Method for toughening a starch gel and use thereof

By controlling the moisture content of starch gel and using high-temperature toughening heat treatment, the problem of simultaneously improving the strength and extensibility of starch gel was solved, resulting in a significant improvement in the mechanical and structural properties of starch gel, which is suitable for starch-based raw materials from various plant sources.

CN123152146APending Publication Date: 2026-11-24QINGDAO AGRI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611627676.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing three-dimensional gel network pore structure of starch gels is not uniform, resulting in insufficient load-bearing capacity. It is prone to local stress concentration during stretching, making it difficult to improve strength and ductility simultaneously. Furthermore, existing modification methods are complex or exceed the composition range of single starch-based foods.

Method used

Toughened starch gel was prepared by controlling the water content of the gelatinized starch gel and subjecting it to high-temperature toughening through heat treatment, including pre-drying or water absorption control, sealed heat treatment, and cooling.

Benefits of technology

It significantly improves the fracture stress and fracture strain of starch gel, enhances mechanical and structural properties, achieves a balance between strength and ductility, and is simple, environmentally friendly, and applicable to various plant-derived starch-based raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152146A_ABST
    Figure CN123152146A_ABST
Patent Text Reader

Abstract

This invention provides a method for toughening starch gel and its application, belonging to the field of starch gel processing technology. The method for toughening starch gel provided by this invention includes gelatinizing a starch-based raw material, adjusting the water content of the resulting pre-formed gel to a mass-volume ratio of 20%~55%, and toughening it by heating at 80~110℃ for 10 min~50 min under sealed conditions, followed by cooling to obtain a toughened starch gel. Using the toughening method described in this invention, the fracture stress and fracture strain of the starch gel are effectively improved compared to the control group; the toughening method also improves the stress retention rate, normalized stress relaxation curve area, shear work, elasticity, and uniform and continuous pore wall structure of the starch gel, and reduces the swelling rate. Therefore, the method described in this invention can be used to control the mechanical and structural properties of starch gels and starch-based materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of starch gel processing technology, specifically relating to a method for toughening starch gel and its application. Background Technology

[0002] After gelatinization and cooling, starch molecules undergo rearrangement, double helix reassociation, and hydrogen bond reconstruction to form a three-dimensional gel network. However, the three-dimensional gel network often suffers from problems such as uneven pore structure, insufficient load-bearing capacity, easy local stress concentration during stretching, and difficulty in simultaneously improving strength and extensibility, which limit its application in high-quality starch gel foods.

[0003] To improve the tensile properties, elasticity, or gel strength of starch gels, existing technologies have developed methods such as composite crosslinking, enzymatic modification, chemical esterification, and raw material defatting combined with mechanical homogenization. For example, patent CN109354719B uses starch, polyvinyl alcohol, and borax as raw materials, and utilizes retrogradation, freeze-thaw cycles, and dynamic crosslinking with borate esters to construct a double crosslinking network, resulting in a starch-based hydrogel with high tensile strength, toughness, and mechanical strength. Patent CN110656139A uses 4-α-glycosyltransferase to enzymatically modify starch, followed by gelatinization and coagulation to obtain a thermally reversible starch-based gel with controllable gel strength. Patent CN114773493A improves the octenyl succinic anhydride starch content by compounding waxy rice starch and waxy potato starch and modifying it with octenyl succinic anhydride esterification. The gel strength of sodium starch powder; Patent US3666557A fully gelatinizes and homogenizes amylose-containing raw materials with bound lipid content reduced to about 0.3% to obtain starch gel with high gel strength, cohesiveness and elasticity, and texture close to gelatin. Although the above technology can improve the tensile strength, elasticity or gel strength of starch gel to a certain extent, it may rely on exogenous polymers such as polyvinyl alcohol and crosslinking agents, or on enzymatic modification and chemical esterification, or require defatted raw materials and specific processing such as high shear homogenization. The process is relatively complicated, and some systems have exceeded the composition range of single starch food. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide a method for toughening starch gel. The toughening method provided by this invention, by controlling the water content of the gelatinized starch gel and performing high-temperature toughening through heat treatment, can effectively improve the fracture stress and fracture strain of the starch gel compared to the group without high-temperature toughening.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for toughening starch gel, characterized by comprising the following steps: Starch-based raw materials are gelatinized and shaped to obtain pre-shaped starch gels; After adjusting the water content of the pre-formed starch gel to 20%~55% by volume, the pre-formed starch gel with adjusted water content is sealed, heat-treated at 80~110 ℃ for 10~50 min, and then cooled to obtain toughened starch gel.

[0006] Preferably, the moisture content control is carried out by pre-drying or water absorption; the pre-drying includes any one of the following: natural drying, hot air drying, constant temperature and humidity drying or vacuum drying; the water absorption includes any one of the following: soaking, spraying and constant humidity balancing.

[0007] Preferably, the heat treatment is performed after sealing the starch gel with adjusted moisture content; the heat treatment method includes any one of the following: water bath heating, steam heating, high-pressure steam treatment, and electromagnetic induction heating.

[0008] Preferably, the cooling method includes any one of the following: cryogenic medium cooling, natural cooling, and forced air cooling.

[0009] Preferably, the cooling process further includes rehydration, which involves placing the toughened starch gel in boiling water until no unhydrated core is visible in the cross-section of the gel.

[0010] Preferably, the starch-based raw material includes at least one of the following: cereal starch, legume starch, potato starch, and starch-containing cereal powder, potato powder, or legume powder.

[0011] This invention provides an application of the toughening method described above in improving the mechanical properties and / or structural properties of starch gels.

[0012] Preferably, the mechanical properties include at least one of the following: tensile properties, stress relaxation stability, shear properties, and textural properties; the textural properties include at least one of hardness, elasticity, and chewiness.

[0013] Preferably, the structural properties include at least one of the following: water retention, stability, and network density.

[0014] This invention provides a starch gel prepared by the aforementioned toughening method.

