A method for preparing a nanofluid composite membrane, products thereof and applications in osmotic energy harvesting

By extracting negatively charged cellulose nanofibers from brown algae and combining them with hydrated calcium silicate, a CNF/CSH nanofluid membrane was constructed, solving the environmental pollution and high cost problems of nanochannel materials and achieving efficient osmotic energy harvesting and stable output.

CN123152137APending Publication Date: 2026-11-24SOUTHEAST UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510654425.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing nanochannel material preparation technologies face environmental pollution risks, high costs, and difficulties in large-scale production. Furthermore, the output power density of existing nanofluid membranes is insufficient.

Method used

Negatively charged cellulose nanofibers (CNFs) were extracted from brown algae using an alkali treatment-mechanical defibrillation method. CNF/CSH composite membranes were constructed by guiding the directional growth of calcium silicate hydrate (CSH) crystal nuclei through interfacial chelation. The layered ordered composite membranes were then prepared using a vacuum-assisted self-assembly strategy.

Benefits of technology

The prepared CNF/CSH composite membrane has high ionic conductivity, low membrane internal resistance and high output power density, and can stably output at low salt concentrations, adapting to different environmental conditions, thus breaking through the performance limitations of traditional nanofluid membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152137A_ABST
    Figure CN123152137A_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a nanofluid composite membrane, and a product and application thereof. The preparation method comprises the following steps: extracting cellulose nanofibers with negative surface charges from seaweed; dissolving the cellulose nanofibers in a solvent in a glove box filled with nitrogen, and then introducing calcium nitrate solution and sodium metasilicate solution into the mixed solution; after the reaction is completed, the mixed solution is cleaned through multiple centrifugations and is subjected to suction filtration to form a membrane, so that the nanofluid composite membrane with osmotic energy collection is obtained. The main raw materials of the application are seaweed, sodium metasilicate and calcium nitrate, which are low in price and environmentally friendly. The nanofluid membrane prepared by the application is different from a traditional ion exchange membrane, has high ion conductivity, low membrane internal resistance, high osmotic energy collection performance and environmental applicability, and is expected to more efficiently collect osmotic energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanofluidic device fabrication technology, specifically relating to a method for preparing a nanofluidic composite membrane, its product, and its application in permeation energy harvesting. Background Technology

[0002] Nanofluids refer to the unique transport phenomena exhibited by fluid media (including liquids, gases, and ionized substances) within a confined space with a characteristic scale of less than 100 nanometers. In charged nanochannel systems, ion transport behavior is mainly regulated by the electric double layer effect formed at the solid-liquid interface: counterions in the solution undergo selective adsorption under the influence of the interfacial potential, forming an electric double layer structure with a space charge density gradient. The positive and negative ions within this layer exhibit asymmetric distribution characteristics, and the coupling effect of their concentration gradient and potential gradient induces the formation of an electrochemical potential field, thereby driving the directional migration of ions and generating differential transport rates. This nanoscale ion transport mechanism is not only an important material basis for physiological processes such as muscle fiber contraction and nerve impulse transmission, but also provides a theoretical basis for the development of novel nanofluidic devices. Research shows that nanofluidic systems based on electric double layer regulation have demonstrated breakthrough application potential in fields such as biosensing technology, microfluidic systems, seawater desalination engineering, and novel energy storage devices. Their unique interfacial charge effect opens up innovative research directions for cross-scale material transport control.

