An antibacterial degradable film and a preparation method thereof

By grafting eugenol onto the PBAT molecular chain and forming covalent crosslinks with PLA, the compatibility and antibacterial properties of PLA/PBAT blend films were solved, and a biodegradable film with both excellent mechanical properties and long-lasting antibacterial function was prepared.

CN123152141APending Publication Date: 2026-11-24河南逸祥领研科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611557819.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

PLA and PBAT blend films have poor thermodynamic compatibility and low interfacial bonding, resulting in insufficient mechanical properties and a lack of antibacterial properties, making it difficult to meet practical application requirements.

Method used

By grafting eugenol onto the PBAT molecular chain and forming covalent cross-links with PLA, a three-dimensional cross-linked network was constructed to prepare a PLA/PBAT-g-eugenol cross-linked blend, which enhanced the interfacial binding force and introduced antibacterial active units.

Benefits of technology

It achieves a balance of high tensile strength, toughness and long-lasting antibacterial properties. The film has an antibacterial rate of ≥90% against Staphylococcus aureus and Escherichia coli, an eugenol migration rate of <5%, and a light transmittance of ≥85%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152141A_ABST
    Figure CN123152141A_ABST
Patent Text Reader

Abstract

This invention provides an antibacterial biodegradable film and its preparation method. The method includes: melting PBAT, adding eugenol and maleic anhydride to induce esterification of eugenol and maleic anhydride to form eugenol maleic acid monoester; then adding BIBP for a free radical grafting reaction to graft the eugenol maleic acid monoester onto the PBAT molecular chain, obtaining PBAT-g-eugenol; mixing PBAT-g-eugenol and PLA, adding BIBP for melt crosslinking blending to form covalent crosslinks at the PLA / PBAT-g-eugenol interface, obtaining a PLA / PBAT-g-eugenol crosslinked blend; and extruding the PLA / PBAT-g-eugenol crosslinked blend to obtain an antibacterial biodegradable film. This invention solves the problems of insufficient mechanical properties and lack of antibacterial properties in related technologies for biodegradable films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of biodegradable polymer material processing technology, and in particular to an antibacterial biodegradable film and its preparation method. Background Technology

[0002] In related technologies, fully biodegradable films are prepared using PLA (polylactic acid) and PBAT (polybutylene adipate / terephthalate). PLA, derived from biomass raw materials such as corn and sugarcane, exhibits high transparency, excellent rigidity, and tensile strength. PBAT is an aliphatic-aromatic biodegradable copolyester; the aliphatic segments impart superior toughness (elongation at break > 500%), while the aromatic segments ensure basic mechanical strength. However, PLA and PBAT have poor thermodynamic compatibility, resulting in severe phase separation and extremely low interfacial bonding during direct melt blending, making it difficult to simultaneously improve strength and toughness, leading to insufficient mechanical properties in the film. Furthermore, the aforementioned films have limited functionality, lacking antibacterial properties, and thus fail to meet practical application requirements. Summary of the Invention

[0003] In view of the above problems, the present invention is proposed to provide a biodegradable antibacterial blend film and a method for preparing the same, which overcomes or at least partially solves the above problems, and solves the problem that biodegradable films in the related art have insufficient mechanical properties and do not have antibacterial properties.

[0004] Specifically, the present invention provides a method for preparing an antibacterial biodegradable film, comprising: After PBAT is melted, eugenol and maleic anhydride are added to induce an esterification reaction between eugenol and maleic anhydride to form eugenol maleic acid monoester; then BIBP is added to carry out a free radical grafting reaction to graft the eugenol maleic acid monoester onto the PBAT molecular chain to obtain PBAT-g-eugenol. After mixing PBAT-g-eugenol and PLA, BIBP is added for melt crosslinking blending to form covalent crosslinking bonds at the interface between PLA and PBAT-g-eugenol, thus obtaining PLA / PBAT-g-eugenol crosslinked blend. The PLA / PBAT-g-eugenol crosslinked blend was extruded and blown into a film to obtain an antibacterial and biodegradable film.

[0005] Optionally, the mass ratio of eugenol to PBAT is (1-5):100; The molar ratio of maleic anhydride to eugenol is (1.0-1.2):1.

[0006] Optionally, the esterification reaction is carried out at a temperature of 140–150°C for a reaction time of 3–8 min.

[0007] Optionally, the amount of BIBP used in the free radical grafting reaction is 0.5 to 1.0 wt% of the mass of PBAT. The free radical grafting reaction is carried out at a temperature of 170–180°C for a reaction time of 3–8 min.

[0008] Optionally, the mass ratio of PLA to PBAT-g-eugenol is 6:4 to 9:1; The amount of BIBP used in the melt crosslinking blend is 0.3–0.6 wt% of the total mass of PLA and PBAT-g-eugenol. The temperature for the melt crosslinking blend is 170–180°C, and the time is 4–8 min.