[0015] This invention provides a method for toughening starch gel. This method, through precise control of the starch gel's moisture content via pre-drying, combined with high-temperature toughening via sealed heat treatment, significantly improves the mechanical properties of the starch gel without the need for chemical cross-linking agents. The toughening method simultaneously increases the gel's fracture stress and fracture strain. Under the preferred 38% moisture content condition, the ANN-38 gel obtained achieves a fracture stress of 111.85 kPa and a fracture strain of 158.65%, which are 3.06 times and 2.88 times that of untreated Native-53, respectively. These represent increases of 75.3% and 67.2% compared to PD-38 (pre-dried but not high-temperature toughened), demonstrating excellent strength-ductility balance. Furthermore, the toughening method also improves the stress retention rate, normalized stress relaxation curve area, shear work, elasticity, and uniform and continuous pore wall structure of the starch gel, while reducing the swelling rate. The overall performance of the starch gel obtained using this method is significantly superior to the comparative example without high-temperature toughening. Furthermore, the method of this invention is simple, has controllable conditions, is green and environmentally friendly, and is universally applicable to starch-based raw materials from different plant sources, such as ordinary corn starch, potato starch, wheat starch, sweet potato starch, pea starch, mung bean starch, and rice flour, providing an effective way to prepare high-performance starch gels. Attached Figure Description

[0016] Figure 1 A flowchart of the starch gel toughening method; Figure 2 The figures show the tensile properties of corn starch gel under different moisture content control and high temperature toughening conditions. In the figures, A is the stress-strain curve before high temperature toughening, B is the stress-strain curve after high temperature toughening, C is the elastic modulus, and D is the tensile toughness. Figure 3 The figures show the stress relaxation behavior of rehydrated corn starch gel and the fitting of the double exponential Maxwell model. In the figure, A is the stress-time curve, B is the normalized stress-time curve, and C is the nonlinear Maxwell model fitting of the ANN-38 sample. Figure 4 X-ray diffraction patterns of corn starch gels with different treatments; Figure 5 Fourier transform infrared spectra and short-range order index diagrams of corn starch gels before and after rehydration under different treatments are shown. In the figure, A is the FTIR spectrum before rehydration, B is the FTIR spectrum after rehydration, C is the R1047 / 1022 ratio before rehydration, and D is the R1047 / 1022 ratio after rehydration. Figure 6 Low-field nuclear magnetic resonance T2 relaxation distribution of corn starch gels with different moisture contents before high-temperature toughening before rehydration; Figure 7The image shows a cross-sectional scanning electron microscope image of a high-temperature toughened corn starch gel before rehydration, where the scale bar of A1~A7 is 50 μm and the scale bar of B1~B7 is 10 μm. Figure 8 The image shows a cross-sectional scanning electron microscope image of the high-temperature toughened corn starch gel after rehydration, where the scale bar of A1~A7 is 50 μm and the scale bar of B1~B7 is 10 μm. Figure 9 The swelling rate of high-temperature toughened corn starch gel under different soaking times is shown in the graph. Figure 10 Representative tensile stress-strain curves of potato starch, wheat starch, sweet potato starch, pea starch, mung bean starch, and rice flour gels before and after high-temperature toughening at 95℃ for 30 min are shown. Among them, A is the engineering stress-strain curve of the potato starch gel control group and the high-temperature toughening group; B is the engineering stress-strain curve of the wheat starch gel control group and the high-temperature toughening group; C is the engineering stress-strain curve of the sweet potato starch gel control group and the high-temperature toughening group; D is the engineering stress-strain curve of the pea starch gel control group and the high-temperature toughening group; E is the engineering stress-strain curve of the mung bean starch gel control group and the high-temperature toughening group; and F is the engineering stress-strain curve of the rice flour gel control group and the high-temperature toughening group. Detailed Implementation

[0017] This invention provides a method for toughening starch gel, comprising the following steps: mixing starch-based raw materials and water to obtain starch slurry; gelatinizing the starch slurry to obtain pre-formed starch gel; adjusting the water content of the pre-formed starch gel to 20%~55%; heat-treating it at 80~110 ℃ for 10~50 min; and cooling it to obtain toughened starch gel.

[0018] In this invention, the gelatinization is performed using any one of the following methods: steaming, boiling, water bath heating, extrusion curing, microwave heating, and pressure heating. In this invention, gelatinization refers to the process by which starch-based raw materials, in the presence of moisture, are heated or subjected to mechanical energy, causing starch granules to absorb water and swell, disrupting their crystalline structure, dissolving amylose, and forming a paste or gel-like system. Steaming refers to placing the starch slurry in a steamer, steam oven, or steam environment, and directly heating it with boiling steam until the starch is fully gelatinized. Cooking refers to adding the starch slurry directly to boiling or hot water, heating and stirring simultaneously until gelatinized. Water bath heating refers to placing a container containing the starch slurry in a constant-temperature water bath, indirectly heating it until gelatinized. Extrusion curing refers to feeding the starch-based raw material into an extruder, where the starch is gelatinized and extruded under the combined action of screw shearing, frictional heat, and external heating. Microwave heating refers to placing the starch slurry in a microwave field, using microwave dielectric heating to rapidly raise the temperature of the moisture, thereby gelatinizing the starch. Pressure heating refers to placing the starch slurry in a sealed or pressurized container and heating it at a temperature higher than the boiling point at atmospheric pressure until gelatinized. The above methods can be used individually or in combination depending on the raw materials and equipment conditions, as long as the starch-based raw material is fully gelatinized. In this invention, when gelatinization is performed by steaming, the preferred steaming temperature is 90-100°C, specifically 92°C, 94°C, 96°C, or 98°C. The preferred steaming time is 2-5 minutes, specifically 3 minutes or 4 minutes. The specific temperature and time for gelatinization effectively disrupt the original crystalline structure of the starch granules, achieving thorough gelatinization. In a specific embodiment of this invention, the steaming is performed by heating with steam at 95°C for 3 minutes.

