一种复合绝缘子内嵌光纤与芯棒的界面增强方法

By plasma treatment and grafting polyglycidyl methacrylate onto the surface of the optical fiber sheath, the problem of insufficient interfacial bonding density in optical fiber composite insulators was solved, achieving stable chemical bonding between the optical fiber and the core rod, and improving the stability and insulation performance of the insulator during long-term service.

CN123152136APending Publication Date: 2026-11-24CHINA ELECTRIC POWER RES INST WUHAN BRANCH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611026645.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In fiber-optic composite insulators, the bonding density between the optical fiber and the core rod is insufficient, resulting in poor long-term service stability. They are easily affected by factors such as moisture infiltration, ultraviolet radiation, thermal cycling, and electrothermal coupling, leading to interface aging and performance degradation, and increasing the risk of partial discharge and flashover.

Method used

By introducing oxygen-containing polar functional groups through plasma treatment of the optical fiber sheath surface, and grafting poly(glycidyl methacrylate) to form a graft layer with epoxy groups in the side chain, a stable interface is formed with the core rod resin matrix through a chemical bonding reaction, thereby enhancing the bonding between the optical fiber and the core rod.

Benefits of technology

It significantly improves the interfacial shear strength between the fiber sheath and the core rod, enhances the tightness of the interfacial bonding and long-term service stability, reduces water diffusion leakage current, and strengthens insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152136A_ABST
    Figure CN123152136A_ABST
Patent Text Reader

Abstract

This invention provides a method for enhancing the interface between embedded optical fiber and core rod in composite insulators. By plasma treatment of the optical fiber sheath, polar functional groups are introduced into the sheath interface and micro-etched, significantly improving surface activity while enhancing the surface roughness of the sheath, providing highly active reaction sites for subsequent chemical grafting. GMA free radical polymerization is initiated by an initiator, allowing it to be firmly grafted onto the optical fiber sheath surface via chemical bonds. The epoxy groups in the GMA molecules further undergo ring-opening copolymerization with the core rod resin matrix, forming a stable covalent bond network between the optical fiber sheath and the resin matrix, greatly improving the interfacial shear strength. The treated optical fiber assembly is then embedded into the core rod resin matrix and cured by heating to form an optical fiber insulating core. This effectively solves the problems of insufficient interfacial compactness and poor long-term service stability in existing technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of transmission line and substation equipment technology, and more specifically, to an interface enhancement method for embedded optical fiber and core rod in composite insulators. Background Technology

[0002] Insulators are fundamental components of the external insulation system in power systems, directly affecting the long-term stable operation of transmission lines and substation equipment. Among various insulator types, post composite insulators are rapidly replacing ceramic insulators due to their advantages such as lightweight design, ease of maintenance, and excellent resistance to pollution flashover. Fiber optic composite insulators further integrate the dual functions of "high-voltage insulation + signal transmission," making them crucial equipment in new power systems that combines insulation and monitoring capabilities. However, the interface between the fiber optic sheath and the core rod is a multi-material coupling region, susceptible to the combined effects of moisture infiltration, ultraviolet radiation, thermal cycling, strong electric fields, and electrothermal coupling during service, leading to interface aging and performance degradation. Once the interface bonding layer degrades, it can cause an increase in micropore defects, weakened intermolecular interactions, softening or loss of adhesion of the bonding layer, resulting in distorted electric field distribution near the interface, inducing local electric field concentration, and significantly increasing the risk of partial discharge, interface flashover, and even insulator failure.

[0003] Therefore, modifying the fiber interface to form a dense and stable bond between the fiber sheath and core rod is an effective way to improve the insulation level and service reliability of fiber-optic composite insulators. Currently, domestic research on fiber-optic composite insulators mainly focuses on overall insulation performance evaluation and macroscopic structural design, with relatively insufficient methods, processes, and evaluation indicators for treating the fiber sheath-core rod interface, and a lack of related technological reserves. Therefore, conducting research on fiber-optic composite insulator interface modification technology is of great significance for breaking through the current domestic research bottlenecks and promoting engineering applications. Summary of the Invention

[0004] In view of this, the present invention proposes an interface enhancement method for embedded optical fiber and core rod in composite insulator, aiming to solve the problems of insufficient interfacial compactness and poor long-term service stability of existing composite insulators.

[0005] This invention proposes a method for enhancing the interface between embedded optical fiber and core rod in a composite insulator, comprising: The surface of the fiber sheath in the fiber optic assembly is subjected to plasma treatment to activate the surface of the fiber sheath and introduce oxygen-containing polar functional groups; wherein, the fiber optic assembly includes an optical fiber and an optical fiber sheath covering the outer periphery of the optical fiber. Polyglycerol methacrylate is grafted onto the surface of the optical fiber sheath after plasma treatment to form a polyglycerol methacrylate graft layer with epoxy groups in the side chain. The grafted optical fiber assembly is embedded in the resin matrix of the core rod. After curing, the epoxy groups in the poly(glycidyl methacrylate) grafted layer undergo a ring-opening addition reaction with the resin matrix of the core rod, thereby constructing a chemical bonding interface between the optical fiber sheath and the core rod.