[0009] Optionally, before mixing the PBAT-g-eugenol and PLA, the method further includes: cooling and granulating the PBAT-g-eugenol; Before extruding and blowing the PLA / PBAT-g-eugenol crosslinked blend into a film, the process further includes cooling and pelletizing the PLA / PBAT-g-eugenol crosslinked blend.

[0010] Optionally, the process parameters for the extrusion blown film forming include: barrel temperatures from the feed inlet to the die head are 150-155℃, 160-165℃, 165-170℃, and 170-175℃ respectively; die head temperature is 170-175℃; screw speed is 40-80 rpm; die gap is 0.8-1.2 mm; blow-up ratio is 2.5-4.0; draw ratio is 3-6; cooling air temperature is 15-25℃; frost line height is 2-4 times the die diameter; and draw speed is 2-5 m / min.

[0011] Optionally, before melting PBAT, the process also includes: PBAT, eugenol, maleic anhydride and BIBP were vacuum dried separately to control the moisture content to ≤0.02wt%.

[0012] Optionally, during the melt crosslinking blending process, the degree of crosslinking is monitored by the change in mixing torque, and the reaction is stopped when the equilibrium torque rises to 1.4 to 1.8 times the initial value.

[0013] On the other hand, the present invention also provides an antibacterial biodegradable film, which is prepared by any of the above-described preparation methods.

[0014] In the preparation method of the antibacterial biodegradable film of the present invention, a two-step crosslinking compatibilization strategy is adopted to prepare PLA / PBAT-g-eugenol crosslinked blends: First, the quenching effect of phenolic hydroxyl groups on free radicals is eliminated by esterification of maleic anhydride with the phenolic hydroxyl groups of eugenol. Then, a free radical grafting reaction is initiated by BIBP to introduce the antibacterial active unit eugenol onto the PBAT molecular chain, thus obtaining a PBAT-g-eugenol graft copolymer. Second, using BIBP as a crosslinking initiator, PLA-PBAT covalent crosslinking bonds are formed at the interface between PLA and PBAT-g-eugenol, constructing a three-dimensional crosslinking network to obtain the PLA / PBAT-g-eugenol crosslinked blend. Through the above two-step crosslinking compatibilization strategy, an antibacterial biodegradable film with both excellent mechanical properties and long-lasting antibacterial function can be prepared.

[0015] Furthermore, in the antibacterial biodegradable film of the present invention, the film thickness is 30~80μm; the film has an antibacterial rate of ≥90% against Staphylococcus aureus and Escherichia coli, and the migration rate of eugenol is <5% after 30-day accelerated migration test; the longitudinal tensile strength is ≥30MPa, the longitudinal elongation at break is ≥150%, the haze is <20%, and the light transmittance is ≥85%.

[0016] The above and other objects, advantages and features of the present invention will become more apparent to those skilled in the art from the following detailed description of specific embodiments of the invention in conjunction with the accompanying drawings. Attached Figure Description

[0017] The following sections will describe some specific embodiments of the invention in detail by way of example and not limitation, with reference to the accompanying drawings. The same reference numerals in the drawings denote the same or similar parts or portions. Those skilled in the art should understand that these drawings are not necessarily drawn to scale. In the drawings: Figure 1 This is a schematic flowchart illustrating a method for preparing an antibacterial biodegradable film according to an embodiment of the present invention. Detailed Implementation

[0018] In the description of this embodiment, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0019] Figure 1 This is a schematic flowchart illustrating a method for preparing an antibacterial biodegradable film according to an embodiment of the present invention, as shown below.Figure 1 As shown in the figure, this invention provides a method for preparing an antibacterial biodegradable film, which may include the following steps: S100, Preparation of PBAT-g-eugenol: After melting PBAT, eugenol and maleic anhydride are added to allow eugenol and maleic anhydride to undergo an esterification reaction to form eugenol maleic acid monoester; then BIBP is added to carry out a free radical grafting reaction to graft the eugenol maleic acid monoester onto the PBAT molecular chain to obtain PBAT-g-eugenol.

[0020] S200, Preparation of cross-linked blends: After mixing PBAT-g-eugenol and PLA, BIBP is added for melt cross-linking blending to form covalent cross-linking bonds at the interface between PLA and PBAT-g-eugenol, thus obtaining PLA / PBAT-g-eugenol cross-linked blends.

[0021] S300, Preparation of antibacterial and biodegradable film: Cross-linked blends are extruded and blown into film to obtain antibacterial and biodegradable film.

