Carbon fiber surface modified epoxy resin composite material, and preparation method and application thereof
By constructing a PEI/PA composite coating on the carbon fiber surface through a layer-by-layer self-assembly technology, the problem of simultaneously achieving flame retardancy and interfacial reinforcement properties in carbon fiber epoxy resin composites has been solved, resulting in a significant improvement in flame retardancy and mechanical properties with low addition levels.
Patent Information
- Application Number
- CN202611324794.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing carbon fiber epoxy resin composites struggle to balance flame retardancy and interfacial reinforcement properties. Traditional flame retardant modification methods may lead to increased resin viscosity, decreased processing performance, and adverse effects on mechanical properties.
A PEI/PA composite coating is constructed on the surface of carbon fiber using a layer-by-layer self-assembly technology. By alternately depositing polyethyleneimine and phytic acid, a multi-layer coating is formed, which is combined with an epoxy resin curing agent to form a tight interface. The flame retardant components are concentrated in the fiber/resin interface area to form a dense carbon layer to block heat transfer and flame spread.
The addition of low amounts significantly improves the flame retardant properties and interfacial bonding ability of composite materials, avoiding the problems of increased viscosity and uneven dispersion caused by the addition of large amounts of flame retardants in traditional methods, and achieving effective improvement of flame retardant properties and synergistic improvement of mechanical properties.
Smart Images

Figure CN123152135A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flame retardant modification technology of carbon fiber epoxy resin composite materials, specifically relating to a carbon fiber surface-modified epoxy resin composite material, its preparation method, and its application. Background Technology
[0002] Carbon fiber reinforced epoxy composites (CFRPs) possess excellent properties such as high specific strength, high specific modulus, low density, fatigue resistance, and corrosion resistance, making them promising for applications in aerospace, rail transportation, new energy equipment, shipbuilding, and high-end construction. However, epoxy resin matrices are flammable polymers that easily undergo thermal decomposition during combustion, releasing large amounts of flammable volatile products. They also exhibit high heat release rates and smoke emissions, limiting the application of CFRPs in applications requiring high flame retardancy. Furthermore, carbon fibers are prone to oxidative damage in high-temperature and aerobic environments, further affecting the high-temperature stability and fire safety performance of the composite material. Compared to ordinary epoxy resin materials, CFRPs also exhibit a certain "wick effect" during combustion. Due to their continuous fiber structure and high thermal conductivity, under thermal action, the melting or pyrolysis products generated by the epoxy resin may migrate along the carbon fibers and their interface regions, thereby promoting the transfer of heat and flammable volatiles and accelerating flame propagation along the fiber direction. Therefore, suppressing the "wick effect" of carbon fibers and reducing the transfer of heat and combustible pyrolysis products is crucial for improving the flame-retardant properties of CFRP. Currently, flame-retardant modification of CFRP mainly includes adding flame retardants to the epoxy resin matrix, reactive flame-retardant modification of the epoxy resin, and surface flame-retardant modification of the carbon fibers. While directly adding flame retardants to the epoxy resin matrix is simple, high amounts can lead to increased resin viscosity, decreased processing performance, and uneven dispersion of the flame retardant, potentially negatively impacting the mechanical properties of the composite material. Reactive flame-retardant modification can introduce flame-retardant structures into the resin molecular chain, but its preparation process is relatively complex and limited by the resin system and reaction conditions. Therefore, functionalizing the carbon fiber surface to impart flame-retardant functionality while reinforcing the interfacial bonding between the fiber and epoxy resin is a promising modification method.
[0003] Layer-by-layer (LBL) self-assembly is a surface modification method that uses electrostatic interactions, hydrogen bonds, and other intermolecular forces to alternately deposit different functional components on a substrate surface to construct a multilayer composite film. This method can form a continuous functional coating on carbon fiber surfaces, and the coating structure and thickness can be controlled by adjusting the number of assembled layers, component concentration, and assembly conditions. Compared with traditional blend-based flame retardant methods, LBL technology can directly introduce flame-retardant functional components into the carbon fiber surface, forming a relatively continuous protective layer with lower amounts of flame-retardant components. It also features simple processing, wide applicability, and flexible component design.