[0006] Furthermore, in the above-mentioned method for enhancing the interface between embedded optical fiber and core rod in composite insulator, the oxygen-containing polar functional groups include hydroxyl, carbonyl and / or carboxyl groups.

[0007] Furthermore, in the above-mentioned method for enhancing the interface between embedded optical fiber and core rod in composite insulator, before plasma treatment of the optical fiber sheath surface, the optical fiber assembly is ultrasonically cleaned in an organic solvent to remove contaminants from the surface of the optical fiber sheath, and then dried to remove solvent residue.

[0008] Furthermore, in the above-mentioned method for enhancing the interface between embedded optical fiber and core rod in composite insulator, the plasma treatment power is 40~80W and the time is 60~180s.

[0009] Furthermore, in the above-mentioned method for enhancing the interface between the embedded optical fiber and the core rod in the composite insulator, the step of grafting polyglycidyl methacrylate is carried out under nitrogen protection, including: Benzoyl peroxide wet powder was added to anhydrous ethanol and stirred to dissolve, thus obtaining an initiator solution; Add glycidyl methacrylate to the initiator solution to a volume fraction of 5-30%, stir until homogeneous, and obtain the grafting reaction solution; The plasma-treated optical fiber assembly is immersed in the grafting reaction solution, stirred at 60-80°C for 40-80 minutes, then removed and dried to obtain an optical fiber assembly with a poly(glycidyl methacrylate) grafted layer on its surface.

[0010] Furthermore, in the above-mentioned method for enhancing the interface between the embedded optical fiber and the core rod in a composite insulator, the step of constructing the chemical bonding interface includes: An epoxy resin, an anhydride curing agent, and a phenol accelerator are mixed, wherein the molar ratio of the epoxy resin to the anhydride curing agent is (4~6):(3~5), and the phenol accelerator accounts for 1~3% of the total mass of the epoxy resin. Add 1-3% of polymer hollow microspheres, which account for the total mass of the core rod resin matrix, stir evenly, and heat in a vacuum environment at 80-85℃ for a period of time to pre-cur the core to obtain a pre-cured core. The grafted optical fiber assembly is fixed in the mold and the two ends of the optical fiber in the optical fiber assembly extend to the outside of the mold. The pre-cured core is filled into the mold and then heated at 100~110°C for a period of time to obtain the insulating core with implanted optical fiber.

[0011] Furthermore, in the above-mentioned method for enhancing the interface between the embedded optical fiber and the core rod in the composite insulator, the molar ratio of the epoxy resin to the anhydride curing agent is 5:4.

[0012] Furthermore, in the above-mentioned method for enhancing the interface between the embedded optical fiber and the core rod in the composite insulator, the anhydride curing agent is methyl hexahydrophthalic anhydride.

[0013] Furthermore, in the above-mentioned method for enhancing the interface between the embedded optical fiber and the core rod in the composite insulator, the phenol promoter is 2,4,6-tris(dimethylaminomethyl)phenol.

[0014] Furthermore, in the above-mentioned method for enhancing the interface between embedded optical fiber and core rod in composite insulator, the polymer hollow microspheres are polyethyl methacrylate polymer hollow microspheres.

[0015] The present invention provides a method for enhancing the interface between embedded optical fiber and core rod in composite insulators. This method involves plasma treatment of the optical fiber sheath of the optical fiber assembly, introducing polar functional groups and performing micro-etching at the sheath interface. This significantly improves surface activity while enhancing the surface roughness of the sheath, providing highly active reaction sites for subsequent chemical grafting. GMA free radical polymerization is initiated by an initiator, allowing it to be firmly grafted onto the optical fiber sheath surface via chemical bonds. The epoxy groups in the GMA molecules further undergo ring-opening copolymerization with the core rod resin matrix, forming a stable covalent bond network between the optical fiber sheath and the core rod resin matrix, greatly improving the interfacial shear strength. The treated optical fiber assembly is then embedded into the core rod resin matrix and cured by heating to form an optical fiber composite insulating core. This method effectively solves the problems of insufficient interfacial compactness and poor long-term service stability in existing technologies. Attached Figure Description

[0016] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 This is a schematic flowchart of the interface enhancement method for embedded optical fiber and core rod in composite insulator provided in an embodiment of the present invention. Figure 2 The diagram shows the shear strength test results of the interface between the embedded optical fiber and the core rod in the embodiments and comparative examples of the present invention. Figure 3 The diagram shows the breakdown voltage test results of the interface between the embedded optical fiber and the core rod in the embodiments and comparative examples of the present invention. Figure 4The diagram shows the leakage current test results at the interface between the embedded optical fiber and the core rod in the embodiments and comparative examples of the present invention. Detailed Implementation

[0017] Exemplary embodiments of the present invention will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the invention to those skilled in the art. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0018] See Figure 1 The interface enhancement method between the embedded optical fiber and the core rod in the composite insulator according to embodiments of the present invention includes: Step S1: Plasma treatment is performed on the surface of the fiber sheath in the fiber optic assembly to activate the surface of the fiber sheath and introduce oxygen-containing polar functional groups; wherein, the fiber optic assembly includes an optical fiber and an optical fiber sheath covering the periphery of the optical fiber.