[0019] In this invention, the moisture content control is preferably performed using pre-drying or water absorption methods; the pre-drying preferably includes any one of the following: natural drying, hot air drying, constant temperature and humidity drying, or vacuum drying; the water absorption preferably includes any one of the following: soaking, spraying, and constant humidity equilibration. In this invention, the moisture content control refers to adjusting the moisture content of the pre-formed starch gel to a target range to facilitate subsequent high-temperature toughening treatment and achieve an ideal strength-ductility balance. The terms "natural drying" and "hot air drying" refer to placing the pre-formed starch gel in a well-ventilated environment at room temperature, allowing it to slowly remove moisture to the target moisture content through natural evaporation. "Hot air drying" refers to placing the gel in a hot air oven or hot air circulation system, introducing hot air at 40-80°C to accelerate moisture evaporation to the target moisture content. "Constant temperature and humidity drying" refers to placing the gel in a constant temperature and humidity chamber, allowing moisture to slowly and evenly dissipate to the target moisture content at 50-70°C and 70%-90% relative humidity. "Vacuum drying" refers to placing the gel in a vacuum drying chamber, allowing moisture to boil and evaporate to the target moisture content under negative pressure and lower temperature. "Soaking" refers to completely immersing the gel in deionized water or a specific solution, controlling the soaking time and temperature to allow it to absorb water to the target moisture content. "Spraying" refers to intermittently or continuously spraying the gel surface with deionized water or a specific solution to gradually allow it to absorb water to the target moisture content. "Constant humidity equilibrium" refers to placing the gel in a closed environment with constant relative humidity, allowing it to reach the target moisture content through moisture absorption or release. The above methods can be used individually or in combination depending on the type of raw materials, equipment conditions, and target moisture content, as long as the moisture content of the preformed starch gel reaches the required range.

[0020] In this invention, when a constant temperature and humidity drying method is used to control the moisture content, the preferred drying temperature is 50-70°C, which can be 55°C, 60°C, or 65°C. The preferred humidity is a relative humidity of 70%-90%, which can be 75%, 80%, or 85%. In a specific embodiment of this invention, the pre-formed starch gel is placed in an oven at 60°C and 80% relative humidity for moisture content control.

[0021] In this invention, the heat treatment is preferably performed after sealing the starch gel with adjusted moisture content. The sealing prevents moisture evaporation and external moisture interference during the high-temperature toughening process, maintaining the starch gel at a preset moisture content, thereby ensuring stable and repeatable high-temperature toughening. The sealing method is preferably any of the following: vacuum sealing, nitrogen-filled sealing, heat sealing, sealed bag sealing, sealed container sealing, retort pouch sealing, aluminum foil bag sealing, high-temperature resistant film sealing, glass container sealing, metal container sealing, self-sealing bag sealing, sealing film sealing, mechanical sealing, etc. Under high-temperature water bath or high-pressure steam conditions, a sealing method that is high-temperature resistant, pressure resistant, and can prevent moisture exchange should be preferred. The above methods can be used individually or in combination, as long as they can prevent moisture evaporation and external moisture ingress during the high-temperature toughening process, maintaining the preset moisture content of the starch gel.

[0022] In this invention, the heat treatment temperature is preferably 80-110℃, but can be 90-100℃, or even 92℃, 94℃, 96℃, or 98℃. The heat treatment time is preferably 10 min-50 min, but can be 20-40 min, or even 25 min, 30 min, or 35 min. The heat treatment refers to sealing the starch gel with adjusted moisture content and placing it in a high-temperature environment for a certain period of time, causing the starch molecular chains to rearrange, hydrogen bonds to reconstruct, and the crystal structure to undergo moderate changes, thereby improving the gel's strength, extensibility, and stress retention capacity, i.e., achieving high-temperature toughening. The heat treatment method preferably includes any one of the following: water bath heating, steam heating, high-pressure steam treatment, and electromagnetic induction heating. The water bath heating refers to completely immersing the sealed starch gel in a constant temperature water bath to ensure uniform heating. Steam heating involves placing the sealed starch gel in a normal or slightly pressurized steam environment, directly heating it to a set temperature using saturated or superheated steam, and maintaining it for a set time. High-pressure steam treatment involves placing the sealed starch gel in a high-pressure steam sterilizer, autoclave, or similar pressurized container, treating it under saturated steam conditions above 100°C to the target temperature, and maintaining it for a set time to achieve a faster or stronger toughening effect. Electromagnetic induction heating involves placing the sealed starch gel in an electromagnetic induction heating device, using an alternating magnetic field to generate eddy currents in the container or heat-conducting medium, thereby indirectly heating the gel to a set temperature and maintaining it for a set time. These methods can be used individually or in combination depending on the type of raw material, equipment conditions, and target toughening level, as long as the sealed starch gel can complete the toughening treatment under high-temperature conditions. In a specific embodiment of this invention, a 95°C water bath for 30 minutes is used for heat treatment.

[0023] In this invention, the cooling method preferably includes any one of the following: low-temperature medium cooling, room temperature natural cooling, and forced-air cooling. The cooling refers to placing the sealed starch gel in a specific environment to cool it down after heat treatment, thereby terminating the high-temperature toughening reaction, fixing the formed gel network structure, and possibly causing some starch retrogradation, thus stabilizing the gel's strength, extensibility, and stress retention capacity. The cooling method preferably includes any one of the following: low-temperature medium cooling, room temperature natural cooling, and forced-air cooling. Low-temperature medium cooling refers to directly immersing the sealed starch gel in ice water, cold water, or a refrigerated environment, or contacting it with a low-temperature cold plate, cold bath, or other medium to rapidly cool it to 0-4°C or room temperature; the cooling time depends on the gel size. Room temperature natural cooling refers to placing the sealed starch gel in a room temperature environment of 20-25°C, allowing it to cool naturally to room temperature without additional refrigeration or forced convection; the cooling time depends on the gel size and environmental conditions. Forced-air cooling refers to placing the sealed starch gel in a forced-air cooling device or a cold air circulation environment, using forced-flowing cold air to accelerate heat dissipation and rapidly cool it to the target temperature. The above methods can be used individually or in combination, as long as they can effectively cool the starch gel after high-temperature toughening and stabilize its structure. In a specific embodiment of this invention, the gel after high-temperature toughening is immediately placed in ice water at 0 ℃ for 15 min to cool.

[0024] In a specific embodiment of the present invention, the cooling process preferably includes rehydration. Rehydration preferably involves placing the toughened starch gel in boiling water until no unhydrated core is visible in the cross-section of the gel, and the mass change rate is less than 1% after two consecutive weighings at 10-second intervals. Rehydration refers to placing the cooled toughened starch gel in a boiling water environment to allow it to reabsorb water and reach swelling equilibrium, thereby restoring the gel's suitable water content and network structure, facilitating subsequent tests such as tensile properties, shear properties, and textural profile analysis. During rehydration, the gel can be directly immersed in boiling water or placed in a boiling water steam environment, preferably directly immersed in boiling water. The rehydration time depends on the sample size, the water content before high-temperature toughening, and the degree of pre-drying. In this application, a dual standard is used to determine the rehydration endpoint: first, the absence of a visible unhydrated core in the gel cross-section indicates that boiling water has penetrated into the gel, and there is no unhydrated area that is wet on the outside and dry on the inside; second, the gel mass is weighed twice consecutively at 10-second intervals. When the mass change rate is less than 1%, it indicates that the gel has nearly reached water saturation, and further rehydration will not significantly increase the water content. This dual standard ensures that different samples are tested at the same rehydration endpoint, avoiding interference from insufficient or excessive rehydration on mechanical property determination. In practice, observing the absence of a visible unhydrated core in the gel cross-section is sufficient.

