Preparation method of sodium carboxymethyl starch graft copolymer and application thereof in thermal response quenching liquid

By preparing sodium carboxymethyl starch graft copolymer, the problem of remelting lag in PAG-type quenching fluid was solved, achieving precise control of cooling rate and improved stability, reducing usage costs, and making it suitable for controllable quenching and cooling treatment of various workpieces.

CN123152117APending Publication Date: 2026-11-24YANTAI THINKING FINECHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611664949.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing PAG-type quenching fluids suffer from polymer re-dissolution lag during use, resulting in a decrease in the concentration of effective components carried out by the workpiece, poor cooling stability, and increased usage costs and maintenance difficulties.

Method used

A sodium carboxymethyl starch graft copolymer was prepared by combining sodium carboxymethyl starch with a low critical solution temperature polymer. Polyetheramine was then linked to the sodium carboxymethyl starch backbone through a chemical grafting method to form a thermally responsive quenching fluid. The fluid's high-temperature hydrophobic association and low-temperature water solubility properties enabled precise control of the cooling rate.

Benefits of technology

It achieves precise control of the cooling rate during quenching, reduces polymer carry-out, improves the cooling stability of the quenching fluid, reduces usage costs, and the material is environmentally friendly and renewable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152117A_ABST
    Figure CN123152117A_ABST
Patent Text Reader

Abstract

This invention relates to the field of heat treatment, and discloses a method for preparing sodium carboxymethyl starch graft copolymer and its application in a thermally responsive quenching fluid. The graft copolymer uses sodium carboxymethyl starch as the backbone and polyetheramine as the temperature-sensitive side chain, and is prepared by covalently grafting polyetheramine onto the sodium carboxymethyl starch backbone via an amidation reaction. This graft copolymer is in a dissolved state below the LCST, exhibiting low viscosity, which facilitates workpiece immersion. In the high-temperature quenching stage above the LCST, hydrophobic association and self-assembly occur, significantly increasing the system viscosity and forming a stable polymer coating on the workpiece surface, effectively suppressing the initial cooling rate and preventing workpiece cracking and deformation. The quenching fluid is an aqueous solution of 2-5 wt% sodium carboxymethyl starch graft copolymer. Compared with existing PAG-based and oil-based quenching fluids, the quenching fluid of this invention has temperature-sensitive and reversible thermal thickening characteristics, controllable cooling rate, and is suitable for controllable quenching and cooling treatment of various workpieces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat treatment, and more particularly to a method for preparing sodium carboxymethyl starch graft copolymer and its application in thermally responsive quenching fluids. Background Technology

[0002] Quenching is the core process in metal heat treatment, which involves rapidly cooling a red-hot workpiece to obtain the desired microstructure and properties. Water-based polymer quenching fluids, due to their combination of the cooling properties of water and oil, safety, environmental friendliness, and adjustable cooling rate, have become the main development direction for quenching media. These fluids mainly include types such as polyalkylene glycol (PAG), polyacrylate (ACR), and polyvinylpyrrolidone (PVP), with PAG quenching fluid being the most widely used.

[0003] However, existing PAG-based quenching fluids suffer from polymer re-dissolution lag in practical applications. Specifically, when a high-temperature workpiece enters the quenching fluid, the PAG polymer forms a coating on the workpiece surface to control the cooling rate; however, once the workpiece temperature drops below the lower critical dissolution temperature (LCST), the PAG polymer molecular chains require a considerable amount of time to completely dissolve back into the quenching fluid. This re-dissolution lag results in the concentration of effective components carried out of the fluid by the workpiece being higher than the average concentration of the quenching fluid. After long-term cumulative operation, the relative concentration of PAG in the quenching fluid continues to decrease, reducing cooling stability and requiring frequent replenishment and adjustment, thus increasing operating costs and maintenance difficulty. Summary of the Invention

[0004] Sodium carboxymethyl starch (CMS) is a widely available, renewable, and environmentally friendly natural polymer derivative that can be used as both a thickener and a disintegrant, exhibiting extremely rapid water solubility and a high molecular weight. By combining sodium carboxymethyl starch with a low critical solution temperature (LCST) polymer, the polymer's properties are utilized: above the LCST, it shrinks and aggregates due to hydrophobic association, resulting in a significant increase in solution viscosity; below the LCST, the polymer chains extend and remain in a dissolved state. Addressing the shortcomings of existing technologies, this invention provides a method for preparing a sodium carboxymethyl starch graft copolymer, and uses this copolymer to prepare a thermally responsive quenching fluid. This overcomes the drawbacks of existing PAG-type quenching fluids, such as high workpiece carry-out and continuous loss of effective components due to polymer remelting lag, achieving precise control of the cooling rate during quenching and rapid polymer remelting after quenching.

