Broadband high-solar-absorption composite film and preparation method thereof
By electrochemically depositing polypyrrole and carboxylated carbon nanotubes under a constant magnetic field, a composite film with a multi-level high curvature microstructure is formed, which solves the problem of insufficient absorption of polypyrrole-based materials in the near-infrared band and achieves efficient photothermal conversion and anti-icing effects across the entire band. It is suitable for wind power, power grid, aviation and other fields.
Patent Information
- Application Number
- CN202611586785.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-24
AI Technical Summary
In existing photothermal de-icing technologies, polypyrrole-based materials have insufficient absorption capacity in the near-infrared band, making it difficult to achieve efficient photothermal conversion across the entire band. Furthermore, the preparation process is inefficient, making it difficult to promote on a large scale in industrial applications.
Under a constant magnetic field, a multi-level high-curvature microstructure is formed by electrochemically depositing polypyrrole and carboxylated carbon nanotube composite materials. Combined with a magnetic field-controlled light trap structure, a wide-band high absorption is achieved, and the preparation time is shortened.
It significantly improves the light absorption rate of the composite film across the entire wavelength range, enhances the photothermal conversion efficiency, delays icing and accelerates melting, and is suitable for large-scale industrial production.
Smart Images

Figure CN123152142A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photothermal materials technology, and particularly relates to a composite film with wide-band high absorption of sunlight and its preparation method. Background Technology
[0002] In industrial and critical infrastructure, ice accumulation can cause serious safety hazards and economic losses, such as leading to the collapse of power transmission line towers, reduced efficiency of wind turbine blades, and damage to aircraft flight safety. Traditional de-icing technologies to address this problem include mechanical de-icing, electrothermal de-icing, chemical de-icing, and manual de-icing. However, these methods have significant limitations, including easy damage to the substrate, high energy consumption, dependence on external power sources, high costs, environmental pollution and facility corrosion, low efficiency, and high risks. In contrast, solar thermal de-icing technology based on solar energy conversion has become a research hotspot due to its high energy efficiency, low operating costs, strong sustainability, and ease of remote control. This technology mainly utilizes photothermal materials to convert solar energy into heat energy, raising the surface temperature through the photothermal effect to delay ice nucleation or accelerate ice melting. Among many photothermal materials, polypyrrole is widely used due to its readily available raw materials, simple synthesis, good chemical stability, high conductivity, and excellent light absorption properties. By combining polypyrrole with materials such as carbon nanotubes with wide-bandgap light absorption characteristics, the photothermal conversion performance of the materials can be further improved.
[0003] From a technical implementation perspective, existing photothermal anti-icing and de-icing technologies primarily construct photothermal coatings by selecting suitable photothermal media and preparation processes. On one hand, the conductive polymer properties of polypyrrole are utilized to introduce other photothermal components through doping or compositing to compensate for its insufficient spectral absorption range; on the other hand, active materials are loaded onto a substrate using methods such as electrochemical deposition. Furthermore, to improve light capture efficiency, existing technologies also attempt to utilize the micro-nano rough structures on the material surface to induce multiple scattering and reflection of light, thereby extending the optical path. Although existing polypyrrole-based materials have developed rapidly, they still face many problems and shortcomings in practical applications. These problems mainly limit further improvements in photothermal conversion efficiency and optimization of preparation processes.
[0004] First, existing polypyrrole-based materials have significant shortcomings in achieving maximum photothermal conversion efficiency, particularly in the absorption and utilization of near-infrared light. Approximately 43% of the solar spectrum's energy is distributed in the near-infrared band. Due to the longer wavelength and stronger penetrating power of photons in this band, existing polypyrrole materials, limited by their band structure, struggle to effectively capture these low-energy photons, thus restricting their full-spectrum absorption efficiency of solar radiation. This inadequacy in utilizing near-infrared light severely hinders breakthroughs in the overall photothermal conversion efficiency of these materials and limits their application in demanding anti-icing scenarios requiring high absorbance and conversion rates. While materials such as carbon nanotubes perform excellently in the near-infrared region, effectively combining them with polypyrrole to maximize this characteristic remains a challenge for current technologies.
[0005] Secondly, from the perspective of microstructure and morphology control, existing technologies struggle to precisely construct composite film structures with high light absorption rates. Light absorption capacity is closely related to microstructure and surface morphology; complex micro / nano rough structures can induce multiple scattering and reflection of light within the material, thereby significantly improving light-harvesting efficiency. However, in conventional electropolymerization processes, there is a lack of effective control methods to precisely manage the ordered assembly of nanosheets or particles, making it difficult to construct ideal macroscopic roughness and microscopic hierarchical structures. Existing preparation strategies are often limited to adjusting chemical components or single electric field parameters, failing to deeply intervene in the mass transfer rate and reaction kinetics during the reaction process. This results in suboptimal product structures, limiting further improvements in light-harvesting efficiency.
