A quick-charging type graphite negative electrode liquid phase coating material and a preparation method and device thereof
By using a high-solubility, high-boiling-point solvent to dissolve cross-linked asphalt or resin, the process flow is simplified, enabling room-temperature coating of graphite anode materials. This solves the problems of low initial charge-discharge efficiency and poor cycle performance of graphite anode materials in existing technologies, and improves the electrochemical performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202510671101.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies for preparing graphite anode materials for lithium-ion batteries suffer from problems such as low initial charge-discharge efficiency, large irreversible capacity loss, and poor cycle performance, especially due to the peeling and pulverization of the graphite layer structure caused by the formation and rupture of the SEI film.
Crosslinked asphalt or resin is dissolved in a high-solubility, high-boiling-point solvent, and then heated and stirred in a mixing tank to prepare a fast-charging graphite negative electrode liquid-phase coating material. This simplifies the process, enables room-temperature coating, and improves the rate performance and cycle stability of the material.
It improves the initial coulombic efficiency and cycle stability of graphite anode materials, enhances the rate performance of graphite anode materials, reduces SEI film rupture and volume expansion, and improves the electrochemical performance of lithium-ion batteries.
Smart Images

Figure CN123152134A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of negative electrode coating material production, and more specifically, to a fast-charging graphite negative electrode liquid phase coating material, its preparation method, and its preparation apparatus. Background Technology
[0002] Using graphite directly as a negative electrode material in lithium-ion batteries has several drawbacks, mainly in two aspects: First, solvent molecules in the electrolyte undergo a reduction reaction with lithium ions during the first charge-discharge cycle, forming an SEI film, resulting in irreversible capacity loss and low initial coulombic efficiency. Second, after lithium ion deintercalation, the co-intercalation of lithium ions and solvent molecules causes the graphite layer structure to peel off and crumble. Furthermore, with charge-discharge cycles, the rupture and formation of the SEI film repeatedly occur, further increasing the irreversible capacity loss of the graphite electrode and impairing its rate performance and cycle performance. Therefore, graphite materials need to be coated with a layer of amorphous carbon to form a composite material with a "core-shell" structure. This reduces adverse reactions such as lithium plating, isolates the graphite particles from the electrolyte, prevents capacity reduction due to solvent molecule co-intercalation, and restricts and buffers the volume expansion of graphite, increasing cycle stability.
[0003] Chinese patent application CN202411504332.3 discloses a nitrogen-containing resin liquid-phase coated modified artificial graphite, its preparation method, and its application. The preparation method of the modified artificial graphite includes: performing a polycondensation reaction of N-phenylmaleimide, phenolic compounds, aldehyde compounds, and a catalyst to obtain a nitrogen-containing phenolic resin; adding the nitrogen-containing phenolic resin and artificial graphite to a solvent for liquid-phase coating, followed by carbonization treatment, to obtain the nitrogen-containing resin liquid-phase coated modified artificial graphite. This technology can effectively accelerate the transport speed of lithium ions during charging and discharging, while having more lithium intercalation sites and a stable SEI film, ultimately obtaining modified artificial graphite with high rate capability, high capacity, and high first-efficiency. This technology uses an alkenyl silane coupling agent to modify artificial graphite, and uses a nitrogen-containing phenolic resin, solvent, and azo initiator to complete the coating, but it requires multiple filtrations and drying, making the process complex and costly.
[0004] Chinese patent application CN202411588627.3 discloses a liquid-phase coated graphite anode material, its preparation method, and a lithium-ion battery. The preparation method of the liquid-phase coated graphite anode material includes: adding asphalt to an organic solvent and mixing thoroughly to obtain an asphalt solution; adding artificial graphite to the asphalt solution and mixing thoroughly; heating and vacuuming to remove the organic solvent; and then carbonizing to obtain the liquid-phase coated graphite anode material. This technology uses asphalt with a softening point of 150℃, but most of the organic solvents used have boiling points below 100℃. In the preparation process, the solvents need to be ground into fine powder to dissolve below their boiling point, resulting in low efficiency.
[0005] Chinese Patent Application No. CN202411275622.5 discloses a fast-charging phosphorus-doped hard carbon-coated graphite anode material, its preparation method, and its application. The preparation method of the fast-charging graphite anode material includes the following steps: 1) placing microcrystalline graphite powder in a dispersion containing polyacrylonitrile and sonicating it to obtain a mixture; 2) heating and stirring the mixture to obtain polyacrylonitrile-coated microcrystalline graphite powder; 3) mixing the polyacrylonitrile-coated microcrystalline graphite powder with a phytic acid solution and then performing a hydrothermal reaction, followed by filtration and freeze-drying to obtain phosphorus-doped polyacrylonitrile-coated microcrystalline graphite powder; 4) subjecting the phosphorus-doped polyacrylonitrile-coated microcrystalline graphite powder to heat treatment to obtain the fast-charging graphite anode material. This technology uses polyacrylonitrile as a coating agent. Due to its high melting point of 317℃, it needs to be dissolved under an ultrasonic field after mixing with a solvent, which is not easily achieved industrially.