[0005] In a first aspect, the present invention provides a method for preparing the above-mentioned sodium carboxymethyl starch graft copolymer, comprising the following steps:

[0006] 1) Disperse sodium carboxymethyl starch in ethanol, adjust the pH with MES, stir until dissolved and homogeneous, and set aside.

[0007] 2) Dissolve the polyetheramine in deionized water, adjust the pH with dilute hydrochloric acid, stir well, and set aside.

[0008] 3) Mix the liquids prepared in steps 1) and 2), add DMTMM, and stir to react;

[0009] 4) Vacuum rotary evaporate the reaction solution from step 3) to obtain a concentrated solution;

[0010] 5) The concentrated solution obtained in step 4) is added dropwise into cold acetone to precipitate the precipitate. After filtering the precipitate, it is washed with cold acetone and dried under vacuum to obtain the sodium carboxymethyl starch graft copolymer.

[0011] Furthermore, in step 1), the degree of substitution of sodium carboxymethyl starch is 0.2–0.8. The degree of substitution (DS) determines the number of -COO atoms that can be grafted onto the sodium carboxymethyl starch backbone. - The number of grafting sites and the hydrophilicity of the main chain are crucial factors. When the DS is below 0.2, there are too few active sites on the backbone that can participate in the amidation reaction, resulting in a low grafting rate and insufficient content of temperature-sensitive side chains in the product. This makes it difficult to form a sufficiently strong hydrophobic association network at high temperatures, leading to insignificant thermal thickening and film-forming cooling effects. When the DS is above 0.8, the main chain is too hydrophilic and the carboxyl group density is too high. On the one hand, this competes with the temperature-sensitive aggregation behavior of the polyetheramine side chains, weakening the LCST responsiveness. On the other hand, the excessive local charge density in the reaction system easily leads to a decrease in DMTMM activation efficiency and excessively high product water solubility, making it difficult to effectively precipitate and form a film at high temperatures. Controlling the DS between 0.2 and 0.8 ensures sufficient grafting sites while maintaining a suitable hydrophilic-hydrophobic balance, allowing the product to possess both low-temperature water solubility and high-temperature thermal thickening capabilities.

[0012] Further, in step 2), the polyetheramine is one of M-600, M-1000, M-2005, M-2070, or M-3058. The molecular weight and EO / PO segment ratio of the polyetheramine directly determine the LCST value and high-temperature film-forming properties of the grafted product. Lower molecular weight polyetheramines such as M-600 and M-1000 have relatively high LCST and shorter segments, resulting in a higher thermal thickening response temperature and a relatively mild thickening amplitude after grafting. Higher molecular weight polyetheramines such as M-2005, M-2070, and M-3058 have a larger proportion of hydrophobic PO segments and relatively lower LCST, allowing the grafted product to undergo hydrophobic association earlier in the quenching and boiling film stage, forming a denser polymer coating. All five polyetheramines mentioned above are commercially available products with stable sources and controllable costs. Furthermore, their terminal amino group reactivity is moderate, ensuring the smooth progress of the amidation grafting reaction with the sodium carboxymethyl starch backbone. Based on the material and cooling rate requirements of the target workpiece, a suitable molecular weight of polyetheramine can be selected within the above range to achieve adjustable design of the LCST and cooling characteristics of the quenching fluid.

[0013] Furthermore, in step 1), the pH is 6-6.7; in step 2), the pH is 5.5-6.5. The DMTMM-mediated carboxyl-amino amidation reaction is highly sensitive to pH. At excessively low pH, the -COO group in sodium carboxymethyl starch... - The amino group at the end of the polyether amine is protonated to -COOH, resulting in decreased nucleophilicity. Simultaneously, the terminal amino group is excessively protonated to -NH3. + The loss of nucleophilic activity leads to a significant decrease in grafting efficiency. At excessively high pH, ​​the DMTMM active ester intermediate is easily hydrolyzed and deactivated, and the terminal amino groups of the polyetheramine may undergo side reactions, resulting in poorer controllability of the product structure. Controlling the pH of the system in step 1) to 6–6.7 and the pH of the polyetheramine solution in step 2) to 5.5–6.5 ensures that the mixed reaction system is in a weakly acidic to near-neutral range, guaranteeing that the carboxyl groups are in the partially dissociated -COO group. - The polyether amine terminal amino group exists in a form that is successfully activated by DMTMM, while ensuring that the free -NH2 form of the polyether amine terminal amino group maintains sufficient nucleophilic reactivity, thereby obtaining a high grafting rate and good product uniformity.