[0003] The realization of nanoconfined fluid effects relies on the construction of a network structure with sub-100-nanometer-scale fluid transport channels within the material, and the channel surface must possess controllable charge properties. Current nanochannel material preparation technologies face three major challenges: first, traditional synthesis processes often involve toxic reagent residues, posing environmental toxicity risks; second, precise control of nanostructures requires complex microfabrication techniques, resulting in poor process repeatability; and third, the demand for high-purity raw materials and precision equipment drives up manufacturing costs. It is noteworthy that existing nanochannel material systems are mostly based on petroleum-based polymers such as polyethyleneimine (PEI), polyvinyl alcohol (PVA), and polystyrene sulfonate (PSS). These non-renewable polymers are difficult to degrade in the natural environment, and their end-of-life disposal can easily lead to environmental risks such as microplastic pollution. This material unsustainability and the conflict with the global green chemistry development concept have sparked a surge of research into novel bio-based biodegradable nanochannel materials. While significant breakthroughs have been achieved in the construction of nanoconfined channels at the laboratory scale, their large-scale fabrication remains constrained by multiple technical bottlenecks. Firstly, photolithography or atomic layer deposition (ALD) processes relying on silicon substrates are highly complex and time-consuming, resulting in high manufacturing costs per unit area. Secondly, existing processes are limited by the requirements of high-cleanliness production environments and precision instruments, leading to poor process compatibility and difficulty in meeting the demands of continuous industrial production. Against this backdrop, developing low-energy self-assembly strategies based on eco-friendly precursors (such as biomass-derived materials) to construct biomimetic nano-ion membranes with both high ion flux and interfacial charge control capabilities has become a key research direction for overcoming the negative environmental externalities of traditional petroleum-based material systems and achieving sustainable development of nanofluidic devices. Currently, some researchers have successfully prepared renewable biomass nanofluidic membranes for permeation energy harvesting by utilizing the advantages of readily available, biodegradable, renewable, and environmentally compatible natural materials, addressing the issues of high cost and environmental pollution. Hu Liangbing et al. successfully fabricated a wood-based permeation energy generator using a top-down method by utilizing the naturally oriented micro- and nano-channels within wood (Adv. Energy Mater. 2020, 10, 1902590.; Adv. Functional Mater. 2019, 29(44), 1902772.; ACS Nano 2021, 15(7), 11244-11252.). However, the aforementioned prior art has a drawback: the construction of nanochannels is based on the randomness of wood growth, requiring compression of the wood or filling with hydrogel to eliminate macropores.Chinese patent application CN115182163B discloses a metal-organic framework (MOF) / cellulose composite nanofluidic channel membrane and its preparation method and application. MOF particles are loaded and grown on cellulose nanofibers, and then a film is formed to form an MOF / cellulose composite membrane. The actual power density of the MOF / cellulose composite membrane can reach 1.9 W / m. -2 The output power density is lower than the commercial standard.

[0004] Therefore, there is an urgent need to find a new method for preparing nanofluid membranes to overcome the above problems. Summary of the Invention

[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for preparing nanofluid membranes.

[0006] The technical problem that this invention also aims to solve is to provide a nanofluid composite membrane with high ionic conductivity, low membrane internal resistance, high output power density, and good environmental adaptability.

[0007] The final technical problem to be solved by this invention is to provide the application of nanofluidic composite membranes in permeation energy harvesting.

[0008] Technical Solution: To solve the above-mentioned technical problems, the present invention provides a method for preparing a nanofluidic composite membrane, comprising the following steps:

[0009] (1) Calcium nitrate solution and sodium metasilicate solution were simultaneously and dropwise injected into a continuously stirred cellulose nanofiber (CNF) dispersion to obtain a mixed solution. The CNF dispersion was obtained by dissolving CNF with negative surface charge extracted from seaweed in a solvent.

[0010] (2) After the reaction is completed, the mixed solution is centrifuged and washed multiple times and vacuum filtered to form a membrane, thus obtaining a nanofluid composite membrane with permeation energy collection.

[0011] In step (1), the CNF with negative surface charge is obtained by separating natural cellulose from brown algae using an alkali treatment-mechanical defibrillation method, and then performing surface carboxyl functionalization modification through a TEMPO oxidation system to obtain a CNF suspension with negative surface charge. Subsequently, a fluffy CNF aerogel is obtained by freeze-drying.