[0004] However, existing flame-retardant coatings for carbon fiber surfaces still suffer from the challenge of simultaneously achieving both flame-retardant properties and interfacial reinforcement. Some flame-retardant coatings exhibit weak bonding with the carbon fiber and epoxy resin matrix, easily leading to interfacial defects and affecting load transfer. Furthermore, coating thickness and component ratios significantly impact resin wetting and interfacial bonding; excessively thin coatings fail to form an effective flame-retardant barrier, while excessively thick coatings may create weak interfaces and cause stress concentration, thereby reducing the mechanical properties of the composite material. Therefore, it is necessary to develop a method to form a stable and uniform composite coating on the carbon fiber surface, enabling it to simultaneously possess flame-retardant and interfacial reinforcement properties, thus achieving a synergistic improvement in the flame-retardant and mechanical properties of CFRP. Summary of the Invention
[0005] The purpose of this invention is to provide a carbon fiber surface-modified epoxy resin composite material, its preparation method and application, in order to solve the technical problems of poor flame retardancy and high addition amount of carbon fiber epoxy resin composite materials in the prior art.
[0006] To achieve the above objectives, the present invention employs the following technical solution: This invention discloses a method for preparing carbon fiber surface-modified epoxy resin composite material, comprising the following steps: S1: PEI / PA-NBL@CF was prepared by a layer-by-layer self-assembly method; S2: Weigh the epoxy resin, heat and stir until uniform, add the curing agent, stir evenly and apply it to PEI / PA-NBL@CF, and after curing, obtain the carbon fiber surface modified epoxy resin composite material.
[0007] Furthermore, in S1, the specific steps for preparing PEI / PA-NBL@CF are as follows: Polyethyleneimine was dissolved in water to obtain a cationic PEI solution; Phytic acid is dissolved in water to obtain an anionic PA solution; Carbon fiber cloth is alternately immersed in cationic PEI solution and anionic PA solution. Each immersion in cationic PEI solution and anionic PA solution constitutes one cycle. Each cycle forms a coating, resulting in PEI / PA-NBL@CF.
[0008] Furthermore, the cationic PEI solution contains 0.1-2 wt% polyethyleneimine and has a pH of 9; the anionic PA solution contains 0.5-5 wt% phytic acid and has a pH of 4.
[0009] Furthermore, the number of coating layers is 1 to 5.
[0010] Further, in S2, the epoxy resin is heated and stirred in a water bath until uniform, then the curing agent H256 is added, and the mixture is heated in a water bath to make it flow. It is then evenly coated onto PEI / PA-NBL@CF, and then placed into a mold preheated to 90 ℃. The mold is then cured using a three-stage heating process to obtain the carbon fiber epoxy resin composite material.
[0011] Furthermore, the mass ratio of the epoxy resin to the curing agent H256 is 100:(25~40).
[0012] Furthermore, the process parameters for the three-stage temperature-curing process are as follows: After holding at 80-100℃ under normal pressure for 1-3 hours, pressurize to 3-8 MPa, then raise the temperature to 110-130℃ and hold for 1-3 hours. In the third stage, maintain the temperature at 140-160℃ for 2-5 hours.
[0013] The present invention also discloses a carbon fiber surface-modified epoxy resin composite material, which is prepared by the above preparation method.
[0014] Furthermore, the maximum heat release rate of the composite material is 675.68 kW / m³. 2 The total heat release is 40.11 MJ / m³. 2 .
[0015] This invention also discloses a carbon fiber surface-modified epoxy resin composite material that improves the interfacial bonding between carbon fiber and epoxy resin matrix, while simultaneously endowing the composite material with excellent flame retardant properties and thermal stability. The resulting composite material can be used as a lightweight flame-retardant structural material in aerospace equipment, new energy vehicle battery structural components, rail transit vehicle parts, wind turbine blade reinforcement materials, and other composite material fields with high requirements for flame retardant safety performance.
