Aramid nanofiber composite based on hydroxypropylated polyrotaxane dynamic topological interlocking

By introducing hydroxypropylated polyrotaxane into ANF films to form a dynamic topological interlocking network, the problem of balancing strength, toughness, and transparency of ANF films in flexible electronic devices is solved, realizing a composite material with high strength, high toughness, and high transparency, suitable for applications such as flexible electronic insulating base films and transparent UV protection films.

CN123152126APending Publication Date: 2026-11-24BEIJING JIAOTONG UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611111719.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-24
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing ANF films are difficult to simultaneously satisfy high strength, toughness, transparency, insulation and heat resistance in flexible electronics and foldable devices. Furthermore, the toughening process of flexible components can easily dilute the rigid support network, leading to a decrease in strength and modulus. The distribution of modified components is uneven, making it difficult to construct a uniform interface.

Method used

During the deprotonation and dissociation of PPTA fibers into ANF, hydroxypropylated polyrotaxane (HyPR) is introduced to form a dynamic topological interlocking network. Through hydroxy-amide hydrogen bonding, molecular chain entanglement and interfacial adsorption, the surface of ANF is coated to construct a sliding and energy-consuming dynamic cross-linking network, thereby improving tensile strength, fracture strain and toughness.

Benefits of technology

While maintaining the intrinsic thermal stability, electrical insulation and UV shielding capabilities of ANF, the tensile strength, fracture strain and toughness of the film were significantly improved, and high visible light transparency was maintained, avoiding stress concentration and interface discontinuity problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152126A_ABST
    Figure CN123152126A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing an aramid nanofiber composite material based on hydroxypropylated polyrotaxane with dynamic topological interlocking, comprising the following steps: preparing hydroxypropylated polyrotaxane containing a dynamic topological interlocking structure; and dissociating para-aramid fibers in a pyrolysis solution containing the aforementioned hydroxypropylated polyrotaxane with a dynamic topological interlocking structure. In the process of deprotonating and dissociating para-aramid fibers into ANF, this invention simultaneously introduces a dynamic crosslinking network that is slippery, energy-dissipating, and capable of forming strong interfacial interactions with ANF. This reconstructs the energy dissipation path of the ANF composite film at the molecular scale, thereby simultaneously improving tensile strength, fracture strain, toughness, crack tolerance, and repeated deformation stability, while preserving the intrinsic thermal stability, electrical insulation, UV shielding ability, and visible light transparency of ANF as much as possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aramid nanofiber technology, and particularly relates to an aramid nanofiber composite material based on hydroxypropylated polyrotaxane dynamic topological interlocking. Background Technology

[0002] Para-aramid (PPTA, poly(p-phenylene terephthalamide)) fiber is a macroscopic precursor of aramid nanofiber (ANF), possessing advantages such as high strength and modulus, high temperature resistance, acid and alkali resistance, and lightweight, and is widely used in aerospace, defense protection, electronics and electrical engineering, and high-performance composite materials. Macroscopic PPTA fibers can be deprotonated and dissociated in a dimethyl sulfoxide (DMSO) / strong alkali system to obtain ANF, which has nanoscale diameter, high aspect ratio, large specific surface area, and abundant surface amide groups, retaining the intrinsic properties of aramid while significantly improving interfacial compatibility. ANF films are currently used in electrical insulating paper, UV-resistant films, thermal management materials, flame retardant materials, composite material reinforcement, and electromagnetic shielding substrates. However, while the rigid molecular chains and dense hydrogen bond stacking of ANF films provide high strength, they also lead to low fracture strain and defect sensitivity. Especially in flexible electronics and foldable devices, the films need to withstand bending, torsion, tension, notch propagation, and environmental aging simultaneously; high strength alone is no longer sufficient to meet practical service requirements.

[0003] Traditional methods for preparing ANF thin films include KOH / DMSO deprotonation, mechanically assisted exfoliation, electrospinning, and polymerization-induced self-assembly. Among these, the KOH / DMSO deprotonation method can better preserve the aramid molecular structure and is a common route for preparing ANF dispersions and ANF thin films. However, pure ANF thin films mainly rely on a rigid hydrogen bond network, exhibiting high strength but insufficient fracture strain, fracture toughness, crack tolerance, and repeated deformation stability.

[0004] To solve the above problems, existing technologies mainly adopt the following approaches: (1) ANF / flexible polymer composite; for example, introducing flexible components such as polyvinyl alcohol (PVA), polyurethane, and cellulose containing a large number of hydroxyl groups into the ANF system can improve fracture strain and film stability. However, ordinary flexible polymers are usually distributed as "soft phases" between ANFs, which can easily reduce the proportion of rigid load-bearing networks. When the flexible component is excessive, the strength and modulus decrease significantly.