[0012] The solvent used in step (1) is placed in a glove box after being treated at high temperature.

[0013] In step (1), the CNF dispersion is prepared by dispersing CNF aerogel in deoxygenated deionized water and then treating it by ultrasonic disruption and high-pressure homogenization.

[0014] In step (1), the titration rate of the calcium nitrate solution and the sodium metasilicate solution is 3-8 mL / h.

[0015] In step (1), sodium metasilicate and calcium nitrate are dissolved in a solvent and ultrasonically treated to obtain sodium metasilicate solution and calcium nitrate solution for later use.

[0016] In step (1), the mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers, and solvent (deionized water) is 0.1-1:0.15-1.18:0.4-2:95-99.

[0017] In step (1), the stirring temperature is 55-80℃.

[0018] In step (2), the vacuum filtration pressure is 0.05-0.1 MPa, the filtration time is 3-8 h, and the filtration temperature is 15-40 °C.

[0019] The present invention also includes the nanofluid composite membrane prepared by the aforementioned preparation method.

[0020] The present invention also includes the application of the aforementioned nanofluid composite membrane in permeation energy harvesting.

[0021] The salinity gradient ratio in the salinity differential power generation is 50:1, and the salt includes one of NaCl, KCl, LiCl, CaCl2, MgCl2 or AlCl3 solution.

[0022] The preparation principle of this invention is as follows: When constructing hydrated calcium silicate (CSH) composite materials in a CNF dispersion system, the abundant hydroxyl / carboxyl functional units on the CNF surface can serve as selective coordination sites for calcium ions, inducing the directional deposition of CSH crystal nuclei through interfacial chelation. This bio-templating effect significantly enhances the preferred orientation growth characteristics of CSH crystals. Based on this, the CSH / CNF structure formed can achieve continuous preparation of layered ordered composite membranes through a vacuum-assisted self-assembly strategy. Notably, by introducing CNF, CSH, and other nanomaterials to construct cross-dimensional structures through a CNF-assisted CSH growth strategy, a dual regulation strategy can be implemented: on the one hand, the zeta potential on the membrane surface is optimized through interfacial charge engineering to enhance the ion selective transport effect; on the other hand, the internal mesoporous channel structure is finely regulated by the topological confinement effect of nanofillers, thereby overcoming the mutual constraint between ion flux and selectivity in traditional homogeneous membrane materials. Experiments show that this type of biomimetic heterostructure nanofluid membrane exhibits breakthrough transport performance in fields such as salinity gradient power generation and ion sieving.

[0023] Beneficial Effects: Compared with existing technologies, this invention has the following significant characteristics: The main raw materials used in this invention are seaweed, calcium nitrate, and sodium metasilicate, which are inexpensive, non-toxic, and environmentally friendly. The nanofluid membrane prepared in this invention differs from traditional commercial or synthetic nanofluid membranes. Its preparation method is simple, it has low internal resistance, and high output performance, and it is expected to collect permeate energy more efficiently for electrical energy conversion to address the energy crisis. The nanofluid membrane of this invention uses CSH nanosheets, which can overcome the mutual constraint between ion flux and selectivity in traditional nanofluid membranes. At low salt concentrations (C... KCl <10 -3 At a concentration of M), the CNF / CSH composite membrane exhibits an ionic conductivity of up to 1.8 μS. Under a 50-fold salinity gradient, the CNF / CSH composite membrane demonstrates stable output for up to 20 days. Under different solution conditions, the CNF / CSH composite membrane exhibits good output power density. Under real seawater and river water conditions, the maximum output power density of the CNF / CSH composite membrane reaches 6.45 W / m³. -2 . Attached Figure Description

[0024] Figure 1 The ionic conductivity diagrams are for the CNF / CSH nanofluid membranes prepared in Examples 1-6.

[0025] Figure 2 The output power density diagrams of the CNF / CSH nanofluid membranes prepared in Examples 1-6 under a 50-fold salinity gradient are shown.