[0016] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a method for preparing carbon fiber surface-modified epoxy resin composite materials. This method first constructs a PEI / PA composite coating on the carbon fiber surface using a layer-by-layer self-assembly technique, rather than directly mixing flame retardants into the epoxy resin matrix. This allows PEI and PA to adhere tightly to the fiber surface in a multi-layered, alternating stacked structure. During combustion, this coating acts as an in-situ barrier layer, providing physical insulation and inhibiting the diffusion of combustible volatiles. Furthermore, because the flame-retardant components are concentrated in the fiber / resin interface region rather than uniformly dispersed throughout the matrix, significant flame-retardant effects can be achieved with relatively low addition amounts, avoiding the problems associated with traditional methods where large amounts of flame retardants are required. Adding excessive amounts of PEI / PA resin leads to problems such as increased resin viscosity, decreased processing performance, and uneven dispersion. Subsequently, epoxy resin containing curing agent is directly applied to the surface of the coated carbon fiber cloth and cured. This ensures that the resin matrix is in close contact with the PEI / PA coating on the fiber surface during the curing process, thus ensuring the formation of a continuous and stable interface transition zone between the coating and the resin matrix. When the composite material is heated and burned, the PEI / PA coating located at the fiber / resin interface can quickly respond to form a dense char layer, effectively blocking the transfer of heat along the fiber direction and the spread of flame. The method of this invention effectively improves flame retardant performance while reducing the amount of flame retardant components added. Attached Figure Description
[0017] Figure 1 The infrared spectrum of the carbon fiber surface-modified epoxy resin composite material of the present invention is shown below. Figure 2 The XPS analysis spectrum of the carbon fiber surface-modified epoxy resin composite material of the present invention is shown below. Figure 3 These are SEM images of the carbon fiber surface-modified epoxy resin composite material and untreated carbon fiber of the present invention. Wherein: a-untreated carbon fiber; b-carbon fiber surface-modified epoxy resin composite material; Figure 4 This is an impact test image of the carbon fiber surface-modified epoxy resin composite material of the present invention. Where: a - Maximum heat release rate (PHRR) graph; b - Maximum total heat release (THR) graph; Figure 5 The image shows the test results of the flame retardant properties of carbon fiber surface-modified epoxy resin composite material. Figure 6 This is a flowchart of the preparation method of the carbon fiber surface modified epoxy resin composite material of the present invention. Detailed Implementation
[0018] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.
[0019] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.
[0020] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values (including integers and fractions) within those ranges.
[0021] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”
[0022] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0023] This invention provides a method for preparing carbon fiber surface-modified epoxy resin composite materials, such as... Figure 6 As shown, it includes the following steps: S1: PEI / PA-NBL@CF was prepared by layer-by-layer self-assembly technology.
[0024] S2: Weigh out epoxy resin, disperse it evenly, add curing agent, stir evenly, apply it to the surface of PEI / PA-NBL@CF carbon fiber, and then cure to obtain PEI / PA-NBL@CF / EP composite material.
[0025] Preferably, S1 specifically includes: S101: Dissolve polyethyleneimine (PEI) in water to obtain a cationic PEI solution; S102: Dissolve phytic acid (PA) in water to obtain anionic PA solution; S103: Alternately immerse the carbon fiber cloth in cationic PEI solution and anionic PA solution, with each cycle corresponding to a bilayer polyelectrolyte.
[0026] More preferably, in S101, the mass fraction of polyethyleneimine in solution A is 0.5 wt%, and the pH value is 9; the mass fraction of phytic acid in S102 is 2 wt%, and the pH value is 4.
[0027] More preferably, in S103, the number of coating layers is 1, 2, 3, 4, or 5.
[0028] In some embodiments, a layer-by-layer self-assembly technique is employed, specifically including: S101: Dissolve the measured amount of PEI in 500 ml of water to obtain solution A; Preferably, the mass fraction of polyethyleneimine is 0.2 wt%.
[0029] S102: Dissolve the measured amount of PA in 500 ml of water to obtain solution B; Preferably, the phytic acid mass fraction is 2 wt%.
[0030] S103: Carbon fiber cloth is alternately immersed in cationic PEI and anionic PA, with each cycle corresponding to a bilayer polyelectrolyte.
[0031] Preferably, S2 specifically includes: S201: Weigh an appropriate amount of epoxy resin, heat it in a water bath and stir until uniform, add curing agent H256, heat it in a water bath to make it flowable, and apply it evenly to a 10 cm × 10 cm carbon fiber cloth. S202: The coated carbon fiber cloth is placed into a mold that has been preheated to 90 ℃, and the mold is cured in a three-stage heating process to obtain a carbon fiber epoxy resin composite material.
[0032] In some embodiments, the process of uniformly dispersing epoxy resin E-51, adding a curing agent, coating it onto carbon fiber cloth, and then curing it to obtain a carbon fiber epoxy resin composite material specifically includes the following steps: S201: Weigh a certain amount of epoxy resin, stir it in a water bath at 60 ℃ for 2 h, then add curing agent H256, and then heat it in a water bath to make it flowable and evenly coat it on a 10 cm × 10 cm carbon fiber cloth. Preferably, the mass ratio of resin to curing agent is 100:32.
[0033] S202: The coated carbon cloth is placed into a mold preheated to 90 ℃, and the mold is placed in a hot press for three-stage heating and curing to obtain carbon fiber epoxy resin composite material.