[0019] Specifically, the use of ether ester-type thermoplastic elastomers (such as Hytrel) as the material for the optical fiber sheath in this embodiment of the invention is not intended to limit the invention. This invention is also applicable to other sheath materials such as polyurethane, silicone rubber, and polyurethane.

[0020] The oxygen-containing polar functional groups include hydroxyl, carbonyl, and / or carboxyl groups; these functional groups activate the α-H atom on their adjacent carbon atom through an inductive effect, providing hydrogen abstraction sites for free radical initiators in surface-initiated polymerization reactions. Polar functional groups are introduced into the fiber optic sheath interface via plasma treatment and micro-etching to enhance the surface roughness and surface activity of the fiber optic sheath.

[0021] In this embodiment, before plasma treatment of the fiber optic sheath surface, the fiber optic assembly is ultrasonically cleaned in an organic solvent to remove contaminants from the fiber optic sheath surface, followed by drying to remove solvent residue. The organic solvent can be ethanol, isopropanol, etc.

[0022] In practice, the optical fiber assembly is ultrasonically cleaned in ethanol for 1-3 hours (e.g., 2 hours) to remove surface contaminants, and then dried in a vacuum environment at 60-80°C (preferably 60°C) for 20-60 minutes to remove ethanol residue.

[0023] In this embodiment, the plasma treatment is carried out in an atmospheric environment (standard conditions of 101 kPa, room temperature 15-30°C, and relative humidity 30-70%), which can directly utilize oxygen and water vapor in the environment as the source of active species. By adjusting the discharge parameters, the surface of the optical fiber sheath can be activated.

[0024] Preferably, the plasma treatment power is 40-80W and the time is 60-180s. Within this parameter range, the active oxygen generated by atmospheric plasma can efficiently break down organic matter on the surface of the optical fiber assembly and generate polar groups such as hydroxyl groups through surface activation, significantly improving the wettability and chemical activity of the optical fiber assembly, thereby ensuring the formation of a strong chemical bond interface between the optical fiber assembly and the core rod resin matrix. Step S2: Grafting polyglycidyl methacrylate onto the surface of the plasma-treated optical fiber sheath to form a polyglycidyl methacrylate graft layer with epoxy groups in the side chains.

[0025] In this embodiment of the invention, the polyglycidyl methacrylate grafted layer is a GMA grafted brush layer.

[0026] Specifically, this step is carried out under nitrogen protection and includes the following steps: Benzoyl peroxide (BPO) wet powder was added to anhydrous ethanol and stirred to dissolve, thus obtaining an initiator solution; Glycidyl methacrylate (GMA) is added to the initiator solution to a volume fraction of 5-30%, and the mixture is stirred until homogeneous to obtain a grafting reaction solution; wherein the mass ratio of BPO to GMA is 1:17-1:30, preferably 1:17.6; correspondingly, the molar ratio of BPO to GMA is 1:30-1:50, preferably 1:30.

[0027] In practice, 9.35 ml of GMA liquid (density 1.07 g / mL) is weighed to be 10 g. Approximately 0.76 g of wet BPO powder is added (mass ratio approximately 1:17.6). After stirring to dissolve, different volumes of anhydrous ethanol are added and mixed thoroughly to achieve a GMA volume fraction of 5%, 10%, 15%, 20%, and 25% in the reaction system, thus obtaining the grafting reaction solution. For example, adding 10 g (9.35 ml) of GMA liquid and 0.57 g of BPO, followed by 52.98 ml of anhydrous ethanol and mixing thoroughly, yields a grafting reaction solution with a volume fraction of 15%.

[0028] The plasma-treated optical fiber assembly is immersed in the grafting reaction solution, stirred at 60-80°C for 40-80 minutes, then removed and dried to obtain an optical fiber assembly with a poly(glycidyl methacrylate) grafted layer on its surface.

[0029] Specifically, the side-chain epoxy groups on the glycidyl methacrylate (GMA) grafted brush layer have the same chemical properties as the E-51 epoxy groups in the resin matrix of the subsequent mandrel. Therefore, during the curing process, the carboxyl groups generated by the ring-opening of the acid anhydride will not only react with the epoxy groups in the resin matrix, but also react with the epoxy groups on the GMA brush layer at the interface, seamlessly participating in the crosslinking reaction.