[0026] Figure 3 A photograph of the CNF / CSH nanofluid membrane prepared in Example 3;

[0027] Figure 4 A scanning electron microscope image of the CNF / CSH nanofluidic film prepared in Example 3;

[0028] Figure 5 The image shows the stable output of the CNF / CSH nanofluid membrane prepared in Example 3 over a period of 20 days.

[0029] Figure 6 The output power density diagram of the CNF / CSH nanofluid membrane prepared in Example 3 under different solution states;

[0030] Figure 7 The output power density diagram of the CNF / CSH nanofluid membrane prepared in Example 3 under real seawater and river water conditions;

[0031] Figure 8 Image of the CNF / CSH nanofluid membrane prepared in Example 5. Detailed Implementation

[0032] Unless otherwise specified, all materials, reagents, and instruments used in the following examples are commercially available. Experimental methods not specifically described in the examples are generally performed under standard conditions or as recommended by the manufacturer.

[0033] Example 1: Preparation of a nanofluidic membrane for osmotic energy harvesting

[0034] 1. Natural cellulose was isolated from brown algae using an alkali treatment-mechanical defibrillation method. The surface was then functionalized with carboxyl groups via a TEMPO oxidation system to obtain a negatively charged CNF suspension. Subsequently, a fluffy CNF aerogel template was obtained through freeze-drying. Specific conditions were followed to prepare the CNF aerogel according to the method described in the literature (Nano Energy, 124, 109450).

[0035] 2. In a nitrogen-filled glove box, CNF aerogel was quantitatively dispersed in deoxygenated deionized water and then ultrasonically (400W) to prepare a CNF dispersion with a mass concentration of 1.25%.

[0036] 3. Under a nitrogen atmosphere, dissolve calcium nitrate hexahydrate (Ca(NO3)2·6H2O, AR) in deoxygenated deionized water and dissolve it with ultrasonic assistance to form a transparent calcium nitrate solution with a mass concentration of 1%. Store the solution in a sealed container away from light.

[0037] 4. Under a nitrogen atmosphere, sodium metasilicate nonahydrate (Na2SiO3·9H2O, AR) is dissolved in deoxygenated deionized water and dissolved with ultrasonic assistance to form a transparent sodium metasilicate solution with a mass concentration of 1.5%.

[0038] 5. Using a flow pump, calcium nitrate solution and sodium metasilicate solution were added dropwise to a continuously stirred CNF dispersion at a simultaneous titration rate of 3 mL / h. The mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers, and deoxygenated deionized water was 0.1:0.15:1:98.75. The stirring temperature was set to 55℃. After titration, the reaction was maintained for 24 h to promote heterogeneous nucleation and directional growth of CSH on the CNF surface, thus obtaining the reaction product CSH / CNF complex.

[0039] 6. Transfer the reaction product, the CSH / CNF complex, to a centrifuge tube and centrifuge at 6000 rpm for 5 min to remove free ions and unreacted precursors. Repeat the washing process several times. After each centrifugation, use ultrasonic-assisted redispersion to ensure particle stability.

[0040] 7. Place the cleaned CSH / CNF complex in a freeze dryer for 48 hours to freeze dry. Accurately weigh the dried product and reconstitute it in deoxygenated deionized water to form a stable colloidal dispersion of the CSH / CNF complex at 0.2 wt%.

[0041] 8. Take 20 mL of 0.2 wt% stable colloidal dispersion and use a vacuum-assisted self-assembly strategy. Specifically, the filtration pressure is 0.05 MPa, the temperature is 15 ℃, the filtration time is 4 h, and after the filtration is completed, let it stand for 24 h to finally obtain a nanocomposite film with a layered ordered structure.

[0042] Example 2:

[0043] 1. A CNF dispersion with a mass concentration of 1%, a calcium nitrate solution with a mass concentration of 2%, and a sodium metasilicate solution with a mass concentration of 3% were prepared according to the preparation method of Example 1.