[0034] Preferably, in S201, the mass ratio of the epoxy resin system to the curing agent H256 is 100:32.
[0035] Preferably, in S202, the three-stage heating and curing process involves holding the product at 90°C under normal pressure for 2 hours, then pressurizing it to 5MPa, heating it to 120°C and holding it for 2 hours, and finally maintaining the temperature at 150°C for 3 hours in the third stage.
[0036] In some embodiments, the carbon fibers are cleaned until no sizing agent remains on the carbon fiber surface before coating the carbon fiber cloth.
[0037] Specifically, through the PN synergistic effect, the two components generate a denser char layer with higher thermal stability. This char layer acts as a physical barrier, inhibiting heat transfer between the combustion zone and the fibers, and suppressing the diffusion of volatile pyrolysis products. PEI provides a nitrogen source and releases non-combustible gases such as NH3 and N2 during decomposition, diluting the concentration of combustible gases and oxygen. PA releases free radicals upon heating, quenching active free radicals in the combustion reaction and terminating the chain reaction.
[0038] In some embodiments, a method for constructing a composite coating on a carbon fiber surface and its flame-retardant reinforcement of an epoxy resin composite material includes the following steps: Step 1: Since carbon fibers undergo sizing before leaving the factory, and sizing agents usually affect fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove sizing agents and other impurities. The specific operation is as follows: Arrange 6 carbon fiber sheets in a Soxhlet extractor containing acetone, reflux extract for 48 h, and vacuum dry at 80 ℃ for 24 h; Step 2: Fabrication of PEI / PA-NBL@CF using layer-by-layer self-assembly First, 2.5 g of PEI was dissolved in 500 mL of water to obtain a cationic PEI solution (pH 9, mass fraction 0.5 wt%). Second, 14.28 g of PA was dissolved in 500 mL of water to obtain an anionic PA solution (pH 4, mass fraction 2 wt%). Then, the carbon fibers were immersed in the cationic PEI solution for 30 min, washed, dried, and then immersed in the anionic PA solution for 30 min, washed, and dried. Each cycle corresponded to one bilayer polyelectrolyte (BL), followed by immersion for 10 minutes each time, then rinsing with deionized water and drying in an oven at 80 ℃. Finally, the assembled carbon fibers were vacuum dried at 80 ℃ for 12 h to obtain PEI / PA-NBL@CF (abbreviated as CF-Ln), where n is the number of assembled layers.
[0039] Step 3: Preparation of PEI / PA-NBL@CF / EP composite material Epoxy resin (E-51) was weighed and stirred in a water bath at 60 ℃ for 2 h. Then, curing agent H256 was added, ensuring a resin-to-curing agent mass ratio of 100:32. The mixture was then heated in a water bath to allow it to flow and evenly coated onto a 10cm × 10cm carbon fiber cloth. The sample was then placed in a mold preheated to 90 ℃ and placed in a hot press. The composite material preparation process adopted a three-stage heating process: first, it was held at 90 ℃ under normal pressure for 2 h, then pressurized to 5 MPa, then heated to 120 ℃ and held for 2 h; finally, the temperature was maintained at 150 ℃ for 3 h. After the mold cooled to room temperature, the composite material was demolded. The resulting composite material was PEI / PA-NBL@CF / EP. The obtained samples were cut to appropriate sizes according to testing requirements for testing.
[0040] The layer-by-layer self-assembly technology offers a relatively simple process and a fast reaction rate. By controlling the number of coatings, suitable conditions for industrial production can be selected. Polyethyleneimine and phytic acid form an interfacial bridge between epoxy resin and carbon fiber, thereby promoting the improvement of interfacial properties and overall material properties, synergistically enhancing the flame retardant and mechanical properties of CFRP.
[0041] This invention discloses a method for constructing a carbon fiber surface composite coating and its flame-retardant reinforcement of epoxy resin composites. The method utilizes a layer-by-layer self-assembly technique to prepare PEI / PA-NBL@CF, a relatively simple and fast process. The flame-retardant effect of the PEI / PA-NBL@CF / EP composite is mainly attributed to the synergistic flame retardancy of phosphorus and nitrogen. During combustion, PA generates acidic species such as phosphoric acid and polyphosphoric acid upon heating, which catalyzes the dehydration and cross-linking of EP pyrolysis products, promoting the formation of a continuous and dense char layer. Simultaneously, the nitrogen-containing structure in PEI further inhibits the combustion reaction through condensed phase and gas-phase flame retardancy, thus forming a PN synergistic flame-retardant effect. The char layer induced by PEI / PA effectively inhibits oxygen and heat diffusion, reducing the escape of combustible volatiles, thereby significantly reducing the heat release rate and combustion intensity of the composite. Furthermore, the N2 and NH3 generated during combustion help dilute oxygen and flammable gases on the surface of the composite, and PA releases free radicals upon heating to quench active free radicals in the combustion reaction and terminate the chain reaction.