[0014] Further, in step 3), according to the -COO in sodium carboxymethyl starch... - The product is mixed with polyetheramine at a molar ratio of -NH2 of 1:(0.1~3). This molar ratio determines the grafting density of the temperature-sensitive side chains in the product. Insufficient polyetheramine content (-NH2 / -COO2) will result in an undesirable grafting density. - When the grafting density is less than 0.1%, the hydrophobic association ability of the product at high temperatures is weak, and the effects of thermal thickening and film-forming cooling are limited; excessive polyetheramine content (-NH2 / -COO) - When the ratio is greater than 3, a large amount of ungrafted free polyetheramine remains in the system, which not only wastes raw materials and increases the purification burden, but may also interfere with the stability of the grafted product performance due to the temperature-sensitive precipitation behavior of the free polyetheramine itself. Controlling the molar ratio at 1:(0.1~3) can ensure sufficient grafting density while taking into account both raw material utilization and product performance, and the LCST and high-temperature thickening range of the product can be flexibly controlled by adjusting this ratio.

[0015] Furthermore, in step 3), the amount of DMTMM is equal to the amount of -COO in sodium carboxymethyl starch. - The dosage of DMTMM, as a condensing agent, directly affects the activation efficiency and grafting rate of the amidation reaction. The dosage should be less than that of -COO. - At 0.1 times the concentration, there are insufficient activation sites, the grafting reaction is incomplete, and the grafting rate of the product is low; when the concentration is higher than that of -COO - When the concentration of DMTMM is four times higher than normal, the excess DMTMM and its hydrolysis byproducts increase, which not only increases the difficulty and cost of purification, but may also cause side reactions such as cross-linking of the sodium carboxymethyl starch backbone, leading to a decrease in the water solubility of the product. The amount of DMTMM should be controlled within the range of -COO. -The concentration is 0.1 to 4 times that of the product, which can ensure the full activation of carboxyl groups and obtain the ideal grafting rate while inhibiting side reactions and reducing residues, thus balancing reaction efficiency and product quality.

[0016] Furthermore, the reaction temperature in step 3) is 20~50℃; the rotary evaporation temperature in step 4) is 40~70℃; and the cold acetone temperature in step 5) is -20℃~-4℃.

[0017] The grafting reaction mechanism in step 3) of the method of the present invention is as follows:

[0018] 1. Overall reaction formula

[0019] CMS-COO - +H2N-PEA→CMS-CONH-PEA;

[0020] That is, the carboxyl groups on the sodium carboxymethyl starch backbone undergo dehydration condensation with the amino groups at the end of the polyether amine to form amide bonds with bridging function.

[0021] 2. Step-by-step mechanism

[0022] Step 1: Carboxyl group activation

[0023] Carboxyl groups (-COO) on the CMS backbone - Under weakly acidic to near-neutral conditions, it partially exists as -COO - DMTMM exists in this form; as a highly efficient condensing agent, it first reacts with -COO... - The reaction produces a highly reactive ester intermediate (DMTMM reactive ester) and releases byproducts such as N-methylmorpholine. The reaction formula is as follows:

[0024] CMS-COO - +DMTMM→CMS-COO-DMT + +byproducts;

[0025] The essence of this step is that DMTMM transforms the carboxyl group, which is originally less nucleophilic and less likely to react directly, into a more electrophilic active ester, making subsequent amino group attack easier.

[0026] Step 2: Nucleophilic attack of amino groups

[0027] The nitrogen atom in the terminal amino group (-NH2) of polyetheramine has a lone pair of electrons and exhibits nucleophilicity. It attacks the carbonyl carbon of the aforementioned reactive ester intermediate to form a tetrahedral intermediate. The reaction formula is as follows:

[0028] CMS-COO-DMT + +H2N-PEA→Tetrahedral intermediate.

