A lithium-containing polysilazaborane ceramic precursor, a preparation method thereof, an electrolyte and application in a lithium ion battery

By forming a Li-Si-BN ceramic interface film in lithium-ion batteries through a process of first containing lithium and then boronizing, problems such as poor stability of electrolyte additives at high temperatures and large expansion of silicon anodes are solved, achieving high ionic conductivity and electrode interface stability, and improving battery performance.

CN123152116APending Publication Date: 2026-11-24SHANGHAI HANFU IND DEVELOPMENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611394316.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing lithium-ion battery electrolyte additives suffer from poor stability at high temperatures, are prone to gas generation, cause large expansion of silicon anodes, and have high interface impedance, making it difficult to simultaneously meet the requirements of interface stability and rapid lithium conduction.

Method used

A two-step modification process, first introducing lithium and then boronizing, is adopted to orderly introduce lithium and boron into the polysilazane molecular network in the form of N-Li bonds and BN bonds, respectively, to form a Li-Si-BN ceramic interface film rich in LiF and LiSi₂N₃ crystalline phases. This film serves as an electrolyte additive to remove acid and moisture and improve electrode interface performance.

Benefits of technology

It achieves electrolyte stability at high temperatures and high ionic conductivity at the electrode interface, suppresses lithium dendrite growth, buffers silicon anode expansion, and improves battery cycle stability and storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152116A_ABST
    Figure CN123152116A_ABST
Patent Text Reader

Abstract

This application relates to a lithium-containing polyborosilazane ceramic precursor, its preparation method, electrolyte, and its application in lithium-ion batteries. The preparation method includes: dissolving a polysilazane monomer in an anhydrous organic solvent; adding a lithium-containing reagent to react and obtain a lithium-containing polysilazane mixed solution; then adding a boron source compound to react and obtain another lithium-containing polyborosilazane mixed solution; and finally removing the solvent by vacuum distillation to obtain the lithium-containing polyborosilazane ceramic precursor. This application, through a two-step modification process of first introducing lithium and then boronizing, allows lithium and boron to be simultaneously introduced into the polysilazane molecular network via chemical bonds, unexpectedly obtaining a ceramic precursor material with synergistic properties of efficient acid and water removal, high-temperature interface stability, and rapid lithium conduction. This precursor can be used as an electrolyte additive to construct a Li-Si-B-N-containing ceramic interface film in situ on the electrode surface, significantly improving the high-temperature cycle life and storage stability of lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of functional materials technology for lithium-ion batteries, and in particular to a lithium-containing polyboron silazane ceramic precursor, its preparation method, electrolyte, and its application in lithium-ion batteries. Background Technology

[0002] Lithium-ion batteries have been widely used in new energy vehicles, energy storage power stations, and consumer electronics. With the continuous improvement of energy density and lifespan requirements, the stability of the electrolyte-electrode interface has become increasingly prominent. Especially under high temperature, high voltage, and silicon-based anode systems, problems such as electrolyte decomposition, electrode corrosion, gas expansion, and lithium dendrite growth seriously restrict further improvement of battery performance.

[0003] Commercial electrolytes commonly use lithium hexafluorophosphate (LiPF6) as the lithium salt, which is extremely sensitive to trace amounts of water and readily hydrolyzes to form hydrofluoric acid (HF) and phosphorus pentafluoride (PF5). HF corrodes electrode materials and triggers electrolyte decomposition, causing capacity decay and gas buildup. To address these issues, various additive strategies have been reported in the prior art: isocyanates can act as acid removers but are highly toxic; film-forming additives such as vinylene carbonate (VC) and vinyl sulfate (DTD) can form interfacial protective films, but their high-temperature resistance is limited, and some varieties are restricted by environmental regulations; novel lithium salts such as lithium difluorooxalate borate (LiODFB) and lithium bis(fluorosulfonyl)imide (LiFSI) have better thermal stability, but LiFSI has the problem of high-temperature corrosion of aluminum foil. In addition, polysilazane materials, due to the presence of Si-N bonds in their main chain, can theoretically be used as acid removers and form silicon-containing interfacial films on the electrode surface. However, ordinary polysilazanes do not contain lithium, and the ion conductivity of the resulting interfacial film is weak, making it difficult to simultaneously meet the dual requirements of interfacial stability and rapid lithium conduction.

[0004] In summary, existing technologies lack electrolyte materials that combine multiple functions such as efficient acid and water removal, stable film formation, lithium conduction, and expansion inhibition. There is an urgent need to develop a new type of functional additive that can solve the above problems simultaneously. Summary of the Invention

[0005] To address the problems of existing electrolyte additives, such as limited functionality, poor high-temperature stability, easy gas generation, large expansion of silicon anodes, and high interfacial impedance, this application provides a lithium-containing polyborosilazane ceramic precursor, its preparation method, electrolyte, and its application in lithium-ion batteries.

