier is 0.1-10% of the mass of the amino-containing polysiloxane adduct.
[0020] In one aspect of the embodiments of this disclosure, preferably, when the polythiol compound is trimethylolpropane tris(3-mercaptopropionate), the molar ratio of the amino-containing silane compound to trimethylolpropane tris(3-mercaptopropionate) is (2.8-3.2):1; when the polythiol compound is pentaerythritol tetra(3-mercaptopropionate), the molar ratio of the amino-containing silane compound to pentaerythritol tetra(3-mercaptopropionate) is (3.8-4.2):1.
[0021] In this disclosure, the number of repeating units 12 in Formula III-A, Formula II-B1, and Formula II-B2 represents the average degree of polymerization calculated based on the molar ratio of the feed.
[0022] According to a second aspect of the present disclosure, a water-based, fluorine-free, scratch-resistant water-repellent finishing agent is provided, wherein the water-based, fluorine-free, scratch-resistant water-repellent finishing agent is prepared by the aforementioned preparation method.
[0023] According to a third aspect of the present disclosure, the application of the aforementioned water-based, fluorine-free, scratch-resistant water-repellent finishing agent in fluorine-free water-repellent finishing of fabrics is provided.
[0024] In one aspect of the present disclosure, the application includes: diluting the water-based fluorine-free, scratch-resistant water-repellent finishing agent with water to prepare a finishing solution, padding the fabric with the solution, and then pre-drying and baking the fabric to complete the fluorine-free water-repellent finishing. The concentration of the water-based, fluorine-free, scratch-resistant water-repellent finishing agent in the finishing solution is 30-90 g / L; the padding rate of the fabric after padding treatment is 60%-80%; the pre-drying temperature is 80-100℃; the baking temperature is 150-170℃ and the time is 1-5 min; the fabric is a cellulose fiber fabric, polyester fiber fabric, polyamide fiber fabric or a blended fabric thereof.
[0025] The technical solutions provided by the embodiments of this disclosure may include the following beneficial effects: As can be seen from the above embodiments, this disclosure constructs an amino-containing polysiloxane adduct by combining a polythiol compound with an amino-containing silane compound through a mercapto-olefin addition reaction. The resulting water-based fluorine-free water-repellent finishing agent imparts excellent water-repellent and wash-resistant properties to the fabric, while also providing a soft hand feel and preventing hand scratches after gripping, thus achieving a synergistic improvement in water repellency, wash resistance, hand feel, and no hand scratches.
[0026] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit this disclosure. Detailed Implementation
[0027] Exemplary embodiments will now be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this disclosure. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this disclosure as detailed in the appended claims.
[0028] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. The embodiments described herein are illustrative in nature and are used to provide a basic understanding of this application. The embodiments of this application should not be construed as limiting this application.
[0029] For the sake of brevity, this article only discloses a few specific numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.
[0030] In this disclosure, the term "alkyl" refers to an aliphatic hydrocarbon group, which can be straight-chain or branched. Branched refers to one or more lower alkyl groups, such as methyl, ethyl, or propyl, that link a linear alkyl chain. "Lower alkyl" refers to a group containing about 1 to about 6 carbon atoms in the chain, which can be straight-chain or branched.
[0031] In this disclosure, the term "alkylene" refers to a divalent aliphatic hydrocarbon group formed by the loss of a hydrogen atom from an alkyl group, having two linking sites, and can be straight-chain or branched. Branching refers to one or more lower alkyl groups, such as methyl, ethyl, or propyl, that link a linear alkylene chain. "Lower alkylene" refers to a divalent group containing about 1 to about 6 carbon atoms in the chain, and can be straight-chain or branched. Alkylenes include, for example, methylene, 1,2-ethylene, 1,3-propylene, 1,4-butylene, isobutylene, and 1,6-hexylene.
[0032] In this disclosure, the term "alkoxy" refers to -O-alkyl. Alkoxy can refer to a straight-chain, branched, or cyclic, saturated or unsaturated oxy-hydrocarbon chain, including, for example, methoxy, ethoxy, propoxy, isopropoxy, butoxy, tert-butoxy, and pentoxy. Alkoxy may optionally be substituted by one or more alkoxy substituents ("substituted alkoxy").