[0006] Finally, existing technologies suffer from low efficiency in the fabrication process. To obtain high-performance photothermal coatings, a relatively long reaction time is often required to ensure film quality. This is mainly because the mass transfer rate at the electrode surface is relatively slow during traditional electrochemical deposition, and there is a lack of effective external energy input to accelerate the reaction process. Although introducing external physical fields to assist fabrication is considered a potential solution, how to effectively couple physical fields such as magnetic fields into the electropolymerization system to achieve high-quality film fabrication in a shorter time remains an unresolved technical challenge. This bottleneck in fabrication efficiency also hinders the large-scale application of high-performance photothermal anti-icing and de-icing technologies. Summary of the Invention
[0007] This invention proposes a composite film with high absorption of sunlight across a wide wavelength range and its preparation method. The invention aims to improve upon the shortcomings of traditional polypyrrole / carbon nanotube composite films, such as insufficient near-infrared absorption and low absorbance across the entire wavelength range. It produces a composite film that achieves high absorption in the 200–2500 nm ultraviolet-visible-near-infrared range. Simultaneously, it addresses the difficulties of precisely controlling the multi-level microscopic roughness of the material's microstructure and effectively constructing light trap structures in conventional electropolymerization processes. This shortens the electropolymerization preparation time, improves film uniformity to suit large-scale industrial production, and enhances the material's comprehensive performance in both light- and dark environments, delaying icing and accelerating melting. It can be applied long-term to anti-icing scenarios in wind power, power grids, and aviation-related substrates. Furthermore, the composite film possesses optical isotropic characteristics, unaffected by the angle of sunlight incidence, and maintains a stable photothermal conversion output effect.
[0008] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing a composite film with wide-band high absorption of sunlight, comprising the following steps: In a constant magnetic field environment, the working electrode and the counter electrode are immersed in a mixture of pyrrole, sodium perfluorononenoxybenzenesulfonate, carboxylated carbon nanotubes, ethanol and water, and deposition is carried out under constant current density. After deposition, the product is cleaned and dried to obtain the composite film with wide-band high absorption of sunlight.
[0009] The core of this invention's performance enhancement of the broadband high-absorption solar composite film lies in the ingenious synergy between the intrinsic properties of the material and the magnetically modulated microstructure. The specific principle is as follows: First: the intrinsic broadband absorption capability of the material This is primarily attributed to two key materials in the composite film. Polypyrrole (PPy): This is a conductive polymer with a conjugated π-electron structure in its molecular chains. This structure allows it to be excited at lower energies, thus effectively absorbing a broad band of light from ultraviolet to near-infrared. Carboxylated carbon nanotubes (CNTs): Carboxylated carbon nanotubes possess excellent broad-band light absorption properties. When the two are combined, polypyrrole uniformly coats the surface of the carboxylated carbon nanotubes, forming a synergistic effect that significantly enhances the light absorption capacity of the composite film across the entire solar spectrum (200–2500 nm).
[0010] Second: Microstructure of light traps induced by magnetic fields This is the key innovation of the invention, achieved through electrochemical deposition in a constant magnetic field (35~170 mT). **Microstructure Control:** The magnetic field induces magnetohydrodynamic effects in the electrodeposition process, acting as a gentle "stirring" mechanism that effectively guides the self-assembly of polypyrrole and carbon nanotubes. This results in a multi-level, high-curvature, rough microstructure (e.g., rod-like structures). **Light Trapping:** This rough microstructure acts like a "light trap" or a "blackbody" surface. When light is incident, it undergoes multiple reflections and scatterings between these high-curvature structures, significantly increasing the propagation path and the chance of photons being trapped within the material. **Enhanced Absorption Efficiency:** This multiple reflection effect significantly suppresses surface reflection of light, ensuring that the vast majority of incident light is absorbed by the material and converted into heat energy, thus achieving high absorption across the entire wavelength range.