[0042] The present invention also discloses a carbon fiber surface-modified epoxy resin composite material prepared by the above preparation method.
[0043] This application focuses on the flame-retardant modification of carbon fiber epoxy resin composites, using a layer-by-layer self-assembly synthesis of PEI / PA-NBL@CF. Simultaneously, SEM, FTIR, XPS, and cone calorimetry were employed to investigate the surface microstructure and surface chemical properties of PEI / PA-NBL@CF. The effect of PEI / PA-NBL@CF addition on the flame-retardant properties of the carbon fiber epoxy resin composite was systematically studied.
[0044] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0045] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.
[0046] Example 1 A method for preparing a carbon fiber surface-modified epoxy resin composite material includes the following steps: Step 1: Since carbon fibers undergo sizing before leaving the factory, and sizing agents usually affect fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove sizing agents and other impurities. The specific operation is as follows: Arrange 6 carbon fiber sheets in a Soxhlet extractor containing acetone, reflux extract for 48 h, and vacuum dry at 80 ℃ for 24 h; Step 2: Fabrication of PEI / PA-NBL@CF using layer-by-layer self-assembly First, 2.5 g of PEI was dissolved in 500 mL of water to obtain a cationic PEI solution (pH 9, mass fraction 0.5 wt%). Second, 14.28 g of PA was dissolved in 500 mL of water to obtain an anionic PA solution (pH 4, mass fraction 2 wt%). Then, the carbon fibers were immersed in the cationic PEI solution for 30 min, washed, dried, and then immersed in the anionic PA solution for 30 min, washed, and dried. Each cycle corresponded to one bilayer polyelectrolyte (BL), followed by immersion for 10 minutes each time, then rinsing with deionized water and drying in an oven at 80 ℃. Finally, the assembled carbon fibers were vacuum dried at 80 ℃ for 12 h to obtain PEI / PA-NBL@CF (abbreviated as CF-L1), where 1 represents the number of assembled layers.
[0047] Step 3: Preparation of PEI / PA-NBL@CF / EP composite material Epoxy resin (E-51) was weighed and stirred in a water bath at 60 ℃ for 2 h. Then, curing agent H256 was added, ensuring a resin-to-curing agent mass ratio of 100:32. The mixture was then heated in a water bath to allow it to flow and evenly coated onto a 10cm × 10cm carbon fiber cloth. The sample was then placed in a mold preheated to 90 ℃ and placed in a hot press. The composite material preparation process adopted a three-stage heating process: first, it was held at 90 ℃ under normal pressure for 2 h, then pressurized to 5 MPa, then heated to 120 ℃ and held for 2 h; finally, the temperature was maintained at 150 ℃ for 3 h. After the mold cooled to room temperature, it was demolded. The resulting composite material was CF-L1 / EP composite material (carbon fiber surface modified epoxy resin composite material). The obtained samples were cut to appropriate sizes according to the testing requirements for testing.
[0048] Example 2 A method for preparing a carbon fiber surface-modified epoxy resin composite material includes the following steps: Step 1: Since carbon fibers undergo sizing before leaving the factory, and sizing agents usually affect fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove sizing agents and other impurities. The specific operation is as follows: Arrange 6 carbon fiber sheets in a Soxhlet extractor containing acetone, reflux extract for 48 h, and vacuum dry at 80 ℃ for 24 h; Step 2: Fabrication of PEI / PA-NBL@CF using layer-by-layer self-assembly First, 2.5 g of PEI was dissolved in 500 mL of water to obtain a cationic PEI solution (pH 9, mass fraction 0.5 wt%). Second, 14.28 g of PA was dissolved in 500 mL of water to obtain an anionic PA solution (pH 4, mass fraction 2 wt%). Then, the carbon fibers were immersed in the cationic PEI solution for 30 min, washed, dried, and then immersed in the anionic PA solution for 30 min, washed, and dried. Each cycle corresponded to one bilayer polyelectrolyte (BL), followed by immersion for 10 minutes each time, then rinsing with deionized water and drying in an oven at 80 ℃. Finally, the assembled carbon fibers were vacuum dried at 80 ℃ for 12 h to obtain PEI / PA-NBL@CF (abbreviated as CF-L2), where 2 represents the number of assembled layers.