[0025] In this invention, the starch-based raw material preferably includes at least one of the following: cereal starch, legume starch, potato starch, and starch-containing cereal flour, potato flour, or legume flour. The cereal starch includes, but is not limited to, corn starch, wheat starch, or rice starch; the legume starch includes, but is not limited to, pea starch or mung bean starch; and the potato starch includes, but is not limited to, potato starch or sweet potato starch. The cereal flour includes, but is not limited to, rice flour, wheat flour, corn flour, or mixed grain flour; the potato flour includes, but is not limited to, potato flour or sweet potato flour; and the legume flour includes, but is not limited to, pea flour or mung bean flour. All of the above raw materials are common starch-based raw materials that are widely available, low in cost, and food-grade safe. They all contain abundant starch and can form a continuous three-dimensional gel network after gelatinization with water, providing a structural basis for subsequent pre-drying, sealing, high-temperature toughening, and cooling. Furthermore, the high-temperature toughening method of this invention does not have strict limitations on the type of starch and has universal applicability. In a specific embodiment of the present invention, without pre-drying, potato starch, wheat starch, sweet potato starch, pea starch, mung bean starch, and indica rice flour gels, after high-temperature toughening at 95 °C for 30 min, showed an increase in fracture stress of 36.5%–164.7% and an increase in fracture strain of 3.6%–158.5%, indicating that the mechanical properties of starch gels from different sources could be improved to varying degrees. For ordinary corn starch gel, when the wet basis moisture content before high-temperature toughening was 38%, the fracture stress and fracture strain after rehydration reached 111.85 kPa and 158.65%, respectively, which were 206.4% and 187.6% higher than those of the untreated gel; the tensile toughness reached 102.18 kJ / m. 3 The shear work reached 35.17±0.36 g·s, demonstrating a good balance between strength and ductility and energy absorption capacity.

[0026] In this invention, the starch-based raw material preferably includes one or more of the following: protein, edible gum, dietary fiber, polysaccharide, salts, sugars, lipids, emulsifier, and water-retaining agent. The above components can be used alone or in combination of two or more. Their dosage can be adjusted according to the texture, water-holding capacity, mechanical properties, and processing requirements of the target gel, preferably 0.5% to 10% of the starch mass, but can be 1% to 5%, or 2%, 3%, or 4%. The above components can be mixed with the starch-based raw material before gelatinization and molding, or added after the formation of the starch paste but before gelation, or added after cooling but before rehydration.

[0027] This invention provides an application of the aforementioned toughening method in improving the mechanical properties and / or structural properties of starch gels. The improvement refers to the enhancement of the mechanical and / or structural properties of the starch gel treated by the aforementioned toughening method compared to a control group that did not undergo high-temperature toughening treatment.

[0028] In this invention, the mechanical properties preferably include at least one of the following: tensile properties, stress relaxation stability, shear properties, and textural properties.

[0029] In this invention, the tensile properties represent the strength and ductility of the gel under tensile load, mainly including fracture stress, fracture strain, elastic modulus, and tensile toughness. Fracture stress reflects the gel's ability to resist tensile fracture, fracture strain reflects the gel's deformation capacity before fracture, elastic modulus reflects the gel's stiffness, and tensile toughness reflects the gel's ability to absorb energy before fracture. In specific embodiments of this invention, compared to the control group without high-temperature toughening, the tensile properties of the gel after high-temperature toughening are generally improved. For example, the fracture stress and fracture strain of ANN-53 are increased by 8.9% and 30.4% respectively compared to Native-53; compared to PD-38 with the same water content, the fracture stress of ANN-38 increases from 63.79 kPa to 111.85 kPa, and the fracture strain increases from 94.87% to 158.65%, representing increases of 75.3% and 67.2% respectively, and are 3.06 times and 2.88 times that of Native-53, respectively. At different moisture contents, as the moisture content before toughening decreases, the fracture stress generally increases, while the fracture strain first increases and then decreases. The strength-ductility balance is optimal near 38% moisture content, while the fracture stress is highest at 22% moisture content, but the fracture strain decreases, exhibiting strength-dominated hardening.

[0030] In this invention, stress relaxation stability represents the gel's ability to maintain stress under constant deformation conditions, typically characterized by stress retention rate, relaxation rate, and normalized area under stress relaxation (AUC). A higher stress retention rate, lower relaxation rate, and larger AUC indicate better relaxation stability of the gel network, enabling it to maintain load under continuous external force. In specific embodiments of this invention, compared to the un-toughened group, ANN-38 exhibits the highest stress retention rate, lowest relaxation rate, and largest AUC. Furthermore, under different water contents, the stress retention rate and AUC show a trend of first increasing and then decreasing with decreasing water content before toughening, with ANN-38 showing the highest values ​​and ANN-22 showing a significant decrease, indicating that excessively low water content is not conducive to stress retention.

[0031] In this invention, the shear performance represents the gel's ability to resist shear failure, mainly including shear work and maximum shear force. Shear work reflects the gel's ability to absorb energy throughout the shear failure process, while maximum shear force reflects the maximum force the gel can withstand against shear deformation. In specific embodiments of this invention, compared to the un-toughened group, the shear work and maximum shear force of each high-temperature toughened group are generally improved. Furthermore, under different water contents, the shear work initially increases and then decreases as the water content decreases before toughening, with ANN-38 showing the highest value, while ANN-22 remains higher than Native-53. The maximum shear force generally increases as the water content decreases before toughening, with ANN-22 showing the highest value. These results indicate that a 38% water content is more conducive to improving the gel's energy absorption capacity throughout the shear failure process.