[0030] Step S3: The grafted optical fiber assembly is embedded in the resin matrix of the core rod. After curing, the epoxy groups in the poly(glycidyl methacrylate) grafted layer undergo a ring-opening addition reaction with the resin matrix of the core rod, thereby constructing a chemical bonding interface between the optical fiber sheath and the core rod.

[0031] Specifically, the steps for constructing the chemical bonding interface include: Sub-step S31 involves mixing epoxy resin, anhydride curing agent, and phenol accelerator, wherein the molar ratio of epoxy resin to anhydride curing agent is (4~6):(3~5), and the phenol accelerator accounts for 1~3% of the total mass of epoxy resin; in this embodiment, the epoxy resin is E51 type epoxy resin.

[0032] The anhydride curing agent is methyl hexahydrophthalic anhydride (MeHHPA).

[0033] The phenol accelerator is 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30).

[0034] The preferred molar ratio of epoxy resin to acid anhydride curing agent is 5:4.

[0035] In sub-step S32, polymer hollow microspheres with a mass fraction of 1-3% of the total mass of the core rod resin matrix are added, stirred evenly, and then pre-cured in a vacuum environment at 80-85℃ for a period of time to obtain a pre-cured core.

[0036] Specifically, the total mass of the core rod resin matrix refers to the sum of the masses of epoxy resin, acid anhydride curing agent, phenol accelerator, and hollow microspheres. The polymer hollow microspheres are polyethyl methacrylate polymer hollow microspheres, and their preferred mass fraction is 2 wt%. Adding hollow microspheres can significantly reduce the weight of the core and offset some of the curing shrinkage stress, while also reducing partial discharge and effectively enhancing the bonding strength and insulation performance at the interface.

[0037] During the mixing process, the stirring speed of the stirring equipment can be 1500~2500r / min, and the stirring time can be 3~5min. After the mixture is evenly mixed, it can be dried under vacuum conditions.

[0038] In practice, a vacuum planetary stirrer is used to stir the mixture at 2000 r / min for 5 minutes. After thorough mixing, the mixture is placed in a vacuum drying oven and heated at 80°C for 1 hour to obtain a pre-cured core.

[0039] In sub-step S33, the grafted optical fiber assembly is fixed in the mold and the two ends of the optical fiber in the optical fiber assembly extend to the outside of the mold. The pre-cured core is filled into the mold and then heated at 100~110°C for a period of time to obtain the insulating core with implanted optical fiber.

[0040] Specifically, the fiber assembly with its outer surface grafted with GMA is centered and fixed along the mold axis, with both ends of the fiber sheath extending outside the mold to keep the internal fiber straight and avoid signal loss. This also facilitates subsequent removal of incompletely cured areas. A pre-cured core is filled into the mold, its viscosity suppressing air bubbles and flow disturbances, preventing erosion damage to the GMA grafting brush layer on the fiber sheath surface, and reducing subsequent curing shrinkage stress. Final curing is then completed at 80-120°C. This temperature is beneficial for the ring-opening reactivity of the GMA epoxy groups and the post-curing characteristics of the core resin matrix, allowing the grafting brush layer to fully participate in interfacial crosslinking, achieving a strong chemical bond between the fiber sheath and the core resin matrix, resulting in a structurally stable fiber composite insulating core.

[0041] The principle of this invention is as follows: Plasma treatment is applied to the optical fiber sheath in an atmospheric environment. High-energy particles, such as oxygen radicals (O·), bombard the polymer molecular chains on the surface of the optical fiber sheath, breaking the weaker CH bonds and abstracting hydrogen atoms, thereby generating macro-radicals on the polymer surface. These surface macro-radicals rapidly react with oxygen or oxygen radicals in the plasma to form intermediate states such as peroxy radicals and hydroperoxides, which are further decomposed or oxidized. Ultimately, various oxygen-containing polar functional groups, such as hydroxyl, carbonyl, and carboxyl groups, are introduced onto the surface of the optical fiber sheath. These polar groups significantly increase the surface energy and polarity of the optical fiber sheath, improving the wettability between the sheath and the epoxy resin matrix. Furthermore, they activate the α-H at the adjacent positions through an inductive effect, providing highly active hydrogen abstraction sites for subsequent BPO radicals, thus efficiently initiating the GMA grafting reaction.