[0005] (2) Metal ion or inorganic particle reinforcement route: For example, CN116926981A discloses a method for iron ion-reinforced ANF thin films: FeCl3·6H2O is dissolved in DMSO, and then PPTA, KOH and water are added. During the pyrolysis process, iron ions / iron hydroxide nanoparticles are introduced in situ, and then the film is obtained by protonation, vacuum filtration, cold pressing and drying. This technical solution improves mechanical and insulation properties through coordination, electrostatic interaction and particle reinforcement, but its core reinforcement is inorganic / ionic crosslinking and particle interface interaction. In addition, although metal ions and inorganic particles can improve local strength, they may bring problems such as agglomeration, interface defects, changes in conductivity, reduced transparency or fixation stress concentration.

[0006] (3) Solvent replacement or densification route: For example, patent CN117416077A discloses a method for preparing a high-strength, high-toughness, and high-transparency ANF film, which improves the strength, toughness, and transparency of the film by replacing the ANF with an aprotic solvent to make the ANFs more tightly bonded and reduce defects. Solvent replacement or densification is mainly used to improve film structure defects, as it is difficult to provide energy-consuming units that can dynamically rearrange under stress at the molecular scale.

[0007] While the above-mentioned approaches can improve some properties, they still generally suffer from the following problems: First, it is difficult to simultaneously achieve strength, toughness, transparency, insulation, and heat resistance; second, fixing crosslinking points, using rigid fillers, or ionic particles may create new stress concentrations; third, post-mixing or multi-step compounding makes it difficult to ensure that the modified components uniformly coat each ANF fiber; fourth, the toughening effect of conventional flexible components can easily dilute the rigid load-bearing network of the ANF, leading to a decrease in strength and modulus. Furthermore, in post-mixing modification, uneven distribution and insufficient coating between the modified components and the already formed ANF are prone to occur, making it difficult to stably construct a uniform interface at the single-fiber scale.

[0008] Polyrotaxane (PR) is a mechanically interlocked molecule formed by a cyclic host molecule encased in a linear axial chain and then capped. The cyclic molecule can slide, rotate, and rearrange along the linear axial chain, dispersing stress and dissipating frictional energy under external forces. It has shown potential for strengthening and toughening gels, elastomers, composite fibers, and some two-dimensional film materials. However, current common applications of PR mainly focus on soft gels, thermoplastics, or two-dimensional sheet materials; its application in ANF (angiotensin-converter) has not yet been observed. Summary of the Invention

[0009] To address the aforementioned technical problems, this invention provides an aramid nanofiber composite material based on hydroxypropylated polyrotaxane with dynamic topological interlocking. During the deprotonation and dissociation of PPTA fibers into ANF, this invention simultaneously introduces a dynamic cross-linking network that is slippery, energy-dissipating, and capable of forming strong interfacial interactions with ANF. This reconstructs the energy dissipation path of the ANF composite film at the molecular scale, thereby simultaneously improving tensile strength, fracture strain, toughness, crack tolerance, and repeated deformation stability, while preserving the intrinsic thermal stability, electrical insulation, UV shielding ability, and visible light transparency of ANF as much as possible.

[0010] To achieve the above objectives, the technical solution adopted by the present invention is as follows: On one hand, the present invention provides a method for preparing aramid nanofiber composite materials based on hydroxypropylated polyrotaxane dynamic topological interlocking, comprising the following steps: (1) Hydroxypropyl modified polyrotaxane (HyPR) is reacted with a polymer containing active group I and active group II to obtain hydroxypropylated polyrotaxane containing a dynamic topological interlocking structure; wherein active group I is a functional group that can form hydrogen bonds with aramid nanofibers (ANF); wherein active group II is a functional group that can form covalent bonds with hydroxypropyl modified polyrotaxane (HyPR), or a functional group that can form covalent bonds with hydroxypropyl modified polyrotaxane (HyPR) activated by N,N'-carbonyldiimidazole (CDI).

[0011] (2) The para-aramid (PPTA) fiber is dissociated in a pyrolysis solution containing hydroxypropylated polyrotaxane with a dynamic topological interlocking structure obtained in step (1), and the hydroxypropylated polyrotaxane with a dynamic topological interlocking structure is coated on the surface of the aramid nanofiber (ANF) obtained by dissociating the para-aramid (PPTA) fiber.

[0012] In a preferred embodiment, in step (1), the active group I is selected from at least one of hydroxyl, carboxyl, amino, amide, carbamate, ether, ester, carbonyl, sulfonyl, primary amine and nitrogen-containing heterocyclic groups.

[0013] Preferably, the active group II is selected from at least one of hydroxyl, carboxyl, amino, borate, isocyanate, aldehyde, azide, alkynyl, alkenyl, and epoxy groups.

[0014] In the technical solution of the present invention, in step (1), the reaction between hydroxypropyl modified polyrotaxane (HyPR) and a polymer containing active group I and active group II is selected from at least one of esterification reaction, urethane esterification reaction, click chemistry reaction, aldehyde-amine dynamic bond reaction, borate esterification reaction, epoxy ring-opening reaction and amidation reaction.

[0015] In some specific embodiments, the hydroxypropyl-modified polyrotaxane is activated by N,N'-carbonyldiimidazole (CDI) and then undergoes an esterification reaction with a polymer containing hydroxyl groups.