[0011] The optical isotropic property does not refer to the material being isotropic at the molecular level, but rather to its macroscopic light absorption performance being independent of the direction of incident light. This is due to the disordered, isotropic, multi-level microstructure induced by a magnetic field. Regardless of the angle from which sunlight shines, the light is effectively captured by these structures, ensuring stable and attenuated photothermal conversion output. The efficiently absorbed light energy is rapidly converted into heat energy, significantly increasing the surface temperature of the composite film, thus enabling the composite film to possess photothermal conversion and anti-icing effects. In low-temperature environments, this manifests as delayed icing (the heat generated by photothermal conversion can delay the surface temperature from dropping to the freezing point) and accelerated melting (the deposited heat can quickly melt the existing ice layer). In summary, this invention, through magnetic field control, combines the intrinsic broadband absorption capability of polypyrrole / carbon nanotube composite materials with a carefully designed microscopic "light trap" structure, achieving efficient and stable photothermal conversion, providing a solid theoretical foundation for its application in anti-icing and other fields.
[0012] Furthermore, the magnitude of the constant magnetic field is 35~170 mT.
[0013] Furthermore, both the working electrode and the counter electrode are stainless steel sheets.
[0014] Further, the ratio of pyrrole, sodium perfluorononenoxybenzenesulfonate, carboxylated carbon nanotubes, ethanol and water is (1.0~4.0) g : (2.0~12.0) g : (0.1~1.0) g : 30 mL : 120 mL, preferably 2.0 g : 6.0 g : 0.5 g : 30 mL : 120 mL.
[0015] Furthermore, the constant current density is 1.2 mA·cm⁻¹. -2 .
[0016] Furthermore, the deposition time is 20 min.
[0017] The present invention also provides a composite film with high absorption of sunlight in a wide band prepared according to the above method, which can achieve high absorption in the ultraviolet-visible-near infrared range of 200~2500 nm.
[0018] This invention also provides the application of the above-mentioned broadband high-absorption solar light composite film in active anti-icing materials.
[0019] Compared with the prior art, the present invention has the following advantages and technical effects: 1. Compared with the control group without magnetic field, the composite film prepared with 100 mT magnetic field has significantly improved the absorption rate of the whole band and near-infrared light, the surface temperature rises higher under light and the photothermal conversion efficiency is stronger. At the same time, the material has optical isotropy and the light absorption effect is stable and has no attenuation under different incident angles of sunlight.
[0020] 2. Under a low-temperature test environment of -10 ℃, compared with stainless steel substrate and non-magnetic field composite film, the optimal sample of this invention (prepared by 100 mT magnetic field) has significantly longer time for dark-state icing and light-induced icing, and faster ice melting speed. It achieves long-term active anti-icing effect by relying on the synergy of multi-level high-curvature rod structure and photothermal effect.
[0021] 3. Compared with traditional non-magnetic electropolymerization, the magnetoelectric synergistic preparation process significantly shortens the film formation time and improves production efficiency. The magnetic fluid stirring brought by the magnetic field makes the film composition uniform and the batch performance stable. The whole process conditions are mild, the raw materials used are green, and the required supporting equipment is simple, which is convenient for large-scale industrial production. Attached Figure Description
[0022] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 Fourier transform infrared spectra comparison of stainless steel substrate (SS), magnetic field-free composite film (B-PPy-CNT-0), and 100 mT magnetic field composite film (B-PPy-CNT-100); Figure 2 Microscopic morphology images of composite films prepared under different magnetic field strengths (0, 35, 70, 100, 135, 170 mT): (a) CNT-COOH, (b) B-PPy-CNT-0, (c) B-PPy-CNT-35, (d) B-PPy-CNT-70, (e) B-PPy-CNT-100, (f) B-PPy-CNT-135, (g) B-PPy-CNT-170; Figure 3The 3D contour roughness test images of composite film surfaces prepared under different magnetic field strengths (0, 35, 70, 100, 135, 170 mT) are shown. (a) is B-PPy-CNT-0, (b) is B-PPy-CNT-35, (c) is B-PPy-CNT-70, (d) is B-PPy-CNT-100, (e) is B-PPy-CNT-135, and (f) is B-PPy-CNT-170. Figure 4 Comparison of absorption spectra of composite films prepared under different magnetic field strengths (0, 35, 70, 100, 135, 170 mT) in the range of 200–2500 nm; Figure 5 The images shown are polarization optical microscope test images of the composite film prepared with the optimal magnetic field (100 mT) in Example 1 (rotated at 0° and 90°), (a) rotated at 0°, (b) rotated at 90°; Figure 6 The images show the infrared thermal imaging temperature comparison of the stainless steel substrate (SS) and each composite film under the same illumination. (a) is SS, (b) is B-PPy-CNT-0, (c) is B-PPy-CNT-35, (d) is B-PPy-CNT-70, (e) is B-PPy-CNT-100, (f) is B-PPy-CNT-135, and (g) is B-PPy-CNT-170. Figure 7 Comparison of icing tests under dark conditions and light conditions for blank substrate (SS), non-magnetic field membrane (B-PPy-CNT-0), and composite membrane of the present invention (B-PPy-CNT-100) under -10 ℃ cold stage conditions. Detailed Implementation
[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0024] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0025] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0026] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0027] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0028] An embodiment of the present invention provides a method for preparing a composite film with wide-band high absorption of sunlight, comprising the following steps: In a constant magnetic field environment, the working electrode and the counter electrode are immersed in a mixture of pyrrole, sodium perfluorononenoxybenzenesulfonate, carboxylated carbon nanotubes, ethanol and water, and deposition is carried out under constant current density. After deposition, the product is cleaned and dried to obtain a composite film with high absorption of sunlight in a wide band.