[0006] In a first aspect, this application provides a method for preparing a lithium-containing polyborosilazane ceramic precursor, employing the following technical solution: A method for preparing a lithium-containing polyborosilazane ceramic precursor includes the following steps: S1. Under inert gas protection, polysilazane monomers are dissolved in an anhydrous organic solvent to prepare a polysilazane solution; S2. Add a lithium-containing reagent to the polysilazane solution obtained in step S1, and react at -78℃ to -10℃ for 1 to 12 hours to obtain a lithium-containing polysilazane mixed solution. S3. Add a boron source compound to the lithium-containing polysilazane mixed solution obtained in step S2, and react at 25℃~80℃ for 3~24h to obtain a lithium-containing polyborosilicate mixed solution. S4. The lithium-containing polyborosilicate mixed solution obtained in step S3 is filtered and the solvent is removed by vacuum distillation to obtain the lithium-containing polyborosilicate ceramic precursor.

[0007] By employing the above preparation steps and a two-step modification process involving lithium inclusion followed by boronizing, lithium and boron can be sequentially introduced into the polysilazane molecular network. In the final product, they exist as N-Li bonds and BN / BC bonds, respectively, forming an ordered distribution of lithium and boron within the molecular network. The N-Li and Si-N bonds formed in the lithium inclusion step react with water or HF, effectively removing acidic and watery impurities from the electrolyte. Simultaneously, the N-Li bonds act as a lithium source during electrode interface film formation, participating in the construction of a ceramicized interface layer rich in LiF and LiSi₂N₃ crystalline phases. The LiSi₂N₃ crystalline phase in this interface layer exhibits high lithium-ion conductivity, which helps reduce interfacial impedance, while the LiF component enhances the electronic insulation and chemical stability of the interface film. The BN bonds formed in the boronizing step are embedded in the molecular backbone, possessing high bond energies that can enhance the thermal stability of the precursor molecular structure to some extent, slowing down molecular chain degradation or cross-linking failure in high-temperature electrolyte environments. The synergistic introduction of lithium and boron enables the in-situ formation of a Li-Si-BN ceramicized interface film rich in LiF and LiSi2N3 after the precursor is pyrolyzed and ceramicized on the electrode surface. In this interface film, the LiSi2N3 crystal phase provides ion transport channels, the LiF component enhances interface stability, and the BN framework network provides structural support. The three work together to give the interface film both high ionic conductivity and strong thermal stability.

[0008] Compared to lithium-free ordinary polysilazanes, the precursor of this application, due to the presence of N-Li bonds, can form a ceramicized interface layer rich in LiF and LiSi₂N₃ crystalline phases after film formation. The presence of the lithium-conducting crystalline phase may contribute to the improvement of interfacial ionic conductivity. Ordinary polysilazanes, lacking lithium, lack lithium-conducting crystalline phases in their pyrolysis products, resulting in relatively limited interfacial ionic conductivity, and they cannot form LiF to optimize the interfacial chemical environment. Compared to polysilazanes containing only lithium but no boron, the introduction of boron in this application forms BN bonds in the molecular framework. These bonds endow the ceramicized interface film with higher thermal stability and structural rigidity, potentially better maintaining the structural integrity of the interface film under high-temperature conditions. Furthermore, the BN framework may have a certain stabilizing effect on the distribution of LiF and LiSi₂N₃ crystalline phases. In addition, the process sequence of first introducing lithium and then boronizing ensures that lithium and boron each have their own sites in the molecular network, avoiding the structural disorder caused by competitive reactions that may occur when lithium and boron are introduced simultaneously, which is conducive to the stable realization of the above-mentioned properties. The above results indicate that the ceramicized interface film rich in LiF and LiSi2N3, the synergistic introduction of lithium and boron, and the specific introduction order may be important factors that distinguish the technical solution of this application from the prior art and produce the corresponding technical effects.

[0009] In one specific implementation scheme, in step S1, the general structural formula of the polysilazane precursor is as follows: Formula I:

[0010] Formula I, Where m is an integer from 0 to 6; n is an integer from 0 to 6; R1, R2, R3, and R4 are each independently selected from H, an aliphatic group, or an aromatic group.

[0011] This application employs a two-step modification process—first lithium-containing and then boronizing—to simultaneously introduce lithium and boron into the aforementioned polysilazane molecular network via chemical bonds, thereby obtaining a ceramic precursor material that combines highly efficient acid and water removal, high-temperature interface stability, and rapid lithium conduction. In the lithium-containing step, the lithium-containing reagent reacts with the NH bonds on the polysilazane backbone, with lithium linked to the nitrogen atoms of the backbone via N-Li bonds. In the boronizing step, the boron source compound reacts with active sites such as Si-H bonds, with boron embedded in the molecular network via BN bonds. The orderly distribution and proper placement of these two components allow for the in-situ formation of a Li-Si-BN ceramicized interface film rich in LiF and LiSi₂N₃ crystalline phases after pyrolysis and ceramization on the electrode surface, exhibiting both high ionic conductivity and strong thermal stability.