[0016] In some specific embodiments, the hydroxypropyl and / or hydroxyl groups of the hydroxypropyl-modified polyrotaxane undergo esterification with a polymer containing carboxyl groups.

[0017] In some specific embodiments, the hydroxypropyl-modified polyrotaxane is activated by N,N'-carbonyldiimidazole (CDI) and then undergoes a carbamate reaction with an amino-containing polymer.

[0018] In some specific embodiments, the hydroxypropyl modified polyrotaxane is activated by N,N'-carbonyldiimidazole (CDI) and then reacts with an amine containing an azide group to introduce an azide group, and then undergoes an azide-alkyne cycloaddition click chemistry reaction with a polymer containing an alkyne group; In some specific embodiments, the hydroxypropyl-modified polyrotaxane, after being modified to introduce thiol groups, undergoes a thiol-alkene click chemical reaction with a polymer containing alkenyl groups in the presence of a photoinitiator or a free radical initiator.

[0019] In some specific embodiments, the hydroxyl groups on the hydroxypropyl-modified polyrotaxane are oxidized or derivatized into aldehyde groups, which then undergo a Schiff base reaction with a polymer containing primary amine groups to generate reversible imine bonds.

[0020] In some specific embodiments, the hydroxypropyl-modified polyrotaxane is activated by N,N'-carbonyldiimidazole (CDI) and then undergoes a borate esterification reaction with a polymer containing boric acid groups.

[0021] In some specific embodiments, the hydroxypropyl groups and / or hydroxyl groups on the hydroxypropyl-modified polyrotaxane undergo a carbamate reaction with the isocyanate-containing polymer.

[0022] In some specific embodiments, the hydroxyl groups on the hydroxypropyl-modified polyrotaxane, or the amino groups introduced through modification, undergo a ring-opening reaction with a polymer containing epoxy groups.

[0023] In some specific embodiments, the activation process of the hydroxypropyl-modified polyrotaxane by N,N'-carbonyldiimidazole (CDI) includes the following steps: heating and stirring the hydroxypropyl-modified polyrotaxane and N,N'-carbonyldiimidazole (CDI) in a solvent. The heating temperature is 60-70°C; the heating and stirring time is 2-4 h; and the mass ratio of the hydroxypropyl-modified polyrotaxane to N,N'-carbonyldiimidazole (CDI) is 1:1-3.

[0024] In a preferred embodiment, the polymer containing active group I and active group II is selected from at least one of polyvinyl alcohol, polyacrylic acid (PAA), polyamide (PA) containing active group II, and polyvinylpyrrolidone containing active group II, more preferably polyvinyl alcohol and / or polyacrylic acid (PAA), and most preferably polyvinyl alcohol.

[0025] In some specific embodiments, the molecular weight of the polyvinyl alcohol is 14,600 to 18,600.

[0026] In some specific implementations, step (1) includes the following steps: Polyvinyl alcohol and hydroxypropyl-modified polyrotaxane activated by N,N'-carbonyldiimidazole (CDI) were esterified in a solvent to obtain hydroxypropylated polyrotaxane containing a dynamic topological interlocking structure.

[0027] Preferably, the mass ratio of the polyvinyl alcohol to the hydroxypropyl-modified polyrotaxane is 20-40:1.

[0028] Preferably, the esterification reaction is carried out at a temperature of 75-85°C.

[0029] Preferably, the esterification reaction takes 4 to 6 hours.

[0030] In a preferred embodiment, the preparation method of the hydroxypropyl-modified polyrotaxane (HyPR) includes the following steps: S1. A host-guest inclusion-extension reaction is carried out by mixing cyclodextrin with polyethylene glycol with carboxyl groups at both ends, so that the cyclodextrin is encased on the polyethylene glycol molecule with carboxyl groups at both ends to obtain quasi-polyrotaxane (PPR). S2. End-capping the polyethylene glycol end in the quasi-polyrotaxane with 1-adamantane to obtain polyrotaxane (PR). S3. Modify the polyrotaxane (PR) with propylene oxide to obtain hydroxypropyl modified polyrotaxane (HyPR).

[0031] Preferably, the cyclodextrin is selected from at least one of α-cyclodextrin (α-CD), β-cyclodextrin (β-CD), γ-cyclodextrin (γ-CD), dimethylcyclodextrin and glucose cyclodextrin and their derivatives and modified compounds.

[0032] In the technical solution of this invention, the polyethylene glycol with carboxyl groups at both ends can be prepared by oxidation of the end groups of polyethylene glycol. In some specific embodiments, the molecular weight of the polyethylene glycol is 20,000 to 35,000.

[0033] Preferably, the mass ratio of the cyclodextrin to the polyethylene glycol with carboxyl groups at both ends is 4~6:1.

[0034] Preferably, in step S1, the temperature of the host-guest encapsulation reaction is 0~10℃ and the time is 8~24 h.