[0006] The paper "Research on the Preparation of Lithium-ion Anode Materials by Asphalt-Coated Artificial Graphite" by Sun Jinghui et al. introduces a liquid-phase coating method for preparing lithium-ion anode materials by coating artificial graphite with asphalt dissolved in CS2. The study analyzes the materials using BET testing, X-ray diffraction, scanning electron microscopy, and electrochemical performance. The results show that this method coats the raw material surface with a uniform layer of asphalt-degraded carbon, significantly improving the electrochemical performance of the coated material: the initial efficiency increases from 64.0% to 91.8%, and the irreversible capacity increases from 175.3 mAh·g⁻¹. -1 Reduced to 30.2 mAh·g -1 This technology uses CS2 to dissolve asphalt, but CS2 is a low-boiling-point solvent, dissolving below its boiling point, so the asphalt must be finely ground.
[0007] Sui Jia proposed a study on "Research on Enhancing the Activity of Electrode Materials by Modifying Graphite Interface with Water-soluble Asphalt," which uses water-soluble asphalt to coat artificial graphite to enhance the electrochemical performance of the material. Water-soluble asphalt was prepared by mixed acid oxidation using medium-temperature asphalt as raw material. The process of coating and modifying artificial graphite with water-soluble asphalt was optimized using response surface methodology, examining factors such as the mass ratio of water-soluble asphalt to graphite, coating time, carbonization isothermal time, and final carbonization temperature. This study uses mixed acid oxidation to prepare water-soluble asphalt, mainly involving steps such as mixed acid oxidation, water washing, filtration, alkali dissolution, filtration, acid addition, centrifugation, washing, and drying. The water-soluble asphalt is dissolved in ammonia water, artificial graphite is slowly added, and after drying, a liquid-phase coated sample is obtained; however, this technique is cumbersome and has little industrial value. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide a fast-charging graphite anode liquid-phase coating material, its preparation method, and its preparation apparatus. This method utilizes a high-solubility, high-boiling-point solvent to dissolve cross-linked asphalt or resin, resulting in good mixing, low solvent consumption, and eliminating the need for complex filtration and drying processes. The process is short, and the prepared liquid-phase coating material can coat graphite anode materials at room temperature, improving the rate performance and cycle stability of the graphite anode material.
[0009] To achieve the above objectives, the present invention adopts the following technical solution:
[0010] The first aspect of this invention provides a method for preparing a fast-charging graphite negative electrode liquid-phase coated material, comprising the following steps:
[0011] S1, one or more blocky solid cross-linked asphalt or resin are fed into the hopper and then sent to the crusher for coarse crushing to a particle size of <2cm, and then sent into the powder silo.
[0012] S2, solid cross-linked asphalt or resin in the powder silo is added to the mixing tank after being measured by the batching and weighing module. High-solubility and high-boiling-point solvents are added to the mixing tank after being measured by the batching and weighing module or flow meter.
[0013] S3, the mixture in the mixing tank is heated by a heater, and nitrogen is introduced through a distributor to heat the mixture to a temperature below the boiling point of a high-solubility, high-boiling-point solvent and then kept at that temperature.
[0014] S4. After stirring the mixture in the mixing tank evenly with a stirrer, turn off the heating, turn off the stirring and stop the nitrogen gas supply. After naturally cooling to below 100°C, open the bottom valve of the mixing tank. After filtering through the filter, obtain the fast-charging graphite negative electrode liquid phase coating material.
[0015] Preferably, in step S1:
[0016] The crosslinked asphalt is a non-graphitized asphalt prepared by a crosslinking reaction using a crosslinking agent and a catalyst; or
[0017] The resin is selected from one or more of coumarone resin, furan resin, thermoplastic phenolic resin, and epoxy resin.
[0018] Preferably, in step S1, the softening point of the solid cross-linked asphalt or resin is 70–125°C.
[0019] Preferably, in step S2:
[0020] The solid crosslinked asphalt or resin comprises 40-60 parts by weight, and the high-solubility, high-boiling-point solvent comprises 40-60 parts by weight; and / or
[0021] The boiling point of the high-solubility, high-boiling-point solvent is 137–250°C, and the high-solubility, high-boiling-point solvent is selected from one or more of xylene, wash oil, N,N-dimethylformamide, ethylene glycol, and dephenolized oil.
[0022] Preferably, in step S3:
[0023] During the heating process, the heating rate is 20–40 °C / h; and / or
[0024] The flow rate of the nitrogen gas is 10-15 m³ / h. 3 / h; and / or
[0025] During the heating process, the temperature below the boiling point of the high-solubility, high-boiling-point solvent is 100–180°C; and / or
[0026] The heat preservation time is 0.5 ± 0.1 h.
[0027] Preferably, in step S4, the stirring time is 1 to 2 hours.
[0028] A second aspect of the present invention provides a method for preparing a fast-charging graphite negative electrode liquid-phase coated material, comprising the following steps:
[0029] (1) A high-solubility, high-boiling-point solvent is added to the mixing tank after being metered by the batching and weighing module or flow meter; then one or more cross-linked asphalt or resin that is liquid at room temperature or high temperature is added to the mixing tank according to the batching and weighing module.