[0049] Step 3: Preparation of PEI / PA-NBL@CF / EP composite material Epoxy resin (E-51) was weighed and stirred in a water bath at 60 ℃ for 2 h. Then, curing agent H256 was added, ensuring a resin-to-curing agent mass ratio of 100:32. The mixture was then heated in a water bath to allow it to flow and evenly spread onto a 10cm × 10cm carbon fiber cloth. The sample was then placed in a mold preheated to 90 ℃ and placed in a hot press. The composite material preparation process adopted a three-stage heating process: first, it was held at 90 ℃ under normal pressure for 2 h, then pressurized to 5 MPa, then heated to 120 ℃ and held for 2 h; finally, the temperature was maintained at 150 ℃ for 3 h. After the mold cooled to room temperature, it was demolded. The resulting composite material was CF-L2 / EP composite material (carbon fiber surface modified epoxy resin composite material). The obtained samples were cut to appropriate sizes according to the testing requirements for testing.
[0050] Example 3 A method for preparing a carbon fiber surface-modified epoxy resin composite material includes the following steps: Step 1: Since carbon fibers undergo sizing before leaving the factory, and sizing agents usually affect fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove sizing agents and other impurities. The specific operation is as follows: Arrange 6 carbon fiber sheets in a Soxhlet extractor containing acetone, reflux extract for 48 h, and vacuum dry at 80 ℃ for 24 h; Step 2: Fabrication of PEI / PA-NBL@CF using layer-by-layer self-assembly First, 2.5 g of PEI was dissolved in 500 mL of water to obtain a cationic PEI solution (pH 9, mass fraction 0.5 wt%). Second, 14.28 g of PA was dissolved in 500 mL of water to obtain an anionic PA solution (pH 4, mass fraction 2 wt%). Then, the carbon fibers were immersed in the cationic PEI solution for 30 min, washed, dried, and then immersed in the anionic PA solution for 30 min, washed, and dried. Each cycle corresponded to one bilayer polyelectrolyte (BL), followed by immersion for 10 minutes each time, then rinsing with deionized water and drying in an oven at 80 ℃. Finally, the assembled carbon fibers were vacuum dried at 80 ℃ for 12 h to obtain PEI / PA-NBL@CF (abbreviated as CF-L3), where 3 represents the number of assembled layers.
[0051] Step 3: Preparation of PEI / PA-NBL@CF / EP composite material Epoxy resin (E-51) was weighed and stirred in a water bath at 60 ℃ for 2 h. Then, curing agent H256 was added, ensuring a resin-to-curing agent mass ratio of 100:32. The mixture was then heated in a water bath to allow it to flow and evenly coated onto a 10cm × 10cm carbon fiber cloth. The sample was then placed in a mold preheated to 90 ℃ and placed in a hot press. The composite material preparation process adopted a three-stage heating process: first, it was held at 90 ℃ under normal pressure for 2 h, then pressurized to 5 MPa, then heated to 120 ℃ and held for 2 h; finally, the temperature was maintained at 150 ℃ for 3 h. After the mold cooled to room temperature, it was demolded. The resulting composite material was CF-L3 / EP composite material (carbon fiber surface modified epoxy resin composite material). The obtained samples were cut to appropriate sizes according to testing requirements for testing.
[0052] Example 4 A method for preparing a carbon fiber surface-modified epoxy resin composite material includes the following steps: Step 1: Since carbon fibers undergo sizing before leaving the factory, and sizing agents usually affect fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove sizing agents and other impurities. The specific operation is as follows: Arrange 6 carbon fiber sheets in a Soxhlet extractor containing acetone, reflux extract for 48 h, and vacuum dry at 80 ℃ for 24 h; Step 2: Fabrication of PEI / PA-NBL@CF using layer-by-layer self-assembly First, 2.5 g of PEI was dissolved in 500 mL of water to obtain a cationic PEI solution (pH 9, mass fraction 0.5 wt%). Second, 14.28 g of PA was dissolved in 500 mL of water to obtain an anionic PA solution (pH 4, mass fraction 2 wt%). Then, the carbon fibers were immersed in the cationic PEI solution for 30 min, washed, dried, and then immersed in the anionic PA solution for 30 min, washed, and dried. Each cycle corresponded to one bilayer polyelectrolyte (BL), followed by immersion for 10 minutes each time, then rinsing with deionized water and drying in an oven at 80 ℃. Finally, the assembled carbon fibers were vacuum dried at 80 ℃ for 12 h to obtain PEI / PA-NBL@CF (abbreviated as CF-L4), where 4 represents the number of assembled layers.