[0035] In some specific embodiments, step S2 includes the following steps: activating quasi-polyrotaxane (PPR) and benzotriazol-1-yl-oxytris(dimethylamino)phosphonium hexafluorophosphate (BOP) and N-ethyldiisopropylamine (DIPEA) in a solvent for 10-20 min, then adding 1-adamantaneamine and reacting for 24-48 h for end-capping. For every 7 g of quasi-polyrotaxane (PPR), the corresponding amount of 1-adamantaneamine is 0.17-0.20 g, the corresponding amount of BOP is 0.25-0.50 g, and the corresponding amount of DIPEA is 100-200 μL.

[0036] In some specific embodiments, step S3 includes the following steps: reacting polyrotaxane (PR) and propylene oxide in NaOH solution in an ice bath, followed by continuing the reaction at room temperature (25-35°C). The ice bath reaction time is 0.5-1 h, and the room temperature reaction time is 36-48 h. For every 0.5 g of polyrotaxane (PR) dissolved in 40-60 mL of 1 M NaOH solution, the corresponding amount of propylene oxide is 3.5-4.5 g.

[0037] In a preferred embodiment, in step (2), the lysis solution also contains KOH, dimethyl sulfoxide (DMSO) and H2O.

[0038] Preferably, the para-aramid (PPTA) fiber is a short fiber.

[0039] In some specific embodiments, for every 1 g of para-aramid (PPTA) fiber, the corresponding mass of dimethyl sulfoxide (DMSO) is 93.75 g, the corresponding mass of H2O is 7.5 g, and the corresponding mass of KOH is 3 g.

[0040] Preferably, the mass of the hydroxypropylated polyrotaxane containing the dynamic topological interlocking structure is 20% to 40% of its total mass with that of the para-aramid (PPTA) fiber.

[0041] In the technical solution of the present invention, during the dissociation process in step (2), PPTA is deprotonated and dissociated into ANF; PVA@PR simultaneously coats the surface of ANF through hydroxyl-amide hydrogen bonds, molecular chain entanglement and interfacial adsorption.

[0042] In a preferred embodiment, the dissociation temperature in step (2) is 25~35℃; Preferably, the dissociation time is 6-8 hours.

[0043] In some specific embodiments, step (2) further includes a protonation precipitation process and a film formation process. The protonation precipitation process includes adding 4 to 6 times the volume of water to the dissociated system. The film formation process is selected from at least one of vacuum-assisted filtration, hot-pressing extension to casting, pressure filtration, spraying, blade coating, layer-to-layer assembly, and roll-to-roll continuous filtration hot-pressing.

[0044] In some specific embodiments, the protonation precipitation process and film formation process are as follows: 4-6 times the volume of water is added to the dissociated system to re-protonate the deprotonated ANF and precipitate it from the system, forming a suspension or wet gel system; stirring is continued to homogenize the system; a gel membrane is obtained by vacuum filtration through a porous filter membrane, dried at 60-70°C for 20-30 min, and then hot-pressed at 0.5-1 MPa and 60-70°C for 20-30 min to obtain an aramid nanofiber composite film based on hydroxypropylated polyrotaxane dynamic topological interlocking. The thickness of the composite film can be adjusted by the filtration volume, solid content, filter membrane size, and hot-pressing conditions.

[0045] On another aspect, the present invention provides an aramid nanofiber composite material based on dynamic topological interlocking of hydroxypropylated polyrotaxane obtained by the above preparation method.

[0046] On another aspect, the present invention provides the use of the above-mentioned aramid nanofiber composite material based on hydroxypropylated polyrotaxane dynamic topological interlocking in the preparation of flexible electronic insulating base film, transparent ultraviolet protection film, heat-resistant flexible packaging substrate, aerospace lightweight protective intermediate layer, foldable electronic device support material or packaging material, electromagnetic shielding material or electrothermal functional composite material.

[0047] The above technical solution has the following advantages or beneficial effects: Compared to conventional ANF / PVA polymer blends, the PVA in the aramid nanofiber composite material provided by this invention is not merely a flexible toughening phase, but is endowed with dynamic topological energy dissipation capabilities by HyPR. Simultaneously, PVA@PR participates in surface coating during the PPTA pyrolysis stage, resulting in a more uniform interface structure and reducing agglomeration and phase separation during post-mixing. Therefore, this invention does not simply rely on flexible segments to improve ductility, but rather provides rearranged and slippery topological energy dissipation channels through HyPR slip rings, actively releasing stress concentration during stress application. Thus, it can significantly improve toughness and fracture strain while maintaining or even enhancing strength.

[0048] Compared to existing polyrotaxane-toughened polymers or two-dimensional material systems, this invention places the polyrotaxane network at the PPTA dissociation stage, enabling the dynamic network to complete surface coating and interface construction during the formation of a single ANF strand. This avoids phase separation and interface discontinuities caused by post-mixing, resulting in more efficient load transfer and a more stable layered structure. Compared to most ANF composite films that emphasize a single function, this invention also considers high breakdown strength, excellent UV shielding, high visible light transparency, and environmental stability, thus possessing stronger comprehensive application potential in the field of flexible insulating transparent protection. Attached Figure Description

[0049] Figure 1 These are TEM images and diameter distribution histograms of the nanofibers ANF, AA@PR-1, AA@PR-2, AA@PR-3, and AA@PR-4 prepared in the embodiments of the present invention at different magnifications.