[0030] (2) The mixture in the mixing tank is heated by a heater, and nitrogen is introduced through a distributor to heat the mixture to a temperature below the boiling point of a high-solubility, high-boiling-point solvent and keep it at that temperature.
[0031] (3) After stirring the mixture in the mixing tank evenly with a stirrer, turn off the heating, turn off the stirring and stop the nitrogen gas supply. After naturally cooling to below 100°C, open the bottom valve of the mixing tank and filter it to obtain the fast-charging graphite negative electrode liquid phase coating material.
[0032] Preferably, in step (1):
[0033] The crosslinked asphalt is a non-graphitized asphalt prepared by a crosslinking reaction using a crosslinking agent and a catalyst; or
[0034] The resin is selected from one or more of coumarone resin, furan resin, thermoplastic phenolic resin, and epoxy resin.
[0035] Preferably, in step (1):
[0036] The solid crosslinked asphalt or resin comprises 40-60 parts by weight, and the high-solubility, high-boiling-point solvent comprises 40-60 parts by weight; and / or
[0037] The boiling point of the high-solubility, high-boiling-point solvent is 137–250°C, and the high-solubility, high-boiling-point solvent is selected from one or more of xylene, wash oil, N,N-dimethylformamide, ethylene glycol, and dephenolized oil.
[0038] Preferably, in step (2):
[0039] During the heating process, the heating rate is 20–40 °C / h; and / or
[0040] The flow rate of the nitrogen gas is 10-15 m³ / h. 3 / h; and / or
[0041] During the heating process, the temperature below the boiling point of the high-solubility, high-boiling-point solvent is 100–180°C; and / or
[0042] The heat preservation time is 0.5 ± 0.1 h.
[0043] Preferably, in step (3), the stirring time is 1 to 2 hours.
[0044] The third aspect of the present invention provides a fast-charging graphite negative electrode liquid phase coating material prepared by the preparation method of the fast-charging graphite negative electrode liquid phase coating material according to the first or second aspect of the present invention, wherein the viscosity at room temperature is 300-1000CP, the residual carbon is 15-30%, the ash content is ≤0.15%, and the magnetic element content is ≤0.8μg / g.
[0045] A fourth aspect of the present invention provides an apparatus for preparing a fast-charging graphite negative electrode liquid phase coating material, comprising a mixing tank and a filter;
[0046] The mixing tank is equipped with a stirrer, and below the stirrer is a distributor connected to nitrogen gas; the top of the mixing tank is equipped with a feed inlet, a liquid inlet, and an exhaust outlet, and the inlet pipe of the liquid inlet is equipped with a flow meter; a heater is installed outside the mixing tank; the mixing tank is equipped with a batching and weighing module for weighing the materials in the mixing tank; the bottom discharge port of the mixing tank is equipped with a bottom valve;
[0047] The filter is connected to the bottom discharge port of the mixing tank, and the filter outlet is connected to the holding device.
[0048] Preferably, it also includes a solid phase conveying and crushing module;
[0049] The solid phase conveying and crushing module includes a hopper, a belt conveyor, a crusher, a conveying device, and a powder silo arranged in sequence; the conveying device is a screw conveyor, a tubular chain conveyor, or a bucket elevator; the powder silo is connected to the feed inlet of the mixing tank.
[0050] Preferably, the holding device is a holding bucket, which is equipped with a holding and weighing module.
[0051] The effects of this invention are as follows:
[0052] This invention uses a high-solution, high-boiling-point solvent to dissolve cross-linked asphalt or resin, which can be solid or liquid. When the cross-linked asphalt or resin is a blocky solid, only coarse crushing is required, without fine grinding. It is then mixed with the high-solution, high-boiling-point solvent and heated to below the solvent's boiling point. When the cross-linked asphalt or resin is a liquid, it is directly mixed with the high-solution, high-boiling-point solvent in a liquid-liquid process. This invention achieves good mixing effect, low solvent consumption, high solid content, and high carbon residue. Due to the excellent fluidity of the fast-charging graphite anode liquid-phase coating material, it can achieve uniform coating of graphite materials at room temperature. After carbonization, the fast-charging graphite anode liquid-phase coating material has good compatibility with graphite and is difficult to peel off or pulverize. This invention, by using the fast-charging graphite anode liquid-phase coating material to coat the graphite anode material, can reduce the rupture of the SEI film, inhibit the volume expansion of graphite, and improve the rate performance and cycle stability of the anode material. Attached Figure Description
[0053] Figure 1 This is a schematic flowchart of the preparation method of the fast-charging graphite negative electrode liquid phase coating material of the first aspect of the present invention;
[0054] Figure 2 This is a schematic flowchart of the preparation method of the fast-charging graphite negative electrode liquid phase coating material according to the second aspect of the present invention;
[0055] Among them, 1. Hopper; 2. Belt conveyor; 3. Crusher; 4. Conveying device; 5. Powder silo; 6-1. Batching and weighing module; 6-2. Container weighing module; 7. Mixing tank; 8. Flow meter; 9. Heater; 10. Distributor; 11. Agitator; 12. Bottom valve; 13. Filter; 14. Container. Detailed Implementation
[0056] To better understand the above-mentioned technical solutions of the present invention, the technical solutions of the present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0057] The present invention provides a method for preparing a fast-charging graphite negative electrode liquid phase coating material, which uses a high-solution, high-boiling-point solvent to dissolve cross-linked asphalt or resin. For solid cross-linked asphalt or resin, it is first coarsely crushed, then mixed with solvent and heated to melt the solid at a certain temperature. Nitrogen gas is introduced and mechanical stirring is performed. If the cross-linked asphalt or resin is in a liquid state, it can be directly mixed with the high-solution, high-boiling-point solvent.