[0053] Step 3: Preparation of PEI / PA-NBL@CF / EP composite material Epoxy resin (E-51) was weighed and stirred in a water bath at 60 ℃ for 2 h. Then, curing agent H256 was added, ensuring a resin-to-curing agent mass ratio of 100:32. The mixture was then heated in a water bath to allow it to flow and evenly coated onto a 10cm × 10cm carbon fiber cloth. The sample was then placed in a mold preheated to 90 ℃ and placed in a hot press. The composite material preparation process adopted a three-stage heating process: first, it was held at 90 ℃ under normal pressure for 2 h, then pressurized to 5 MPa, then heated to 120 ℃ and held for 2 h; finally, the temperature was maintained at 150 ℃ for 3 h. After the mold cooled to room temperature, the composite material was demolded. The resulting composite material was CF-L4 / EP composite material (carbon fiber surface modified epoxy resin composite material). The obtained samples were cut to appropriate sizes according to the testing requirements for testing.
[0054] Example 5 A method for preparing a carbon fiber surface-modified epoxy resin composite material includes the following steps: Step 1: Since carbon fibers undergo sizing before leaving the factory, and sizing agents usually affect fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove sizing agents and other impurities. The specific operation is as follows: Arrange 6 carbon fiber sheets in a Soxhlet extractor containing acetone, reflux extract for 48 h, and vacuum dry at 80 ℃ for 24 h; Step 2: Fabrication of PEI / PA-NBL@CF using layer-by-layer self-assembly First, 2.5 g of PEI was dissolved in 500 mL of water to obtain a cationic PEI solution (pH 9, mass fraction 0.5 wt%). Second, 14.28 g of PA was dissolved in 500 mL of water to obtain an anionic PA solution (pH 4, mass fraction 2 wt%). Then, the carbon fibers were immersed in the cationic PEI solution for 30 min, washed, dried, and then immersed in the anionic PA solution for 30 min, washed, and dried. Each cycle corresponded to one bilayer polyelectrolyte (BL), followed by immersion for 10 minutes each time, then rinsing with deionized water and drying in an oven at 80 ℃. Finally, the assembled carbon fibers were vacuum dried at 80 ℃ for 12 h to obtain PEI / PA-NBL@CF (abbreviated as CF-L5), where 5 represents the number of assembled layers.
[0055] Step 3: Preparation of PEI / PA-NBL@CF / EP composite material Epoxy resin (E-51) was weighed and stirred in a water bath at 60 ℃ for 2 h. Then, curing agent H256 was added, ensuring a resin-to-curing agent mass ratio of 100:32. The mixture was then heated in a water bath to allow it to flow and evenly coated onto a 10cm × 10cm carbon fiber cloth. The sample was then placed in a mold preheated to 90 ℃ and placed in a hot press. The composite material preparation process adopted a three-stage heating process: 1) holding at 90 ℃ under normal pressure for 2 h, then pressurizing to 5 MPa, then heating to 120 ℃ and holding for 2 h; 2) maintaining the temperature at 150 ℃ for 3 h. After the mold cooled to room temperature, the composite material was demolded. The resulting composite material was CF-L5 / EP composite material (carbon fiber surface modified epoxy resin composite material). The obtained sample was cut to an appropriate size according to the testing requirements for testing.
[0056] To characterize the morphological features, Fourier transform infrared spectroscopy (FTIR) was performed on the target product. Figure 1 The image shows the infrared spectrum of PEI / PA-NBL@CF. Characteristic absorption peaks for PEI and PA are present at 3400 cm⁻¹. - ¹ NH stretching vibration peak, 880 cm⁻¹ -1 NH bending vibration, 1000 cm -1 The POC stretching vibration peak and the 1250 cm peak. - The stretching vibration at P=O at point ¹ preliminarily proves that the PEI / PA composite coating was successfully loaded onto the carbon fiber surface.
[0057] Figure 2This is a schematic diagram of the carbon fiber before scanning. The surface of the untreated carbon fiber is relatively rough, with clearly visible grooves. After PEI / PA coating, as shown in 2(b), the grooves on the carbon fiber surface are effectively filled, and a uniform, dense, and smooth coating gradually forms as the coating thickens.