[0029] Step 3: Amide bond formation and DMT departure

[0030] The tetrahedral intermediate is unstable and undergoes rearrangement. DMT is released as a leaving group, simultaneously forming a stable amide bond (-CONH-), thereby covalently attaching the polyether amine chain to the CMS backbone. The reaction formula is as follows:

[0031] Tetrahedral intermediate → CMS-CONH-PEA+DMT-OH;

[0032] The final product is the CMS-g-PEA graft copolymer.

[0033] DMTMM, as a condensing agent, has the following advantages in the method of this invention: 1. It can be completed in one step. DMTMM can directly activate the carboxyl group and react with the amino group, without the need to add NHS to prepare intermediates, making the operation simpler; 2. Fewer side reactions. The active ester intermediate of DMTMM is relatively stable and has a slow hydrolysis rate, which is conducive to the full attack of the amino group and improves the grafting rate; 3. The reaction conditions are mild and can be carried out at room temperature in a weakly acidic to near-neutral aqueous system, which is suitable for natural polymer backbones such as sodium carboxymethyl starch, avoiding the degradation of the main chain caused by high temperature or strong acid and strong alkali; 4. The by-products have good water solubility. DMT and other by-products are easily soluble in water and can be effectively removed by subsequent precipitation with acetone, making product purification convenient.

[0034] Secondly, the present invention provides a thermally responsive quenching fluid, which is an aqueous solution of sodium carboxymethyl starch graft copolymer obtained by the method of the present invention. Specifically, the thermally responsive quenching fluid of the present invention is composed of the following substances in weight percentage: 2wt%~5wt% sodium carboxymethyl starch graft copolymer, 0.3wt%~1wt% rust inhibitor, 0.01wt%~0.1wt% defoamer, 0~0.1wt% bactericide, 0~0.1wt% antioxidant, 0~0.05wt% anti-hard water agent, and the balance being water.

[0035] Furthermore, the rust inhibitor is one or a combination of triethanolamine, diisopropanolamine, sebacic acid, and sodium adipic acid; the defoamer is polyether or polyether-modified silicone. The rust inhibitor and defoamer are essential additives, their function being to prevent workpiece corrosion during quenching, while simultaneously suppressing excessive foam generation during stirring or cooling circulation, preventing foam overflow from affecting the operating environment and cooling efficiency.

[0036] Furthermore, the bactericide is benzisothiazolinone or BK; the antioxidant is a water-soluble phenolic compound antioxidant; and the anti-hard water agent is one or more of sodium gluconate and disodium EDTA. These three additives are optional and can be added selectively according to the application scenario. Among them, the bactericide can inhibit the growth of microorganisms in the quenching fluid during long-term use, preventing the system from becoming smelly and deteriorating; the antioxidant can inhibit the oxidative degradation of polymer molecular chains during long-term cyclic use, maintaining stable cooling performance; and the anti-hard water agent can chelate hardness ions such as calcium and magnesium in the water, preventing hardness ions from affecting the polymer's solubility stability and extending the service life of the quenching fluid.

[0037] The beneficial effects of this invention are as follows:

[0038] 1. This invention involves chemically grafting temperature-sensitive side-chain polyetheramine onto a sodium carboxymethyl starch backbone. The hydrophilicity of the sodium carboxymethyl starch backbone facilitates rapid and uniform dispersion of the polymer in aqueous solution, while the grafted polyetheramine segments exhibit excellent anti-solution film-forming properties at high temperatures. The overall integrity and stability of the molecular structure after chemical bonding are significantly superior to that of a physically mixed system. The synergistic effect of the two structures through chemical bonding results in a uniform, dense, and highly flexible viscous polymer coating on the workpiece surface during quenching, which is less prone to rupture, thereby achieving the effect of controlling the cooling rate.

[0039] 2. The sodium carboxymethyl starch graft copolymer obtained in this invention requires less material and uses environmentally friendly and renewable raw materials compared to traditional quenching media. The graft copolymer solution is a uniform, low-viscosity solution below the LCST. When a red-hot workpiece enters the solution and the temperature rises, the graft copolymer undergoes self-assembly, forming a uniform, viscous polymer film on the workpiece surface. When the workpiece temperature drops below the LCST, the strong hydrophilicity of the carboxyl and hydroxyl groups in sodium carboxymethyl starch causes the copolymer to rapidly dissolve back into a uniform, low-viscosity liquid, thus greatly reducing the risk of polymer carryover.