[0033] In this disclosure, the term "alkeneoxy" refers to -O-alkylene. Alkeneoxy can refer to a straight-chain, branched, or cyclic, saturated, or unsaturated oxy-alkylene chain, including, for example, methyleneoxy, ethoxy, propoxy, isopropoxy, butoxy, and pentyleoxy. Alkeneoxy may optionally be substituted with one or more alkoxy substituents ("substituted alkeneoxy").
[0034] In this disclosure, the term "cycloalkyl" refers to a non-aromatic mono- or polycyclic ring system, preferably containing about 5 to about 7 ring atoms. The cycloalkyl group may optionally be substituted with one or more "cyclic substituents," which may be the same or different, as defined above. Suitable monocyclic cycloalkyl groups, without limitation, include cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, etc. Suitable polycyclic cycloalkyl groups, without limitation, include 1-decahydronaphthyl, norcamphenyl, adamantyl, etc. In this disclosure, the term "cycloalkoxy" refers to a group in which one or more carbon atoms in the mono- or polycyclic ring system of the "cycloalkyl" group are substituted with oxygen atoms.
[0035] In this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0036] In this description, unless otherwise stated, "above" and "below" include the stated number.
[0037] Unless otherwise stated, the terms used in this disclosure have their common meanings as commonly understood by those skilled in the art. Unless otherwise stated, the values of the parameters mentioned in this disclosure can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this disclosure).
[0038] The term "about" is used to describe and indicate small variations. When used in conjunction with an event or situation, the term may refer to examples in which the event or situation occurred precisely or in examples in which the event or situation occurred very approximately. For example, when used in conjunction with numerical values, the term may refer to a range of variation less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. Additionally, quantities, ratios, and other numerical values are sometimes presented in range format herein. It should be understood that such range format is for convenience and brevity and should be interpreted flexibly to include not only numerical values explicitly specified as range limits but also all individual numerical values or subranges covered within the range, as if each numerical value and subrange were explicitly specified.
[0039] The list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms can mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another instance, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0040] The present disclosure will be further described below by way of specific embodiments. Unless otherwise specified, all chemical reagents used in the embodiments of the present disclosure are obtained through conventional commercial means. Unless otherwise specified, all contents mentioned below are mass contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.
[0041] Example Example 1: Example 1 includes the following steps: 1. Preparation of amino-containing silane compounds (Formula III-A): 1.1. Preparation of vinyldimethylsilane: 46.25 g of N,N-dimethylformamide, 39.6 g of deionized water and 1.3 g of acetic acid were added to a flask, and stirring was started. 185.42 g of 1,3-divinyl-1,1,3,3-tetramethyldisilazane was slowly added dropwise at room temperature. After the addition was complete, nitrogen gas was bubbled through the system for 1 h to remove ammonia. After drying with anhydrous sodium sulfate, an N,N-dimethylformamide solution of vinyldimethylsilane was obtained. 1.2. Preparation of α-vinyl-ω-hydroxy polydimethylsiloxane: Under nitrogen protection, 100 g of the above-mentioned vinyl dimethylsilanol N,N-dimethylformamide solution, 200.00 g of toluene and 564.72 g of hexamethylcyclotrisiloxane were added to a flask, and 14.00 g of 1,8-diazabicycloundec-7-ene was added as a catalyst. The ring-opening polymerization reaction was carried out at room temperature for 5 h. 5.52 g of acetic acid was added for neutralization for 10 min, and the mixture was washed 5 times with deionized water. After drying the organic phase with anhydrous sodium sulfate, toluene and N,N-dimethylformamide were removed under reduced pressure to obtain colorless and transparent α-vinyl-ω-hydroxy polydimethylsiloxane; it has the following structural formula:
[0042] 1.3. Preparation of compound III-A: Under nitrogen protection, 99 g of the above-mentioned α-vinyl-ω-hydroxy polydimethylsiloxane, 15.70 g of aminoethylaminopropyltrimethoxysilane and 1.66 g of 1,8-diazabicycloundec-7-ene were added to a flask and the mixture was heated to 69 °C and reacted for 3 h; then, unreacted aminoethylaminopropyltrimethoxysilane was removed from the system at 150 °C and -0.095 MPa to obtain a pale yellow transparent liquid, which is the amino-containing silane compound shown in formula III-A.