[0032] In this invention, the textural properties include at least one of hardness, elasticity, and chewiness. Hardness represents the gel's resistance to compression deformation, elasticity represents the gel's recovery ability after deformation, and chewiness represents the energy required to chew the gel, typically related to hardness, elasticity, and cohesion. In specific embodiments of this invention, compared to the un-toughened group, the overall hardness and chewiness of each high-temperature toughened group are improved. Hardness increases with decreasing water content before toughening, and at different water contents, both hardness and chewiness increase with decreasing water content. Elasticity is optimal around 38% water content; excessively low water content mainly leads to gel hardening, while 38% water content is more conducive to balancing hardness and deformation recovery.

[0033] In this invention, the structural performance preferably includes at least one of the following: water retention, stability, and network density.

[0034] In this invention, the water-holding capacity represents the gel's ability to retain moisture, restrict water movement, and bind water to the gel network, primarily including the hydrogen bonding environment and T... 21 T 22 The relaxation time is shortened. The hydrogen bonding environment can be characterized by the peak shift of the OH stretching vibration and the R1047 / 1022 ratio in the Fourier transform infrared spectrum. A shift of the OH peak to a lower wavenumber and an increase in R1047 / 1022 generally indicate enhanced hydrogen bonding and improved short-range order. In a specific embodiment of the present invention, the OH stretching vibration peak of the high-temperature toughened group after rehydration is located at 3284.68~3291.86 cm⁻¹. -1 It is lower than Native-53's 3310.14 cm. -1 This indicates that the treatment altered the hydroxyl-related hydrogen bond environment; before rehydration, R1047 / 1022 increased from 0.23 in Native-53 to 0.42 in ANN-38, and then decreased to 0.35 in ANN-22. After rehydration, the differences between groups decreased, but the overall high-temperature toughened group was still higher than Native-53. 21 and T 22The shortening of relaxation time can be measured by low-field nuclear magnetic resonance (NMR), T 21 and T 22 The shorter the length, the more restricted the movement of water, and the tighter the binding between water and the gel network. In a specific embodiment of the present invention, as the water content decreases before high-temperature toughening, T... 21 and T 22 The significant shortening indicates that water movement is more restricted.

[0035] In this invention, stability represents the gel's ability to maintain structural integrity and stable performance under external conditions such as heat and water, mainly including any one of relative crystallinity, swelling rate, and thermal properties. The relative crystallinity can be determined by X-ray diffraction, reflecting the relative number of long-range ordered structures in the gel. In a specific embodiment of this invention, the relative crystallinity increased from 3.14% for Native-53 to 5.49% for ANN-38 and 6.48% for ANN-22, and generally increased with decreasing water content before toughening, indicating that high-temperature toughening promoted starch molecular chain rearrangement and partial recrystallization. The swelling rate can be determined by immersion testing, reflecting the degree of water absorption and swelling of the gel in water. In a specific embodiment of this invention, after immersion for 48 h, the swelling rates of Native-53, ANN-38, and ANN-22 were 133.57%, 60.95%, and 42.86%, respectively. High-temperature toughening significantly reduced the gel swelling rate, and the swelling rate decreased with decreasing water content before toughening. The thermal properties can be determined by differential scanning calorimetry, mainly including enthalpy ΔH, which reflects the energy contribution of the fusible ordered region under test conditions. In a specific embodiment of the present invention, the ΔH of the high-temperature toughening group is generally higher than that of Native-53, with ANN-53 being the highest, then decreasing as the moisture content before treatment decreases, and ANN-22 being the lowest.

[0036] In this invention, the network density represents the compactness and structural uniformity of the gel micronetwork, mainly including the pore structure, which includes any one of pore size, pore wall thickness, and pore size variation coefficient. In a specific embodiment of this invention, compared with Native-53, the pore size of each high-temperature toughening group before rehydration is generally smaller and the pore wall is generally thicker, and the pore size further decreases and the pore wall further thickens as the water content before toughening decreases. Among them, the pore size variation coefficient of ANN-38 after rehydration is 3.73%, and the pore wall thickness is 9.22±0.80 μm, forming a continuous and relatively uniform pore wall structure.

[0037] The toughening method provided by this invention can generally improve the water retention, stability, and network density of starch gels. However, different indicators show different trends with decreasing water content before toughening: water retention increases with decreasing water content; relative crystallinity and swelling ratio increase or decrease with decreasing water content in terms of stability; thermal properties decrease with decreasing water content; and network density increases with decreasing water content but may decrease uniformity. Overall, the structural properties are better around a water content of 38%. While excessively low water content can improve network density and reduce swelling ratio, it may lead to increased structural non-uniformity and decreased ductility.

[0038] This invention also provides a starch gel prepared by the aforementioned toughening method. Because this starch gel, after moisture content regulation and sealed high-temperature toughening treatment, possesses improved mechanical and structural properties, such as better tensile properties, stress relaxation stability, shear properties, textural characteristics, water retention, stability, and network density, it can be widely used in applications requiring strength, extensibility, water retention, and swelling resistance. For example, it can be used as a gelling agent, thickener, stabilizer, water-retaining agent, or edible film material in products such as jelly, vermicelli, fruit jelly, soft candy, meat products, noodle products, dairy products, and biomimetic foods; in the biomedical field, it can be used as a tissue engineering scaffold, wound dressing, hydrogel, cell culture medium, drug sustained-release carrier, or biodegradable implant material; in the agricultural field, it can be used as a soil water-retaining agent, seed coating agent, or fertilizer sustained-release carrier; and in the industrial field, it can be used as a thickener, stabilizer, gelling agent, or adsorbent material. Unless otherwise specified, the materials and equipment used in this invention are commercially available products in the field.

[0039] To further illustrate the present invention, the solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0040] Example 1 A method for toughening starch gel, comprising the following steps: (1) Mix corn starch and deionized water at a mass ratio of 1:1 and stir evenly to obtain starch slurry. The corn starch is ordinary corn starch composed of about 22% to 28% amylose and 72% to 78% amylopectin.

[0041] (2) Take 4 mL of the starch slurry prepared in step (1) and inject it into a silicone mold of 90 mm × 18 mm × 2 mm. Steam it in boiling water steam for 4 min, cool it and demold it to obtain a pre-formed corn starch gel with an initial water content of 53%.

[0042] (3) The pre-formed corn starch gel prepared in step (2) was pre-dried in an environment of 60 ℃ and 80% relative humidity for 2 h to achieve a moisture content of 38%. The moisture content was determined by drying at 105 ℃ to constant weight and calculated using the following formula: (4) The corn starch gel with a water content of 38% prepared in step (3) is vacuum sealed and treated in a 95 ℃ water bath for 30 min. Then it is immediately placed in 0 ℃ ice water to cool for 15 min to obtain a high-temperature toughened starch gel, which can also be named ANN-38.

