A spherical nanomicelle, a protein hydrogel enhanced by the same, and a preparation method and application thereof

CN123152127APending Publication Date: 2026-11-24GUANGZHOU INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611664160.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing protein hydrogels have poor mechanical strength, and traditional cross-linking methods are inefficient, cumbersome, and pose biosafety risks, making it difficult to achieve large-scale production.

Method used

Spherical nanomicelles were prepared using polymerization-induced self-assembly technology. The shell ends contain phthalaldehyde functional groups, which can rapidly cross-link with proteins under physiological conditions to form a three-dimensional network structure, simplifying the preparation process and improving efficiency.

Benefits of technology

The preparation process is simple and efficient, and the resulting protein hydrogel has good mechanical strength and biocompatibility, making it suitable for large-scale production, and it also has drug loading and sustained release capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152127A_ABST
    Figure CN123152127A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of protein hydrogel preparation, and particularly relates to a spherical nanomicelle, a protein hydrogel reinforced therefrom, its preparation method, and its applications. This invention obtains a macromolecular chain transfer agent with terminal phthalaldehyde protecting groups through chain transfer polymerization. This agent is then polymerized with nucleating monomers in a selective solvent to induce self-assembly, resulting in spherical nanomicelles with phthalaldehyde functional groups at the shell ends. These micelles are then mixed with proteins in PBS buffer. The phthalaldehyde functional groups at the micelle shell ends undergo a rapid, irreversible click reaction with the primary amine groups of the protein, forming a three-dimensional network hydrogel with micelles as cross-linking nodes. The spherical nanomicelles prepared by this invention are highly efficient and simple to operate. The resulting protein hydrogel exhibits good mechanical strength and biocompatibility, while also possessing drug loading and sustained-release capabilities, showing promising application prospects in the field of drug sustained-release.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of protein hydrogel preparation, and more particularly to a spherical nanomicelle, a protein hydrogel reinforced therefrom, a preparation method thereof, and its applications. Background Technology

[0002] Protein hydrogels are widely considered a class of biomedical materials with great application potential due to their advantages such as good biocompatibility, biodegradability, and low immunogenicity, and have attracted increasing attention in areas such as tissue repair and regeneration, and drug delivery. However, protein hydrogels generally suffer from poor mechanical strength, and their mechanical properties under physiological conditions often fail to meet the requirements of practical applications, which seriously restricts their clinical translation and industrialization.

[0003] Currently, some studies have attempted to utilize polymer micelles as crosslinking nodes to enhance the mechanical properties of protein hydrogels, but existing technologies still have many shortcomings. On the one hand, current micelle preparation involves polymerization followed by assembly. To ensure each micelle has sufficient free volume for chain rearrangement and thermodynamically stable configuration during formation, the assembly process often employs a dilute solution self-assembly strategy with extremely low solid content, resulting in low preparation efficiency, cumbersome steps, and difficulty in large-scale production. On the other hand, the crosslinking reaction between micelles and proteins still relies on traditional chemical crosslinking systems, such as the reversible reaction between aldehydes and amino groups, the coupling reaction between N-hydroxysuccinimide and amino groups, and the addition reaction between double bonds and thiol groups. These systems generally suffer from reversible reaction equilibrium, easy hydrolysis and inactivation of crosslinking agents, and the need for catalysts or initiators, which not only affect crosslinking efficiency and long-term gel stability but also increase system complexity and may introduce biosafety risks. Therefore, developing a method for constructing micelle-enhanced protein hydrogels that is efficient, simple to operate, has mild crosslinking conditions, and produces stable products is a pressing issue in this field. Summary of the Invention

[0004] Based on this, the present invention provides spherical nanomicelles, protein hydrogels reinforced therefrom, their preparation methods, and applications. The spherical nanomicelles are simple to prepare; their shell ends contain phthalaldehyde functional groups, exhibiting high reactivity. When mixed with proteins, they can rapidly crosslink under physiological conditions to form a three-dimensional network structure, thus producing a protein hydrogel. This hydrogel possesses good mechanical strength and biocompatibility, while also exhibiting drug loading and sustained-release capabilities, making it applicable to the field of drug sustained-release.