[0058] Combination Figure 1 As shown, the first aspect of the present invention describes a method for preparing a fast-charging graphite negative electrode liquid-phase coated material using bulk solid cross-linked pitch or resin as raw material, comprising the following steps:
[0059] S1, one or more blocky solid cross-linked asphalt or resin are fed into hopper 1, then sent to crusher 3 for coarse crushing and then sent to powder silo 5.
[0060] This step involves conveying and crushing solids. One or more blocky solid cross-linked asphalt or resins with a softening point of 70-125℃ are fed into hopper 1. The material in hopper 1 falls evenly onto belt conveyor 2 and is then conveyed by belt conveyor 2 to crusher 3. The material is coarsely crushed by crusher 3 into small particles with a particle size of <2cm, and then conveyed into powder silo 5 by conveying device 4 (screw conveyor, tubular chain conveyor or bucket elevator).
[0061] The cross-linked asphalt used above is a non-graphitized asphalt prepared by cross-linking reaction using a cross-linking agent and catalyst; the resin is selected from one or more of coumarone resin, furan resin, thermoplastic phenolic resin, and epoxy resin. The softening point of the solid cross-linked asphalt or resin is 70–125℃.
[0062] S2, solid cross-linked asphalt or resin in powder silo 5 is added to mixing tank 7 after being measured by batching and weighing module 6-1. High-solubility and high-boiling-point solvents are added to mixing tank 7 after being measured by batching and weighing module 6-1 or flow meter 8.
[0063] This step involves material metering and mixing. The cross-linked asphalt or resin comprises 40–60 parts by weight, and the high-solubility, high-boiling-point solvent comprises 40–60 parts by weight. The high-solubility, high-boiling-point solvent has a boiling point of 137–250°C, and its solubility is reflected in the product's viscosity index; good solubility results in low viscosity and good flowability. This high-solubility, high-boiling-point solvent is selected from one or more of xylene, wash oil, N,N-dimethylformamide, ethylene glycol, and dephenolized oil.
[0064] S3, the mixture in the mixing tank 7 is heated by the heater 9, and nitrogen is introduced through the distributor 10 to heat the mixture to a temperature below the boiling point of the high-solubility, high-boiling-point solvent and keep it at that temperature.
[0065] This step involves heating the mixture. The mixture (solid-liquid) in mixing tank 7 is slowly heated by heater 9 at a rate of 20–40 °C / h. Simultaneously, nitrogen gas is introduced through distributor 10, with the flow rate controlled at 10–15 m³ / h. 3 The mixture is heated to complete melting at a temperature of / h, and then kept at a temperature below the boiling point of the high-solubility, high-boiling-point solvent (100–180℃) for 0.5 ± 0.1 h. Nitrogen gas serves to isolate the combustion-supporting gas to ensure safety, and also acts as a stirrer.
[0066] S4. After the mixture in the mixing tank 7 is stirred evenly by the stirrer 11, the heating is turned off, the stirring is turned off and the nitrogen gas supply is stopped. After natural cooling, the bottom valve 12 of the mixing tank 7 is opened. After filtration by the filter 13, the fast-charging graphite negative electrode liquid phase coating material is obtained.
[0067] In this step, the mixture in the mixing tank 7 is stirred by the stirrer 11 for 1 to 2 hours to ensure uniform mixing. Then, the heating is turned off, the stirring is turned off and the nitrogen gas supply is stopped. After the mixture is naturally cooled to below 100°C, the bottom valve 12 of the mixing tank 7 is opened. The material is filtered through the filter 13 to remove particulate impurities and then loaded into a barrel (measured by the weighing module 6-2) to obtain the fast-charging graphite negative electrode liquid phase coating material.
[0068] The second aspect of the present invention describes a method for preparing a fast-charging graphite negative electrode liquid-phase coated material using liquid cross-linked pitch or resin as a raw material, comprising the following steps:
[0069] (1) A high-solubility, high-boiling-point solvent is added to the mixing tank 7 after being metered by the batching and weighing module 6-1 or the flow meter 8; then one or more cross-linked asphalt or resin that is liquid at room temperature or high temperature is added to the mixing tank 7 after being metered by the batching and weighing module 6-1.
[0070] This step mainly involves material metering and mixing. High-solubility, high-boiling-point solvents are metered using the batching and weighing module 6-1 or the flow meter 8 and then added to the mixing tank 7. Next, one or more cross-linked asphalt or resins that are liquid at room temperature or high temperature are metered using the batching and weighing module 6-1 and added to the mixing tank 7. In this step, the liquid cross-linked asphalt or resin may be a high-temperature liquid. In this case, the room-temperature solvent should be added first, followed by the high-temperature liquid, to avoid solvent evaporation at high temperatures and potential safety accidents.