[0029] In a preferred embodiment of the present invention, the magnitude of the constant magnetic field is 35~170 mT, more preferably 70~135 mT, more preferably 70~100 mT, and most preferably 100 mT.
[0030] In a preferred embodiment of the present invention, both the working electrode and the counter electrode are stainless steel sheets.
[0031] In a preferred embodiment of the present invention, the ratio of pyrrole, sodium perfluorononenoxybenzenesulfonate, carboxylated carbon nanotubes, ethanol and water is (1.0~4.0) g∶(2.0~12.0) g∶(0.1~1.0) g∶30 mL∶120 mL, preferably 2.0 g∶6.0 g∶0.5 g∶30 mL∶120 mL.
[0032] In a preferred embodiment of the present invention, the constant current density is 1.2 mA·cm. -2 .
[0033] In a preferred embodiment of the invention, the deposition time is 20 min.
[0034] Embodiments of the present invention also provide a composite film with high absorption of sunlight over a wide band, prepared according to the above method, which can achieve high absorption in the ultraviolet-visible-near infrared range of 200~2500 nm.
[0035] Embodiments of the present invention also provide the application of the above-mentioned broadband high-absorption solar radiation composite film in active anti-icing materials.
[0036] Unless otherwise specified, the room temperature in this invention is 25±2℃.
[0037] All raw materials used in the embodiments of this invention were purchased commercially. For example, carboxylated carbon nanotubes were purchased from Shenzhen Guosen Leading Technology Co., Ltd., CAS number 308068-56-6, with a purity >98%, a diameter of 10~20nm, a length of 5~15μm, and a specific surface area of 210~280m². 2 / g, with a bulk density of 0.04~0.09g / cm³. 3 .
[0038] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0039] The technical solution of the present invention will be further illustrated by the following embodiments.
[0040] Example 1 A method for preparing a composite film with wide-band high absorption of sunlight, comprising the following steps: In a constant magnetic field of 100 mT, stainless steel sheets (SS) were used as the working and counter electrodes, respectively, immersed in a mixture of pyrrole (Py, 2.0 g), sodium perfluorononenoxybenzenesulfonate (OBS, 6.0 g), carboxylated carbon nanotubes (CNT-COOH, 0.5 g), ethanol (30 mL), and deionized water (120 mL). Subsequently, the magnetic field was subjected to a constant magnetic field of 1.2 mA·cm⁻¹. -2 Deposition was performed at a constant current density for 20 min. After deposition, the composite membrane was rinsed with deionized water to remove residual reagents and impurities, and dried at 60 °C to obtain a broadband high-absorption solar composite membrane (B-PPy-CNT composite membrane), denoted as B-PPy-CNT-100.
[0041] Example 2 A method for preparing a composite film with wide-band high absorption of sunlight is the same as in Example 1, except that the constant magnetic field is 35 mT. The resulting composite film with wide-band high absorption of sunlight is denoted as B-PPy-CNT-35.
[0042] Example 3 A method for preparing a composite film with wide-band high absorption of sunlight is the same as in Example 1, except that the constant magnetic field is 70 mT. The resulting composite film with wide-band high absorption of sunlight is denoted as B-PPy-CNT-70.
[0043] Example 4 A method for preparing a composite film with wide-band high absorption of sunlight is the same as in Example 1, except that the constant magnetic field is 135 mT. The resulting composite film with wide-band high absorption of sunlight is denoted as B-PPy-CNT-135.
[0044] Example 5 A method for preparing a composite film with wide-band high absorption of sunlight is the same as in Example 1, except that the constant magnetic field is 170 mT. The resulting composite film with wide-band high absorption of sunlight is denoted as B-PPy-CNT-170.
[0045] Comparative Example 1 A method for preparing a composite membrane is the same as in Example 1, except that no magnetic field is applied during the preparation of the composite membrane, and the prepared composite membrane is denoted as B-PPy-CNT-0.