[0043] (5) Place the ANN-38 prepared in step (4) in boiling water for 100 s to rehydrate until there is no visible unhydrated core in the cross section of the gel, and the mass change rate of two consecutive weighings at 10 s intervals is less than 1%. The water content after rehydration is 51.65%.

[0044] Example 2 The difference between this embodiment and embodiment 1 is that this embodiment does not perform the pre-drying in step (3), and the water content of the pre-formed corn starch gel is 53%; the rehydration time in step (5) is 10 s, and the water content after rehydration is 53.20%. The obtained high-temperature toughened starch gel can also be named ANN-53. The remaining steps are the same as in embodiment 1.

[0045] Example 3 The difference between this embodiment and embodiment 1 is that the pre-drying time in step (3) of this embodiment is 0.5 h, so that the water content of the pre-formed corn starch gel reaches 50%; the rehydration time in step (5) is 20 s, and the water content after rehydration is 52.32%. The obtained high-temperature toughened starch gel can also be named ANN-50. The remaining steps are the same as in embodiment 1.

[0046] Example 4 The difference between this embodiment and embodiment 1 is that the pre-drying time in step (3) of this embodiment is 1.5 h, so that the water content of the pre-formed corn starch gel reaches 44%; the rehydration time in step (5) is 60 s, and the water content after rehydration is 51.93%. The obtained high-temperature toughened starch gel can also be named ANN-44. The remaining steps are the same as in embodiment 1.

[0047] Example 5 The difference between this embodiment and embodiment 1 is that the pre-drying time in step (3) of this embodiment is 3 h, so that the water content of the pre-formed corn starch gel reaches 25%; the rehydration time in step (5) is 150 s, and the water content after rehydration is 50.30%. The obtained high-temperature toughened starch gel can also be named ANN-25. The remaining steps are the same as in embodiment 1.

[0048] Example 6 The difference between this embodiment and embodiment 1 is that the pre-drying time in step (3) of this embodiment is 5 h, so that the water content of the pre-formed corn starch gel reaches 22%; the rehydration time in step (5) is 330 s, and the water content after rehydration is 48.57%. The obtained high-temperature toughened starch gel can also be named ANN-22. The remaining steps are the same as in embodiment 1.

[0049] Example 7 The difference between this embodiment and embodiment 2 is that potato starch is used instead of corn starch as the starch-based raw material in this embodiment, while the remaining steps are the same as in embodiment 2.

[0050] Example 8 The difference between this embodiment and embodiment 2 is that wheat starch is used instead of ordinary corn starch as the starch-based raw material in this embodiment, while the remaining steps are the same as in embodiment 2.

[0051] Example 9 The difference between this embodiment and embodiment 2 is that sweet potato starch is used instead of ordinary corn starch as the starch-based raw material in this embodiment, while the remaining steps are the same as in embodiment 2.

[0052] Example 10 The difference between this embodiment and embodiment 2 is that pea starch is used instead of ordinary corn starch as the starch-based raw material in this embodiment, while the remaining steps are the same as in embodiment 2.

[0053] Example 11 The difference between this embodiment and embodiment 2 is that in this embodiment, mung bean starch is used instead of ordinary corn starch as the starch-based raw material, while the remaining steps are the same as in embodiment 2.

[0054] Example 12 The difference between this embodiment and embodiment 2 is that in this embodiment, rice flour is used instead of ordinary corn starch as the starch-based raw material, while the remaining steps are the same as in embodiment 2.

[0055] Comparative Example 1 The difference between this comparative example and Example 2 is that this comparative example does not perform the sealing high-temperature toughening treatment in step (4) and the subsequent cooling treatment, nor does it perform the rehydration treatment in step (5), resulting in a corn starch gel that has not undergone pre-drying and high-temperature toughening treatment, named Native-53.

[0056] Comparative Example 2 The difference between this comparative example and Example 3 is that this comparative example does not perform the sealing high-temperature toughening treatment in step (4) and the subsequent cooling treatment, and obtains corn starch gel that has only been pre-dried and adjusted to a wet base moisture content of 50% without high-temperature toughening treatment; before testing, rehydration is performed according to the rehydration endpoint described in step (5) of Example 3, and the resulting gel is named PD-50.

[0057] Comparative Example 3 The difference between this comparative example and Example 4 is that this comparative example does not perform the sealing high-temperature toughening treatment in step (4) and the subsequent cooling treatment, and obtains corn starch gel that has only been pre-dried and adjusted to a wet base moisture content of 44% without high-temperature toughening treatment; before testing, rehydration is performed according to the rehydration endpoint described in step (5) of Example 4, and the resulting gel is named PD-44.

[0058] Comparative Example 4 The difference between this comparative example and Example 1 is that this comparative example does not perform the sealing high-temperature toughening treatment in step (4) and the subsequent cooling treatment, and obtains corn starch gel that has only been pre-dried and adjusted to a wet base moisture content of 38% without high-temperature toughening treatment; before testing, rehydration is performed according to the rehydration endpoint described in step (5) of Example 1, and the resulting gel is named PD-38.

[0059] Comparative Example 5 The difference between this comparative example and Example 5 is that this comparative example does not perform the sealing high-temperature toughening treatment in step (4) and the subsequent cooling treatment, and obtains corn starch gel that has only been pre-dried and adjusted to a wet base moisture content of 25% without high-temperature toughening treatment; before testing, rehydration is performed according to the rehydration endpoint described in step (5) of Example 5, and the resulting gel is named PD-25.

[0060] Comparative Example 6 The difference between this comparative example and Example 6 is that this comparative example does not perform the sealing high-temperature toughening treatment in step (4) and the subsequent cooling treatment, and obtains corn starch gel that has only been pre-dried and adjusted to a wet base moisture content of 22% without high-temperature toughening treatment; before testing, rehydration is performed according to the rehydration endpoint described in step (5) of Example 6, and the resulting gel is named PD-22.