[0005] To achieve the above objectives, the present invention includes the following technical solutions: In a first aspect, the present invention provides a method for preparing spherical nanomicelles containing phthalaldehyde functional groups, comprising the following steps: S1: A chain transfer agent with a terminal phthalaldehyde protecting group, a hydrophilic monomer, and a first initiator are added to a solvent, stirred until homogeneous and fully dissolved, nitrogen gas is introduced, the mixture is heated to react, and after cooling, it is precipitated in diethyl ether to obtain a macromolecular chain transfer agent with a terminal phthalaldehyde protecting group; wherein the phthalaldehyde protecting group is a closed active acetal structure formed by two active aldehyde groups in the phthalaldehyde functional group; S2: The macromolecular chain transfer agent, nucleating monomer, and second initiator are added to a selective solvent and stirred until fully dissolved. Nitrogen gas is introduced, and the mixture is heated to polymerize. After cooling, excess trifluoroacetic acid is added for deprotection, releasing the active aldehyde groups. The precipitate is then placed in diethyl ether and washed with diethyl ether to obtain spherical nanomicelles with o-phthalaldehyde groups at the ends. The selective solvent is soluble in hydrophilic segments and insoluble in nucleating segments.

[0006] In step S1, the chain transfer agent initiates the polymerization of hydrophilic monomers under the action of an initiator. Uniform chain growth is achieved through a chain transfer reaction, yielding a macromolecular chain transfer agent with phthalaldehyde (OPA) protecting groups at the ends. The initiator decomposes upon heating to generate free radicals, which initiate the polymerization of hydrophilic monomers to form polymer chains with active centers. Subsequently, these polymer chains with active centers undergo a reversible chain transfer reaction with the chain transfer agent containing phthalaldehyde protecting groups at the ends. This allows the active centers to be continuously transferred between polymer chains, resulting in uniform chain growth for each polymer chain. This synthesizes a macromolecular chain transfer agent with controllable molecular weight and uniform chain length, containing phthalaldehyde protecting groups at the ends. The two active aldehyde groups in the phthalaldehyde functional group are linked to the ends of the chain transfer agent in an acetal structure, remaining stable under heating and free radical conditions and not participating in the polymerization reaction. This ensures that the acetal structure is completely preserved at the ends of each macromolecular chain, laying the foundation for subsequent release of active aldehyde groups and functionalization. After the reaction, precipitation with diethyl ether is used to wash away unreacted small molecule impurities, yielding the pure target macromolecular chain transfer agent. Step S2 utilizes polymerization-induced self-assembly technology to prepare spherical nanomicelles with terminal phthalaldehyde functional groups containing active aldehyde groups. The macromolecular chain transfer agent obtained in step S1, along with nucleating monomers and an initiator, is dissolved in a selective solvent to form a homogeneous solution. After heating to initiate polymerization, the nucleating monomers gradually attach to the ends of the macromolecular chain transfer agent to form nucleating segments. As the nucleating segments grow, their solubility in the selective solvent gradually decreases. When a critical value is reached, these block copolymers can no longer dissolve in a monomolecular state and spontaneously aggregate to form spherical nanomicelle structures with nucleating segments as the core and hydrophilic segments as the shell. Polymerization and assembly are completed simultaneously, requiring no external conditions, and a stable micelle dispersion can be directly obtained at high concentrations. After polymerization, trifluoroacetic acid is added. Its acidity cleaves the protecting groups on the OPA, releasing the active aldehyde groups. This deprotection process can be completed at room temperature without destroying the formed micelle structure. Finally, residual small molecule impurities are removed by ether precipitation and washing to obtain pure spherical nanomicelles with terminal active OPA aldehyde groups.