[0071] The aforementioned crosslinked asphalt is a non-graphitized asphalt prepared by crosslinking with a crosslinking agent and catalyst. The resin is selected from one or more of coumarone resin, furan resin, thermoplastic phenolic resin, and epoxy resin. The liquid crosslinked asphalt or resin comprises 40–60 parts by weight, and the high-solubility, high-boiling-point solvent comprises 40–60 parts by weight; the boiling point of the high-solubility, high-boiling-point solvent is 137–250℃, and the high-solubility, high-boiling-point solvent is selected from one or more of xylene, wash oil, N,N-dimethylformamide, ethylene glycol, and dephenolized oil.
[0072] (2) The mixture in the mixing tank 7 is heated by the heater 9, and nitrogen is introduced through the distributor 10 to heat the mixture to a temperature below the boiling point of the high-solubility, high-boiling-point solvent and keep it at that temperature.
[0073] This step involves heating the mixture. The mixture (liquid-liquid) in mixing tank 7 is slowly heated by heater 9 at a rate of 20–40 °C / h. Simultaneously, nitrogen gas is introduced through distributor 10, with the flow rate controlled at 10–15 m³ / h. 3 The mixture is heated to complete melting at a temperature of / h, and then kept at a temperature below the boiling point of the high-solubility, high-boiling-point solvent (100–180℃) for 0.5 ± 0.1 h. Nitrogen gas serves to isolate the combustion-supporting gas to ensure safety, and also acts as a stirrer.
[0074] (3) After stirring the mixture in the mixing tank 7 evenly with the stirrer 11, turn off the heating, turn off the stirring and stop the nitrogen gas supply. After natural cooling, open the bottom valve 12 of the mixing tank 7 and filter it through the filter 13 to obtain the fast-charging graphite negative electrode liquid phase coating material.
[0075] In this step, the mixture in the mixing tank 7 is stirred by the stirrer 11 for 1 to 2 hours to ensure uniform mixing. Then, the heating is turned off, the stirring is turned off and the nitrogen gas supply is stopped. After the mixture is naturally cooled to below 100°C, the bottom valve 12 of the mixing tank 7 is opened. The material is filtered through the filter 13 to remove particulate impurities and then loaded into a barrel (measured by the weighing module 6-2) to obtain the fast-charging graphite negative electrode liquid phase coating material.
[0076] The fast-charging graphite anode liquid phase coating materials prepared by the above two methods achieve a suitable viscosity, with a viscosity of 300-1000 CP at room temperature. The residual carbon content of the fast-charging graphite anode liquid phase coating material is 15-30%, the ash content is ≤0.15%, and the magnetic element content is ≤0.8μg / g. It can be used as a coating material for graphite anodes of lithium batteries.
[0077] Natural or artificial graphite, after undergoing granulation, demagnetization, shaping, and grading processes, is heated and stirred with the aforementioned fast-charging graphite negative electrode liquid phase coating material to complete the coating. After filtration and heating to remove organic solvents, a precursor is obtained. Then, it is carbonized at a high temperature of 1200–1500°C under a nitrogen atmosphere to obtain resin liquid phase coated modified natural graphite.
[0078] Combination Figure 1 As shown, the preparation apparatus for fast-charging graphite negative electrode liquid phase coating material includes a mixing tank 7 and a filter 13. A stirrer 11 is installed inside the mixing tank 7, and a distributor 10 connected to nitrogen is located below the stirrer 11. The top of the mixing tank 7 has an inlet, a liquid feed port, and an exhaust port. Liquid cross-linked asphalt or resin (or coarsely crushed blocky solid cross-linked asphalt or resin) at room temperature or high temperature is added to the mixing tank 7 through the inlet. A high-solubility, high-boiling-point solvent is added to the mixing tank 7 through the liquid feed port. A flow meter 8 is installed on the inlet pipe of the liquid feed port. A heater 9 is installed outside the mixing tank 7. A weighing module 6-1 for weighing the materials inside the mixing tank 7 is installed on the mixing tank 7. A bottom valve 12 is installed at the bottom discharge port of the mixing tank 7. The filter 13 is connected to the bottom discharge port of the mixing tank 7, and the outlet of the filter 13 is connected to a holding device 14.
[0079] Combination Figure 1 As shown, the preparation device for fast-charging graphite negative electrode liquid phase coating material also includes a solid phase conveying and crushing module; the solid phase conveying and crushing module includes a hopper 1, a belt conveyor 2, a crusher 3, a conveying device 4 and a powder silo 5 arranged in sequence; the conveying device 4 is a screw conveyor, a tubular chain conveyor or a bucket elevator; the powder silo 5 is connected to the feed inlet of the mixing tank 7.
[0080] Combination Figure 1 As shown, the holding device 14 is a holding bucket, which is equipped with a weighing module 6-2.
[0081] Example 1
[0082] The preparation method of the fast-charging graphite negative electrode liquid-phase coated material in this embodiment is as follows:
[0083] (1) Add lumpy solid coumarone resin with a softening point of 71℃ to the hopper. The lumpy solid material in the hopper falls evenly into the belt conveyor. The material falls from the end of the belt conveyor into the crusher, where it is crushed into particles <2cm. It is then sent to the powder silo via a screw conveyor. 60 parts of coumarone resin in the powder silo are weighed according to the batching weighing module and added to the mixing tank. 40 parts of xylene solvent (boiling point of 137℃) are added to the mixing tank through the batching weighing module or a flow meter.