[0012] In one specific implementation scheme, in step S1, the anhydrous organic solvent is selected from one or more of tetrahydrofuran, diethyl ether, ethyl acetate, acetone, N,N-dimethylformamide, dichloromethane, 1,4-dioxane, toluene, xylene, and n-hexane; more preferably, in step S1, the anhydrous organic solvent is selected from tetrahydrofuran.

[0013] This application selects tetrahydrofuran as an anhydrous organic solvent, taking advantage of its good solubility and storage safety for both polysilazane and lithium-containing reagents. This provides a homogeneous reaction system for lithium-containing reactions, which is conducive to the uniform introduction of lithium into the side chains of polysilazane in the form of N-Li bonds. It avoids insufficient lithium content caused by differences in solubility or uneven local concentration, thereby obtaining lithium-containing polysilazane precursor materials.

[0014] In one specific implementation scheme, in step S2, the lithium-containing reagent is selected from one or more of methyllithium, phenyllithium, lithium ethylenediamine complex, trimethylsilylacetylene, lithium cyclopentadiene, lithium hydride, lithium chloride, lithium bromide, lithium iodide, lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, n-butyllithium, sec-butyllithium, tert-butyllithium, tert-butoxide, lithium borohydride, lithium amino, diisopropylaminolithium, bistrimethylsilylaminolithium, and 2,2,6,6-tetramethylpiperidinelithium; the molar ratio of the lithium-containing reagent to the polysilazane is (0.1-0.8):1; more preferably, in step S2, the lithium-containing reagent is selected from sec-butyllithium.

[0015] By adopting the above technical solution, sec-butyllithium can selectively react with the NH bond on the polysilazane backbone under low temperature conditions, and introduce lithium into the molecular network in a controllable manner in the form of N-Li bonds; the larger alkyl substituents of sec-butyllithium can, to a certain extent, regulate the lithium-containing reaction rate, avoiding excessive lithium content that leads to a sharp increase in molecular weight or excessive cross-linking.

[0016] The molar ratio of lithium-containing reagent to polysilazane determines the content of N-Li bonds in the precursor. Controlling it within the above range can introduce an appropriate amount of lithium reaction sites into the molecular network. On the one hand, the number of N-Li bonds directly affects the reactivity of the precursor with HF / H2O in the electrolyte. If the lithium content is too low, the deacidification and dehydration effect may be insufficient. If the lithium content is too high, it may affect the solubility and storage stability of the precursor. On the other hand, at this lithium content, active sites that can be used for subsequent borylation reactions are retained on the molecular chain, which is conducive to the embedding of boron source compounds into the molecular network in the form of BN bonds in the S3 step, thereby achieving an ordered distribution of lithium and boron in the polysilazane molecular backbone.

[0017] The sequential process of first introducing lithium and then boronizing ensures that lithium and boron occupy their respective positions, avoiding structural disorder caused by competition for the same reaction site when they are introduced simultaneously. This may be beneficial for the formation of a more uniform ceramicized interface layer after the precursor is deposited. Furthermore, the synergistic introduction of lithium and boron enables the in-situ formation of a Li-Si-BN ceramicized interface film rich in LiF and LiSi₂N₃ crystalline phases after the precursor is pyrolyzed and ceramicized on the electrode surface. The LiSi₂N₃ crystalline phase provides a fast lithium-ion transport channel, the LiF component helps enhance interface stability, and the BN framework network provides high-temperature structural support. The combined effect of these three factors gives the interface film both high ionic conductivity and strong thermal stability.

[0018] In one specific implementation, in step S3, the boron source compound is selected from one or more of boric acid, 3-bromo-5-methylphenylboronic acid, 1-octylboronic acid, n-hexylboronic acid, n-dodecanoboronic acid, 6-ethoxy-2-naphthoboronic acid, phenylboronic acid, 3-methoxyphenylboronic acid, 4-methoxyphenylboronic acid, trimethyl borate, p-methylphenylboronic acid, 3-isopropylphenylboronic acid, n-decylboronic acid, 4-(4-fluorophenyl)phenylboronic acid, 4-methylbiphenylboronic acid, 4-chloro-1-naphthoboronic acid, heptylboronic acid, boron trichloride, dimethyl borane sulfide, pyridine borane, 4-isopropylthiophenylboronic acid, dibenzofuran-3-boronic acid, 4-(methoxymethyl)phenylboronic acid, ammonia borane, and pinacol borane; more preferably, the boron source compound is selected from trimethyl borate.

[0019] This application utilizes trimethyl borate as the boron source. Its molecular structure contains three methoxy groups, exhibiting high reactivity with lithium-containing polysilazanes. It can react with Si-H and NH sites on the main chain, embedding boron into the polysilazane molecular network via BN and BC bonds. Introducing boron into the lithium-containing structure allows for an ordered distribution of lithium and boron within the molecular framework, providing a structural basis for the subsequent formation of a Li-Si-BN ceramicized interface film with both high ionic conductivity and strong thermal stability.