[0007] Existing technologies for preparing micelles typically employ dilute solution self-assembly methods, which suffer from poor preparation efficiency and difficulty in mass production. Furthermore, most related studies primarily focus on controlling micelle morphology, and the resulting micelles still require additional steps to introduce reactive groups when used as hydrogel crosslinking agents, making the process complex. This invention addresses this issue by utilizing the acetal structure at the end of the chain transfer agent in step S1 to ensure the stability of the phthalaldehyde functional group throughout the polymerization process. Step S2 employs polymerization-induced self-assembly technology, simultaneously completing the polymerization of nucleating monomers and in-situ formation of micelles within the same system, eliminating the need for step-by-step operations, significantly simplifying the preparation process and improving efficiency. After polymerization, trifluoroacetic acid is added for deprotection under mild conditions, yielding an active aldehyde group at the end of the micelle shell. This aldehyde group, located at the outermost end of the hydrophilic chain of the micelle with minimal steric hindrance, can subsequently undergo a rapid and irreversible crosslinking reaction with the primary amine groups of proteins under physiological conditions. The entire preparation process requires only conventional heating and stirring, making it simple to operate and simultaneously achieving the preparation of micelles and the introduction of active functional groups. This provides a micelle raw material preparation scheme that is easy to scale up and possesses high crosslinking activity.

[0008] Preferably, the chain transfer agent with a terminal phthalaldehyde protecting group in step S1 has the following structure:

[0009] Furthermore, the hydrophilic monomer in step S1 is selected from one of dimethacrylamide, hydroxyethylacrylamide, polyethylene glycol acrylate, polyethylene glycol methacrylate, and acrylamide. The preferred hydrophilic monomers described above possess good biocompatibility and do not contain primary amine groups. They will not undergo side reactions with the OPA functional groups during free radical polymerization, thus ensuring the stability of the OPA functional groups and OPA protecting groups.

[0010] Furthermore, the nucleating monomer in step S2 is selected from one or more hard monomers such as styrene, methyl methacrylate, ethyl methacrylate, benzyl methacrylate, and benzyl acrylate. The segments formed after polymerization of the above-preferred nucleating monomers are highly hydrophobic, providing sufficient driving force for phase separation in selective solvents to ensure that the block copolymer spontaneously assembles into well-structured micelles. Simultaneously, the above-preferred nucleating monomers do not contain reactive groups that react with OPA functional groups, ensuring the stability of OPA functional groups and OPA protecting groups during polymerization, and maintaining high reactivity of the OPA aldehyde groups at the ends of the micelle shell after deprotection.

[0011] Furthermore, in step S1, the molar ratio of chain transfer agent, hydrophilic monomer, and initiator is 1:(40~70):(0.1~0.4), and the total concentration of the reaction system solution is 20wt%~50wt%. If the total concentration of the reaction system solution is too low, the collision frequency of the reactants is too low, and the reaction rate is too slow; if the total concentration of the reaction system solution is too high, the collision frequency between molecules increases, side reactions increase, and the viscosity of the reaction system increases significantly, making it difficult to effectively dissipate the heat released by the polymerization reaction, causing abnormal local temperature rises, which can easily lead to runaway reaction.

[0012] Furthermore, in step S2, the molar ratio of the macromolecular chain transfer agent, nucleating monomer, and initiator is 1:(80~150):(0.1~0.4), and the solid content of the polymerization system is 15wt%~50wt%. Polymerization-induced self-assembly refers to the in-situ self-assembly of block copolymers to form nanomicelles during the polymerization process. Too low a solid content results in low preparation efficiency and is not conducive to the aggregation of nanoparticles to form high-dimensional micelle structures. Too high a solid content easily leads to excessive particle aggregation and precipitation.

[0013] Preferably, the initiator in steps S1 and S2 is one of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide.

[0014] Preferably, the solvent in steps S1 and S2 is one of methanol, ethanol, and isopropanol.

[0015] Preferably, the amount of trifluoroacetic acid added in step S2 is 300 mol% to 1000 mol% of the molar amount of the macromolecular chain transfer agent. In the deprotection reaction, trifluoroacetic acid participates in the cleavage reaction of the protecting group as a reactant, and also serves as the acidic medium for the reaction. An excess of trifluoroacetic acid ensures the completeness of the deprotection reaction and maintains the acidic environment of the reaction system, preventing side reactions of the deprotected OPA aldehyde group.

[0016] Secondly, the present invention provides a micelle-reinforced protein hydrogel prepared from the above-mentioned spherical nanomicelles. The micelle-reinforced protein hydrogel is prepared from the spherical nanomicelles with phthalaldehyde functional groups at their ends and a protein; the phthalaldehyde functional groups at the ends of the spherical nanomicelle shells react with the primary amine groups of the protein via a click reaction to form a crosslinked network.