[0040] 3. The thermally responsive quenching fluid of the present invention has temperature-sensitive and reversible thermal thickening characteristics. Compared with existing PAG-type quenching fluids and oil-based quenching fluids, it not only has a controllable cooling rate, but also has the advantages of safety, environmental friendliness and low cost. It is suitable for controllable quenching and cooling treatment of various workpieces. Attached Figure Description

[0041] Figure 1 A photograph of the sodium carboxymethyl starch graft copolymer powder obtained in Example 1;

[0042] Figure 2 The infrared spectrum of sodium carboxymethyl starch used in Example 1;

[0043] Figure 3 The infrared spectrum of the sodium carboxymethyl starch graft copolymer obtained in Example 1 is shown below.

[0044] Figure 4 To adopt Figure 1 Photograph of a 3wt% quenching fluid prepared from sodium carboxymethyl starch graft copolymer powder;

[0045] Figure 5 for Figure 4 Photographs of the quenching fluid after one month of continuous use;

[0046] Figure 6 This is a schematic diagram illustrating the working mechanism of the thermally responsive quenching fluid of the present invention;

[0047] Figure 7 This is a viscosity-temperature curve of the sodium carboxymethyl starch graft copolymer of the present invention. Detailed Implementation

[0048] The present invention will be described below with reference to embodiments. The embodiments are only used to explain the present invention and are not intended to limit the scope of the present invention.

[0049] Example 1

[0050] A method for preparing a sodium carboxymethyl starch graft copolymer includes the following steps:

[0051] 1) Weigh 5 parts by weight of sodium carboxymethyl starch with a degree of substitution of 0.8, disperse it in a small amount of ethanol, dissolve it in MES buffer, adjust the pH to 6, and set aside.

[0052] 2) Disperse 2.89 parts by weight of polyetheramine M-600 in 30 mL of deionized water, and adjust the pH to 6 with 0.1 M HCl for later use;

[0053] 3) Mix the liquids prepared in steps 1) and 2), quickly add 0.82 parts by weight of DMTMM, monitor and adjust the pH to 6 during the reaction, and continue stirring at room temperature for 24 hours to obtain the crude product;

[0054] 4) The crude product from step 3) is subjected to vacuum rotary evaporation at 40°C to remove most of the water, yielding a concentrated solution;

[0055] 5) The concentrated solution obtained in step 4) is dropped into cold acetone at -20°C to precipitate the polymer. After filtration, washing with cold acetone, and vacuum drying, the product is obtained.

[0056] Example 2

[0057] A method for preparing a sodium carboxymethyl starch graft copolymer includes the following steps:

[0058] 1) Weigh 5 parts by weight of sodium carboxymethyl starch with a degree of substitution of 0.5, disperse it in a small amount of ethanol, dissolve it in MES buffer, adjust the pH to 6.5, and set aside.

[0059] 2) Disperse 4.82 parts by weight of polyetheramine M-1000 in 30 mL of deionized water, and adjust the pH to 5.5 with 0.1 M HCl for later use;

[0060] 3) Mix the liquids prepared in steps 1) and 2), quickly add 0.11 parts by weight of DMTMM, monitor and adjust the pH to 6 during the reaction, and stir continuously at 20°C for 30 hours to obtain the crude product;

[0061] 4) The crude product from step 3) is subjected to vacuum rotary evaporation at 50°C to remove most of the water, yielding a concentrated solution;

[0062] 5) The concentrated solution obtained in step 4) is dropped into cold acetone at -10℃ to precipitate the polymer. After filtration, washing with cold acetone, and vacuum drying, the polymer is obtained.

[0063] Example 3

[0064] A method for preparing a sodium carboxymethyl starch graft copolymer includes the following steps:

[0065] 1) Weigh 5 parts by weight of sodium carboxymethyl starch with a degree of substitution of 0.3, disperse it in a small amount of ethanol, dissolve it in MES buffer, adjust the pH to 6.7, and set aside.

[0066] 2) Disperse 9.63 parts by weight of polyetheramine M-2070 in 30 mL of deionized water, and adjust the pH to 6.5 with 0.1 M HCl for later use;

[0067] 3) Mix the liquids prepared in steps 1) and 2), quickly add 0.24 parts by weight of DMTMM, monitor and adjust the pH to 6 during the reaction, and stir continuously at 40°C for 16 hours to obtain the crude product;

[0068] 4) The crude product from step 3) is subjected to vacuum rotary evaporation at 60°C to remove most of the water, yielding a concentrated solution;

[0069] 5) The concentrated solution obtained in step 4) is dropped into cold acetone at -15℃ to precipitate the polymer. After filtration, washing with cold acetone, and vacuum drying, the polymer is obtained.