[0043] 2. Preparation of amino-containing polysiloxane adducts (Formula II-B1): Under nitrogen protection, 100 g of the obtained compound III-A was mixed with 11.2 g of trimethylolpropane tris(3-mercaptopropionate), and 1.1 g of azobisisobutyronitrile was added. After stirring evenly, the mixture was heated to 70 °C and subjected to a mercapto-olefin addition reaction for 4 h. After the reaction was completed, the low-boiling-point substances were removed under reduced pressure to obtain a pale yellow transparent viscous liquid, which is the amino-containing polysiloxane adduct shown in formula II-B1. 3. Emulsification: Mix 100 g of the II-B1 adduct obtained in step (2) with 5 g of isotridecyl alcohol polyoxyethylene ether evenly, add 1.5 g of glacial acetic acid, and continue stirring for 20 min; then add deionized water in portions under shear conditions of 4000 r / min, shear emulsify for 2 h, and add deionized water to adjust the solid content to 30% to obtain a semi-transparent blue light emulsion, which is the water-based fluorine-free, scratch-free water-repellent finishing agent of this embodiment.
[0044] Example 2: Example 2 includes the following steps: 1. Preparation of amino-containing silane compounds (Formula III-A): The steps here are the same as in Example 1.
[0045] 2. Preparation of amino-containing polysiloxane adducts (Formula II-B2): Under nitrogen protection, 100 g of compound III-A obtained in step (1) was mixed with 10.3 g of pentaerythritol tetra(3-mercaptopropionate), and 1.1 g of azobisisoheptanenitrile was added. After stirring evenly, the mixture was heated to 75 °C and subjected to a mercapto-olefin addition reaction for 3.5 h. After the reaction was completed, the low-boiling substances were removed under reduced pressure to obtain a pale yellow transparent viscous liquid, which is the amino-containing polysiloxane adduct shown in formula II-B2.
[0046] 3. Emulsification: 100 g of the obtained formula II-B2 adduct was mixed with 3 g of isotridecyl alcohol polyoxyethylene ether until homogeneous, 2.0 g of glacial acetic acid was added, and stirring was continued for 15 min; then deionized water was added in portions under shear conditions of 3500 r / min, and shear emulsification was carried out for 2.5 h. Deionized water was added to adjust the solid content to 28%, and a semi-transparent blue light emulsion was obtained, which is the water-based fluorine-free, scratch-free water-repellent finishing agent of this embodiment.
[0047] Example 3: Example 3 includes the following steps: 1. Preparation of amino-containing silane compounds (Formula III-A): The steps here are the same as in Example 1.
[0048] 2. Preparation of amino-containing polysiloxane adduct: Under nitrogen protection, 100 g of compound III-A obtained in step 1 was mixed with 6.3 g of 1,6-hexanedithiol, and 1.1 g of azobisisobutyronitrile was added. After stirring evenly, the mixture was heated to 65°C to carry out a mercapto-olefin addition reaction for 4.5 h. After the reaction was completed, the low-boiling substances were removed under reduced pressure to obtain the amino-containing polysiloxane adduct of this embodiment.
[0049] 3. Emulsification: Mix 100 g of the adduct obtained in step 2 with 5 g of isotridecyl alcohol polyoxyethylene ether evenly, add 1.5 g of glacial acetic acid, and continue stirring for 20 min; then add deionized water in portions under shear conditions of 4000 r / min, shear emulsify for 2 h, and add deionized water to adjust the solid content to 30% to obtain the emulsion, which is the water-based fluorine-free, scratch-resistant, and water-repellent finishing agent of this embodiment.
[0050] Example 4: Example 4 includes the following steps: 1. Preparation of amino-containing silane compounds (Formula III-A): The steps here are the same as in Example 1.