[0017] Thirdly, the present invention provides a method for preparing the micelle-reinforced protein hydrogel as described above, comprising the following steps: The protein and the spherical nanomicelles were dispersed evenly in PBS buffer, and air bubbles were removed to obtain two dispersions. The two dispersions were then rapidly injected into a mold, allowed to stand, poured out of the mold, and freeze-dried to obtain a micelle-reinforced protein hydrogel.

[0018] Proteins and spherical nanomicelles with terminal OPA functional groups were separately dispersed in PBS buffer. After mixing the two dispersions, the OPA functional groups, located at the free ends of the hydrophilic shell of the micelles, exhibited good extensibility and accessibility in solution, enabling them to rapidly undergo nucleophilic addition reactions with primary amine groups on the protein molecular chains to form stable amide bonds without any catalyst. Since each spherical nanomicelle contains a large number of OPA functional groups, and the protein molecular chain contains multiple primary amine groups, one micelle can react with multiple protein chains simultaneously, and one protein chain can react with multiple micelles, forming a three-dimensional cross-linked network structure with micelles as cross-linking nodes and proteins as the network backbone, thus achieving rapid formation of protein hydrogels. The entire preparation process was carried out at room temperature, atmospheric pressure, and physiological pH conditions. The mild reaction conditions and pure reaction system are beneficial for maintaining the native conformation and biological function of the proteins, ensuring the biosafety of the product, and making it suitable for large-scale preparation.

[0019] Furthermore, the protein is selected from one or more of silk fibroin, bovine serum albumin, soy protein, casein, and gelatin.

[0020] Furthermore, the mass ratio of the protein to the spherical nanomicelles is 1:(0.1~1.2); the total mass fraction of the protein and spherical nanomicelles in the protein hydrogel is 1wt%~20wt%. An excessively high or low feed ratio of micelles to protein will lead to an excess of a certain functional group in the system, reducing the cross-linking density and resulting in a sparse network structure and insufficient mechanical strength of the hydrogel.

[0021] Fourthly, the present invention provides the application of the micelle-enhanced protein hydrogel in drug sustained release.

[0022] Beneficial Effects: This invention utilizes polymerization-induced self-assembly technology to simultaneously polymerize and self-assemble micelles within the same system. The preparation process requires no step-by-step operations, only conventional heating and stirring, making it simple and efficient. Furthermore, the micelle shells contain phthalaldehyde functional groups at their ends. These functional groups are located at the outermost end of the hydrophilic segments, exhibiting low steric hindrance and high reactivity. Based on these spherical nanomicelles, they can be rapidly cross-linked with proteins in a buffer solution to obtain protein hydrogels. This cross-linking reaction is mild, the resulting cross-links are irreversible, and the resulting protein hydrogel network structure is stable. In addition, this protein hydrogel possesses drug loading and sustained-release capabilities, making it applicable to the field of drug sustained-release. Attached Figure Description

[0023] Figure 1 This is a gel chromatography chromatogram of the polydimethylacrylamide macromolecular chain transfer agent in Example 1.

[0024] Figure 2 The spherical nanomicelles dissolved in Example 11 H NMR spectrum.

[0025] Figure 3 This is a scanning electron microscope image of the spherical nanomicelles in Example 1.

[0026] Figure 4 The swelling rate-time curve of the bovine serum albumin hydrogel prepared in Example 1 is shown.

[0027] Figure 5 The bar chart shows the cytotoxicity analysis of the protein hydrogels prepared in Examples 1-4 and Comparative Example 1.

[0028] Figure 6 The stress-strain curves are shown for the protein hydrogels prepared in Examples 1-4 and Comparative Example 1.

[0029] Figure 7 The bar chart shows the drug loading rate of the protein hydrogels prepared in Examples 1-4.