[0070] Example 4

[0071] A method for preparing a sodium carboxymethyl starch graft copolymer includes the following steps:

[0072] 1) Weigh 5 parts by weight of sodium carboxymethyl starch with a degree of substitution of 0.2, disperse it in a small amount of ethanol, dissolve it in MES buffer, adjust the pH to 6, and set aside.

[0073] 2) Disperse 14.45 parts by weight of polyetheramine M-3050 in 30 mL of deionized water, and adjust the pH to 6 with 0.1 M HCl for later use;

[0074] 3) Mix the liquids prepared in steps 1) and 2), quickly add 0.30 parts by weight of DMTMM, monitor and adjust the pH to 6 during the reaction, and stir continuously at 50°C for 12 hours to obtain the crude product;

[0075] 4) The crude product from step 3) is subjected to vacuum rotary evaporation at 70°C to remove most of the water, yielding a concentrated solution;

[0076] 5) The concentrated solution obtained in step 4) is dropped into cold acetone at -4°C to precipitate the polymer. After filtration, washing with cold acetone, and vacuum drying, the polymer is obtained.

[0077] The sodium carboxymethyl starch graft copolymers obtained in Examples 1 to 4 were formulated into quenching liquids at concentrations of 2 wt%, 3 wt%, 4 wt%, and 5 wt%, respectively. The additives and their contents in each quenching liquid were as follows: triethanolamine 0.6 wt%, THIX-288 polyether defoamer (Yantai Hengxin Chemical Technology Co., Ltd.) 0.06 wt%, BK bactericide 0.05 wt%, antioxidant 702 0.03 wt%, disodium EDTA 0.02 wt%, and the balance being water.

[0078] The cooling characteristics of quenching agents with different concentrations are shown in Tables 1-4. As can be seen from Tables 1-4, with the increase of quenching fluid concentration, T600, T400, and T200 of each embodiment gradually increase, while V300 and maximum cooling rate gradually decrease. This indicates that increasing the polymer concentration enhances the coating thickness and density of the workpiece surface, effectively suppressing the cooling rate. Comparing different embodiments, at the same concentration, the quenching fluid obtained in Example 4 has the lowest V300 and maximum cooling rate, and the longest T600 and T400. Example 3 is next, while Examples 1 and 2 are relatively higher. This is consistent with the trend of increased molecular weight of polyetheramine side chains, enhanced hydrophobic association, and increased thermal thickening. Those skilled in the art can flexibly control the cooling characteristics by selecting different types of polyetheramine and adjusting the quenching fluid concentration according to the material, size, and cooling rate requirements of the target workpiece.

[0079] Table 1. Cooling characteristics of quenching fluids with different concentrations of sodium carboxymethyl starch graft copolymer in Example 1

[0080]

[0081] Table 2. Cooling characteristics of sodium carboxymethyl starch graft copolymer quenching fluids of different concentrations in Example 2.

[0082]

[0083] Table 3. Cooling characteristics of sodium carboxymethyl starch graft copolymer quenching fluids of different concentrations in Example 3.

[0084]

[0085] Table 4. Cooling characteristics of sodium carboxymethyl starch graft copolymer quenching fluids at different concentrations as described in Example 4.

[0086]

[0087] Figure 1 The image shows the sodium carboxymethyl starch graft copolymer powder obtained in Example 1. The powder has a uniform color. Since it was obtained by filtering the reaction solution, there is some agglomeration, but it does not affect its solubility in water.

[0088] Figure 2 and Figure 3 The images show the infrared spectra of sodium carboxymethyl starch used in Example 1 and the obtained sodium carboxymethyl starch graft copolymer, respectively. (Comparison) Figure 2 and Figure 3 It can be seen Figure 3 The curve retains the original characteristic skeleton of sodium carboxymethyl starch (OH, CO0). - CO), at approximately 1650cm -1 A new C=O stretching vibration absorption peak appeared at approximately 1550 cm⁻¹. -1 The appearance of the bending vibration peak characteristic of NH in PEA indicates that DMTMM successfully mediated the reaction between the carboxyl group of sodium carboxymethyl starch and the amino group of polyetheramine in the method of Example 1. The thermosensitive side chain of polyetheramine was covalently grafted onto the sodium carboxymethyl starch backbone, and the target product CMS-g-PEA was successfully synthesized.