[0042] Subsequently, the treated optical fiber assembly was placed in a solution containing benzoyl peroxide (BPO) and glycidyl methacrylate (GMA) and heated. Under heating conditions, the peroxide bonds in the BPO molecule undergo homolytic cleavage, generating highly reactive benzoyloxy radicals. These radicals may further decarboxylate, generating phenyl radicals. These radicals abstract the ortho-activated α-H atoms of the aforementioned polar groups, generating new surface macroradicals on the optical fiber sheath surface. These surface macroradicals attack the double bonds of the GMA monomers in the solution, initiating graft polymerization. During polymerization, the newly generated chain-end radicals continue to react with GMA, ultimately forming a GMA polymer brush layer firmly anchored to the optical fiber sheath surface by covalent bonds. In the subsequent mandrel molding and curing process, the side-chain epoxy groups on the GMA graft brush layer react with the carboxyl groups generated by ring-opening of the anhydride and embed into the epoxy resin cross-linking structure of the mandrel resin matrix, causing covalent bridging between the optical fiber sheath and the epoxy-anhydride matrix, thereby fundamentally enhancing the interfacial bonding strength and compatibility.

[0043] The present invention will now be described in detail with reference to several embodiments.

[0044] Example 1 (1) Fiber plasma treatment: The fiber optic assembly was ultrasonically cleaned in ethanol for 2 h to remove surface contaminants, and then vacuum dried at 60 ℃ for 30 min to remove ethanol residue. Then, the fiber optic sheath was plasma treated in an atmospheric environment with the equipment power set to 60W and 120s respectively. Active functional groups, such as carboxyl groups (-COOH) and hydroxyl groups (-OH), were generated on the surface of the fiber optic sheath. (2) Using BPO to initiate GMA grafting: Weigh a certain mass of wet BPO powder and add anhydrous ethanol to it. Stir with a magnetic stirrer for 10 min until dissolved. Then add GMA solution according to the total volume of GMA-anhydrous ethanol mixture of 5 vol%. Stir with a magnetic stirrer for 2 min until the solution is completely mixed and homogeneous to obtain the grafting reaction solution. Completely immerse the plasma-treated optical fiber assembly in the grafting reaction solution, heat to 70℃ with a magnetic stirrer and stir for 60 min. Take out the optical fiber assembly and put it in an oven to dry at 60℃ for 1 h to obtain the GMA-grafted optical fiber assembly. The whole process should be carried out under nitrogen protection. (3) Molding of composite insulating core: E51 type epoxy resin, methyl hexahydrophthalic anhydride, 2,4,6-tris(dimethylaminomethyl)phenol and polymethyl methacrylate polymer hollow microspheres are placed in a vacuum stirrer and stirred at 2000 r / min for 5 min. After being fully mixed, the mixture is placed in a vacuum drying oven and heated at 80℃ for 1 h to obtain a pre-cured core. The molar ratio of epoxy resin to methyl hexahydrophthalic anhydride is 5:4, the mass fraction of 2,4,6-tris(dimethylaminomethyl)phenol in the total mass of E51 type epoxy resin is 1.0 wt%, and the mass fraction of polymethyl methacrylate polymer hollow microspheres in the total mass of core rod resin matrix is ​​2.0 wt%. The prepared optical fiber assembly is fixed in the mold and extends from both ends to fill the prepared pre-cured core. Then it is heated at 100℃ for 2 h to obtain the insulating core after implantation of optical fiber.

[0045] Example 2 (1) Fiber plasma treatment: The fiber optic assembly was ultrasonically cleaned in ethanol for 1 h to remove surface contaminants, and then vacuum dried at 65 °C for 40 min to remove ethanol residue. Then, the fiber optic sheath was subjected to plasma treatment in an atmospheric environment with the equipment power set to 40W and 180s respectively. Active functional groups, such as carboxyl groups (-COOH) and hydroxyl groups (-OH), were generated on the surface of the fiber optic sheath. (2) Using BPO to initiate GMA grafting: Weigh a certain mass of wet BPO powder and add anhydrous ethanol to it. Stir with a magnetic stirrer for 10 min until dissolved. Then add GMA solution according to the total volume of GMA-anhydrous ethanol mixture of 10 vol%. Stir with a magnetic stirrer for 2 min until the solution is completely mixed and homogeneous to obtain the grafting reaction solution. Completely immerse the plasma-treated optical fiber assembly in the grafting reaction solution, heat to 60℃ with a magnetic stirrer and stir for 80 min. Take out the optical fiber assembly and put it in an oven to dry at 60℃ for 1 h to obtain the GMA-grafted optical fiber assembly. The whole process should be carried out under nitrogen protection. (3) Molding of composite insulating core: E51 type epoxy resin, methyl hexahydrophthalic anhydride, 2,4,6-tris(dimethylaminomethyl)phenol and polymethyl methacrylate polymer hollow microspheres are placed in a vacuum stirrer and stirred at 2500 r / min for 4 min. After being fully mixed, the mixture is placed in a vacuum drying oven and heated at 85℃ for 1 h to obtain a pre-cured core. The molar ratio of epoxy resin to methyl hexahydrophthalic anhydride is 6:4, the mass fraction of 2,4,6-tris(dimethylaminomethyl)phenol in the total mass of E51 type epoxy resin is 2.0 wt%, and the mass fraction of polymethyl methacrylate polymer hollow microspheres in the total mass of the core rod resin matrix is ​​3.0 wt%. The prepared optical fiber assembly is fixed in the mold and extends from both ends to fill the prepared pre-cured core. Then it is heated at 100℃ for 2 h to obtain the insulating core after the optical fiber is implanted.