[0030] Figure 8 The graphs show the cumulative release rate-time curves of the protein hydrogels prepared in Examples 1-4. Detailed Implementation

[0031] This invention provides a method for preparing spherical nanomicelles containing phthalaldehyde functional groups, comprising the following steps: S1: Add the chain transfer agent with a terminal phthalaldehyde protecting group, hydrophilic monomer, and initiator to the solvent, stir until uniform and fully dissolved, purge with nitrogen for 30 min, heat to 65℃ for 4 h to 6 h, cool and precipitate in diethyl ether to obtain a macromolecular chain transfer agent with a terminal phthalaldehyde protecting group. S2: Add macromolecular chain transfer agent, nucleating monomer and initiator to selective solvent and stir until fully dissolved. Purge with nitrogen for 30 min, heat to 65℃ and polymerize for 12 h. After cooling, add excess trifluoroacetic acid and continue the reaction for 1 h to 2 h. The precipitate is placed in diethyl ether and washed 3 times with diethyl ether. After drying, spherical nanomicelles with o-phthalaldehyde functional groups at the ends are obtained.

[0032] The chain transfer agent with a terminal phthalaldehyde protecting group has the following structure:

[0033] The chain transfer agent can be prepared according to the methods reported in existing literature (see: Huang JB, Shi M, Liang H, Lu J. An efficient O-phthalaldehyde-amine coupling reaction for the synthesis of a bottlebrush polymer under physiological conditions. PolymerChemistry, 2022, 13(5):649-654.).

[0034] In step S1, the molar ratio of chain transfer agent, hydrophilic monomer, and initiator is 1:(40~70):(0.1~0.4), and the concentration of the reaction system solution is 20wt%~50wt%. The hydrophilic monomer is selected from one of dimethacrylamide, hydroxyethylacrylamide, polyethylene glycol acrylate, polyethylene glycol methacrylate, and acrylamide. In step S2, the molar ratio of macromolecular chain transfer agent, nucleating monomer, and initiator is 1:(80~150):(0.1~0.4), and the solid content of the polymerization system is 15wt%~50wt%. The nucleating monomer is selected from one or more of hard monomers such as styrene, methyl methacrylate, ethyl methacrylate, benzyl methacrylate, and benzyl acrylate. The initiator in steps S1 and S2 is one of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide, and the solvent is one of methanol, ethanol, and isopropanol; the amount of trifluoroacetic acid added in step S2 is 300mol% to 1000mol% of the molar amount of the macromolecular chain transfer agent.

[0035] The spherical nanomicelle shells obtained by the above preparation method contain phthalaldehyde functional groups at their ends, which can undergo click reactions with the primary amine groups of proteins to form a cross-linked network. Therefore, this invention also provides a method for preparing micelle-reinforced protein hydrogels using the above-mentioned spherical nanomicelles, comprising the following steps: The protein and the spherical nanomicelles were dispersed evenly in PBS buffer (pH=7.4), and air bubbles were removed by negative pressure and nitrogen purging to obtain two dispersions. The two dispersions were then rapidly injected into a mold, allowed to stand at room temperature for 3-6 hours, poured out of the mold, and freeze-dried to obtain a micelle-enhanced protein hydrogel.

[0036] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0037] Unless otherwise specified, all reagents and materials used in the following examples and comparative examples are commercially available.

[0038] Example 1 (1) Preparation of spherical nanomicelles containing phthalaldehyde functional groups S1: 10.0 g of chain transfer agent with phthalaldehyde protecting group at the end, 107.0 g of dimethacrylamide, and 0.58 g of azobisisobutyronitrile were added to 275.0 g of ethanol and stirred until fully dissolved. Nitrogen gas was purged for 30 min, and the mixture was heated to 65 °C for 4 h. After cooling, the mixture was precipitated in diethyl ether to obtain 110.2 g of polydimethacrylamide macromolecular chain transfer agent with phthalaldehyde protecting group at the end.

[0039] The chain transfer agent with a terminal phthalaldehyde protecting group has the following structure:

[0040] S2: Add 20.0g of macromolecular chain transfer agent, 33.0g of styrene, and 0.17g of azobisisobutyronitrile to 124.0g of ethanol and stir until fully dissolved. Purge with nitrogen for 30min, heat to 65℃ and polymerize for 12h. Cool, add 2.0g of trifluoroacetic acid, and continue the reaction for 1h~2h to remove the protecting groups. The precipitate is then placed in diethyl ether and washed 3 times with diethyl ether. After drying, 48.3g of spherical nanomicelles with o-phthalaldehyde functional groups at the ends are obtained.