[0022] Specifically, "PBAT-g-eugenol" refers to a eugenol-grafted PBAT copolymer, where "g" indicates grafting. PBAT is used as the matrix component, providing flexibility; PLA is used as the matrix component, providing rigidity; eugenol is used as a natural antibacterial monomer; maleic anhydride is used as an esterifying agent, protecting the phenolic hydroxyl groups and introducing double bonds; and BIBP is used as a free radical initiator or crosslinking agent.

[0023] In this embodiment, a two-step cross-linking compatibilization strategy is adopted, which involves chemically grafting PBAT with eugenol and then further cross-linking it with PLA to prepare a PLA / PBAT-g-eugenol antibacterial biodegradable film with excellent mechanical properties and antibacterial function.

[0024] In step S100, the chemical grafting of eugenol onto PBAT is achieved: by using the esterification reaction of maleic anhydride and the phenolic hydroxyl group of eugenol, the quenching effect of the phenolic hydroxyl group on free radicals is eliminated, and an antibacterial active unit is introduced into the PBAT molecular chain to obtain PBAT-g-eugenol.

[0025] Step S200 constructs a PLA / PBAT-g-eugenol three-dimensional cross-linked network: using BIBP as a cross-linking initiator, PLA-PBAT covalent cross-linking bonds are formed at the PLA and PBAT-g-eugenol interface, which solves the problem of debonding at the interface of the two phases from the root, and simultaneously realizes interface compatibilization, melt strengthening and further anchoring of antibacterial units.

[0026] Step S300 achieves the preparation of a high-performance antibacterial and biodegradable film: through extrusion blown film forming, an antibacterial and biodegradable film with high tensile strength, high elongation at break, high light transmittance and long-lasting antibacterial effect is obtained, providing a green alternative for the field of flexible packaging.

[0027] In some embodiments of the present invention, PBAT is commercial grade polybutylene adipate / terephthalate with a melt index of 3-5 g / 10 min (190°C, 2.16 kg).

[0028] PLA is commercial-grade polylactic acid with a melt index of 5–10 g / 10 min (190℃, 2.16 kg) and a weight-average molecular weight of 100,000–200,000 g / mol.

[0029] Eugenol was of analytical grade, with a purity ≥98% and a molecular weight of 164.2 g / mol.

[0030] Maleic anhydride was of analytical grade, with a purity ≥99% and a molecular weight of 98.1 g / mol.

[0031] BIBP is industrial grade with a purity of ≥98% (odorless DCP).

[0032] In some embodiments, before mixing the PBAT-g-eugenol and PLA, the preparation method further includes: cooling and granulating the PBAT-g-eugenol.

[0033] Before extruding and blowing the PLA / PBAT-g-eugenol crosslinked blend into a film, the preparation method further includes: cooling and pelletizing the PLA / PBAT-g-eugenol crosslinked blend.

[0034] In some embodiments of the present invention, in step S100, the mass ratio of eugenol to PBAT is (1-5):100; the molar ratio of maleic anhydride to eugenol is (1.0-1.2):1.

[0035] Specifically, the amount of eugenol directly affects the antibacterial and mechanical properties of the film, while the amount of maleic anhydride directly affects the protective effect of the phenolic hydroxyl groups and the efficiency of subsequent grafting reactions. In this embodiment, by limiting the mass ratio of eugenol to PBAT to (1-5):100 and the molar ratio of maleic anhydride to eugenol to (1.0-1.2):1, the phenolic hydroxyl groups of eugenol are completely esterified and protected by maleic anhydride, eliminating the quenching effect of phenolic hydroxyl groups on free radicals. The free radicals generated by the decomposition of BIBP can efficiently initiate the grafting reaction, grafting eugenol units onto the PBAT molecular chain via covalent bonds, resulting in the highest grafting rate. The obtained PBAT-g-eugenol graft copolymer has a moderate loading of antibacterial active units, ensuring both the long-lasting antibacterial function of the film and maintaining excellent mechanical properties.

[0036] In some embodiments of the present invention, the esterification reaction temperature is 140–150°C and the reaction time is 3–8 min.

[0037] Specifically, the esterification temperature affects the protection of phenolic hydroxyl groups, while the reaction time affects the esterification efficiency. In this embodiment, the esterification temperature is limited to 140–150°C and the reaction time to 3–8 min. This temperature is higher than the melting point of PBAT (approximately 120–130°C), ensuring that all components melt sufficiently and that the reaction time is sufficient for complete esterification. At the same time, it avoids excessively long reaction times that could lead to thermal degradation of PBAT, resulting in a high esterification rate and complete protection of phenolic hydroxyl groups, thus balancing reaction efficiency and product quality.

[0038] In some embodiments of the present invention, the amount of BIBP used in the free radical grafting reaction is 0.5 to 1.0 wt% of the mass of PBAT; the temperature of the free radical grafting reaction is 170 to 180°C, and the reaction time is 3 to 8 min.