[0046] Example 3 (1) Fiber plasma treatment: The fiber optic assembly was ultrasonically cleaned in ethanol for 3 h to remove surface contaminants, and then vacuum dried at 70 ℃ for 45 min to remove ethanol residue. Then, the fiber optic sheath was plasma treated in an atmospheric environment with the equipment power set to 80W and 60s respectively. Active functional groups, such as carboxyl groups (-COOH) and hydroxyl groups (-OH), were generated on the surface of the fiber optic sheath. (2) Using BPO to initiate GMA grafting: Weigh a certain mass of wet BPO powder and add anhydrous ethanol to it. Stir with a magnetic stirrer for 10 min until dissolved. Then add GMA solution according to the total volume of GMA-anhydrous ethanol mixture at 15 vol%. Stir with a magnetic stirrer for 2 min until the solution is completely mixed and homogeneous to obtain the grafting reaction solution. Completely immerse the plasma-treated optical fiber assembly in the grafting reaction solution, heat to 65℃ with a magnetic stirrer and stir for 80 min. Take out the optical fiber assembly and put it in an oven at 60℃ for 1 h to dry to obtain the GMA-grafted optical fiber assembly. The whole process should be carried out under nitrogen protection. (3) Molding of composite insulating core: E51 type epoxy resin, methyl hexahydrophthalic anhydride, 2,4,6-tris(dimethylaminomethyl)phenol and polymethyl methacrylate polymer hollow microspheres are placed in a vacuum stirrer and stirred at 2000 r / min for 3 min. After being fully mixed, the mixture is placed in a vacuum drying oven and heated at 80℃ for 1 h to obtain a pre-cured core. The molar ratio of epoxy resin to methyl hexahydrophthalic anhydride is 5:4, the mass fraction of 2,4,6-tris(dimethylaminomethyl)phenol in the total mass of E51 type epoxy resin is 1.0 wt%, and the mass fraction of polymethyl methacrylate polymer hollow microspheres in the total mass of core rod resin matrix is ​​2.0 wt%. The prepared optical fiber assembly is fixed in the mold and extends from both ends to fill the prepared pre-cured core. Then it is heated at 110℃ for 1 h to obtain the insulating core after implantation of optical fiber.

[0047] Example 4 (1) Fiber plasma treatment: The fiber optic assembly was ultrasonically cleaned in ethanol for 2 h to remove surface contaminants, and then vacuum dried at 75 ℃ for 50 min to remove ethanol residue. Then, the fiber optic sheath was subjected to plasma treatment in an atmospheric environment with the equipment power set to 70W and 110s respectively. Active functional groups, such as carboxyl groups (-COOH) and hydroxyl groups (-OH), were generated on the surface of the fiber optic sheath. (2) Using BPO to initiate GMA grafting: Weigh a certain mass of wet BPO powder and add anhydrous ethanol to it. Stir with a magnetic stirrer for 10 min until dissolved. Then add GMA solution according to the total volume of GMA-anhydrous ethanol mixture of 20 vol%. Stir with a magnetic stirrer for 2 min until the solution is completely mixed and homogeneous to obtain the grafting reaction solution. Completely immerse the plasma-treated optical fiber assembly in the grafting reaction solution, heat to 75℃ with a magnetic stirrer and stir for 45 min. Take out the optical fiber assembly and put it in an oven at 60℃ for 1 h to dry to obtain the GMA-grafted optical fiber assembly. The whole process should be carried out under nitrogen protection. (3) Molding of composite insulating core: E51 type epoxy resin, methyl hexahydrophthalic anhydride, 2,4,6-tris(dimethylaminomethyl)phenol and polymethyl methacrylate polymer hollow microspheres are placed in a vacuum stirrer and stirred at 2500 r / min for 3 min. After being fully mixed, the mixture is placed in a vacuum drying oven and heated at 80℃ for 1 h to obtain a pre-cured core. The molar ratio of epoxy resin to methyl hexahydrophthalic anhydride is 6:3, the mass fraction of 2,4,6-tris(dimethylaminomethyl)phenol in the total mass of E51 type epoxy resin is 1.0 wt%, and the mass fraction of polymethyl methacrylate polymer hollow microspheres in the total mass of core rod resin matrix is ​​3.0 wt%. The prepared optical fiber assembly is fixed in the mold and extends from both ends to fill the prepared pre-cured core. Then it is heated at 110℃ for 3 h to obtain the insulating core after implantation of optical fiber.