[0041] The polydimethylacrylamide macromolecular chain transfer agent with terminal phthalaldehyde protecting groups obtained in step S1 of this embodiment was analyzed by 1H NMR spectroscopy, and its actual degree of polymerization was 58, and its molecular weight was 6300. Gel chromatography analysis was performed, and the results are as follows: Figure 1 As shown, its number-average molecular weight was measured to be 4800, which is smaller than the actual molecular weight. This may be because polydimethylacrylamide is highly polar and has a strong adsorption effect on the chromatographic column, resulting in a longer elution time and a smaller molecular weight.

[0042] The spherical nanomicelles with terminal phthalaldehyde functional groups obtained in step S2 of this embodiment were characterized. The dissolved spherical nanomicelles... 1 H NMR spectrum as shown Figure 2 As shown, the signal peak with a chemical shift around 10.5 is attributed to the characteristic hydrogen of the aldehyde group in the phthalaldehyde functional group, and the signal peak with a chemical shift of 6-8 is attributed to the characteristic hydrogen of the benzene ring, indicating that a block copolymer with phthalaldehyde functional groups at the ends has been synthesized. The spherical nanomicelles were observed using scanning electron microscopy (SEM), and the results are as follows... Figure 3 As shown, the micelles exhibit a regular spherical structure with a particle size of approximately 80 nm.

[0043] (2) Micelle-enhanced synthesis of protein hydrogels 1.0 g bovine serum albumin and 1.0 g spherical nanomicelles were dispersed evenly in 20 mL of PBS buffer (pH=7.4). The air bubbles were removed by negative pressure and nitrogen purging to obtain two dispersions. The two dispersions were then rapidly injected into a mold and allowed to stand for 5 h. The mold was then poured out and freeze-dried to obtain bovine serum albumin hydrogel.

[0044] Example 2 This embodiment uses the same spherical nanomicelles as in Example 1. The difference between Example 2 and Example 1 is that in the synthesis step of micelle-enhanced protein hydrogel, bovine serum albumin is replaced with silk fibroin. The remaining steps and conditions are the same as in Example 1, and silk fibroin hydrogel is obtained.

[0045] Example 3 This embodiment uses the same spherical nanomicelles as in Example 1. The difference between Example 3 and Example 1 is that in the synthesis step of micelle-enhanced protein hydrogel, bovine serum albumin is replaced with casein. The remaining steps and conditions are the same as in Example 1, and casein hydrogel is obtained.

[0046] Example 4 This embodiment uses the same spherical nanomicelles as in Example 1. The difference between Example 4 and Example 1 is that in the synthesis step of micelle-enhanced protein hydrogel, bovine serum albumin is replaced with soy protein. The remaining steps and conditions are the same as in Example 1, and soy protein hydrogel is obtained.

[0047] Comparative Example 1 2.0 g bovine serum albumin was dispersed evenly in 20 mL of PBS buffer (pH=7.4), and air bubbles were removed by negative pressure and nitrogen purging. 10 mL of 0.2 mol / L genipin aqueous solution was added, mixed evenly, and then quickly injected into a mold and allowed to stand for 5 h. The mold was then poured out and freeze-dried to obtain genipin crosslinked bovine serum albumin hydrogel.

[0048] Performance testing: 1. Swelling rate test The swelling rate of the bovine serum albumin hydrogel prepared in Example 1 was tested, and the specific steps are as follows: A certain mass of lyophilized protein hydrogel was immersed in PBS buffer (pH=7.4) at 37℃ for a certain period of time, then removed, the surface moisture was wiped off, and the sample was weighed. Swelling rate = (m-m0) / m0, where m is the weight after water absorption and m0 is the mass of the lyophilized sample.

[0049] The swelling rate variation curves of bovine serum albumin hydrogel at different soaking times are shown in the figure below. Figure 4As shown, the bovine serum albumin hydrogel reached swelling equilibrium after soaking in PBS buffer for approximately 20 hours, with an equilibrium swelling ratio of approximately 6%. This indicates that an effective cross-linking reaction occurred between the phthalaldehyde functional groups at the ends of the spherical nanomicelle shells and the primary amine groups of the protein, forming a stable covalently cross-linked network that cannot dissolve in water without detaching from the network structure. Simultaneously, this result demonstrates that the protein hydrogel possesses certain hydrophilicity and suitable water absorption.