[0044] 2. Calcium nitrate and sodium metasilicate solutions were injected dropwise into a continuously stirred CNF dispersion at a simultaneous titration rate of 5 mL / h using a flow pump. The mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers, and solvent (deionized water) was 0.2:0.3:0.8:98.7. The stirring temperature was 80℃. After titration, the reaction was maintained for 24 h to promote heterogeneous nucleation and directional growth of CSH on the CNF surface, thus obtaining the reaction product CSH / CNF complex.

[0045] 3. Transfer the reaction product, the CSH / CNF complex, to a centrifuge tube and centrifuge at 6000 rpm for 5 min to remove free ions and unreacted precursors. Repeat the washing process several times. After each centrifugation, use ultrasonic-assisted redispersion to ensure particle stability.

[0046] 4. Place the cleaned CSH / CNF complex in a freeze dryer for 48 hours to freeze dry. Accurately weigh the dried product and reconstitute it in deoxygenated water to form a stable colloidal dispersion of 0.2 wt%.

[0047] 5. Take 20 mL of the composite dispersion for later use. Using a vacuum-assisted self-assembly strategy, select a filtration pressure of 0.1 MPa, a filtration time of 6 h, and a filtration temperature of 40 °C. After the filtration is completed, let it stand for 24 h to finally obtain a nanocomposite film with a layered ordered structure.

[0048] Example 3

[0049] 1. A CNF dispersion with a mass concentration of 1.3%, a calcium nitrate solution with a mass concentration of 10%, and a sodium metasilicate solution with a mass concentration of 10% were prepared according to the preparation method of Example 1.

[0050] 2. Calcium nitrate and sodium metasilicate solutions were injected dropwise into a continuously stirred CNF dispersion at a simultaneous titration rate of 8 mL / h using a flow pump. The mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers, and solvent was 1:1:0.4:97.6. The stirring temperature was 65℃. After titration, the reaction was maintained for 24 h to promote heterogeneous nucleation and directional growth of CSH on the CNF surface, thus obtaining the reaction product CSH / CNF complex.

[0051] 3. Transfer the reaction product, the CSH / CNF complex, to a centrifuge tube and centrifuge at 6000 rpm for 5 min to remove free ions and unreacted precursors. Repeat the washing process several times. After each centrifugation, use ultrasonic-assisted redispersion to ensure particle stability.

[0052] 4. Place the cleaned CSH / CNF complex in a freeze dryer for 48 hours to freeze dry. Accurately weigh the dried product and reconstitute it in deoxygenated water to form a stable colloidal dispersion of 0.2 wt%.

[0053] 5. Take 20 mL of the composite dispersion for later use. Using a vacuum-assisted self-assembly strategy, select a filtration pressure of 0.1 MPa, a filtration time of 8 h, and a filtration temperature of 30 °C. After the filtration is completed, let it stand for 24 h to finally obtain a nanocomposite film with a layered ordered structure.

[0054] Example 4

[0055] 1. A CNF dispersion with a mass concentration of 2%, a calcium nitrate solution with a mass concentration of 10%, and a sodium metasilicate solution with a mass concentration of 12% were prepared according to the preparation method of Example 1.

[0056] 2. Calcium nitrate and sodium metasilicate solutions were injected dropwise into a continuously stirred CNF dispersion at a simultaneous titration rate of 7 mL / h using a flow pump. The mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers, and solvent was 1:1.18:2:95.82. The stirring temperature was 60℃. After titration, the reaction was maintained for 24 h to promote heterogeneous nucleation and directional growth of CSH on the CNF surface, thus obtaining the reaction product CSH / CNF complex.

[0057] 3. Transfer the reaction product, the CSH / CNF complex, to a centrifuge tube and centrifuge at 6000 rpm for 5 min to remove free ions and unreacted precursors. Repeat the washing process several times. After each centrifugation, use ultrasonic-assisted redispersion to ensure particle stability.