[0048] Example 5 (1) Fiber plasma treatment: The fiber optic assembly was ultrasonically cleaned in ethanol for 2 h to remove surface contaminants, and then vacuum dried at 80℃ for 60 min to remove ethanol residue. Then, the fiber optic sheath was plasma treated in an atmospheric environment with the equipment power set to 50W and 150s respectively. Active functional groups, such as carboxyl groups (-COOH) and hydroxyl groups (-OH), were generated on the surface of the fiber optic sheath. (2) Using BPO to initiate GMA grafting: Weigh a certain mass of wet BPO powder and add anhydrous ethanol to it. Stir with a magnetic stirrer for 10 min until dissolved. Then add GMA solution according to the total volume of GMA-anhydrous ethanol mixture of 25 vol%. Stir with a magnetic stirrer for 2 min until the solution is completely mixed and homogeneous to obtain the grafting reaction solution. Completely immerse the plasma-treated optical fiber assembly in the grafting reaction solution, heat to 80℃ with a magnetic stirrer and stir for 40 min. Take out the optical fiber assembly and put it in an oven at 60℃ for 1 h to dry to obtain the GMA-grafted optical fiber assembly. The whole process should be carried out under nitrogen protection. (3) Molding of composite insulating core: E51 type epoxy resin, methyl hexahydrophthalic anhydride, 2,4,6-tris(dimethylaminomethyl)phenol and polymethyl methacrylate polymer hollow microspheres are placed in a vacuum stirrer and stirred at 2500 r / min for 5 min. After being fully mixed, the mixture is placed in a vacuum drying oven and heated at 80℃ for 1 h to obtain a pre-cured core. The molar ratio of epoxy resin to methyl hexahydrophthalic anhydride is 4:3, the mass fraction of 2,4,6-tris(dimethylaminomethyl)phenol in the total mass of E51 type epoxy resin is 2.0 wt%, and the mass fraction of polymethyl methacrylate polymer hollow microspheres in the total mass of core rod resin matrix is ​​3.0 wt%. The prepared optical fiber assembly is fixed in the mold and extends from both ends to fill the prepared pre-cured core. Then it is heated at 100℃ for 2 h to obtain the insulating core after implantation of optical fiber.

[0049] Comparative Example Except for the absence of plasma treatment and GMA grafting treatment on the optical fiber sheath, all other process conditions were the same as in Example 1.

[0050] The cured insulating core samples from Examples 1-5 and the comparative examples were cut into corresponding shapes and sizes for performance testing. The main test items included interfacial shear strength, breakdown voltage, and water diffusion leakage current.

[0051] Interfacial shear strength test: The interfacial shear strength (IFSS) of optical fiber was measured using a YG-163 electronic microsphere debonding tester. The speed of the fixture was set to 2 mm / min, and it was slowly moved upward until the fixture scraped off the epoxy resin microspheres. The embedding length and maximum load were measured and the interfacial shear strength was calculated.

[0052] Combination Figure 2 It can be seen that: the interfacial shear strength of the comparative example is 2.101 MPa; the interfacial shear strength of Example 1 is 3.084 MPa; the interfacial shear strength of Example 2 is 3.376 MPa; the interfacial shear strength of Example 3 is 3.779 MPa; the interfacial shear strength of Example 4 is 3.601 MPa; and the interfacial shear strength of Example 5 is 3.422 MPa.

[0053] Breakdown voltage test: The breakdown voltage test was conducted according to GB / T 1408.1-2016 standard. The breakdown strength of the sample under an alternating electric field was measured at a voltage increase rate of 1 kV / s. The sample thickness was 2 ± 0.1 mm. Electrodes were placed at the fiber optic interface and the center of the composite foam material, respectively. The ambient temperature was 25 ℃. Ball-to-ball electrodes were used for testing. The breakdown voltage data were analyzed using the Weibull distribution function.

[0054] Combination Figure 3 It can be seen that: the breakdown voltage of the comparative example is 23.25 kV / mm; the breakdown voltage of Example 1 is 26.59 kV / mm; the breakdown voltage of Example 2 is 28.97 kV / mm; the breakdown voltage of Example 3 is 30.23 kV / mm; the breakdown voltage of Example 4 is 29.08 kV / mm; and the breakdown voltage of Example 5 is 26.85 kV / mm.

[0055] Water diffusion leakage current test: conducted according to GB-T 19519-2014. A 30 mm high core sample was boiled in a 0.1% NaCl solution for 100 h, removed and dried, and the leakage current value was collected using a Rigio-DM3068 measuring instrument under a 12 kV flat plate electrode.

[0056] Combination Figure 4 As can be seen, the leakage current of the comparative example is 53.65 μA; the leakage current of Example 1 is 50.93 μA; the leakage current of Example 2 is 49.09 μA; the leakage current of Example 3 is 46.43 μA; the leakage current of Example 4 is 47.03 μA; and the leakage current of Example 5 is 49.16 μA.