[0039] Specifically, the amount of BIBP used affects the grafting reaction efficiency, while temperature and time affect the BIBP decomposition rate and grafting degree. This embodiment, through the above limitations, ensures that BIBP fully decomposes to generate free radicals, initiating an efficient grafting reaction with a moderate grafting rate. Simultaneously, it avoids excessive cross-linking due to excessive dosage or insufficient grafting due to insufficient dosage, thus balancing grafting efficiency and product performance.

[0040] In some embodiments of the present invention, the mass ratio of PLA to PBAT-g-eugenol is 6:4 to 9:1. For example, the mass ratio of PLA to PBAT-g-eugenol is 6:4, 7:3, 8:2 or 9:1.

[0041] This embodiment achieves a balance between the rigidity of PLA and the toughness of PBAT-g-eugenol by limiting the mass ratio of PLA to PBAT-g-eugenol, while ensuring a moderate crosslinking network density, thus taking into account both the mechanical properties and blown film stability of the film.

[0042] In some embodiments of the present invention, the amount of BIBP used in the melt crosslinking blend is 0.3 to 0.6 wt% of the total mass of PLA and PBAT-g-eugenol. The melt crosslinking blending temperature is 170 to 180°C, and the time is 4 to 8 minutes.

[0043] Specifically, the amount of BIBP affects the crosslinking density, while temperature and time affect the degree of crosslinking reaction. In this embodiment, by limiting the amount of BIBP to 0.3–0.6 wt% of the total mass of PLA and PBAT-g-eugenol, the melt crosslinking temperature to 170–180°C, and the time to 4–8 min, a moderate crosslinking density is achieved, balancing interfacial compatibilization and melt strength, while maintaining melt processability and avoiding poor mechanical properties due to insufficient crosslinking or loss of flowability due to excessive crosslinking.

[0044] In some embodiments, the process parameters for extrusion blown film forming include: barrel temperatures from the feed inlet to the die head are 150–155°C, 160–165°C, 165–170°C, and 170–175°C respectively; die head temperature is 170–175°C; screw speed is 40–80 rpm; die gap is 0.8–1.2 mm; blow-up ratio is 2.5–4.0; draw ratio is 3–6; cooling air temperature is 15–25°C; frost line height is 2–4 times the die diameter; and draw speed is 2–5 m / min.

[0045] This embodiment, by limiting the above-mentioned extrusion blown film process parameters, enables the crosslinked blend to be gradually plasticized, uniformly extruded, stably blown, and uniformly cooled during the extrusion blown film process. This results in a film bubble that does not rupture or wrinkle, a uniform film thickness, and balanced longitudinal and transverse orientation, balancing the film's mechanical and optical properties with continuous production stability. In other words, within this parameter range, the crosslinked network provides sufficient melt strength, enabling stable blown film production even with a high PLA content system. The resulting film has a thickness of 30–80 μm, balanced longitudinal and transverse tensile strength, low haze, and high light transmittance, allowing for continuous and stable production.

[0046] In some embodiments of the present invention, before “PBAT melting”, the method for preparing the antibacterial biodegradable film further includes the following steps: vacuum drying PBAT, eugenol, maleic anhydride and BIBP respectively, and controlling the water content to ≤0.02wt%.

[0047] Specifically, because PBAT and PLA molecular chains contain a large number of ester bonds (-COO-), at high molten states (>170℃), oxygen atoms in water molecules act as nucleophiles, attacking the carbonyl carbon of the ester bonds, initiating hydrolysis and chain scission, thus reducing the polymer's molecular weight. This polyester hydrolysis reaction exhibits autocatalytic properties—the generated carboxyl end groups further accelerate the hydrolysis. When the water content is >0.02wt%, the PLA molecular weight can decrease by 10-30% within 10 minutes; therefore, the water content must be strictly controlled below 0.02wt%.

[0048] Furthermore, the anhydride bond (-COOCO-) of maleic anhydride is highly sensitive to water. In humid environments, water molecules attack the carbonyl carbon of the anhydride, causing it to undergo ring-opening hydrolysis to form maleic acid, which cannot undergo esterification with eugenol. Therefore, maleic anhydride must be stored in a sealed container after drying and used quickly.

[0049] Through the above steps, this embodiment can effectively prevent the hydrolysis and chain breakage of PLA and PBAT ester bonds caused by moisture during high-temperature processing, ensuring the efficiency of grafting and crosslinking reactions, while avoiding membrane bubble rupture and film pinholes caused by water vapor during blown film.