[0050] 2. Cytotoxicity analysis The protein hydrogels prepared in Examples 1-4 and Comparative Example 1 were used to evaluate the proliferation activity of L929 cells on the surface of the protein hydrogels using CCK-8 assay. The specific steps are as follows: The protein hydrogel, after being fully swollen in PBS buffer (pH=7.4), was cut into discs with a diameter of 2.5 cm. These discs were sterilized with 75% medical alcohol (v / v), washed three times with PBS buffer, and then sterilized under UV light for 2 hours. The protein hydrogel discs were then fixed into the wells of a 24-well plate using cell fixation loops. L929 cells were then introduced at a rate of 4 x 10⁻⁶ cells / well. 4 Inoculate the protein hydrogel surface at a density of 100 cells / mL and incubate at 37°C with 5% carbon dioxide for 7 days (changing the medium every 2 days). After incubation, wash three times with PBS, add 100 μL of CCK-8 reagent, and continue incubation for 4 hours. Transfer 100 μL of the supernatant to a 96-well plate and measure the absorbance at 450 nm using a microplate reader.

[0051] Figure 5 As for the cytotoxicity test results, the cell survival rate of the four micelle-enhanced protein hydrogels prepared in Examples 1-4 was 98%-105%, which is close to or slightly higher than that of the protein hydrogel prepared in Comparative Example 1, indicating that the micelle-enhanced protein hydrogel of the present invention is non-cytotoxic and has good biocompatibility.

[0052] 3. Mechanical performance evaluation The protein hydrogels prepared in Examples 1-4 and Comparative Example 1 were subjected to dynamic mechanical analysis to assess their compressibility. The specific steps are as follows: Protein hydrogels completely swollen in PBS buffer (pH=7.4) were formed into cylindrical samples with a height of 0.2 cm and a diameter of 0.5 cm. In the compression test, the pressure was increased from 0 to 18 N at a rate of 0.5 N / min, and the maximum compressive strain was set to 80%.

[0053] Genipin is commonly used as a crosslinking site in the preparation of polysaccharide and protein hydrogels. Therefore, the bovine serum albumin hydrogel crosslinked with genipin prepared in Comparative Example 1 is used as a comparison. The stress-strain curves of Examples 1-4 and the protein hydrogel prepared in Comparative Example 1 are shown below. Figure 6As shown, the four protein hydrogels obtained in Examples 1-4 all exhibit significantly better compressibility than the bovine serum albumin hydrogel crosslinked with genipin obtained in Comparative Example 1.

[0054] 4. Drug loading and sustained release The protein hydrogels prepared in Examples 1-4 were subjected to drug loading and sustained-release analysis. The specific steps are as follows: Weigh a certain mass (m) D The lyophilized protein hydrogel was immersed in 5 mg / mL diclofenac sodium PBS buffer for 48 h, then removed, the surface was wiped dry, and lyophilized to obtain the drug-loaded protein hydrogel, which was then weighed (m). L ), calculate the load factor using the following formula: Load factor = (m L -m D ) / m D .

[0055] The protein hydrogel loaded with diclofenac sodium was immersed in 20 mL of PBS buffer solution (pH=7.4) and released by shaking in a shaker at 37 °C. At intervals, 1 mL of the release solution was taken, diluted with the same PBS buffer solution, and the absorbance at 269 nm was measured by UV-Vis spectrophotometer. After each sampling, 1 mL of fresh PBS buffer was added to keep the total volume of the release system constant.

[0056] The loading rates of the four micelle-reinforced protein hydrogels prepared in Examples 1-4 are as follows: Figure 7 As shown, the loading rates ranged from 13% to 16%. The cumulative drug release rate-time curves for the four micelle-reinforced protein hydrogels are shown below. Figure 8 As shown. By Figure 8 It can be seen that bovine serum albumin hydrogel reaches peak drug release at 12 hours, with a cumulative release rate of approximately 73%; silk fibroin hydrogel reaches peak drug release at 11 hours, with a cumulative release rate of approximately 67%; casein hydrogel reaches peak drug release at 9 hours, with a cumulative release rate of approximately 80%; and soybean protein hydrogel reaches peak drug release at 15 hours, with a cumulative release rate of approximately 71%.