[0061] Experimental Example 1 In this experiment, the tensile properties of ANN-38, ANN-53, ANN-50, ANN-44, ANN-25, and ANN-22 prepared in Examples 1-6, and Native-53, PD-50, PD-44, PD-38, PD-25, and PD-22 prepared in Comparative Examples 1-6 were measured to investigate the effects of moisture content before high-temperature toughening and heat treatment on the tensile properties of corn starch gel. Furthermore, the tensile stress relaxation, shear properties, texture profile analysis, X-ray diffraction, Fourier transform infrared spectroscopy, differential scanning calorimetry, low-field nuclear magnetic resonance spectroscopy, scanning electron microscopy morphology, and swelling properties of ANN-53, ANN-50, ANN-44, ANN-38, ANN-25, and ANN-22 prepared in Examples 1-6, and Native-53 prepared in Comparative Example 1 were measured.

[0062] Numerical statistical analysis: All samples underwent at least three parallel tests, and results are expressed as mean ± standard deviation. SPSS 27.0 software was used to perform one-way ANOVA and Duncan's multiple comparisons for significance testing of the results. p A value < 0.05 is considered statistically significant. Use Origin 2025 for plotting. In the following tables, different lowercase letters after the same indicator data indicate statistically significant differences between groups. p <0.05).

[0063] (1) Tensile property determination The tensile properties of the composite hydrogel were determined using a TA.XT Plus C texture analyzer and an A / TG tensile fixture. The initial gauge length was 10 mm, and the speeds before, during, and after the test were 3.0 mm / s, 1.0 mm / s, and 3.0 mm / s, respectively. The trigger force was 5 g. The sample width was 18 mm, the thickness was 2 mm, and the cross-sectional area was 36 mm². 2 Calculate the stress and strain of the engineering structure based on the force-displacement curve, see [reference needed]. Figure 2 In sections A and B; the elastic modulus is taken at the same slope in the initial linear strain interval, see... Figure 2 Medium C; tensile toughness is the area under the stress-strain curve before fracture, see... Figure 2 D.

[0064] Depend on Figure 2 The results show that when the moisture content before annealing is about 53%, ANN-53 achieved a fracture stress of 39.74 kPa and a fracture strain of 71.93%, which are 8.9% and 30.4% higher than Native-53, respectively.

[0065] When the moisture content before annealing was approximately 44%, ANN-44 showed a significant change in stress compared to PD-44, in addition to an increase in strain. When the moisture content before annealing was approximately 38%, ANN-38 achieved a fracture stress of 111.85 kPa and a fracture strain of 158.65%. Compared to PD-38 with the same moisture content, gel-state heat annealing increased the fracture stress from 63.79 kPa to 111.85 kPa and the fracture strain from 94.87% to 158.65%, representing increases of 75.3% and 67.2%, respectively. At this point, the fracture stress and fracture strain of ANN-38 were 3.06 times and 2.88 times that of Native-53, respectively, while maintaining high fracture stress and strain, demonstrating a good strength-ductility balance. When the moisture content before annealing was approximately 25%, ANN-44 showed a significant increase in both stress and strain compared to PD-44. When the moisture content before annealing was approximately 22%, ANN-44 showed a significant increase in stress after toughening, reaching 198.61 kPa, compared to PD-44. However, its fracture strain was 113.39%, which was 45.26 percentage points lower than that of ANN-38. This indicates that the tensile response of the gel exhibits a non-monotonic change under different moisture contents before high-temperature toughening. Lower moisture contents primarily result in strength-driven hardening, while a better strength-ductility balance is achieved at a moisture content of 38%.

[0066] (2) Tensile stress relaxation measurement The specimen was stretched to 30% strain at 3 mm / s and held for 180 s, and the stress decay was recorded. Normalized to the initial stress σ0, a double-exponential generalized Maxwell model was used for fitting, and the fitting formula is as follows: , Formula II.

[0067] The coefficient of determination R for the fit of all samples 2 All are greater than 0.99. This represents the apparent residual stress retention term over a 180 s observation timescale. Results are shown in... Figure 3 See Table 1.

[0068] Table 1 Stress relaxation parameters of rehydrated corn starch gel

[0069] The data in the table are expressed as mean ± standard deviation (n=3); AUC is the area under the normalized stress relaxation curve in the range of 0–180 s.

[0070] Depend on Figure 3 The results in Table 1 show that ANN-38 had the highest stress retention rate, the lowest relaxation rate, and the largest AUC, with the AUC being significantly higher than the other groups. p≤0.05). AUC represents the area under the normalized stress relaxation curve within 0~180 s. The higher the AUC value, the stronger the stress retention ability of the gel under constant deformation conditions and the better the network relaxation stability. ANN-38 has the largest AUC, indicating that this high-temperature toughening gel can better maintain the load under continuous external force.

[0071] (3) Shear property determination Shear performance was determined using HDP / LKBF blades. The speeds before, during, and after the test were 3.0 mm / s, 1.0 mm / s, and 3.0 mm / s, respectively, with a trigger force of 5 g. The maximum shear force and the area under the shear force-time curve were recorded. The results are shown in Table 2.

[0072] Table 2 Shear properties of rehydrated corn starch gel

[0073] The results in Table 2 show that the shear work of ANN-38 is 35.17 ± 0.36 g·s, which is 2.13 times that of Native-53 and higher than that of the other high-temperature toughening groups; the maximum shear force generally increases with decreasing water content before high-temperature toughening. These results indicate that a water content of 38% is more beneficial for improving the energy absorption capacity of the gel throughout the shear failure process.

[0074] (4) Texture profile analysis (TPA) Texture profile analysis was performed using a P36R probe. The velocities before, during, and after the measurement were 3.0 mm / s, 1.0 mm / s, and 3.0 mm / s, respectively. Two 50% compressions were performed with a trigger force of 5 g. The results are shown in Table 3.

[0075] Table 3. Main textural parameters of rehydrated corn starch gel

[0076] The results in Table 3 show that ANN-38 has a hardness of 3772.66 ± 166.18 g and an elasticity of 0.948 ± 0.02 g; ANN-22 has the highest hardness and chewiness, but its elasticity is lower than that of ANN-38. These results indicate that excessively low water content mainly leads to gel hardening, while a water content of 38% is more conducive to balancing hardness and deformation recovery.

[0077] (5) X-ray diffraction (XRD) X-ray diffraction was performed using Cu Kα radiation at a voltage of 40 kV and a current of 40 mA. The 2θ scan range was 4°–40°, the scan rate was 1° / min, and the step size was 0.01°. The relative crystallinity was calculated using JADE software by integration within the 2θ range of 8°–32°. The relative crystallinity (%) was determined using the following formula: Depend on Figure 4 The results showed that all gels exhibited broad peaks dominated by an amorphous structure, with weakly broad peaks at approximately 17° and 20°. The relative crystallinity increased from 3.14±0.12% for Native-53 to 5.49±0.05% for ANN-38 and 6.48±0.06% for ANN-22. While ANN-22 had a higher relative crystallinity than ANN-38, its fracture strain and stress retention capabilities were lower, indicating that relative crystallinity alone cannot determine the overall mechanical properties of the gel.