[0084] (2) The solid-liquid mixture in the mixing tank is slowly heated by a heater at a rate of 20°C / h, while nitrogen gas is introduced at a rate of 10m³ through a distributor. 3 Heating to 100℃ in the mixing tank for 0.5 hours, then stirring for 1 hour to ensure uniformity. Afterwards, turning off heating, stirring, and nitrogen, and allowing it to cool naturally to below 90℃, the bottom valve is opened. The material passes through a 200-mesh filter (13) to remove particulate impurities, resulting in a fast-charging graphite anode liquid-phase coating material. This material is then packed into barrels with a weight of 220±1 kg. The fast-charging graphite anode liquid-phase coating material achieves 350 CP, 15% residual carbon, 0.10% ash, and 0.78 μg / g magnetic elements at room temperature, making it suitable for use as a coating material for lithium-ion battery graphite anodes.
[0085] (3) The natural graphite (D) after granulation, demagnetization, shaping and grading 50 =13.75μm) and the above liquid-phase coated asphalt (solid content accounts for 10% of natural graphite) are heated to 80℃ and stirred and mixed. After 1 hour, the coating is completed. After filtration, the organic solvent is removed by heating and vacuuming to obtain the precursor. Then, it is calcined at 1300℃ for 5 hours under nitrogen atmosphere to obtain resin liquid-phase coated modified natural graphite.
[0086] Example 2
[0087] The preparation method of the fast-charging graphite negative electrode liquid-phase coated material in this embodiment is as follows:
[0088] (1) 40 parts of dephenolized oil (boiling point 170℃) were added to the mixing tank after being measured by a flow meter; 60 parts of furan resin, which is liquid at room temperature, were added to the mixing tank by weighing.
[0089] (2) The liquid-liquid mixture in the mixing tank is slowly heated by a heater at a rate of 30°C / h, while nitrogen gas is introduced at a rate of 15m³ through a distributor. 3Heating is carried out at 140℃ in the mixing tank for 0.4 hours. The mixture is then stirred for 1 hour to ensure uniformity. Heating, stirring, and nitrogen gas are then stopped, and the mixture is allowed to cool naturally to below 100℃. The bottom valve is opened, and the material is passed through a 200-mesh filter to remove particulate impurities, yielding a fast-charging graphite anode liquid-phase coating material. This material is then packaged into drums weighing 1000±5 kg. The fast-charging graphite anode liquid-phase coating material achieves 800 CP at room temperature, with 19% residual carbon, 0.08% ash, and 0.70 μg / g magnetic elements, making it suitable for use as a coating material for graphite anodes in lithium-ion batteries.
[0090] (3) Artificial graphite (D) obtained by granulating, demagnetizing, shaping, classifying, and graphitizing petroleum needle coke. 50 =13.47μm) and the above fast-charging graphite negative electrode liquid phase coating material (solid content accounts for 8% of artificial graphite) are heated to 90°C and stirred and mixed. After 2 hours, the coating is completed. After filtration, the organic solvent is removed by heating and vacuuming to obtain the precursor. Then, it is calcined at 1500°C for 3 hours under a nitrogen atmosphere to obtain resin liquid phase coated modified artificial graphite.
[0091] Example 3
[0092] The preparation method of the fast-charging graphite negative electrode liquid-phase coated material in this embodiment is as follows:
[0093] (1) A block of solid thermoplastic phenolic resin with a softening point of 101℃ is fed into a hopper. The solid material in the hopper falls evenly into a belt conveyor. The material falls from the end of the belt conveyor into a crusher, where it is crushed into particles <1cm. The crushed material is then sent to a powder silo via a bucket elevator. 40 parts of thermoplastic phenolic resin in the powder silo are weighed according to the batching and weighing module and added to a mixing tank. 30 parts of N,N-dimethylformamide (DMF, boiling point 153℃) and 30 parts of ethylene glycol (boiling point 197℃) are added to the mixing tank through a flow meter.
[0094] (2) The solid-liquid mixture in the mixing tank is slowly heated by a heater at a rate of 25°C / h, while nitrogen gas is introduced at a rate of 10m³ through a distributor. 3 Heating is carried out at a rate of / h until the material temperature in the mixing tank reaches 145℃, and stabilizing for 0.6h. The agitator is then turned on and stirred for 1.5h to ensure uniformity. Heating, stirring, and nitrogen are then stopped, and the mixture is allowed to cool naturally to below 100℃. The bottom valve is opened, and the material is passed through a 200-mesh filter to remove particulate impurities, yielding a fast-charging graphite anode liquid-phase coating material. The material is then packaged into drums, with a drum weight of 220±1kg. The fast-charging graphite anode liquid-phase coating material achieves 500CP at room temperature, with 17% residual carbon, 0.14% ash, and 0.75μg / g magnetic elements, making it suitable for use as a coating material for graphite anodes in lithium batteries.