[0050] In some embodiments, during the melt crosslinking blending process, the degree of crosslinking is monitored by changes in the mixing torque, and the reaction is stopped when the equilibrium torque rises to 1.4 to 1.8 times the initial value. Through the above steps, the crosslinking density can be precisely controlled within a suitable range, ensuring sufficient interfacial compatibilization and melt strengthening effects while maintaining melt processability, and avoiding poor mechanical properties due to insufficient crosslinking or loss of flowability due to excessive crosslinking.

[0051] This invention also provides an antibacterial biodegradable film, which is prepared by any of the above-described methods.

[0052] To further illustrate the present invention, the following detailed description is provided in conjunction with specific embodiments.

[0053] Example 1 A method for preparing an antibacterial and biodegradable film includes the following steps: S100, Preparation of PBAT-g-eugenol: S110, Raw material drying pretreatment: Place PBAT granules in a vacuum drying oven and dry at 70℃ for 15 hours; eugenol, maleic anhydride, and BIBP are vacuum dried at 40℃ for 4 hours, 4 hours, and 8 hours, respectively. All raw materials are sealed and stored after drying, and weighed after cooling to room temperature before use. Maleic anhydride must be quickly weighed after cooling in a desiccator and used immediately to prevent moisture absorption and hydrolysis. The moisture content of all raw materials must be controlled to ≤0.02wt%.

[0054] S120, Esterification reaction: Preheat the internal mixer to 140℃, rotor speed 40rpm. Add 50.0g of dried PBAT to the internal mixer and pressurize and melt plasticize for 2min. After the PBAT is completely melted, add the pre-mixed eugenol (1.0g, 2wt% of PBAT) and maleic anhydride (0.7g, molar ratio to eugenol 1.17:1), and react for 5min at 140℃~150℃ and 40rpm.

[0055] Specifically, the phenolic hydroxyl group (-OH) of eugenol undergoes a nucleophilic acyl substitution reaction with maleic anhydride. The oxygen atom of the phenolic hydroxyl group attacks the carbonyl carbon of the maleic anhydride, causing the anhydride to open its ring and form eugenol maleic acid monoester. The reaction formula is as follows: .

[0056] This reaction achieves three functions: First, the phenolic hydroxyl group is converted into an ester bond, completely losing its free radical quenching ability; second, after maleic anhydride ring-opening, it retains the C=C double bond, providing an active site for subsequent grafting; third, the product is connected to eugenol at one end and contains an active double bond at the other end, acting as a "molecular bridge".

[0057] S130, Temperature transition: Raise the internal mixer temperature from 140℃ to 175℃ in about 2 minutes, while maintaining the speed at 40 rpm.

[0058] Specifically, BIBP decomposes extremely slowly at 140°C, with a half-life lasting several hours, making it ineffective at providing free radicals. When the temperature rises above 170°C, the peroxy bonds in the BIBP molecule absorb heat and undergo homolytic cleavage, shortening the half-life to 1–2 minutes. 175°C is the temperature at which BIBP has a 1-minute half-life, meaning that approximately 50% of the BIBP molecules decompose to generate free radicals every minute. Raising the temperature to 175°C is to rapidly decompose BIBP, providing sufficient free radicals for subsequent grafting reactions.

[0059] The 2-minute rapid heating shortens the residence time of the material in the intermediate temperature range, reducing the thermo-oxidative degradation of PBAT.

[0060] S140, free radical grafting reaction: After the temperature is raised to 175℃, BIBP (0.375g, 0.75wt% of PBAT) is added, and the mixture is continued to be kneaded at 175℃ and 50rpm for 5min. The change in kneading torque is closely observed, and the reaction is stopped when the torque tends to stabilize (total kneading time is about 15min).

[0061] Specifically, this step involves three consecutive reactions: (1) The peroxide bond in the BIBP molecule undergoes homolytic cleavage at 175℃, generating two highly reactive alkoxy radicals; the reaction formula is: .

[0062] (2) The alkoxy radical abstracts a hydrogen atom from the CH bond of the PBAT molecular chain and is reduced to a stable alcohol molecule (RH). A macromolecular radical (PBAT•) is formed on the PBAT backbone. Hydrogen abstraction preferentially occurs on the methylene carbon (-COO-CH2-) adjacent to the ester group. The reaction formula is: .

[0063] (3) The free radicals of the PBAT macromolecule attack the C=C double bond of eugenol maleic acid monoester, resulting in free radical addition and the formation of a new C-C covalent bond. This grafts the eugenol unit onto the PBAT backbone, achieving chemical anchoring of the antibacterial unit. The reaction formula is: .

[0064] The change in mixing torque is the main indicator of reaction progress. As grafting and cross-linking proceed, the molecular weight and viscosity of the system increase, and the torque continues to rise. When the torque tends to stabilize, it indicates that BIBP has been basically decomposed and the reaction is complete, at which point the material can be discharged.