[0020] Secondly, this application provides a lithium-containing polyborosilazane ceramic precursor, which adopts the following technical solution: A lithium-containing polyborosilazane ceramic precursor is prepared using the method described in the first aspect for preparing lithium-containing polyborosilazane ceramic precursors. The lithium-containing polyborosilazane ceramic precursor has a number-average molecular weight of 500-5000 and a solid content of 65-95%. The molecular structure of the lithium-containing polyborosilazane ceramic precursor simultaneously contains a Si-N backbone, BN bonds, and N-Li bonds. The lithium-containing polyborosilazane ceramic precursor is pyrolyzed and ceramicized at 600℃~1000℃ to obtain lithium silicon nitride ceramics containing the LiSi2N3 crystalline phase.

[0021] The precursor obtained in this application has a moderate molecular weight and high solid content, and is liquid at room temperature, which is beneficial for uniform dispersion and addition in the electrolyte. Its molecular structure simultaneously contains a Si-N backbone, BN bonds, and N-Li bonds, indicating that lithium and boron are chemically introduced into the polysilazane network, rather than being physically mixed. After pyrolysis of this precursor at 600℃~1000℃, a lithium silicon nitride ceramic containing the LiSi2N3 crystalline phase can be generated. This crystalline phase has high lithium-ion conductivity, and its application at the electrode interface is expected to provide a continuous lithium-ion transport channel, which is beneficial for reducing interfacial impedance and improving the cycle stability of the battery.

[0022] Thirdly, this application provides an electrolyte, which adopts the following technical solution: An electrolyte comprising a lithium salt, an organic solvent, and a lithium-containing polyborosilazane ceramic precursor; wherein the amount of the lithium-containing polyborosilazane ceramic precursor added is 0.1-5 wt% of the total mass of the electrolyte. By adding the precursor as an additive to the electrolyte, the Si-N and N-Li bonds in its molecular structure can react with HF and H2O in the electrolyte, effectively removing acid and water. Simultaneously, the released lithium ions can participate in the formation of the interfacial film on the electrode surface. The precursor, added in a moderate amount, exhibits good solubility and dispersibility in the electrolyte. An addition range of 0.1–5 wt% allows it to effectively modify the electrode interface without significantly affecting the basic physicochemical properties of the electrolyte (such as viscosity and conductivity). During formation or charge / discharge processes, it forms a Li-Si-BN-containing ceramic interfacial film in situ, thereby improving the stability of the electrode interface and lithium-ion transport performance.

[0023] In one specific implementation, the lithium salt is selected from one or more of LiPF6, LiFSI, and LiBF4, and the concentration of the lithium salt in the electrolyte is 0.8~1.3 mol / L.

[0024] By adopting the above technical solutions, lithium salts provide lithium ion sources for the electrolyte, ensuring that the electrolyte has sufficient ionic conductivity. LiPF6 has balanced overall performance and is the most widely used lithium salt in commercial electrolytes; LiFSI has high thermal stability, a higher decomposition temperature than LiPF6, and a higher degree of dissociation in carbonate solvents, which helps to reduce interfacial impedance; LiBF4 performs well at low temperatures and has relatively low sensitivity to water.

[0025] Maintaining the lithium salt concentration within the range of 0.8–1.3 mol / L provides a sufficient lithium-ion source, ensuring the electrolyte possesses suitable ionic conductivity. Simultaneously, this concentration range exhibits good compatibility with the aforementioned precursor addition amount (0.1–5 wt%), avoiding both excessively high concentrations that reduce precursor solubility and excessively low concentrations that affect lithium-ion supply to the interfacial film. The combined use of multiple lithium salts leverages their respective advantages—LiPF6 provides basic electrochemical performance, LiFSI enhances high-temperature stability, and LiBF4 improves low-temperature performance—thus broadening the electrolyte's operating temperature range without compromising the precursor's film-forming and acid-removing functions.

[0026] In one specific implementation, the organic solvent is selected from at least two of EC, DMC, EMC, and PC.

[0027] By employing the above technical solutions, EC exhibits a high dielectric constant and good lithium salt solubility, which helps promote the dissociation of lithium salt in the electrolyte; DMC, EMC, and PC have low viscosity and good low-temperature performance, which is beneficial for the rapid migration of lithium ions in the electrolyte. Using at least two of the cyclic carbonates (EC / PC) and chain carbonates (DMC / EMC) in combination allows the electrolyte to possess both a high dielectric constant and low viscosity, thereby achieving suitable ionic conductivity. Simultaneously, this mixed solvent system exhibits good solubility and dispersibility for lithium-containing polyborosilicate precursors, enabling the precursors to exist stably and be uniformly distributed in the electrolyte, which is beneficial for their uniform film formation on the electrode surface.