[0089] Figure 4 To adopt Figure 1 The photo shows a 3wt% quenching solution prepared from sodium carboxymethyl starch graft copolymer powder. It can be seen that the quenching solution is light yellow, without precipitation or turbidity, and has good overall light transmittance.

[0090] Figure 5 for Figure 4 The photo shows the quenching fluid after one month of continuous use (regular replenishment, only adding and not replacing). The color of the quenching fluid has slightly darkened and it has become somewhat cloudy, but it still maintains good uniformity.

[0091] Figure 6 This is a schematic diagram illustrating the mechanism of action of sodium carboxymethyl starch graft copolymer in the thermally responsive quenching fluid of the present invention during quenching. When the hot workpiece enters the thermally responsive quenching fluid, the temperature-sensitive side chains of the copolymer undergo self-assembly. After the temperature decreases, due to the strong hydrophilicity of the main chain backbone, it rapidly dissolves back into the system.

[0092] Figure 7The graphs show the viscosity changes of sodium carboxymethyl starch graft copolymers obtained in Examples 1 (S1) and 2 (S2) and sodium carboxymethyl starch (CMS-Na) after heating. As can be seen from the curves, the viscosity of the sodium carboxymethyl starch graft copolymers obtained in Examples 1 and 2 increases sharply at 78°C, indicating that the copolymers have significant thermal thickening response characteristics near the critical melting temperature (LCST). In contrast, the ungrafted sodium carboxymethyl starch did not exhibit obvious thermal thickening behavior, verifying that polyetheramine graft modification is the key to imparting temperature-sensitive responsiveness to the product.

[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing sodium carboxymethyl starch graft copolymer, characterized in that, Includes the following steps: 1) Disperse sodium carboxymethyl starch in ethanol, adjust the pH with MES, stir until dissolved and homogeneous, and set aside. 2) Dissolve the polyetheramine in deionized water, adjust the pH with dilute hydrochloric acid, stir well, and set aside. 3) Mix the liquids prepared in steps 1) and 2), add DMTMM, and stir to react; 4) Vacuum rotary evaporate the reaction solution from step 3) to obtain a concentrated solution; 5) The concentrated solution obtained in step 4) is added dropwise into cold acetone to precipitate the precipitate. After filtering the precipitate, it is washed with cold acetone and dried under vacuum to obtain the sodium carboxymethyl starch graft copolymer.

2. The method according to claim 1, characterized in that, In step 1), the degree of substitution of the sodium carboxymethyl starch is 0.2 to 0.

8.

3. The method according to claim 1, characterized in that, In step 2), the polyetheramine is one of M-600, M-1000, M-2005, M-2070 or M-3058.

4. The method according to claim 1, characterized in that, In step 1), the pH is 6-6.7; in step 2), the pH is 5.5-6.

5.

5. The method according to claim 1, characterized in that, In step 3), according to the -COO in sodium carboxymethyl starch - It is mixed with polyetheramine in a molar ratio of -NH2 of 1:(0.1~3).

6. The method according to claim 1, characterized in that, In step 3), the amount of DMTMM is equal to the amount of -COO in sodium carboxymethyl starch. - 0.1 to 4 times that.

7. The method according to claim 1, characterized in that, The reaction temperature in step 3) is 20~50℃; the rotary evaporation temperature in step 4) is 40~70℃; and the cold acetone temperature in step 5) is -20℃~-4℃.

8. A thermally responsive quenching fluid, characterized in that, The thermally responsive quenching fluid is composed of the following substances in weight percentages: 2 wt% to 5 wt% of sodium carboxymethyl starch graft copolymer prepared by the method of any one of claims 1 to 7, 0.3 wt% to 1 wt% of rust inhibitor, 0.01 wt% to 0.1 wt% of defoamer, 0 to 0.1 wt% of bactericide, 0 to 0.1 wt% of antioxidant, 0 to 0.05 wt% of anti-hard water agent, and the balance being water.

9. The thermally responsive quenching fluid according to claim 8, characterized in that, The rust inhibitor is one or a combination of triethanolamine, diisopropanolamine, sebacic acid, and sodium adipic acid; the defoamer is polyether or polyether-modified silicone.