[0051] 2. Preparation of amino-containing polysiloxane adduct: Under nitrogen protection, 100 g of compound III-A obtained in step 1 was mixed with 8.6 g of 1,10-decanedithiol, and 1.1 g of azobisisobutyronitrile was added. After stirring evenly, the mixture was heated to 70 °C to carry out a mercapto-olefin addition reaction for 4 h. After the reaction was completed, the low-boiling substances were removed under reduced pressure to obtain the amino-containing polysiloxane adduct of this embodiment.
[0052] 3. Emulsification: Mix 100 g of the adduct obtained in step 2 with 4 g of isotridecyl alcohol polyoxyethylene ether evenly, add 1.5 g of glacial acetic acid, and continue stirring for 20 min; then add deionized water in portions under shear conditions of 3800 r / min, shear emulsify for 2 h, and add deionized water to adjust the solid content to 30%, thus obtaining the water-based fluorine-free, scratch-resistant, water-repellent finishing agent of this embodiment.
[0053] Example 5: Example 5 includes the following steps: 1. Preparation of amino-containing silane compounds (Formula III-A): The steps here are the same as in Example 1.
[0054] 2. Preparation of amino-containing polysiloxane adduct: Under nitrogen protection, 100 g of compound III-A obtained in step 1 was mixed with 12.3 g of 1,6-hexanediol bis(3-mercaptopropionate), and 1.1 g of azobisisoheptanenitrile was added. After stirring evenly, the mixture was heated to 60 °C to carry out a mercapto-olefin addition reaction for 5 h. After the reaction was completed, the low-boiling substances were removed under reduced pressure to obtain the amino-containing polysiloxane adduct of this embodiment.
[0055] 3. Emulsification: Mix 100 g of the adduct obtained in step 2 with 5 g of isotridecyl alcohol polyoxyethylene ether evenly, add 2.0 g of glacial acetic acid, and continue stirring for 15 min; then add deionized water in portions under shear conditions of 3500 r / min, shear emulsify for 2.5 h, and add deionized water to adjust the solid content to 28%, thus obtaining the water-based fluorine-free, scratch-resistant, water-repellent finishing agent of this embodiment.
[0056] Comparative Example 1: Comparative Example 1 includes the following steps: 1. Preparation of modified nano-TiO2: 15 g tetrabutyl titanate and 0.5 g polyethylene glycol were dispersed in 50 g ethanol solution (ethanol to water mass ratio of 6:1). After sonication at room temperature for 10 min, 10 g ethanol solution of acetic acid (acetic acid, ethanol and water mass ratio of 1:7:2) was slowly added dropwise, and sonication was continued for 10 min to obtain nano-TiO2 solution; 20 g vinyltriethoxysilane was added to nano-TiO2 solution, and the mixture was stirred at 150 r / min at 40 °C for 4 h. Impurities were removed by rotary evaporation to obtain modified nano-TiO2. 2. Preparation of the first preemulsion: 10 g of modified nano TiO2, 11 g of polyethylene oxide alkyl aryl ether, 6 g of hexadecyltrimethylammonium bromide, 33 g of octadecyl acrylate, 12.5 g of isobornyl methacrylate and 100 g of water were added to a container. The mixture was heated to 60 °C at a stirring rate of 250 r / min until all the raw materials were dissolved. Then, it was sheared and emulsified at a speed of 1500 r / min for 45 min and homogenized at 25 °C to obtain the first preemulsion. 3. Preparation of the second preemulsion: Add 66 g of octadecyl methacrylate, 37.5 g of isobornyl methacrylate, 20 g of methoxy polyethylene glycol methacrylate, 20 g of monovinyl-terminated dimethyl polysiloxane, 20 g of isopropanol, 22 g of polyethylene oxide alkyl aryl ether, 12 g of hexadecyltrimethylammonium bromide and 300 g of deionized water to a container, and emulsify in the same manner as in step 2 to obtain the second preemulsion; 4. Polymerization: The first preemulsion was heated to 58 °C, and 2.6 g of azobisisobutyronitrile was added at a stirring rate of 250 r / min. The reaction was carried out for 10 min to obtain the first reaction solution. The second preemulsion and 7.5 g of azobisisobutyronitrile were simultaneously added dropwise to the first reaction solution over a period of 30 min. After the addition was completed, the stirring rate and temperature were maintained for 2 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the fluorine-free waterproof finishing agent of Comparative Example 1 was obtained.