[0058] Figure 3 The image shows XPS spectra. Further characterization of the coating formation is needed.
[0059] Figure 4 The image shows an impact test result, which indicates that the impact strength is improved after the PEI / PA coating is applied.
[0060] Figure 5 For flame retardant performance testing. (a) shows the maximum heat release rate (PHRR) graph; (b) shows the maximum total heat release (THR) graph. It can be observed from the graphs that the carbon fiber epoxy composite material without any added flame retardant has the highest maximum heat release rate (PHRR) and maximum total heat release (THR).
[0061] Table 1 further illustrates the results of the cone calorimetry test, clearly showing that the heat release and total heat release of the composite material are reduced after the PEI / PA coating. This indicates that the coating can effectively improve the flame retardant properties of the composite material.
[0062] Table 1. Cone calorimetry test results of composite materials
[0063] In summary, this invention improves the flame retardant properties of carbon fiber epoxy composites by obtaining coated carbon fibers through a layer-by-layer self-assembly technique. These coated carbon fibers are then combined with epoxy resin to form a carbon fiber epoxy resin composite. The changes in morphology, thermal stability, and flame retardant properties with different numbers of layers were investigated. Polyethyleneimine and phytic acid form interfacial bridges between the carbon fibers and epoxy resin, enhancing the mechanical and flame retardant properties of the carbon fiber epoxy resin composite.
[0064] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.
Claims
1. A method for preparing a carbon fiber surface-modified epoxy resin composite material, characterized in that, Includes the following steps: S1: PEI / PA-NBL@CF was prepared by a layer-by-layer self-assembly method; S2: Weigh the epoxy resin, heat and stir until uniform, add the curing agent, stir evenly and apply it to PEI / PA-NBL@CF, and after curing, obtain the carbon fiber surface modified epoxy resin composite material.
2. The method for preparing a carbon fiber surface-modified epoxy resin composite material according to claim 1, characterized in that, In S1, the specific steps for preparing PEI / PA-NBL@CF are as follows: Polyethyleneimine was dissolved in water to obtain a cationic PEI solution; Phytic acid is dissolved in water to obtain an anionic PA solution; Carbon fiber cloth is alternately immersed in cationic PEI solution and anionic PA solution. Each immersion in cationic PEI solution and anionic PA solution constitutes one cycle. Each cycle forms a coating, resulting in PEI / PA-NBL@CF.
3. The method for preparing a carbon fiber surface-modified epoxy resin composite material according to claim 2, characterized in that, The cationic PEI solution contains 0.1-2 wt% polyethyleneimine and has a pH of 9; the anionic PA solution contains 0.5-5 wt% phytic acid and has a pH of 4.
4. The method for preparing a carbon fiber surface-modified epoxy resin composite material according to claim 2, characterized in that, The number of coating layers is 1 to 5.
5. The method for preparing a carbon fiber surface-modified epoxy resin composite material according to claim 1, characterized in that, In S2, epoxy resin is heated and stirred in a water bath until uniform, then curing agent H256 is added, and the mixture is heated in a water bath to make it flow. It is then evenly coated onto PEI / PA-NBL@CF, and then placed into a mold preheated to 90 ℃. The mold is then cured using a three-stage heating process to obtain carbon fiber epoxy resin composite material.
6. The method for preparing a carbon fiber surface-modified epoxy resin composite material according to claim 5, characterized in that, The mass ratio of the epoxy resin to the curing agent H256 is 100:(25~40).
7. The method for preparing a carbon fiber surface-modified epoxy resin composite material according to claim 5, characterized in that, The process parameters for the three-stage temperature-curing process are as follows: After holding at 80-100℃ under normal pressure for 1-3 hours, pressurize to 3-8 MPa, then raise the temperature to 110-130℃ and hold for 1-3 hours. In the third stage, maintain the temperature at 140-160℃ for 2-5 hours.
8. A carbon fiber surface-modified epoxy resin composite material, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 7.
9. The carbon fiber surface-modified epoxy resin composite material according to claim 8, characterized in that, The maximum heat release rate of the composite material is 676.68 kW / m³. 2 The total heat release is 40.11 MJ / m³. 2 .
10. The application of the carbon fiber surface-modified epoxy resin composite material as described in claim 8 or 9 in the preparation of lightweight flame-retardant structural materials, aerospace equipment, new energy vehicle battery structural components, rail transit vehicle components, or wind turbine blade reinforcement materials.