[0050] Figure 2 These are the proton NMR spectra and Fourier transform infrared spectra of HyPR, α-CD, and PEG in the embodiments of the present invention.

[0051] Figure 3 This is a comparison of the full-spectrum hydrogen NMR spectra of PVA@PR and PVA prepared in the embodiments of the present invention. 1 H NMR).

[0052] Figure 4 These are the Fourier transform infrared spectrum, X-ray diffraction pattern, and X-ray photoelectron spectrum of the corresponding samples prepared in the embodiments of the present invention.

[0053] Figure 5 These are the stress-strain curves and toughness modulus diagrams of the thin films prepared according to embodiments of the present invention.

[0054] Figure 6 This is a fracture morphology diagram of the thin film prepared in an embodiment of the present invention.

[0055] Figure 7 This is a graph showing the test results of the film prepared according to the embodiments of the present invention in terms of its resistance to extreme environments.

[0056] Figure 8 This is a graph showing the test results of the electrical insulation properties of the thin film prepared according to an embodiment of the present invention.

[0057] Figure 9 This is a graph showing the test results of the ultraviolet shielding performance of the thin film prepared in the embodiments of the present invention. Detailed Implementation

[0058] The following embodiments are merely some, not all, of the embodiments of the present invention. Therefore, the detailed descriptions of the embodiments provided below are not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0059] In this invention, unless otherwise specified, all equipment and raw materials are commercially available or commonly used in the industry. The methods described in the following embodiments are conventional methods in the art, unless otherwise specified.

[0060] Example 1: Step S1: Preparation of terminal carboxylated PEG: 10 g of PEG (M w Approximately 20,000 mg of 2,2,6,6-tetramethylpiperidine oxide (TEMPO), 100 mg of NaBr, and 10 mL of NaClO solution with an effective chlorine content of 6% were added to 100 mL of deionized water. The pH was adjusted to approximately 11 with NaOH, and the reaction was carried out at room temperature for approximately 30 min. After the reaction, ethanol was added to consume the NaClO, and then the pH was adjusted to <2 with hydrochloric acid. HOOC-PEG-COOH was obtained by extraction with dichloromethane, rotary evaporation, hot ethanol recrystallization, and vacuum drying.

[0061] Step S2: Preparation of pseudo-polyrotaxane (PPR): Dissolve 2 g HOOC-PEG-COOH in 9 mL of water; dissolve 8 g α-CD in 58 mL of water; after mixing the two, let stand at 4°C overnight and freeze dry to obtain white solid PPR.

[0062] Step S3: Preparation of polyrotaxane (PR): 7 g of PPR was activated with 0.25 g of BOP Carter condensing agent and 100 μL of N-ethyldiisopropylamine (DIEPA) in 100 mL of anhydrous N,N-dimethylformamide (DMF) for 10 min, and then 0.173 g of 1-adamantaneamine was added and reacted for 24 h for end-capping. After the reaction, the mixture was centrifuged, washed with DMF / methanol, dissolved in DMSO, reprecipitated in water, and freeze-dried to obtain PR.

[0063] Step S4: Preparation of hydroxypropyl-modified polyrotaxane (HyPR): 0.5 g of PR was dissolved in 50 mL of 1 M NaOH solution. After cooling in an ice bath, 3.83 g of propylene oxide was added dropwise. The reaction was first carried out in an ice bath for 0.5 h, and then the temperature was raised to 25 °C and the reaction was continued for 48 h. After the reaction was completed, the mixture was dialyzed for 4 days, freeze-dried, and purified with dichloromethane / acetone to obtain HyPR. This step can improve the solubility and slip ring sliding ability of polyrotaxane.

[0064] Step S5: Dissolve PVA (molecular weight 14600~18600) in 12 mL DMSO at 75 °C according to the dosage shown in Table 1; add HyPR and CDI to 5 mL DMSO at a mass ratio of 1:1, and stir at 60 °C for 2 h to obtain an activated mixture (activated HyPR); then transfer the activated mixture to the PVA DMSO solution, and continue stirring at 75 °C for about 4 h to obtain a PVA@PR / DMSO solution. In this step, the hydroxypropyl hydroxyl groups on HyPR undergo esterification with the hydroxyl groups on the PVA chain to form covalent grafting sites, resulting in a dynamic network with both flexible PVA segments and slippery polyrotaxane units.

[0065] Step S6: In-situ pyrolysis and surface coating: PPTA fibers with a fineness of 200 denier, 0.6 g KOH, and 1.5 g H2O were added to the PVA@PR / DMSO system obtained in step S5 according to the dosages shown in Table 1. The system was stirred at 25°C for 6 h, and the mixture turned dark red, yielding an ANF / PVA@PR dispersion. During this process, PPTA was deprotonated and dissociated into ANF; PVA@PR simultaneously coated the ANF surface through hydroxyl-amide hydrogen bonds, molecular chain entanglement, and interfacial adsorption.