[0058] 4. Place the cleaned CSH / CNF complex in a freeze dryer for 48 hours to freeze dry. Accurately weigh the dried product and reconstitute it in deoxygenated water to form a stable colloidal dispersion of 0.2 wt%.

[0059] 5. Take 20 mL of the composite dispersion for later use. Using a vacuum-assisted self-assembly strategy, the filtration pressure is selected as 0.08 MPa, the filtration time is 7 h, and the filtration temperature is 29 °C. After the filtration is completed, let it stand for 24 h to finally obtain a nanocomposite film with a layered ordered structure.

[0060] Example 5

[0061] 1. A CNF dispersion with a mass concentration of 0.5%, a calcium nitrate solution with a mass concentration of 20%, and a sodium metasilicate solution with a mass concentration of 20% were prepared according to the preparation method of Example 1.

[0062] 2. Calcium nitrate and sodium metasilicate solutions were injected dropwise into a continuously stirred CNF dispersion at a simultaneous titration rate of 4 mL / h using a flow pump. The mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers, and solvent was 2:2:0.5:95.5. The stirring temperature was 70℃. After titration, the reaction was maintained for 24 h to promote heterogeneous nucleation and directional growth of CSH on the CNF surface, thus obtaining the reaction product CSH / CNF complex.

[0063] 3. Transfer the reaction product, the CSH / CNF complex, to a centrifuge tube and centrifuge at 6000 rpm for 5 min to remove free ions and unreacted precursors. Repeat the washing process several times. After each centrifugation, use ultrasonic-assisted redispersion to ensure particle stability.

[0064] 4. Place the cleaned CSH / CNF complex in a freeze dryer for 48 hours to freeze dry. Accurately weigh the dried product and reconstitute it in deoxygenated water to form a stable colloidal dispersion of 0.2 wt%.

[0065] 5. Take 20 mL of the composite dispersion for later use. Use a vacuum-assisted self-assembly strategy, select a filtration pressure of 0.1 MPa, a filtration time of 4 h, and a filtration temperature of 38 °C. After filtration, let it stand for 24 h.

[0066] 6. The vacuum self-assembly results of this embodiment are as follows: Figure 8 As shown, the membrane exhibits a broken state, which is due to the discontinuity of the internal network caused by excessive calcium nitrate and sodium metasilicate.

[0067] Example 6:

[0068] 1. A stable colloidal dispersion of 0.2 wt% was prepared using the same method as in Example 1.

[0069] 2. Take 20 mL of 0.2 wt% stable colloidal dispersion and use a vacuum-assisted self-assembly strategy. Specifically, the filtration pressure is 0.05 MPa, the filtration time is 8 h, the filtration temperature is 40 °C, and after the filtration is completed, let it stand for 24 h to finally obtain the cellulose film.

[0070] Experimental example:

[0071] 1. The transmembrane ion transport properties of the composite films prepared in Examples 1-6 were systematically characterized using a reverse electrodialysis testing system (refer to Nano Energy, 124, 109450). The results show that... Figure 1 , 2 As shown. At low salt concentrations (C KCl <10 -3 The ionic conductivity of Example 1 was 1.2 μS, that of Example 2 was 1.5 μS, that of Example 3 was 1.8 μS, that of Example 4 was 0.8 μS, and that of Example 6 was 1.1 μS. The addition of an appropriate amount of CSH successfully enhanced ion transport capability; however, excessive addition hindered ion transport. Under a 50-fold NaCl salt concentration gradient, the output power density of Example 1 was 2.95 W / m³. 2 The output power density of Example 2 is 4.01 W / m². 2 The output power density of Example 3 is 6.21 W / m². 2 The output power density of Example 4 is 2.03 W / m². 2 The output power density of Example 6 is 1.48 W / m². 2 .