[0028] Fourthly, this application provides an application of a lithium-containing polyborosilazane ceramic precursor in lithium-ion batteries, employing the following technical solution: A lithium-containing polyboron silazane ceramic precursor is used as an electrolyte deacidification and dehydration additive, an electrode interface modifier, a silicon anode expansion buffer layer, or a solid-state battery interface modification layer.

[0029] Previously, the precursor contained Si-N and N-Li bonds in its molecular structure, which enabled it to react chemically with HF and H2O in the electrolyte, thereby removing acid and water and inhibiting the decomposition of LiPF6. Therefore, it could be used as an additive for removing acid and water from electrolytes.

[0030] Previously, the precursor could be pyrolyzed and ceramicized in situ on the electrode surface to form a Li-Si-BN ceramicized interface film rich in LiF and LiSi2N3 crystalline phases. This interface film has high ionic conductivity, strong thermal stability and dense structure, which can improve the compatibility of the electrode / electrolyte interface and reduce the interface impedance. Therefore, it can be used as an electrode interface modifier.

[0031] The ceramicized interface film of this precursor has high mechanical strength and toughness, and can maintain structural integrity during the volume expansion and contraction of silicon-based anodes, providing physical constraints and buffering for the expansion of silicon particles. Therefore, it can be used as an expansion buffer layer for silicon anodes.

[0032] In solid-state batteries, the precursor can form a ceramicized transition layer with good interfacial contact in situ between the electrode and the solid electrolyte, improving solid-solid interface contact and reducing interfacial impedance. Therefore, it can be used as an interface modification layer for solid-state batteries.

[0033] In summary, this application includes at least one of the following beneficial technical effects: 1. This application employs a two-step modification process of first introducing lithium and then boronizing, which allows lithium and boron to be introduced into the polysilazane molecular network in an orderly manner through chemical bonds, thereby obtaining a precursor material that is liquid at room temperature, has a moderate molecular weight, and can be used directly as an additive, exhibiting good dispersibility and ease of operation.

[0034] 2. This application uses the precursor as an electrolyte additive to remove HF and H2O from the electrolyte by utilizing Si-N and N-Li bonds, and forms a Li-Si-BN ceramic interface film rich in LiF and LiSi2N3 crystal phases in situ on the electrode surface. This film has both high ionic conductivity and strong thermal stability, effectively improving the electrode interface performance.

[0035] 3. This application utilizes the prior material in lithium-ion batteries to suppress lithium dendrite growth and buffer the volume expansion of silicon anodes by forming a ceramicized interface film in situ. It can also be used as an acid and water removal additive, an electrode interface modifier, a silicon anode expansion buffer layer, and a solid-state battery interface modification layer, which has broad application prospects. Attached Figure Description

[0036] Figure 1 The Fourier transform infrared spectrum is that of the lithium-containing polyborosilazane ceramic precursor prepared in Example 1 of this application. Detailed Implementation

[0037] The present application will be further described in detail below with reference to embodiments and comparative examples: Some of the raw materials used in the examples and comparative examples: Polysilazane, model: XSC-N4501, number average molecular weight: 760, purchased from Zhejiang Xinshichen New Material Co., Ltd. Lithium-containing reagent: sec-butyllithium (1.3mol / L, n-hexane, EnergySeal), model: W420382-25ml-YLG, purchased from Anhui Zesheng Technology Co., Ltd. Boron source compound: Trimethyl borate, model number: W320027, purchased from Anhui Zesheng Technology Co., Ltd.; Anhydrous organic solvent: anhydrous tetrahydrofuran, model: W310076-0010, purchased from Anhui Zesheng Technology Co., Ltd.

[0038] Unless otherwise specified, all raw materials used in the examples and comparative examples are commercially available products. Example Example 1

[0039] (1) The preparation of the lithium-containing polyborosilazane precursor (named PLSBN) is as follows: S1. Under argon protection, 20.0g of polysilazane was dissolved in 30mL of anhydrous tetrahydrofuran to prepare a polysilazane solution; S2. Add 16 mL of sec-butyllithium solution dropwise to the polysilazane solution obtained in step S1 using a constant pressure dropping funnel at -60°C. After the addition is complete, continue the reaction at -60°C for 3 h to obtain a lithium-containing polysilazane mixed solution. S3. Add 3.2g of trimethyl borate to the lithium-containing polysilazane mixed solution obtained in step S2, and react at 60℃ for 24h to obtain the lithium-containing polyborosilicate mixed solution. S4. The lithium-containing polyborosilicate mixed solution obtained in step S3 is filtered and the solvent is removed by vacuum distillation to obtain the lithium-containing polyborosilicate ceramic precursor.

[0040] According to GPC testing, the number average molecular weight of the PLSBN prepared in this embodiment is 1800; according to thermogravimetric analysis, the solid content of the PLSBN prepared in this embodiment is 85%.