[0066] Step S7: Protonation precipitation: Add about 4 times the volume of deionized water to the dispersion to reprotonate the ANF obtained by deprotonation and precipitate it from the DMSO system to form a yellowish-white aqueous suspension or wet gel system; continue stirring for about 0.5 h to promote system homogenization.

[0067] Step S8: Film formation: The protonated suspension is vacuum filtered through a porous filter membrane to form a stable gel membrane; it is dried at 75°C for 20 min, and then hot-pressed at 0.5 MPa and 70°C for 30 min to obtain a dense AA@PR composite film.

[0068] Table 1

[0069] Structural characterization and performance testing: (1) Microscopic coating and dispersibility.

[0070] Figure 1 The figures shown are TEM images (a1-a3, a2-e2) and diameter distribution histograms (a3-e3) of the nanofibers ANF (a1-a3), AA@PR-1 (b1-b3), AA@PR-2 (c1-c3), AA@PR-3 (d1-d3), and AA@PR-4 (e1-e3) prepared in the embodiments of the present invention at different magnifications. The specific process is as follows: The dispersion obtained in step S6 was diluted with DMSO to approximately 0.01 mg / mL, added dropwise to a carbon film copper grid, and allowed to dry naturally before TEM observation. The diameters of at least 100 nanofibers were statistically analyzed to obtain TEM images and diameter distribution histograms at different magnifications. The figures show that as the PVA@PR content increased from 0 to approximately 38.08 wt%, the diameter of the nanofibers in the dispersion gradually increased from approximately 8.04 ± 1.91 nm to approximately 19.75 ± 5.25 nm, indicating that PVA@PR formed a uniform coating layer on the ANF surface.

[0071] (2) Chemical structure and interfacial interaction.

[0072] Figure 2 The above are the 1H NMR spectra of the raw materials HyPR, α-CD, and PEG used in the examples. 1 1H NMR (Figure a) and Fourier transform infrared spectrum (FTIR, Figure b). Figure 3 In the figure, a is a comparison of the full-spectrum hydrogen NMR spectra of PVA@PR and PVA, b is a local magnified and integrated plot of PVA@PR in the 4.1~4.7 ppm range, and c is a local magnified and integrated plot of PVA in the same range. Figure 4 The Fourier transform infrared spectrum (FTIR, ad plot), X-ray diffraction pattern (XRD, e plot), and X-ray photoelectron spectrum (XPS, fh plot) of the corresponding samples are shown.

[0073] As can be seen from the figure: FTIR and 1 ¹H NMR confirmed the formation of ester bonds between HyPR and PVA; FTIR of the AA@PR film retained the characteristic peaks of ANF, while PVA@PR-related -CH₂ / -CH absorption peaks appeared; the redshift of the C=O peak and the change in OH / NH vibration indicated an enhanced hydrogen bonding interaction between ANF and PVA@PR. XRD showed that the ANF crystallization peak intensity decreased and broadened after the introduction of PVA@PR, indicating that PVA@PR altered the orderly packing of ANF through interfacial interactions. XPS further confirmed the presence of C, O, N elements and the chemical environment including CO, C=O, and NC=O.

[0074] (3) Mechanical properties.

[0075] Table 2

[0076] Figure 5Table 2 shows the stress-strain curve and toughness modulus diagram of the film prepared in this embodiment, and Table 3 shows the mechanical property test results of the film prepared in this embodiment. From the above results, it can be seen that the mechanical properties of the AA@PR film exhibit a volcano-like change, first increasing and then decreasing with the PVA@PR content. The optimal sample AA@PR 2, with a PVA@PR content of 29.07 wt%, achieved a tensile strength of 414.2 ± 15.8 MPa, a fracture strain of 26.3 ± 0.6%, a toughness of 70.5 ± 1.9 MJ / m³, and a Young's modulus of 4.6 ± 0.4 GPa; compared with pure ANF, the strength, fracture strain, and toughness increased by approximately 2.1 times, 2.3 times, and 5.1 times, respectively.

[0077] (4) Microscopic morphology Figure 6 SEM images of the fracture morphology of the ANF and AA@PR2 films are shown. Images a and c are low-magnification and high-magnification cross-sectional views of the ANF film, respectively, while images b and d are low-magnification and high-magnification cross-sectional views of the AA@PR2 film, respectively. These images illustrate that the excellent toughness of the AA@PR2 film stems from its unique fracture morphology.