[0072] 2. The composite film prepared in Example 3 was examined using a field emission scanning electron microscope. Figure 3 (To perform cross-scale morphological characterization.) Figure 4 As shown, the membrane surface exhibits a highly ordered layered topological structure, as illustrated in the cross-sectional analysis. Figure 4 This further confirms the presence of gradient-distributed nano-confined channels within the device. To evaluate its practicality, a 20-day cyclic stability test was conducted under constant temperature and humidity conditions (25℃, 60% RH) (50 times the concentration of NaCl solution was placed on both sides of the membrane, and the solution was replaced before each test). Figure 5 As shown, the membrane output power remains stable, overcoming the interface failure bottleneck commonly found in existing nanofluidic devices. Further verification was achieved through multiple solution systems (0.5M / 0.01M NaCl, KCl, LiCl, CaCl2, MgCl2, AlCl3 solutions, and 0.5M / 0.01M NaCl solutions at different pH values ​​(pH = 5, 6, 7, 8, 9)). Figure 6 This demonstrates excellent environmental adaptability. Notably, the CNF / CSH nanofluid membrane prepared in Example 3 achieved an output power density of 6.45 W / m³ in the salinity gradient between the Bohai Sea and the Yellow River. 2 ( Figure 7 ).

Claims

1. A method for preparing a nanofluidic composite membrane, characterized in that, Includes the following steps: (1) Calcium nitrate solution and sodium metasilicate solution were simultaneously and dropwise injected into a continuously stirred CNF dispersion to obtain a mixed solution. The CNF dispersion was obtained by dissolving cellulose nanofibers with negative surface charge extracted from seaweed in a solvent. (2) After the reaction is completed, the mixed solution is centrifuged and washed multiple times and vacuum filtered to form a membrane, thus obtaining a nanofluid composite membrane with permeation energy collection.

2. The method for preparing the nanofluidic composite membrane according to claim 1, characterized in that, In step (1), the cellulose nanofibers with negative surface charge are obtained by separating natural cellulose from brown algae using an alkali treatment-mechanical defibrillation method, and then modifying the surface carboxyl groups through a TEMPO oxidation system to obtain a CNF suspension with negative surface charge. Subsequently, a fluffy CNF aerogel is obtained by freeze-drying.

3. The method for preparing the nanofluidic composite membrane according to claim 2, characterized in that, The CNF dispersion mentioned in step (1) is prepared by dispersing CNF aerogel in deoxygenated deionized water and then treating it by ultrasonic disruption and high-pressure homogenization.

4. The method for preparing the nanofluidic composite membrane according to claim 1, characterized in that, The titration rate of the calcium nitrate solution and sodium metasilicate solution in step (1) is 3~8 mL / h.

5. The method for preparing the nanofluidic composite membrane according to claim 1, characterized in that, The mass ratio of sodium metasilicate, calcium nitrate, cellulose nanofibers and solvent in step (1) is 0.1~1: 0.15~1.18: 0.4~2: 95~99.

6. The method for preparing the nanofluidic composite membrane according to claim 1, characterized in that, The stirring temperature in step (1) is 55~80℃.

7. The method for preparing the nanofluidic composite membrane according to claim 1, characterized in that, In step (2), the vacuum filtration pressure is 0.05~0.1 MPa, the filtration time is 3~8 h, and the filtration temperature is 15~40 ℃.

8. The nanofluid composite membrane prepared by the preparation method according to any one of claims 1 to 7.

9. The application of the nanofluid composite membrane according to claim 8 in permeation energy harvesting.

10. The application according to claim 9, characterized in that, The energy harvesting includes salinity gradient power generation or ion sieving, wherein the salinity gradient ratio in the salinity gradient power generation is 50:1.

Citation Information

Patent Citations

  • A MOF / cellulose composite nanofluid channel membrane and its preparation method and application

    CN115182163B