[0057] Comparative Example 2: Comparative Example 2 includes the following steps: 1. Synthesis of side-chain hydrogen-containing silicone oil: 200 g of octamethylcyclotetrasiloxane, 3 g of hexamethyldisiloxane, 20 g of tetramethylcyclotetrasiloxane and 8 g of solid acid resin were added to a four-necked flask, heated to 60 ℃, stirred for 7 h, and filtered after the reaction was completed to obtain side-chain hydrogen-containing silicone oil. 2. Synthesis of modified silicone oil: 100 g of the side-chain hydrogen-containing silicone oil obtained in step 1, 4-vinylepoxycyclohexane and octadecyl methacrylate were added to a three-necked flask. The molar ratio of the side-chain hydrogen-containing silicone oil, 4-vinylepoxycyclohexane and octadecyl methacrylate was 1:12:3. Nitrogen gas was introduced, the temperature was raised to 90℃, chloroplatinic acid catalyst was slowly added dropwise, and the reaction was carried out for 5 h to obtain epoxy-methacrylate co-modified silicone oil. 3. Synthesis of amino-modified silicone oil: The modified silicone oil obtained in step 2 was mixed with 3-aminopropyltriethoxysilane at a molar ratio of 1:2. The dropping time of 3-aminopropyltriethoxysilane was controlled to be 1.2 h, and the mixture was reacted at 60 °C for 5 h to obtain amino-modified silicone oil. 4. Preparation of nonionic silicone surfactant: 50 g of the side-chain hydrogen-containing silicone oil obtained in step 1 and 30 g of allyl polyethylene glycol with a molecular weight of 600 were added to a reaction vessel, heated to 90 °C under nitrogen protection, and reacted for 5 h to obtain a nonionic silicone surfactant. 5. Emulsification: Mix 100 g of the amino-modified silicone oil obtained in step 3, 8 g of the nonionic silicone surfactant obtained in step 4, and 1.3 g of 80% acetic acid solution. Use a high-speed shear disperser to shear emulsify at a speed of 4000 r / min. Slowly add water to adjust the emulsion solid content to 30% to obtain the organosilicon waterproofing agent of Comparative Example 2.
[0058] Comparative Example 3: Comparative Example 3 includes the following steps: 1. Preparation of amino-containing silane compounds (Formula III-A): The steps here are the same as in Example 1.
[0059] 2. Emulsification: Mix 100 g of the compound of formula III-A obtained in step 1 with 5 g of isotridecyl alcohol polyoxyethylene ether evenly, add 1.5 g of glacial acetic acid, and continue stirring for 20 min; then add deionized water in portions under shear conditions of 4000 r / min, shear emulsify for 2 h, and add deionized water to adjust the solid content to 30% to obtain the finishing agent of Comparative Example 3.
[0060] Comparative Example 4: Comparative Example 4 includes the following steps: 1. Preparation of α-vinyl-ω-hydroxy polydimethylsiloxane: The steps here are consistent with steps 1.1 and 1.2 in Example 1; 2. Preparation of polysiloxane adduct: Under nitrogen protection, 100 g of α-vinyl-ω-hydroxy polydimethylsiloxane obtained in step 1 was mixed with 13.2 g of trimethylolpropane tris(3-mercaptopropionate), and 1.1 g of azobisisobutyronitrile was added. After stirring evenly, the mixture was heated to 70 °C for a mercapto-olefin addition reaction for 4 h. After the reaction was completed, the low-boiling-point substances were removed under reduced pressure to obtain an amino-free polysiloxane adduct. 3. Emulsification: Mix 100 g of the adduct obtained in step 2 with 20 g of isotridecyl alcohol polyoxyethylene ether evenly, add deionized water in portions under shear conditions of 4000 r / min, shear emulsify for 2 h, and add deionized water to adjust the solid content to 30% to obtain the finishing agent of Comparative Example 4.