[0057] In summary, compared to the untreated fiber optic assembly in the comparative example, Example 3 showed a 79.87% improvement in interfacial shear strength; a 30.02% improvement in breakdown voltage at a 63.2% breakdown probability; and a 13.46% reduction in water diffusion leakage current. Among all examples, Example 3 exhibited the best overall performance (the grafting density and thickness of the GMA brush layer on the fiber sheath surface can be controlled by adjusting the volume fraction of the GMA monomer. The brush layer structure formed when the volume fraction of GMA is 15 vol% achieves the optimal interfacial bonding state), indicating that optimizing the interfacial bonding state improves interfacial adhesion, which is beneficial for enhancing the mechanical and electrical properties of the fiber sheath-core interface.

[0058] In summary, this invention, through plasma treatment of the optical fiber sheath, introduces polar functional groups at the sheath interface and performs micro-etching, significantly improving surface activity while enhancing the surface roughness of the sheath, providing highly active reaction sites for subsequent chemical grafting. GMA free radical polymerization is initiated by an initiator, allowing it to be firmly grafted onto the optical fiber sheath surface via chemical bonds. The epoxy groups in the GMA molecules further undergo ring-opening copolymerization with the core rod resin matrix, forming a stable covalent bond network between the optical fiber sheath and the core rod, greatly improving the interfacial shear strength. The treated optical fiber assembly is then embedded into the core rod resin matrix and cured by heating to form an optical fiber composite insulating core, effectively solving the problems of insufficient interfacial compactness and poor long-term service stability in existing technologies.

[0059] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for enhancing the interface between embedded optical fiber and core rod in a composite insulator, characterized in that, include: The surface of the fiber sheath in the fiber optic assembly is subjected to plasma treatment to activate the surface of the fiber sheath and introduce oxygen-containing polar functional groups; wherein, the fiber optic assembly includes an optical fiber and an optical fiber sheath covering the outer periphery of the optical fiber. Polyglycerol methacrylate is grafted onto the surface of the optical fiber sheath after plasma treatment to form a polyglycerol methacrylate graft layer with epoxy groups in the side chain. The grafted optical fiber assembly is embedded in the resin matrix of the core rod. After curing, the epoxy groups in the poly(glycidyl methacrylate) grafted layer undergo a ring-opening addition reaction with the resin matrix of the core rod, thereby constructing a chemical bonding interface between the optical fiber sheath and the core rod.

2. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 1, characterized in that, The oxygen-containing polar functional groups include hydroxyl, carbonyl, and / or carboxyl groups.

3. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 1, characterized in that, Before plasma treatment of the fiber sheath surface, the fiber assembly is ultrasonically cleaned in an organic solvent to remove contaminants from the fiber sheath surface, and then dried to remove solvent residue.

4. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 1, characterized in that, The plasma treatment has a power of 40-80W and a duration of 60-180s.

5. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 1, characterized in that, The grafting of polyglycidyl methacrylate is carried out under nitrogen protection and includes: Benzoyl peroxide wet powder was added to anhydrous ethanol and stirred to dissolve, thus obtaining an initiator solution; Add glycidyl methacrylate to the initiator solution to a volume fraction of 5-30%, stir until homogeneous, and obtain the grafting reaction solution; The plasma-treated optical fiber assembly is immersed in the grafting reaction solution, stirred at 60-80°C for 40-80 minutes, then removed and dried to obtain an optical fiber assembly with a poly(glycidyl methacrylate) grafted layer on its surface.

6. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 1, characterized in that, The steps for constructing the chemically bonded interface include: An epoxy resin, an anhydride curing agent, and a phenol accelerator are mixed to form a core rod resin matrix, wherein the molar ratio of the epoxy resin to the anhydride curing agent is (4~6):(3~5), and the phenol accelerator accounts for 1~3% of the total mass of the epoxy resin. Add 1-3% of polymer hollow microspheres, which account for the total mass of the core rod resin matrix, stir evenly, and heat in a vacuum environment at 80-85℃ for a period of time to pre-cur the core to obtain a pre-cured core. The grafted optical fiber assembly is fixed in a mold and the two ends of the optical fiber in the optical fiber assembly extend to the outside of the mold. The pre-cured core is filled into the mold and then heated at 100~110°C for a period of time to obtain an insulating core with implanted optical fiber.

7. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 6, characterized in that, The molar ratio of epoxy resin to acid anhydride curing agent is 5:

4.

8. The interface enhancement method for embedded optical fiber and core rod in composite insulator as described in claim 6, characterized in that, The anhydride curing agent is methyl hexahydrophthalic anhydride.

9. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 6, characterized in that, The phenol accelerator is 2,4,6-tris(dimethylaminomethyl)phenol.

10. The interface enhancement method for embedded optical fiber and core rod in composite insulator according to claim 6, characterized in that, The polymer hollow microspheres are polyethyl methacrylate polymer hollow microspheres.