[0046] Figure 1 Infrared spectra of SS, B-PPy-CNT-0, and B-PPy-CNT-100 composite films are presented. The spectrum of SS exhibits a smooth curve lacking characteristic absorption peaks, indicating that its surface does not display a distinct functional group structure. In contrast, the spectral characteristics of B-PPy-CNT-0 and B-PPy-CNT-100 are highly consistent, both showing significant fingerprint region characteristic peaks. This result strongly confirms that magnetic field treatment did not lead to changes in the chemical composition of the B-PPy-CNT composite film. (Located at 1287 cm⁻¹) -1 and 1450 cm -1 The absorption peaks at 1540 cm⁻¹ correspond to the stretching vibrations of the CN bonds in the pyrrole ring, while the peaks at 1540 cm⁻¹ correspond to the stretching vibrations of the CN bonds in the pyrrole ring. -1 The peak at that point is attributed to the skeletal vibration of the pyrrole ring. Furthermore, the characteristic peak originating from the OBS component is also clearly visible: 957 cm⁻¹. -1 The peak at 1025 cm⁻¹ is attributed to the stretching vibration of the S=O bond in the sulfonic acid group. -1 The peak at 1173 cm⁻¹ corresponds to the vibration of the CS bond, while the peak at 1173 cm⁻¹ corresponds to the vibration of the CS bond. -1 The peak at 1700 cm⁻¹ originates from the antisymmetric stretching vibration of the CF bond. Meanwhile, at 1700 cm⁻¹... -1 The characteristic peak appearing at this point can be attributed to the stretching vibration of the C=O bond in CNT-COOH.
[0047] Figure 2 SEM images of CNT-COOH and B-PPy-CNT composite membranes are shown. Figure 2 As shown in (a), pure CNT-COOH exhibits a slender tubular structure, but due to their intertwining, it forms a cluster structure with a diameter of approximately 2 μm. The B-PPy-CNT-0 composite film was prepared under magnetic field-free conditions, and its microstructure is consistent with the results reported in the literature, namely, it consists of a flat and dense base film and large clusters scattered on the surface. Figure 2 (b) High-magnification images show that these clusters are composed of a large number of small particles with a diameter of approximately 100 nm, and no complete CNT-COOH is clearly observed. This phenomenon indicates that under no magnetic field conditions, the film formed after 20 min of electrodeposition is mainly PPy, while complete CNT-COOH is not fully deposited on the film due to its large steric hindrance. However, after applying a magnetic field during the electrodeposition process, the prepared B-PPy-CNT composite film exhibits a completely different microstructure. Compared with the no magnetic field conditions, the number of loose clusters on the surface of the B-PPy-CNT composite film is significantly increased, and the tubular structure of CNT-COOH can be clearly observed. Figure 2 (c)~(g)). Taking B-PPy-CNT-35 as an example, tubular CNT-COOH and particulate PPy are co-deposited on the surface of the base film, forming a loose, multi-level micro / nano structure. Figure 2 (c)). With further increase in magnetic field strength, the particles on the surface of the B-PPy-CNT-70, B-PPy-CNT-100, and B-PPy-CNT-135 composite films gradually aggregate into a relatively regular rod-shaped structure, and its diameter increases from 10 μm to approximately 30 μm with increasing magnetic field strength. Figure 2 (d)~(f)). High-magnification images further reveal that the increase in magnetic field strength significantly accelerated the polymerization reaction of pyrrole, causing PPy to rapidly aggregate into smaller and more numerous particles. Simultaneously, CNT-COOH, due to the accelerated polymerization rate, failed to be fully encapsulated by PPy, instead remaining entangled and dispersed on the PPy surface. For B-PPy-CNT-170, when the magnetic field strength increased to 170 mT, the polymerization reaction of pyrrole further accelerated, leading to a continuous increase in the diameter of the rod-shaped agglomerates and their interconnection, ultimately returning to a disordered state. Figure 2 (g) Clearly, the presence of the magnetic field significantly affects the growth process of the composite film, and changes in the magnetic field strength further regulate the microstructure of the composite film, thus achieving magnetic field control of the B-PPy-CNT composite film structure. Furthermore, taking B-PPy-CNT-100 as an example, EDS images were used to demonstrate the elemental distribution of the magneto-polymerized B-PPy-CNT composite film. The images show that the brightness is relatively uniform in different parts of the film, indicating that the elements on the film surface are uniformly distributed.