[0041] from Figure 1 The FT-IR spectrum shows that the PLSBN prepared in this embodiment exhibits an NH stretching vibration peak at 3393 cm⁻¹ and a peak at 1156 cm⁻¹. -1 The NH bending vibration peak of Si-NH-Si appears at 915 cm⁻¹. -1 and 824cm -1 The presence of a Si-N stretching vibration peak at 1464 cm⁻¹ indicates that the product retains the main chain structure of the polysilazane. Compared with the raw polysilazane, the product exhibits a higher Si-N stretching vibration peak at 1464 cm⁻¹. -1 A new BC absorption peak appears at 773 cm⁻¹. -1 The presence of a Si-NB bending vibration peak at 1460 cm⁻¹, coupled with a significant decrease in the intensity of the Si-H peak, indicates that boron has been introduced into the polymer network via a dehydrogenation borylation reaction. Crucially, this product exhibits a peak at 1460 cm⁻¹. -1 and 1046cm -1The appearance of new characteristic absorption peaks can be attributed to the stretching vibrations of Li-N and Si-N-Li, respectively, while the raw material polysilazane has no absorption peak at this point, indicating that lithium has been successfully introduced into the polysilazane backbone through chemical bonds (N-Li bonds) rather than through physical mixing.

[0042] (2) The electrolyte is prepared as follows: In an argon glove box, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are mixed evenly in a mass ratio of 1:1:1. PLSBN is added at 0.5% of the total mass of the electrolyte, and the mixture is ultrasonically stirred until completely dissolved. Then, LiPF6 is slowly added to make the concentration of LiPF6 in the electrolyte 1.0 mol / L, and the mixture is stirred until completely dissolved to obtain the electrolyte. Example 2

[0043] The preparation method of the electrolyte in Example 2 is the same as that in Example 1. The only difference between Example 2 and Example 1 is that in step S2 of the preparation of the lithium-containing polyborosilazane precursor, 16 mL of sec-butyllithium solution is replaced with 8 mL of sec-butyllithium solution. Example 3

[0044] The preparation method of the electrolyte in Example 3 is the same as that in Example 1. The only difference between Example 3 and Example 1 is that in step S2 of the preparation of the lithium-containing polyborosilazane precursor, 16 mL of sec-butyllithium solution is replaced with 2 mL of sec-butyllithium solution. Example 4

[0045] The preparation method of the electrolyte in Example 4 is the same as that in Example 1. The only difference between Example 4 and Example 1 is that in step S2 of the preparation of the lithium-containing polyborosilazane precursor, 16 mL of sec-butyllithium solution is replaced with 1 mL of sec-butyllithium solution. Example 5

[0046] The preparation method of the electrolyte in Example 5 is the same as that in Example 1. The only difference between Example 5 and Example 1 is that in step S2 of the preparation of the lithium-containing polyborosilazane precursor, 16 mL of sec-butyllithium solution is replaced with 24 mL of sec-butyllithium solution. Example 6

[0047] Example 6 uses the same method as Example 1 to prepare lithium-containing polyborosilicate ceramic precursor PLSBN. The only difference from Example 1 is that, during the electrolyte preparation process, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte is added instead of 0.1% of the above-mentioned PLSBN based on the total mass of the electrolyte. Example 7

[0048] Example 7 uses the same method as Example 1 to prepare lithium-containing polyborosilicate ceramic precursor PLSBN. The only difference from Example 1 is that, during the electrolyte preparation process, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte is added instead of 5% of the above-mentioned PLSBN based on the total mass of the electrolyte. Example 8

[0049] Example 8 uses the same method as Example 1 to prepare lithium-containing polyborosilicate ceramic precursor PLSBN. The only difference from Example 1 is that, during the electrolyte preparation process, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte is added instead of 0.05% of the above-mentioned PLSBN based on the total mass of the electrolyte. Example 9

[0050] Example 9 uses the same method as Example 1 to prepare lithium-containing polyborosilicate ceramic precursor PLSBN. The only difference from Example 1 is that, during the electrolyte preparation process, instead of adding 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte, 6% of the above-mentioned PLSBN based on the total mass of the electrolyte is added. Example 10

[0051] Example 10 uses the same method as Example 1 to prepare lithium-containing polyborosilicate ceramic precursor PLSBN. The only difference between Example 1 and Example 1 is that, in the electrolyte preparation process, instead of mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a mass ratio of 1:1:1, ethylene carbonate (EC) and dimethyl carbonate (DMC) in a mass ratio of 1:1 are mixed evenly.

[0052] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that the electrolyte of Comparative Example 1 does not contain the PLSBN prepared in Example 1.

[0053] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that, in Comparative Example 2, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte was added to the electrolyte, instead of 0.5% of vinylene carbonate (VC) based on the total mass of the electrolyte.

[0054] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is that, in Comparative Example 3, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte was added to the electrolyte, instead of 0.5% of vinyl sulfate (DTD) based on the total mass of the electrolyte.