[0061] Performance testing: The finishing agents prepared in Examples 1-5 and Comparative Examples 1-4 were diluted with deionized water to prepare finishing solutions with a concentration of 40 g / L. The fabrics were subjected to two dips and two nips with a nip-out ratio of 70%, and then pre-dried at 100 °C for 4 min and baked at 160 °C for 3 min to complete the finishing process. The fabrics used were polyester woven fabrics and pure cotton woven fabrics.
[0062] 1. Water repellency test: The water repellency rating of the finished fabric was determined according to GB / T 4745-2012 "Test and evaluation of water resistance of textiles - Water repellency method". 2. Wash resistance test: The finished fabric was washed 20 times with standard detergent according to the 4N procedure in GB / T 8629-2017 "Testing procedures for textiles - Household washing and drying". After drying, the water repellency rating was determined according to the above method.
[0063] 2. Hand scratch test: Lay the finished fabric flat on a table, pinch the fabric with your fingers, squeeze and rub it 5 times, then release. Observe the scratches on the fabric and how well the scratches recede after standing at room temperature for 1 minute. Evaluate according to the following standards: a) No visible scratches; b) Slight scratches, which disappear on their own within 1 minute; c) Obvious scratches, which partially recede after standing for 1 minute; d) Obvious white scratches, which do not recede after standing for 1 minute.
[0064] 3. Hand feel test: Referring to AATCC EP5-2011, 5 trained evaluators conducted subjective hand feel evaluations of the finished fabric. The hand feel level was 1-5, with level 5 indicating the softest and smoothest hand feel and level 1 indicating the stiffest and roughest hand feel. The results were taken as the average value.
[0065] The test results are shown in Table 1-2.
[0066] Table 1: Performance Test Results of Polyester Fabrics
[0067] Table 2: Performance Test Results of Pure Cotton Fabrics
[0068] As shown in Tables 1 and 2, the water-based fluorine-free, scratch-resistant water-repellent finishing agent prepared in Examples 1-2 of this disclosure has good performance on both polyester and pure cotton fabrics. This is because the polythiols containing ester bonds (trimethylolpropane tris(3-mercaptopropionate) and pentaerythritol tetra(3-mercaptopropionate)) have three and four thiol functional groups, respectively. After the thiol-olefin addition reaction, a star-shaped multi-arm structure containing amino polysiloxane adduct is obtained, with three or four amino-containing siloxane segments connected to the same core. During the baking process, the methoxysilyl groups at the ends of the siloxane segments hydrolyze and condense, forming a covalent bond with the hydroxyl groups on the fiber surface on the one hand, and constructing a three-dimensional cross-linked network in the membrane on the other hand, so that the finishing agent forms a firmly anchored elastic siloxane network membrane on the fabric surface. When gripped by external force, the elastic network membrane undergoes reversible deformation and pulls the yarn back into place. The scratches disappear automatically after release, leaving no visible hand marks. Simultaneously, the integrity of the network membrane, the electrostatic adsorption of amino groups to the fibers, and the covalent interaction of silicon-oxygen bonds ensure that the water-repellent properties of the finishing agent do not diminish after 20 washes. In contrast, the dithiol used in Examples 3-5 is a bifunctional group, resulting in an adduct with a linear two-arm structure. This leads to a relatively lower crosslinking density and elastic recovery ability in the film, resulting in scratches and a slight decrease in water repellency after washing.
[0069] Comparative Example 1's water-repellent finishing agent is mainly composed of an acrylate copolymer hard film. Although its initial water repellency rating can reach level 4, the film is hard and brittle. When gripped, the film breaks brittlely, forming irreversible white scratches, and feels stiff. Comparative Example 2's amino-modified silicone oil feels soft, but it lacks a cross-linked network structure in its molecules. When gripped, the yarn slips, and the film layer cannot bring the yarn back into place, forming obvious scratches. Furthermore, its water repellency and wash resistance are poor. Comparative Example 3 did not undergo mercapto-olefin addition, Formula III... Compound A exists in single-chain form and cannot form a three-dimensional network. The bonding force between the membrane and the fiber and its own cohesion are insufficient, resulting in a comprehensive decline in water repellency, wash resistance, and scratch resistance. Although the adduct of Comparative Example 4 has a star-shaped network structure and acceptable scratch performance, it does not contain amino groups in its molecule and cannot achieve acidification self-emulsification. It requires the addition of 20% emulsifier to emulsify. A large amount of emulsifier remains in the membrane and dissolves during washing, resulting in a low initial water repellency level and significant deterioration of water repellency after 20 washes.