[0048] 3D images visually demonstrate the three-dimensional morphology of the B-PPy-CNT composite film surface. Figure 3 Without an applied magnetic field, the surface of B-PPy-CNT-0 exhibits minimal undulation and is relatively smooth overall, with a roughness of only 1.4 μm. Figure 3 (a)). As the magnetic field strength increases, a peak-like structure gradually appears on the film surface, forming a distinct uneven morphology, and the roughness also increases accordingly. Figure 3 (b)~(d)). When the magnetic field strength reaches 100 mT, the roughness of the B-PPy-CNT-100 composite film reaches its maximum value of 30.3 μm. Afterward, with further increases in magnetic field strength, the roughness shows a slight decrease (…). Figure 3 (e)~(f)). In summary, the surface roughness of the B-PPy-CNT composite film is significantly affected by the magnetic field strength.
[0049] Figure 4The absorption spectra of B-PPy-CNT composite films prepared under different magnetic field strengths (0, 35, 70, 100, 135, and 170 mT) in the ultraviolet-visible-near-infrared band (200–2500 nm) are presented. The results show that the light absorption characteristics of the B-PPy-CNT composite films change significantly with increasing magnetic field strength. Without a magnetic field, the B-PPy-CNT-0 composite film has the lowest average absorbance, exhibiting high absorbance only in the visible light region, while the absorbance in the ultraviolet and near-infrared regions still has considerable room for improvement. In contrast, after applying a magnetic field, the absorbance of all B-PPy-CNT composite films significantly increases. Specifically, the absorbance of B-PPy-CNT-35 to B-PPy-CNT-170 composite films prepared under a magnetic field increases to over 95% in the ultraviolet region, while also showing a slight increase from the over 98% absorbance in the visible light region. It is noteworthy that the applied magnetic field has a more significant impact on the absorbance of the B-PPy-CNT composite film in the near-infrared region. When the magnetic field strength increases from 0 mT to 100 mT, the absorbance of the B-PPy-CNT composite film in the near-infrared region increases sharply to approximately 98%. However, when the magnetic field strength continues to increase to 170 mT, the absorbance of the composite film in the near-infrared region decreases slightly to approximately 95% and remains relatively stable. Finally, at a magnetic field strength of 100 mT, the average absorbance of the B-PPy-CNT-100 composite film reaches its highest value of 98.57%. Furthermore, the absorbance of the B-PPy-CNT-100 composite film exhibits high consistency in the 200–2500 nm wavelength range, effectively compensating for the insufficient absorbance in the near-infrared band. This significant improvement in absorbance can be attributed to the optimization of the composite film structure through the magnetron electropolymerization method. Without a magnetic field, the surface of the B-PPy-CNT-0 composite film is relatively flat, with only scattered clusters, making effective light absorption difficult. However, after applying a magnetic field, the number of clusters on the composite film surface increases significantly, and they aggregate to form more regular rod-like structures, thereby increasing the probability of light contact with the composite film surface. Furthermore, these rod-like structures are composed of interwoven PPy nanoparticles and CNT-COOH tubular structures; this unique micro-nano structure facilitates the formation of light traps, further enhancing the light absorption rate of the composite film.
[0050] The B-PPy-CNT-100 composite film was tested using a polarizing optical microscope (POM), and the results are as follows: Figure 5As shown, under polarized light illumination, rotating the B-PPy-CNT-100 composite film by 0° and 90° respectively did not result in significant changes in brightness. This phenomenon indicates that light passing through the B-PPy-CNT-100 composite film is not affected by birefringence. Regardless of the incident angle of the light, different parts of the composite film can uniformly reflect or refract light, showing insensitivity to the incident angle, thus eliminating the need for additional adjustments or compensation based on the light direction. Based on this, it can be determined that the B-PPy-CNT-100 composite film possesses optical isotropy. This uniformity in optical performance helps ensure that the composite film exhibits consistent light absorption characteristics in different directions.
[0051] To visually demonstrate the photothermal conversion capability of the B-PPy-CNT composite film, thermal images of the SS substrate and the B-PPy-CNT composite film under sunlight were captured using an infrared thermal imager. The results are as follows: Figure 6 As shown. Under sunlight, the surface temperature of the SS substrate is close to room temperature, only 25.9 ℃ ( Figure 6 (a)). In contrast, the surface temperature of the B-PPy-CNT-0 composite membrane reaches 35.3℃ ( Figure 6 In (b), the temperature was nearly 10 °C higher than that of the SS substrate, while the surface temperatures of the B-PPy-CNT-35 to B-PPy-CNT-170 composite films were all above 36 °C. Figure 6 (c)~(g)). Furthermore, the temperature variation trend of the B-PPy-CNT composite film is related to its absorbance ( Figure 4 The trends are basically consistent, indicating that the photothermal conversion capability of the B-PPy-CNT composite film is mainly determined by its absorbance. This result further verifies the potential of the composite film in photothermal conversion applications.