[0055] Comparative Example 4 The only difference between Comparative Example 4 and Example 1 is that, in Comparative Example 4, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte was added to the electrolyte, instead of 0.5% of polysilazane based on the total mass of the electrolyte.

[0056] Comparative Example 5 The only difference between Comparative Example 5 and Example 1 is that, in Comparative Example 5, 0.5% of the above-mentioned PLSBN based on the total mass of the electrolyte was added to the electrolyte, instead of 0.35% of polysilazane, 0.1% of LiCl and 0.05% of trimethyl borate based on the total mass of the electrolyte.

[0057] The electrolytes prepared in each embodiment and comparative example were used to assemble NCM523 / SiO2. x @C soft-pack battery. Specific steps include: (1) Preparation of positive electrode sheet: The positive electrode active material LiNi0.5Co0.2Mn0.3O2 (NCM523), conductive agent (acetylene black) and binder (PVDF) are mixed evenly in a mass ratio of 90:5:5, coated on aluminum foil, and then dried, rolled and cut to obtain the positive electrode sheet.

[0058] (2) Preparation of negative electrode: SiO x @C negative electrode active material, conductive agent (Super P), binder (SBR+CMC) are mixed evenly in a mass ratio of 70:20:10, coated on copper foil, and then dried, rolled, and cut to obtain the negative electrode sheet.

[0059] (3) Battery assembly: The positive electrode, negative electrode and separator (PE / PP composite separator) are wound into a cell, and the soft pack battery is obtained through the processes of encapsulation, liquid injection, formation, aging and capacity testing.

[0060] The pouch cells prepared in the above embodiments and comparative examples were subjected to the following performance tests: 1. High-temperature cycle performance: Each pouch battery was subjected to charge-discharge cycle test in a 60℃ constant temperature chamber with a 1C / 1C current density within a voltage range of 2.75-4.2V. The initial discharge capacity and the discharge capacity after 1000 cycles were recorded, and the capacity retention rate after 1000 cycles was calculated. 2. High-temperature storage performance: Each pouch battery was stored at 60℃ in a fully charged state for 14 days. The battery volume before and after storage was tested using the water displacement method or the size measurement method, and the volume expansion rate was calculated. After 14 days of storage, the battery was discharged at 0.2C to the cutoff voltage, and the capacity recovery rate was calculated. 3. Electrochemical Impedance Spectroscopy (EIS) Test: Perform EIS tests before and after battery cycling (e.g., after 1000 cycles), with a frequency range of 100kHz-10mHz and an amplitude of 5mV, and compare the increase in interfacial impedance before and after cycling.

[0061] The test results are summarized in Table 1 below. Table 1. Performance test data of each pouch battery

[0062] Based on Examples 1-10 and Table 1, it can be seen that variations in lithium content and dosage directly affect the performance of the precursor. When the lithium content is too low, the number of N-Li bonds is insufficient, preventing the formation of a sufficient lithium-conducting crystalline phase; when the lithium content is too high, the solubility and dispersibility of the precursor decrease, and the interface modification effect weakens. When the dosage is too low, the interface film coverage is insufficient; when the dosage is too high, the electrolyte viscosity is too high, and ion conduction is hindered. This indicates that controlling the lithium content and dosage within a reasonable range is necessary. Furthermore, the precursor maintains good performance under different solvent systems, indicating its good compatibility with carbonate solvents.

[0063] Combining Example 1 and Comparative Examples 1-5, and referring to Table 1, it can be seen that the performance indicators of the precursor of this application are significantly better than those of no additive, conventional additives (VC / DTD), ordinary polysilazane, and physical mixing schemes. Crucially, the performance of Comparative Example 4 (i.e., adding ordinary polysilazane) and Comparative Example 5 (i.e., adding physically mixed lithium salt + boron source ordinary polysilazane) is significantly lower than that of Example 1, indicating that physical mixing alone cannot achieve the interface modification effect brought about by the introduction of chemical bonding. The above comparative results further corroborate the structural advantage of this application in simultaneously introducing lithium and boron into the polysilazane molecular network through chemical bonding.

[0064] This application employs a two-step modification process, first introducing lithium and then boronizing, to orderly introduce lithium and boron into the polysilazane molecular network in the form of N-Li bonds and BN bonds, respectively. This yields a lithium-containing polyborosilicate ceramic precursor whose molecular structure simultaneously contains a Si-N backbone, BN bonds, and N-Li bonds. As an electrolyte additive, this precursor utilizes Si-N and N-Li bonds to remove HF and H2O from the electrolyte, inhibiting LiPF6 decomposition. It also forms a Li-Si-BN ceramicized interface film rich in LiF and LiSi2N3 crystalline phases in situ on the electrode surface, exhibiting both high ionic conductivity and strong thermal stability. This significantly improves the high-temperature cycle life and storage stability of lithium-ion batteries, while simultaneously suppressing lithium dendrite growth and buffering the volume expansion of the silicon anode.