[0070] Other embodiments of this disclosure will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This disclosure is intended to cover any variations, uses, or adaptations of this disclosure that follow the general principles of this disclosure and include common knowledge or customary techniques in the art not disclosed herein.
Claims
1. A method for preparing a water-based, fluorine-free, scratch-resistant, water-repellent finishing agent, characterized in that, The preparation method includes: Step 1: Prepare an amino-containing silane compound; the amino-containing silane compound has the structure represented by the following formula IA: Wherein, n1 is selected from 6-20; R 11 R 12 R 15 R 16 Each is independently selected from hydrogen, substituted or unsubstituted C1-C30 alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted 3-30 membered heterocyclic, or substituted or unsubstituted 5-30 membered heteroaryl; R 13 R 14 Each is independently selected from substituted or unsubstituted C1-C30 alkyl groups, or substituted or unsubstituted C1-C30 alkoxy groups; R 17 R 18 Each is independently selected from substituted or unsubstituted C1-C10 alkylene groups or substituted or unsubstituted C1-C30 alkene groups; Step 2: Mix the amino-containing silane compound obtained in Step 1 with the polythiol compound, and carry out a mercapto-olefin addition reaction in the presence of a free radical initiator to obtain the amino-containing polysiloxane adduct. Step 3: The amino-containing polysiloxane adduct obtained in Step 2 is mixed with organic acid and water, and then sheared and emulsified to obtain the water-based fluorine-free, scratch-resistant, water-repellent finishing agent.
2. The preparation method of the water-based, fluorine-free, scratch-resistant water-repellent finishing agent according to claim 1, characterized in that, The polythiol compound is a compound containing two or more thiol groups, selected from one or more of C2-C18 alkylene dithiols and polythiols containing ester bonds; The C2-C18 alkylene dithiol is selected from one or more of 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, and 1,12-dodecanedithiol. The polythiols containing ester bonds are selected from one or more of ethylene glycol bis(3-mercaptopropionate), 1,4-butanediol bis(3-mercaptopropionate), 1,6-hexanediol bis(3-mercaptopropionate), neopentyl glycol bis(3-mercaptopropionate), ethylene glycol bis(mercaptoacetate), trimethylolpropane tri(3-mercaptopropionate), and pentaerythritol tetra(3-mercaptopropionate).
3. The preparation method of the water-based, fluorine-free, scratch-resistant water-repellent finishing agent according to claim 1, characterized in that, In step 2, the free radical initiator is selected from thermal initiators and / or photoinitiators; the thermal initiator is selected from one or more of azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobiscyanopentanoic acid, azobisisobutyramidazoline hydrochloride, benzoyl peroxide, and di-tert-butyl peroxide; the photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and benzophenone; the amount of the free radical initiator is 0.1%-2% of the total mass of the amino-containing silane compound and the polythiol compound; In step 3, the organic acid is selected from one or more of formic acid, acetic acid, propionic acid, lactic acid, glycolic acid, and citric acid.
4. The preparation method of the water-based, fluorine-free, scratch-resistant water-repellent finishing agent according to claim 1, characterized in that, The amino-containing silane compound has the structure represented by the following formula II-A: Wherein, n1 is selected from 6-20; R 17 R 18 R 19 R 20 Each is independently selected from C1-C10 alkylene groups.
5. The preparation method of the water-based, fluorine-free, scratch-resistant, water-repellent finishing agent according to claim 2 or 4, characterized in that, The polythiol compound is selected from trimethylolpropane tris(3-mercaptopropionate) or pentaerythritol tetra(3-mercaptopropionate); The amino-containing polysiloxane adduct obtained in step 2 has the structure represented by formula I-B1 or formula I-B2: Wherein, n1 is selected from 6-20; R 17 R 18 Each is independently selected from C1-C5 alkylene groups; R 19 R 20 Each is independently selected from C1-C5 alkyl groups.