[0052] Five μL water droplets were placed on the surfaces of SS, B-PPy-CNT-0, and B-PPy-CNT-100 composite membranes, respectively, and their dark-state icing, light-induced melting, and light-induced icing processes were observed at -10 °C. The results are as follows: Figure 7As shown in the figure, due to the hydrophobic nature of the SS surface, water droplets form beads on its surface, while the B-PPy-CNT-0 and B-PPy-CNT-100 composite films are superhydrophilic, allowing water droplets to spread and wet completely. In the dark, water droplets on the SS surface freeze within 30 s, while the B-PPy-CNT-0 composite film extends the freezing time by nearly 8 times. In contrast, the B-PPy-CNT-100 composite film further extends the freezing time to 254 s, exhibiting superior delayed freezing performance. To investigate the effect of light on the freezing process, the above experiment was repeated under one intensity of sunlight. The results show that the freezing time on the SS surface does not change much compared to the dark conditions, indicating that light has a limited effect on the freezing behavior of pure metal substrates. However, the freezing time of the B-PPy-CNT-0 composite film under light is more than doubled compared to the dark conditions, reaching 508 s. Notably, after 3700 seconds of illumination, the B-PPy-CNT-100 composite membrane only developed frost on both sides, while the central area remained completely unfrozen, demonstrating excellent anti-icing capabilities. This indicates that the B-PPy-CNT composite membrane, especially the magnetically modulated B-PPy-CNT-100 composite membrane, can efficiently absorb near-infrared light and convert it into heat energy, thereby significantly extending the icing time.
[0053] Although the B-PPy-CNT-0 and B-PPy-CNT-100 composite films are superhydrophilic and theoretically more prone to freezing, they can still delay freezing under dark conditions (indoor environments not completely shaded), attributed to their photothermal conversion capabilities. Under illumination, the differences in freezing and melting times between the two composite films are more significant, closely related to their microstructure and composition. Compared to the relatively smooth surface of the B-PPy-CNT-0 composite film, the B-PPy-CNT-100 composite film has a macroscopic granular structure, increasing its surface curvature. A high-curvature surface leads to a higher chemical potential, which is unfavorable for ice nucleus formation, thus increasing the difficulty of freezing. Furthermore, the B-PPy-CNT-0 composite film only has a micron-scale structure, making it easily reflected after light incidence, resulting in low light utilization and difficulty in accumulating sufficient heat, thus limiting its performance in delaying freezing and accelerating melting. In contrast, the micro-nano structure formed by the B-PPy-CNT-100 composite film under magnetic field control enables multi-level internal reflection of light, extending the light propagation path and thus efficiently converting light into heat, significantly improving anti-icing performance. Simultaneously, the magnetic field accelerates the electropolymerization reaction of pyrrole, incorporating more CNT-COOH into the B-PPy-CNT-100 composite film, thereby enhancing its absorption of near-infrared light. Given that near-infrared light accounts for approximately 43% of total solar radiation, its efficient conversion into heat energy is a key factor in improving the anti-icing performance of the B-PPy-CNT-100 composite film. In conclusion, the B-PPy-CNT-100 composite film exhibits excellent broadband high light absorption capability, providing significant value for its application in the anti-icing field.
[0054] Furthermore, under a 100 mT magnetic field, this invention investigated the effect of different raw material ratios on the composite film layer, as detailed below: Example 6 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of Py used is 1.0 g, and the resulting composite film is designated as B-PPy-CNT-100-1. The B-PPy-CNT-100-1 composite film has an average absorption rate of 96.83% in the 200~2500 nm wavelength range, and its surface temperature under sunlight irradiation is 35.8 ℃.
[0055] Example 7 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of Py used is 3.0 g, and the resulting composite film is designated as B-PPy-CNT-100-2. The B-PPy-CNT-100-2 composite film has an average absorption rate of 98.61% in the 200~2500 nm wavelength band, and its surface temperature under sunlight irradiation is 36.3 ℃.
[0056] Example 8 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of Py used is 4.0 g, and the resulting composite film is designated as B-PPy-CNT-100-3. The B-PPy-CNT-100-3 composite film has an average absorption rate of 98.39% in the 200~2500 nm wavelength range, and its surface temperature under sunlight irradiation is 36.2 ℃.