[0065] S150, Discharge, Cooling and Pelletizing: Remove the molten material at approximately 155°C and place it on a cooling tray to cool rapidly to room temperature.

[0066] Specifically, rapid cooling quickly "freezes" the molecular chain conformation and cross-linking / grafting structure in the high-temperature molten state, preventing residual heat from continuing to drive side reactions (such as further cross-linking or thermal degradation) after discharge, while reducing oxidative discoloration in a high-temperature aerobic environment.

[0067] The cooled product was crushed into uniform particles of 3-5 mm by a pelletizer, dried under vacuum at 70°C for 6 hours, sealed and stored away from light, and labeled as PBAT-g-eugenol.

[0068] S200, preparation of cross-linked blends: S210, Drying Pretreatment: Place PLA granules and PBAT-g-eugenol granules prepared in step S100 separately in a vacuum drying oven and dry at 70℃ for 6 hours. BIBP is vacuum dried at 40℃ for 8 hours. Ensure that the moisture content of all raw materials is ≤0.02wt%.

[0069] Specifically, PLA has a higher hydrolysis rate than PBAT. Besides thermal degradation, hydrolysis is the primary pathway for the decrease in PLA's molecular weight at high temperatures. The tertiary C-hydrogen atoms on the PLA backbone give the adjacent carbonyl carbons of the ester bonds a higher positive charge, making them more susceptible to water molecule attack. The carboxyl end groups generated during hydrolysis can autocatalyze the hydrolysis of more ester bonds, forming a positive feedback degradation chain. The water content must be controlled below 0.02 wt% to ensure the retention of PLA's molecular weight.

[0070] S220, Melt Crosslinking Blending: Preheat the internal mixer to 175℃, rotor speed 60rpm. Premix 35.0g of dry PLA and 15.0g of dry PBAT-g-eugenol (mass ratio 7:3) evenly, then add them to the internal mixer and pressurize for melt plasticization for 2 minutes. After the matrix is ​​completely melted, add BIBP (0.225g, i.e., 0.45wt% of the total matrix mass), and continue internal mixing at 175℃ and 60rpm for 5.5 minutes.

[0071] Specifically, the role of this step is to initiate the PLA / PBAT-g-eugenol interfacial crosslinking reaction via BIBP, which involves five consecutive processes: (1) BIBP thermal decomposition produces alkoxy radicals; (2) Alkoxy radicals simultaneously abstract hydrogen atoms in both the PLA and PBAT-g-eugenol phases, generating two types of macromolecular radicals: PLA· and PBAT-g-eugenol·. ; BIBP, as a small molecule (molecular weight of about 338 g / mol), has a certain solubility in both PLA and PBAT and can be uniformly distributed in the two phases under shear action.

[0072] (3) When PLA· and PBAT-g-eugenol· meet at the interface, unpaired electron spin coupling forms a new C-C covalent bond: ; The covalent bond energy is about 350 kJ / mol, which is two orders of magnitude higher than the van der Waals force of physical compatibilizers (about 5~10 kJ / mol), fundamentally eliminating the possibility of interfacial debonding.

[0073] (4) Free radicals of the same macromolecule can also couple to form cross-linked networks within each phase: ; Homogeneous crosslinking has three functions: first, it enhances melt strength and provides stable film bubbles for blown film; second, it compensates for the loss of molecular weight due to thermal degradation during high-temperature processing of PLA; and third, it further locks the eugenol units into the three-dimensional network, reducing the migration rate.

[0074] (5) Monitor the change in internal mixing torque in real time. Stop the reaction and discharge the material when the equilibrium torque rises to 1.6 times the initial value. A torque of 1.6 times the initial value corresponds to a gel content of about 20%. This crosslinking density can provide sufficient interfacial compatibilization and melt strengthening effects while maintaining the processability of the melt. Crosslinking is insufficient if it is below 1.3 times, and excessive crosslinking if it is above 2.0 times, which leads to a serious decrease in melt fluidity.

[0075] S230, Discharge, Cooling and Pelletizing: Remove the molten blend at approximately 160°C and rapidly cool it to room temperature on a cooling tray.

[0076] Specifically, the purpose of rapid cooling is to "lock in" the cross-linked network structure. At high temperatures, the molecular chains in the cross-linked network have high mobility. If the cooling rate is too slow, the network structure may rearrange or loosen, reducing the cross-linking efficiency. Rapid cooling can reduce the time from 175°C to room temperature to within 1-2 minutes, effectively fixing the network structure.

[0077] The material was crushed into uniform particles of 3-5 mm by a pelletizer and then vacuum dried at 70℃ for 6 hours. This material was designated as "crosslinked PLA / PBAT-g-eugenol blend".