[0057] In summary, the spherical nanomicelles prepared by the polymerization-induced self-assembly technology of this invention can rapidly cross-link with proteins under physiological conditions to form a stable three-dimensional network structure. The resulting protein hydrogel is not only simple and efficient to prepare, but also has good compressibility and biosafety, while also having drug loading and sustained-release functions. It has good application prospects in biomedical fields such as tissue repair and drug delivery.

[0058] The above description is merely a preferred embodiment of the present invention and is only used to illustrate the technical solution of the present invention. It is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the technical solution of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the technical solution of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for preparing a spherical nanomicelle containing an o- phthaldehyde functional group, characterized by, Includes the following steps: S1: A chain transfer agent with a terminal phthalaldehyde protecting group, a hydrophilic monomer, and a first initiator are added to a solvent, stirred until homogeneous and fully dissolved, nitrogen gas is introduced, the mixture is heated to react, and after cooling, it is precipitated in diethyl ether to obtain a macromolecular chain transfer agent with a terminal phthalaldehyde protecting group; wherein the phthalaldehyde protecting group is a closed active acetal structure formed by two active aldehyde groups in the phthalaldehyde functional group; S2: The macromolecular chain transfer agent, nucleating monomer, and second initiator are added to a selective solvent and stirred until fully dissolved. Nitrogen gas is introduced, and the mixture is heated to polymerize. After cooling, excess trifluoroacetic acid is added for deprotection, releasing the active aldehyde groups. The precipitate is then placed in diethyl ether and washed with diethyl ether to obtain spherical nanomicelles with o-phthalaldehyde functional groups at the ends. The selective solvent is soluble in hydrophilic segments and insoluble in nucleating segments.

2. The method for preparing a spherical nanomicelle containing an o-phthaldehyde functional group according to claim 1, characterized by, The hydrophilic monomer in step S1 is selected from one of dimethacrylamide, hydroxyethylacrylamide, polyethylene glycol acrylate, polyethylene glycol methacrylate, and acrylamide.

3. The method of claim 1, wherein the preparation of the spherical nanomicelles containing the o-phthaldehyde functional group is characterized by, The nucleating monomer in step S2 is selected from one or more hard monomers such as styrene, methyl methacrylate, ethyl methacrylate, benzyl methacrylate, and benzyl acrylate.

4. The method of claim 1, wherein the preparation of the spherical nanomicelles containing the o-phthaldehyde functional group is characterized by, In step S1, the molar ratio of chain transfer agent, hydrophilic monomer, and initiator is 1:(40~70):(0.1~0.4), and the total concentration of the reaction system solution is 20wt%~50wt%.

5. The method for preparing spherical nanomicelles containing phthalaldehyde functional groups according to claim 1, characterized in that, In step S2, the molar ratio of macromolecular chain transfer agent, nucleating monomer, and initiator is 1:(80~150):(0.1~0.4), and the solid content of the polymerization system is 15wt%~50wt%.

6. A micelle-reinforced protein hydrogel, characterized in that, It is prepared from proteins and spherical nanomicelles obtained by the preparation method according to any one of claims 1 to 5.

7. A method for preparing the micelle-reinforced protein hydrogel as described in claim 6, characterized in that, Includes the following steps: The protein and the spherical nanomicelles were dispersed evenly in PBS buffer, and air bubbles were removed to obtain two dispersions. The two dispersions were then rapidly injected into a mold, allowed to stand, poured out of the mold, and freeze-dried to obtain a micelle-reinforced protein hydrogel.

8. The method for preparing micelle-reinforced protein hydrogel according to claim 7, characterized in that, The protein is selected from one or more of silk fibroin, bovine serum albumin, soy protein, casein, and gelatin.

9. The method for preparing the micelle-reinforced protein hydrogel according to claim 7, characterized in that, The mass ratio of the protein to the spherical nanomicelles is 1:(0.1~1.2); the total mass fraction of the protein and spherical nanomicelles in the protein hydrogel is 1wt%~20wt%.

10. The use of the micelle-reinforced protein hydrogel as described in claim 6 in the preparation of a drug sustained-release carrier.