[0078] As shown in the figure, both ANF and AA@PR 2 films possess a pearl-like layered structure formed by vacuum-assisted filtration self-assembly, which is the structural basis for their excellent mechanical properties. Compared with pure ANF films, AA@PR 2 films exhibit a denser layered stack with numerous fiber bridges between layers. These bridges effectively inhibit crack initiation and propagation. From a fracture morphology perspective, the pure ANF film has a smooth, flat fracture surface with clear interlayer boundaries, exhibiting typical brittle fracture characteristics, with a large interlayer spacing and no obvious fiber bridges or filler filling. In contrast, the AA@PR 2 film shows a significantly tortuous fracture path, a rough fracture surface, and numerous fibrillated structures and fiber pull-out. This tortuous fracture path effectively extends the crack propagation distance during tensile testing, while the fiber pull-out process consumes a large amount of energy through interfacial friction, thus significantly improving the film's toughness and damage tolerance. The difference in fracture morphology stems from the regulation of interfacial interactions by the PVA@PR network: the polyrotaxane sliding ring in PVA@PR undergoes reversible slip along the PEG axis when subjected to force, and with the dynamic breaking and reconstruction of hydrogen bonds, uniform stress distribution and continuous energy dissipation are achieved, ultimately manifesting as tough fracture characteristics such as crack deflection and fiber pull-out.

[0079] (5) Resistance to extreme environments.

[0080] Figure 7Figures show the test results of the extreme environmental resistance of the ANF film and the AA@PR2 film prepared in this embodiment. Figure a shows a photograph of the AA@PR2 film after immersion in liquid nitrogen and bending; Figure b shows a photograph of the AA@PR2 film before and after being burned by an alcohol lamp flame; Figure c shows the tensile stress-strain curves of the AA@PR2 film after immersion in HCl aqueous solution (pH=3), KOH aqueous solution (pH=11), deionized water, and anhydrous ethanol; Figures d and e show the thermogravimetric and differential thermogravimetric curves of the ANF film and the AA@PR2 film, respectively; Figure f shows the tensile stress-strain curve of the ANF film after immersion in the above media. During testing, the films were cut into strips of 10 mm × 50 mm with a gauge length of 20 mm and stretched at 5 mm / min; the liquid immersion time was 24 h; the thermogravimetric test was conducted under a nitrogen atmosphere with a temperature increase to 800℃ at 10℃ / min.

[0081] As shown in the figure, the AA@PR 2 film maintained its structural integrity after repeated bending in liquid nitrogen (-196°C); no significant deformation occurred after being burned in an alcohol lamp flame at approximately 400°C. Thermogravimetric analysis showed that AA@PR 2 underwent PVA@PR-related thermal degradation at approximately 200°C, and ANF began to lose significant weight at approximately 500°C, with a residual mass of approximately 37.4% at 800°C, indicating that the introduction of PVA@PR did not significantly damage the intrinsic heat resistance properties of the aramid material. After immersion in acid (pH=3), alkali (pH=11), water, and anhydrous ethanol for 24 h, the tensile strength and strain at break of the AA@PR 2 film were all above 90%.

[0082] (6) Electrical insulation performance.

[0083] Figure 8 The figures show the test results of the electrical insulation properties of the thin films. The left figure is a Weibull fitting plot based on the breakdown probability, and the right figure is a statistical graph of the breakdown strength of ANF, AA@PR-1, AA@PR-2, AA@PR-3, and AA@PR-4 films. Each test group included at least five samples, and the breakdown strength was averaged and the standard deviation was given. As can be seen from the figures, the characteristic breakdown strength of the AA@PR-2 film is 59.95 kV / mm, which is lower than pure ANF but significantly higher than commercial Nomex paper (approximately 17 kV / mm). This result demonstrates that the thin film prepared in this invention achieves high strength and toughness while still maintaining the electrical insulation capability required for flexible electronic and electrical insulation applications.

[0084] (7) Ultraviolet shielding and transparency.

[0085] Figure 9Figure 1 shows the UV shielding performance test results of the thin film prepared in this embodiment. Figures a and b are the UV-Vis spectra of the AAPR 2 film and the ANF film, respectively, and figure c shows the UV and visible light transmittance test results of the film. As can be seen from the figure, the transmittance of the AAPR 2 film is less than 0.5% in the 200-400 nm UV band, while the transmittance in the visible light band is as high as 77.5%. This is because the aromatic rings and amide bonds in ANF can absorb UV light through electronic transitions, and the multilayer nanofiber network further enhances UV scattering and absorption; since the diameter of ANF is much smaller than the wavelength of visible light, its scattering of visible light is weak, thus achieving a balance between UV blocking and visible transparency.

[0086] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing an aramid nanofiber composite material based on hydroxypropylated polyrotaxane dynamic topological interlocking, characterized in that, Includes the following steps: (1) Hydroxypropyl-modified polyrotaxane is reacted with a polymer containing active group I and active group II to obtain hydroxypropylated polyrotaxane containing a dynamic topological interlocking structure; wherein active group I is a functional group that can form hydrogen bonds with aramid nanofibers; wherein active group II is a functional group that can form covalent bonds with hydroxypropyl-modified polyrotaxane, or a functional group that can form covalent bonds with hydroxypropyl-modified polyrotaxane activated by N,N'-carbonyldiimidazole; (2) The para-aramid fiber is dissociated in a pyrolysis solution containing the hydroxypropylated polyrotaxane with a dynamic topological interlocking structure obtained in step (1), and the hydroxypropylated polyrotaxane with a dynamic topological interlocking structure is coated on the surface of the aramid nanofiber (ANF) obtained by dissociating the para-aramid fiber.