[0078] S300, for preparing antibacterial and biodegradable films: S310, Extrusion Blown Film: The dried cross-linked blend granules are added to the hopper of a single-screw extrusion blown film mill, and blown film is performed according to the following parameters: The barrel temperatures from the feed inlet to the die head are 152℃ (barrel zone 1), 162℃ (barrel zone 2), 167℃ (barrel zone 3), and 172℃ (barrel zone 4), with the die head temperature at 172℃.

[0079] The screw speed is 60 rpm, the die opening gap is 1.0 mm, the blow-up ratio is 3.0, the traction ratio is 4.0, the cooling air temperature is 20℃, the frost line height is 3 times the die opening diameter, and the traction speed is 3 m / min.

[0080] The melt is extruded into a tube blank through an annular die, blown into a film bubble by compressed air, cooled and shaped by an air ring, gathered by a herringbone plate, sizing by traction clamping rollers, and wound up under constant tension by a winding device to obtain a tubular film.

[0081] Specifically, this step involves physical / physicochemical processes such as melt plasticizing, biaxial stretching orientation, cooling crystallization, and cross-linking network strengthening.

[0082] During the melt plasticizing process, the cross-linked blend particles undergo three stages in the extruder barrel: solid conveying, melt compression, and melt homogenization. The temperature gradually increases from 152℃ to 172℃, ensuring that PLA and PBAT-g-eugenol are completely melted and uniformly mixed. The temperature in each stage is controlled below 175℃ to prevent the continued decomposition of residual BIBP, which could lead to excessive cross-linking, and to avoid a sudden increase in melt viscosity, excessive extrusion pressure, or even melt rupture.

[0083] During the membrane bubble inflation and biaxial stretching orientation process, the melt is extruded into a tube blank through an annular die. Compressed air causes it to expand radially (expansion ratio 3.0), while traction rollers apply axial stretching (traction ratio 4.0), achieving biaxial stretching. Molecular chains align along the MD and TD directions. The orientation enhancement mechanism is as follows: the alignment of molecular chains along the force direction increases the number of covalent bonds bearing the stress, thus improving tensile strength; orientation induces crystallization, with crystalline regions acting as physical cross-linking points to strengthen the network; the orientation structure reduces stress concentration and delays crack propagation. The cross-linking network restricts long-range slip of molecular chains, resulting in more uniform orientation, and the cross-linking points "freeze" the orientation structure, reducing the tendency for shrinkage.

[0084] During the cooling and crystallization process of the membrane bubble, the air ring outputs 20°C cooling air to lower the temperature of the membrane bubble. The frost line is the position where the melt crystallizes and solidifies. If the frost line is too high, it will cause the orientation molecular chains to loosen and the membrane bubble to sag and become unstable; if the frost line is too low, it will cause excessively rapid cooling, insufficient crystallization, and brittle film. The cross-linking network improves the melt's resistance to sag and tearing, and significantly enhances the stability of the membrane bubble; it also widens the processing window, improves thickness uniformity, allows for higher blow-up ratios, and facilitates the production of thinner films.

[0085] S320, Finished Product Storage: Store the rolled-up tubular film in a sealed, dry place away from light.

[0086] Specifically, the allyl double bond in the eugenol molecule can absorb ultraviolet light (wavelength 280–320 nm) under illumination, undergoing a photo-oxidation reaction to generate peroxides and carbonyl compounds, leading to a darkening of the film color and a decrease in antibacterial activity. Storage away from light can effectively inhibit this photo-oxidation reaction. Sealed and dry storage can prevent moisture absorption by the film, which can cause hydrolytic degradation of PLA and changes in film size.

[0087] Performance testing: The thin film samples prepared in Example 1 were subjected to performance tests, including film thickness, mechanical properties, optical properties, antibacterial properties, and eugenol migration. The test methods and sampling requirements are as follows: (1) Film thickness: in accordance with GB / T 6672-2001, with 5 parallel samples per group.

[0088] (2) Mechanical properties: Performed in accordance with GB / T 1040.3-2006, longitudinal tensile strength, longitudinal elongation at break, transverse tensile strength and transverse elongation at break were tested respectively, with 5 parallel samples in each group.

[0089] (3) Optical performance: The haze and transmittance were tested according to GB / T 2410-2008, with 3 parallel samples in each group.

[0090] (4) Antibacterial properties: Performed in accordance with GB / T 31402-2015, using Staphylococcus aureus and Escherichia coli as test species, with 3 parallel samples for each species.

[0091] (5) Migration rate: The migration test method for food contact materials was followed, with 30 days of accelerated migration conditions and 3 parallel samples.