[0095] (3) Artificial graphite (D) obtained by granulating, demagnetizing, shaping, classifying, and graphitizing coal-series needle coke. 50 =15.23μm) and the above fast-charging graphite negative electrode liquid phase coating material (solid content accounts for 8% of artificial graphite) are stirred and mixed at room temperature. After 1.5h, the coating is completed. After filtration, the organic solvent is removed by heating and vacuuming to obtain the precursor. Then, it is calcined at 1200℃ for 5h in a nitrogen atmosphere to obtain resin liquid phase coated modified artificial graphite.
[0096] Example 4
[0097] The preparation method of the fast-charging graphite negative electrode liquid-phase coated material in this embodiment is as follows:
[0098] (1) Blocky solid cross-linked asphalt with a softening point of 124℃ is fed into the hopper. The solid material in the hopper falls evenly into the belt conveyor. The material falls from the end of the belt conveyor into the crusher, where it is crushed into particles <1.5cm. It is then sent to the powder silo via a bucket elevator. 50 parts of the cross-linked asphalt in the powder silo are weighed according to the batching and weighing module and added to the mixing tank. 50 parts of wash oil (boiling point of 240℃) are added to the mixing tank after being weighed by a flow meter.
[0099] (2) The solid-liquid mixture in the mixing tank is slowly heated by a heater at a rate of 40°C / h, while nitrogen gas is introduced at a rate of 10m³ through a distributor. 3 Heating is carried out at 180℃ in the mixing tank for 0.5 hours. The agitator is then turned on and stirred for 2 hours to ensure uniformity. Heating, stirring, and nitrogen gas are then stopped, and the mixture is allowed to cool naturally to below 100℃. The bottom valve is opened, and the material is passed through a 200-mesh filter to remove particulate impurities, yielding a fast-charging graphite anode liquid-phase coating material. This material is then packaged into drums weighing 220±1 kg. The fast-charging graphite anode liquid-phase coating material achieves 990 CP, 30% residual carbon, 0.10% ash, and 0.61 μg / g magnetic elements at room temperature, making it suitable for use as a coating material for graphite anodes in lithium batteries.
[0100] (3) Artificial graphite (D) obtained by granulating, demagnetizing, shaping, classifying, and graphitizing pitch coke. 50 =13.45μm) and the above fast-charging graphite negative electrode liquid phase coating material (solid content accounts for 6% of artificial graphite) are heated to 90°C and stirred and mixed. After 1 hour, the coating is completed. After filtration, the organic solvent is removed by heating and vacuuming to obtain the precursor. Then, it is calcined at 1400°C for 4 hours in a nitrogen atmosphere to obtain resin liquid phase coated modified artificial graphite.
[0101] The modified graphite materials prepared in Examples 1-4 were used as negative electrodes. The electrochemical performance of the coin cell was tested. Charge-discharge cycle tests were conducted at 1C / 1C or 3C / 1C rates until the capacity of the lithium-ion battery decayed to 80% of the initial capacity. The number of cycles was recorded, and the results are shown in Table 1 below.
[0102] Table 1 Electrochemical performance of coin cells
[0103]
[0104] As shown in Table 1, after modifying the graphite anode with the fast-charging graphite anode liquid-phase coating materials prepared in Examples 1-4, the initial discharge capacity of the lithium-ion battery is 356.4–360.1 L, the initial coulombic efficiency reaches over 93.5%, and the 1C / 1C cycle count and 3C / 1C cycle count both exceed 1200 cycles. Therefore, the fast-charging graphite anode liquid-phase coating material of this invention can improve the rate performance and cycle stability of the graphite anode material.
[0105] Those skilled in the art should recognize that the above embodiments are merely illustrative of the present invention and are not intended to limit the present invention. Any variations or modifications to the above embodiments that are within the spirit and essence of the present invention will fall within the scope of the claims of the present invention.
Claims
1. A preparation method of a fast-charging type graphite negative electrode liquid phase coating material, characterized by, Includes the following steps: S1, one or more blocky solid cross-linked asphalt or resin are put into the hopper, and then conveyed by the belt conveyor to the crusher for coarse crushing to a particle size of <2cm before being sent into the powder silo. S2, solid cross-linked asphalt or resin in the powder silo is added to the mixing tank after being measured by the batching and weighing module. High-solubility and high-boiling-point solvents are added to the mixing tank after being measured by the batching and weighing module or flow meter. S3, the mixture in the mixing tank is heated by a heater, and nitrogen is introduced through a distributor to heat the mixture to a temperature below the boiling point of a high-solubility, high-boiling-point solvent and then kept at that temperature. S4. After stirring the mixture in the mixing tank evenly with a stirrer, turn off the heating, turn off the stirring and stop the nitrogen gas supply. After naturally cooling to below 100°C, open the bottom valve of the mixing tank. After filtering through the filter, obtain the fast-charging graphite negative electrode liquid phase coating material.
2. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 1, characterized in that, In step S1: The crosslinked asphalt is a non-graphitized asphalt prepared by a crosslinking reaction using a crosslinking agent and a catalyst; or The resin is selected from one or more of coumarone resin, furan resin, thermoplastic phenolic resin, and epoxy resin.
3. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 1, characterized in that, In step S1, the softening point of the solid cross-linked asphalt or resin is 70–125°C.
4. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 1, characterized in that, In step S2: The crosslinked asphalt or resin comprises 40-60 parts by weight, and the high-solubility, high-boiling-point solvent comprises 40-60 parts by weight; and / or The boiling point of the high-solubility, high-boiling-point solvent is 137–250°C, and the high-solubility, high-boiling-point solvent is selected from one or more of xylene, wash oil, N,N-dimethylformamide, ethylene glycol, and dephenolized oil.
5. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 1, characterized in that, In step S3: During the heating process, the heating rate is 20–40 °C / h; and / or The flow rate of the nitrogen gas is 10 to 15 m 3 / h; and / or During the heating process, the temperature below the boiling point of the high-solubility, high-boiling-point solvent is 100–180°C; and / or The heat preservation time is 0.5 ± 0.1 h.
6. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 1, characterized in that: In step S4, the stirring time is 1 to 2 hours.
7. A method for preparing a fast-charging graphite negative electrode liquid-phase coated material, characterized in that, Includes the following steps: (1) A high-solubility, high-boiling-point solvent is added to the mixing tank after being metered by the batching and weighing module or flow meter; then one or more cross-linked asphalt or resin that is liquid at room temperature or high temperature is added to the mixing tank after being metered by the batching and weighing module. (2) The mixture in the mixing tank is heated by a heater, and nitrogen is introduced through a distributor to heat the mixture to a temperature below the boiling point of a high-solubility, high-boiling-point solvent and keep it at that temperature. (3) After stirring the mixture in the mixing tank evenly with a stirrer, turn off the heating, turn off the stirring and stop the nitrogen gas supply. After naturally cooling to below 100°C, open the bottom valve of the mixing tank and filter it to obtain the fast-charging graphite negative electrode liquid phase coating material.
8. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 7, characterized in that: In step (1): The crosslinked asphalt is a non-graphitized asphalt prepared by a crosslinking reaction using a crosslinking agent and a catalyst; or The resin is selected from one or more of coumarone resin, furan resin, thermoplastic phenolic resin, and epoxy resin.
9. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 7, characterized in that: In step (1): The liquid crosslinked asphalt or resin comprises 40-60 parts by weight, and the high-solubility, high-boiling-point solvent comprises 40-60 parts by weight; and / or The boiling point of the high-solubility, high-boiling-point solvent is 137–250°C, and the high-solubility, high-boiling-point solvent is selected from one or more of xylene, wash oil, N,N-dimethylformamide, ethylene glycol, and dephenolized oil.
10. The preparation method of the fast-charging graphite negative electrode liquid-phase coating material according to claim 7, characterized in that: In step (2): During the heating process, the heating rate is 20–40 °C / h; and / or The flow rate of the nitrogen gas is 10 to 15 m 3 / h; and / or During the heating process, the temperature below the boiling point of the high-solubility, high-boiling-point solvent is 100–180°C; and / or The heat preservation time is 0.5 ± 0.1 h.
11. The preparation method of the fast-charging graphite negative electrode liquid-phase coated material according to claim 7, characterized in that: In step (3), the stirring time is 1 to 2 hours.
12. A fast-charging graphite anode liquid-phase coated material prepared by the preparation method according to any one of claims 1 to 11, characterized in that: Its viscosity at room temperature is 300–1000 CP, carbon residue is 15–30%, ash content is ≤0.15%, and magnetic elements are ≤0.8 μg / g.
13. A preparation apparatus for a fast-charging graphite negative electrode liquid-phase coating material, characterized in that: Includes mixing tank and filter; The mixing tank is equipped with a stirrer, and below the stirrer is a distributor connected to nitrogen gas; the top of the mixing tank is equipped with a feed inlet, a liquid inlet, and an exhaust outlet, and the inlet pipe of the liquid inlet is equipped with a flow meter; a heater is installed outside the mixing tank; the mixing tank is equipped with a batching and weighing module for weighing the materials in the mixing tank; the bottom discharge port of the mixing tank is equipped with a bottom valve; The filter is connected to the bottom discharge port of the mixing tank, and the filter outlet is connected to the holding device.
14. The apparatus for preparing fast-charging graphite negative electrode liquid-phase coated material according to claim 13, characterized in that: It also includes a solid phase conveying and crushing module; The solid phase conveying and crushing module includes a hopper, a belt conveyor, a crusher, a conveying device, and a powder silo arranged in sequence; the conveying device is a screw conveyor, a tubular chain conveyor, or a bucket elevator; the powder silo is connected to the feed inlet of the mixing tank.
15. The apparatus for preparing fast-charging graphite negative electrode liquid-phase coated material according to claim 13, characterized in that: The holding device is a holding bucket, which is equipped with a holding and weighing module.
Citation Information
Patent Citations
A fast-charging phosphorus-doped hard carbon-coated graphite negative electrode material and its preparation method and application
CN119069678B
Nitrogen-containing resin liquid phase coated modified artificial graphite as well as preparation method and application thereof
CN119480958A
Liquid-phase coated graphite negative electrode material, preparation method thereof and lithium ion battery
CN119480968A