6. The preparation method of the water-based, fluorine-free, scratch-resistant water-repellent finishing agent according to claim 4, characterized in that, The amino-containing silane compound has the structure represented by the following formula III-A: The amino-containing silane compound having the structure represented by Formula III-A is prepared by the following steps: Step 1-1: Mix N,N-dimethylformamide, deionized water, and acetic acid. Slowly add 1,3-divinyl-1,1,3,3-tetramethyldisilazane dropwise while stirring at room temperature. After the addition is complete, purge with nitrogen gas for 0.5-2 hours to remove the ammonia gas generated in the reaction. Then dry with a drying agent to obtain a vinyl dimethylsilanol N,N-dimethylformamide solution. The mass ratio of 1,3-divinyl-1,1,3,3-tetramethyldisilazane to deionized water is 1:(0.15-0.25), and the amount of acetic acid used is 0.5%-1.5% of the mass of 1,3-divinyl-1,1,3,3-tetramethyldisilazane. Step 1-2: Under nitrogen protection, the N,N-dimethylformamide solution of vinyl dimethylsilanol obtained in Step 1-1, hexamethylcyclotrisiloxane, and toluene are mixed, and 1,8-diazabicycloundec-7-ene is added as a catalyst. The ring-opening polymerization reaction is carried out at room temperature for 3-8 hours. Then, acetic acid is added to neutralize and terminate the reaction. After washing with water, drying, and removing toluene and N,N-dimethylformamide under reduced pressure, α-vinyl-ω-hydroxy polydimethylsiloxane is obtained. The molar ratio of vinyl dimethylsilanol to hexamethylcyclotrisiloxane is 1:(2-15), and the amount of 1,8-diazabicycloundec-7-ene is 2%-3% of the mass of hexamethylcyclotrisiloxane. The α-vinyl-ω-hydroxy polydimethylsiloxane has the following structural formula: Steps 1-3: Under nitrogen protection, the α-vinyl-ω-hydroxy polydimethylsiloxane obtained in step 1-2 is mixed with aminoethylaminopropyltrialkoxysilane, and 1,8-diazabicycloundec-7-ene is added as a catalyst. The mixture is reacted at 60-75°C for 2-4 hours. Then, unreacted aminoethylaminopropyltrialkoxysilane is removed at 140-160°C and -0.095 MPa to obtain the amino-containing silane compound shown in Formula III-A.
7. The preparation method of the water-based, fluorine-free, scratch-resistant water-repellent finishing agent according to claim 6, characterized in that, The amino-containing polysiloxane adduct obtained in step 2 has the structure represented by formula II-B1 or II-B2: 。 8. The method for preparing the water-based, fluorine-free, scratch-resistant water-repellent finishing agent according to any one of claims 1-7, characterized in that, Step 2 includes: Under nitrogen protection, the amino-containing silane compound obtained in step 1 is mixed with trimethylolpropane tris(3-mercaptopropionate) or pentaerythritol tetra(3-mercaptopropionate), a free radical thermal initiator is added, and after stirring evenly, the mixture is heated to 60-80°C to carry out a mercapto-olefin addition reaction for 3-5 hours. After the reaction is completed, the low-boiling-point substances are removed under reduced pressure to obtain an amino-containing polysiloxane adduct; the free radical thermal initiator is azobisisobutyronitrile and / or azobisisoheptanenitrile. Step 3 includes: The amino-containing polysiloxane adduct obtained in step 2 is mixed with an emulsifier, stirred evenly, and then acetic acid is added. Stirring is continued for 10-30 minutes. Then, deionized water is added in portions under shear conditions of 2500-5000 r / min. Shear emulsification is carried out for 1-3 hours to obtain the water-based fluorine-free, scratch-free, water-repellent finishing agent. The emulsifier is a nonionic emulsifier selected from one or more of fatty alcohol polyoxyethylene ether and isomeric fatty alcohol polyoxyethylene ether, and the amount of the emulsifier is 0.1-10% of the mass of the amino-containing polysiloxane adduct.
9. A water-based, fluorine-free, scratch-resistant water-repellent finishing agent, characterized in that, The water-based, fluorine-free, scratch-resistant, water-repellent finishing agent is prepared by the preparation method described in any one of claims 1-8.