[0092] Table 1. Test results of the mechanical and optical properties of the thin film in Example 1 Note: 1. Longitudinal (MD) is the film traction direction, and transverse (TD) is the blowing direction; 2. Three parallel samples are used for haze and transmittance, so parallel samples 4 and 5 are indicated by "-"; 3. The average value in the table is the arithmetic mean of each parallel sample.

[0093] Table 2. Test results of antibacterial properties and migration rate of the film in Example 1. Note: 1. The inhibition rates of Staphylococcus aureus (Gram-positive) and Escherichia coli (Gram-negative) were determined after inoculation and culture according to GB / T31402-2015; 2. The migration rate is the percentage of eugenol migrated from the film to the simulated food medium under accelerated migration conditions for 30 days, relative to the total amount of eugenol in the film; 3. The average values ​​in the table are the arithmetic mean of all parallel samples.

[0094] As shown in Tables 1 and 2, the film thickness obtained in this embodiment is 30μm~45μm; longitudinal tensile strength is 38.5MPa, transverse tensile strength is 32.1MPa; longitudinal elongation at break is 185%, transverse elongation at break is 210%; haze is 14.8%, light transmittance is 86.3%; the antibacterial rate against Staphylococcus aureus and Escherichia coli is ≥90%; and the eugenol migration rate is <5% after 30-day accelerated migration test. The film bubble is stable, without wrinkles or bubble breakage, and can be continuously and stably wound up.

[0095] Therefore, those skilled in the art should recognize that although numerous exemplary embodiments of the present invention have been shown and described in detail herein, many other variations or modifications conforming to the principles of the present invention can be directly determined or derived from the disclosure of the present invention without departing from the spirit and scope of the invention. Thus, the scope of the present invention should be understood and construed as covering all such other variations or modifications.

Claims

1. A method for preparing an antibacterial and biodegradable film, characterized in that, include: After PBAT is melted, eugenol and maleic anhydride are added to induce an esterification reaction between eugenol and maleic anhydride to form eugenol maleic acid monoester. Then, BIBP was added to carry out a free radical grafting reaction to graft eugenol maleic acid monoester onto the PBAT molecular chain to obtain PBAT-g-eugenol. After mixing PBAT-g-eugenol and PLA, BIBP is added for melt crosslinking blending to form covalent crosslinking bonds at the interface between PLA and PBAT-g-eugenol, thus obtaining PLA / PBAT-g-eugenol crosslinked blend. The PLA / PBAT-g-eugenol crosslinked blend was extruded and blown into a film to obtain an antibacterial and biodegradable film.

2. The preparation method according to claim 1, characterized in that, The mass ratio of eugenol to PBAT is (1-5):100; The molar ratio of maleic anhydride to eugenol is (1.0-1.2):

1.

3. The preparation method according to claim 1, characterized in that, The esterification reaction is carried out at a temperature of 140–150°C for a reaction time of 3–8 minutes.

4. The preparation method according to claim 1, characterized in that, The amount of BIBP used in the free radical grafting reaction is 0.5–1.0 wt% of the mass of PBAT. The free radical grafting reaction is carried out at a temperature of 170–180°C for a reaction time of 3–8 min.

5. The preparation method according to claim 1, characterized in that, The mass ratio of PLA to PBAT-g-eugenol is 6:4 to 9:1; The amount of BIBP used in the melt crosslinking blend is 0.3–0.6 wt% of the total mass of PLA and PBAT-g-eugenol. The temperature for the melt crosslinking blend is 170–180°C, and the time is 4–8 min.

6. The preparation method according to claim 1, characterized in that, Before mixing the PBAT-g-eugenol and PLA, the method further includes: cooling and granulating the PBAT-g-eugenol; Before extruding and blowing the PLA / PBAT-g-eugenol crosslinked blend into a film, the process further includes cooling and pelletizing the PLA / PBAT-g-eugenol crosslinked blend.

7. The preparation method according to claim 1, characterized in that, The process parameters for extrusion blown film forming include: barrel temperatures from the feed inlet to the die head are 150-155℃, 160-165℃, 165-170℃, and 170-175℃ respectively; die head temperature is 170-175℃; screw speed is 40-80 rpm; die gap is 0.8-1.2 mm; blow-up ratio is 2.5-4.0; draw ratio is 3-6; cooling air temperature is 15-25℃; frost line height is 2-4 times the die diameter; and draw speed is 2-5 m / min.

8. The preparation method according to claim 1, characterized in that, Before melting PBAT, the process also includes: PBAT, eugenol, maleic anhydride and BIBP were vacuum dried separately to control the moisture content to ≤0.02wt%.

9. The preparation method according to claim 1, characterized in that, During the melt crosslinking blending process, the degree of crosslinking is monitored by the change in mixing torque. The reaction is stopped when the equilibrium torque rises to 1.4 to 1.8 times the initial value.

10. An antibacterial biodegradable film, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 9.