2. The preparation method according to claim 1, characterized in that, In step (1), the active group I is selected from at least one of hydroxyl, carboxyl, amino, amide, carbamate, ether, ester, carbonyl, sulfonyl, primary amine and nitrogen-containing heterocyclic groups; Preferably, in step (1), the active group II is selected from at least one of hydroxyl, carboxyl, amino, borate, isocyanate, aldehyde, azide, alkynyl, alkenyl and epoxy groups; Preferably, the process of activating the hydroxypropyl-modified polyrotaxane with N,N'-carbonyldiimidazole includes the following steps: heating and stirring the hydroxypropyl-modified polyrotaxane and N,N'-carbonyldiimidazole in a solvent; the heating temperature is 60~70℃; the heating and stirring time is 2~4 h; and the mass ratio of the hydroxypropyl-modified polyrotaxane to N,N'-carbonyldiimidazole is 1:1~3. Preferably, the polymer containing active group I and active group II is selected from at least one of polyvinyl alcohol, polyacrylic acid, polyamide containing active group II and polyvinylpyrrolidone containing active group II, more preferably polyvinyl alcohol and / or polyacrylic acid, and most preferably polyvinyl alcohol.

3. The preparation method according to claim 1, characterized in that, Step (1) includes the following steps: Polyvinyl alcohol and hydroxypropyl-modified polyrotaxane activated by N,N'-carbonyldiimidazole were esterified in a solvent to obtain hydroxypropylated polyrotaxane containing a dynamic topological interlocking structure. Preferably, the mass ratio of the polyvinyl alcohol to the hydroxypropyl-modified polyrotaxane is 20-40:1; Preferably, the temperature of the esterification reaction is 75~85℃; Preferably, the esterification reaction takes 4 to 6 hours.

4. The preparation method according to claim 1, characterized in that, The preparation method of the hydroxypropyl-modified polyrotaxane includes the following steps: S1. A host-guest inclusion-extension reaction is carried out by mixing cyclodextrin with polyethylene glycol with carboxyl groups at both ends, so that the cyclodextrin is encased on the polyethylene glycol molecule with carboxyl groups at both ends to obtain quasi-polyrotaxane; S2. End-capping the polyethylene glycol in the quasi-polyrotaxane with 1-adamantane to obtain polyrotaxane; S3. Modify the polyrotaxane with propylene oxide to obtain hydroxypropyl-modified polyrotaxane; Preferably, the cyclodextrin is selected from at least one of α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, dimethylcyclodextrin and glucose cyclodextrin and their derivatives and modified compounds; Preferably, the mass ratio of the cyclodextrin to the polyethylene glycol with carboxyl groups at both ends is 4~6:1; Preferably, in step S1, the temperature of the host-guest encapsulation reaction is 0~10℃ and the time is 8~24 h.

5. The preparation method according to claim 1, characterized in that, In step (2), the lysis solution also contains KOH, dimethyl sulfoxide and H2O; Preferably, the para-aramid fiber is a short fiber.

6. The preparation method according to claim 1, characterized in that, In step (2), the mass of the hydroxypropylated polyrotaxane containing the dynamic topological interlocking structure is 20% to 40% of its total mass with that of the para-aramid fiber.

7. The preparation method according to claim 1, characterized in that, In step (2), the dissociation temperature is 25~35℃; Preferably, the dissociation time is 6-8 hours.

8. The preparation method according to claim 1, characterized in that, Step (2) also includes a protonation precipitation process and a film formation process; the protonation precipitation process includes adding 4 to 6 times the volume of water to the dissociated system; the film formation process is selected from at least one of vacuum-assisted filtration, hot pressing extended to casting, pressure filtration, spraying, scraping, layer-to-layer assembly and roll-to-roll continuous filtration hot pressing; Preferably, the protonation precipitation process and film formation process are as follows: 4-6 times the volume of water is added to the dissociated system to re-protonate the ANF obtained after deprotonation and precipitate it from the system to form a suspension or wet gel system; stirring is continued to homogenize the system; a gel membrane is obtained by vacuum filtration through a porous filter membrane, dried at 60-70℃ for 20-30 min, and then hot-pressed at 0.5-1 MPa and 60-70℃ for 20-30 min to obtain an aramid nanofiber composite film based on hydroxypropylated polyrotaxane dynamic topological interlocking.

9. The aramid nanofiber composite material based on dynamic topological interlocking of hydroxypropylated polyrotaxane obtained by the preparation method according to any one of claims 1-8.

10. The use of the aramid nanofiber composite material based on hydroxypropylated polyrotaxane dynamic topological interlocking as described in claim 9 in the preparation of flexible electronic insulating base film, transparent ultraviolet protection film, heat-resistant flexible packaging substrate, aerospace lightweight protective intermediate layer, foldable electronic device support material or packaging material, electromagnetic shielding material or electrothermal functional composite material.

Citation Information

Patent Citations

  • Iron ion enhanced aramid nanofiber film and preparation method thereof

    CN116926981A