[0057] Example 9 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of OBS used is 2.0 g, and the resulting composite film is designated as B-PPy-CNT-100-4. The B-PPy-CNT-100-4 composite film has an average absorption rate of 92.76% in the 200~2500 nm wavelength range, and its surface temperature under sunlight irradiation is 34.7 ℃.
[0058] Example 10 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of OBS used is 4.0 g, and the resulting composite film is designated as B-PPy-CNT-100-5. The B-PPy-CNT-100-5 composite film has an average absorption rate of 96.18% in the 200~2500 nm wavelength band, and its surface temperature under sunlight irradiation is 35.7 ℃.
[0059] Example 11 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of OBS used is 8.0 g, and the resulting composite film is designated as B-PPy-CNT-100-6. The B-PPy-CNT-100-6 composite film has an average absorption rate of 98.36% in the 200~2500 nm wavelength band, and its surface temperature under sunlight irradiation is 36.2 ℃.
[0060] Example 12 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of OBS used is 10.0 g, and the resulting composite film is designated as B-PPy-CNT-100-7. The B-PPy-CNT-100-7 composite film has an average absorption rate of 97.33% in the 200~2500 nm wavelength band, and its surface temperature under sunlight irradiation is 36.0 ℃.
[0061] Example 13 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of OBS used is 12.0 g, and the resulting composite film is designated as B-PPy-CNT-100-8. The B-PPy-CNT-100-8 composite film has an average absorption rate of 95.29% in the 200~2500 nm wavelength band, and its surface temperature under sunlight irradiation is 35.3 ℃.
[0062] Example 14 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of CNT-COOH used is 0.1 g, and the resulting composite film is designated as B-PPy-CNT-100-9. The B-PPy-CNT-100-9 composite film has an average absorption rate of 91.87% in the 200~2500nm wavelength range, and its surface temperature under sunlight irradiation is 33.8 ℃.
[0063] Example 15 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of CNT-COOH used is 0.3 g, and the resulting composite film is designated as B-PPy-CNT-100-10. The B-PPy-CNT-100-10 composite film has an average absorption rate of 93.45% in the 200~2500 nm wavelength range, and its surface temperature under sunlight irradiation is 35.1 ℃.
[0064] Example 16 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of CNT-COOH used is 0.8 g, and the resulting composite film is designated as B-PPy-CNT-100-11. The B-PPy-CNT-100-11 composite film has an average absorption rate of 98.80% in the 200~2500 nm wavelength range, and its surface temperature under sunlight irradiation is 36.3 ℃.
[0065] Example 17 A method for preparing a broadband high-absorption solar composite film is the same as in Example 1, except that the amount of CNT-COOH used is 1.0 g, and the resulting composite film is designated as B-PPy-CNT-100-12. The B-PPy-CNT-100-12 composite film has an average absorption rate of 98.63% in the 200~2500 nm wavelength range, and its surface temperature under sunlight irradiation is 36.3 ℃.
[0066] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a composite film with wide-band high absorption of sunlight, characterized in that, Includes the following steps: In a constant magnetic field environment, the working electrode and the counter electrode are immersed in a mixture of pyrrole, sodium perfluorononenoxybenzenesulfonate, carboxylated carbon nanotubes, ethanol and water, and deposition is carried out under constant current density. After deposition, the product is cleaned and dried to obtain the composite film with wide-band high absorption of sunlight.
2. The method for preparing a broadband high-absorption solar composite film according to claim 1, characterized in that, The magnitude of the constant magnetic field is 35~170 mT.
3. The method for preparing a broadband high-absorption solar composite film according to claim 1, characterized in that, Both the working electrode and the counter electrode are stainless steel sheets.
4. The method for preparing a broadband high-absorption solar composite film according to claim 1, characterized in that, The ratio of pyrrole, sodium perfluorononenoxybenzenesulfonate, carboxylated carbon nanotubes, ethanol and water is (1.0~4.0) g : (2.0~12.0) g : (0.1~1.0) g : 30 mL : 120 mL.
5. The method for preparing a broadband high-absorption solar composite film according to claim 1, characterized in that, The constant current density is 1.2 mA·cm. -2 .
6. The method for preparing a broadband high-absorption solar composite film according to claim 1, characterized in that, The deposition time was 20 minutes.
7. A composite film with wide-band high absorption of sunlight, characterized in that, The preparation method according to any one of claims 1 to 6 yields a product that can achieve high absorption in the 200-2500 nm ultraviolet-visible-near-infrared range.
8. The application of a composite film with wide-band high absorption of sunlight as described in claim 7 in active anti-icing materials.