[0065] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A method for preparing a lithium-containing polyborosilazane ceramic precursor, characterized in that, Includes the following steps: S1. Under inert gas protection, polysilazane monomers are dissolved in an anhydrous organic solvent to prepare a polysilazane solution; S2. Add a lithium-containing reagent to the polysilazane solution obtained in step S1, and react at -78℃ to -10℃ for 1 to 12 hours to obtain a lithium-containing polysilazane mixed solution. S3. Add a boron source compound to the lithium-containing polysilazane mixed solution obtained in step S2, and react at 25℃~80℃ for 3~24h to obtain a lithium-containing polyborosilicate mixed solution. S4. The lithium-containing polyborosilicate mixed solution obtained in step S3 is filtered and the solvent is removed by vacuum distillation to obtain the lithium-containing polyborosilicate ceramic precursor.

2. The method for preparing the lithium-containing polyboronsilazane ceramic precursor according to claim 1, characterized in that, In step S1, the general structural formula of the polysilazane precursor is as follows: Formula I: Formula I, Where m is an integer from 0 to 6; n is an integer from 0 to 6; R1, R2, R3, and R4 are each independently selected from H, an aliphatic group, or an aromatic group.

3. The method for preparing the lithium-containing polyboronsilazane ceramic precursor according to claim 1, characterized in that, In step S1, the anhydrous organic solvent is selected from one or more of tetrahydrofuran, diethyl ether, ethyl acetate, acetone, N,N-dimethylformamide, dichloromethane, 1,4-dioxane, toluene, xylene, and n-hexane.

4. The method for preparing the lithium-containing polyboronsilazane ceramic precursor according to claim 1, characterized in that, In step S2, the lithium-containing reagent is selected from one or more of methyllithium, phenyllithium, lithium ethylenediamine complex, trimethylsilylacetylene, lithium cyclopentadiene, lithium hydride, lithium chloride, lithium bromide, lithium iodide, lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, lithium borohydride, lithium amino, diisopropylaminolithium, bistrimethylsilylaminolithium, and 2,2,6,6-tetramethylpiperidinelithium; the molar ratio of the lithium-containing reagent to the polysilazane is (0.1-0.8):

1.

5. The method for preparing the lithium-containing polyboronsilazane ceramic precursor according to claim 1, characterized in that, In step S3, the boron source compound is selected from one or more of the following: boric acid, 3-bromo-5-methylphenylboronic acid, 1-octylboronic acid, n-hexylboronic acid, n-dodecanoboronic acid, 6-ethoxy-2-naphthoboronic acid, phenylboronic acid, 3-methoxyphenylboronic acid, 4-methoxyphenylboronic acid, trimethyl borate, p-methylphenylboronic acid, 3-isopropylphenylboronic acid, n-decylboronic acid, 4-(4-fluorophenyl)phenylboronic acid, 4-methylbiphenylboronic acid, 4-chloro-1-naphthoboronic acid, heptylboronic acid, boron trichloride, dimethyl borane sulfide, pyridine borane, 4-isopropylthiophenylboronic acid, dibenzofuran-3-boronic acid, 4-(methoxymethyl)phenylboronic acid, ammonia borane, and pinacol borane.

6. A lithium-containing polyborosilazane ceramic precursor, characterized in that, The lithium-containing polyborosilicate ceramic precursor is prepared by the preparation method of any one of claims 1-5, wherein the number-average molecular weight of the lithium-containing polyborosilicate ceramic precursor is 500-5000 and the solid content is 65-95%; the molecular structure of the lithium-containing polyborosilicate ceramic precursor simultaneously contains a Si-N main chain, BN bonds and N-Li bonds; the lithium-containing polyborosilicate ceramic precursor is pyrolyzed and ceramicized at 600℃~1000℃ to obtain lithium silicon nitrogen ceramic containing LiSi2N3 crystal phase.

7. An electrolyte, characterized in that, It includes lithium salt, organic solvent and lithium-containing polyborosilazane ceramic precursor as described in claim 6; the amount of lithium-containing polyborosilazane ceramic precursor added is 0.1~5 wt% of the total mass of the electrolyte.

8. The electrolyte according to claim 7, characterized in that, The lithium salt is selected from one or more of LiPF6, LiFSI, and LiBF4, and the concentration of the lithium salt in the electrolyte is 0.8~1.3 mol / L.

9. The electrolyte according to claim 7, characterized in that, The organic solvent is selected from at least two of EC, DMC, EMC, and PC.

10. The application of the lithium-containing polyborosilazane ceramic precursor as described in claim 6 in a lithium-ion battery, characterized in that, The lithium-containing polyboron silazane ceramic precursor is used as an electrolyte deacidification and dehydration additive, an electrode interface modifier, a silicon anode expansion buffer layer, or a solid-state battery interface modification layer.