[0078] (6) Fourier transform infrared spectroscopy (FTIR) The scanning wavenumber range of Fourier transform infrared spectroscopy is 4000–400 cm⁻¹. -1 The resolution is 4 cm. -1 64 scans were performed; a 1047 cm⁻¹ chromatograph was used. -1 With 1022 cm -1 The ratio of absorbance intensities at different locations characterizes the short-range order of starch molecules. Results are shown in [Figure number missing]. Figure 5 .

[0079] Depend on Figure 5 The results showed that no new characteristic absorption bands appeared in any group. Before rehydration, R1047 / 1022 increased from 0.23±0.01 in Native-53 to 0.42±0.02 in ANN-38, and then decreased to 0.35±0.01 in ANN-22. After rehydration, the differences between groups decreased, but the overall R1047 / 1022 ratio in the high-temperature toughened group was still higher than that in Native-53. The OH stretching vibration peak of the high-temperature toughened group after rehydration was located at 3284.68~3291.86 cm⁻¹. -1 It is lower than Native-53's 3310.14 cm. -1 This indicates that the treatment altered the hydroxyl-associated hydrogen bond environment.

[0080] (7) Differential scanning calorimetry (DSC) Approximately 3 mg of lyophilized powder was weighed, added to twice the mass of deionized water, and allowed to equilibrate for 24 h before differential scanning calorimetry (DSC) was performed. The scanning temperature range was 25–110 °C, and the heating rate was 10 °C / min. The results are shown in Table 4.

[0081] Table 4 Thermal properties of corn starch gel

[0082] The results in Table 4 show that the ΔH of the high-temperature toughened group decreased with decreasing water content before treatment, while the relative crystallinity increased. X-ray diffraction reflects the relative number of long-range ordered structures, and ΔH reflects the energy contribution of the fusible ordered region under the test conditions. Therefore, the comprehensive mechanical properties of the gel cannot be determined by a single relative crystallinity or enthalpy change index.

[0083] (8) Low-field nuclear magnetic resonance (LF-NMR) measurement Low-field NMR measurements were performed using a CPMG sequence with a waiting time of 4500 ms, 32 scans, a resonance frequency of 20 MHz, an echo time of 0.200 ms, and an echo number of 12000. Results are shown below. Figure 6 See Table 5.

[0084] Table 5. Low-field NMR T2 relaxation time and peak area percentage of corn starch gel.

[0085] Depend on Figure 6 The results in Table 5 show that T was detected in all groups. 21 T 22 and T 23 Three water relaxation components, of which T 22 The corresponding non-flowing water is the main water component, and the PT of each group 22 All were above 81%, while PT 23 All were below 1.3%. As the moisture content decreased before high-temperature toughening, T... 21 and T 22 Significantly shorten ( p <0.05), indicating that water movement is more severely restricted; T 23 The peak area ratio of ANN-22 was relatively low and fluctuated significantly, therefore, the overall performance of each treatment group was not ranked based on this. ANN-22 had the lowest T22, but its fracture strain, stress retention rate, and shear work after rehydration were all lower than those of ANN-38, indicating that the highest degree of moisture restriction does not necessarily equate to the best overall mechanical performance.

[0086] (9) Scanning electron microscopy morphology determination (SEM) Samples were pre-frozen at -80 °C for at least 12 h and then freeze-dried at -80 °C for 72 h. After gold sputtering onto the cross-sections of the samples, scanning electron microscopy was performed at an accelerating voltage of 5 kV. Pore size and pore wall thickness were determined using ImageJ software, and the coefficient of variation for each individual gel was calculated using the following formula: See results Figure 7 , Figure 8 See Table 6.

[0087] Table 6 Pore structure parameters of corn starch gel before and after rehydration

[0088] In the table, “—” indicates that no reliably segmented pore structure was observed in the corresponding cross-section, and therefore no quantification was performed.

[0089] Depend on Figure 7 , Figure 8 As shown in Table 6, the coefficient of variation for pore size of ANN-38 after rehydration is 3.73%, and the pore wall thickness is 9.22±0.80 μm, forming a continuous and relatively uniform pore wall structure. In contrast, the coefficient of variation for pore size of ANN-22 after rehydration is 48.50%, and the pore wall thickness is 19.51±2.44 μm, indicating higher non-uniformity in its rehydrated structure. These results are consistent with the relatively balanced strength, ductility, and stress retention capacity of ANN-38.

[0090] (10) Determination of swelling properties Unreconstituted hydrogel samples measuring 20 mm × 18 mm × 2 mm were immersed in deionized water and weighed at 1, 6, 18, 24, and 48 h. The swelling ratio was calculated using the following formula: Where W0 is the sample mass before soaking, W t The mass of the sample after soaking for time t is given. Results are shown below. Figure 9 .

[0091] Depend on Figure 9 The results showed that after soaking for 48 h, the swelling rates of Native-53, ANN-38, and ANN-22 were 133.57%, 60.95%, and 42.86%, respectively. ANN-22 had the lowest swelling rate, but its fracture strain and stress retention capacity were not the highest, indicating that the lowest swelling rate is not a sufficient condition for obtaining the optimal strength-ductility balance.

[0092] Experimental Example 2 This experimental example tested the tensile properties of high-temperature toughened gels of potato starch, wheat starch, sweet potato starch, pea starch, mung bean starch, and indica rice flour prepared in Examples 7-12, as well as the corresponding gels without high-temperature toughening treatment. The difference between the preparation method of the gel without high-temperature toughening treatment and that in Examples 7-12 is that high-temperature toughening and cooling treatment after high-temperature toughening are not performed.

[0093] The method for determining tensile properties is the same as step (1) in Test Example 1. From Figure 10The results showed that, without pre-drying, after high-temperature toughening treatment at 95 ℃ for 30 min, the fracture stress of the six starch-based gels increased by 36.5%–164.7%, and the fracture strain increased by 3.6%–158.5%. The increase varied among different plant sources, but both indicators showed a numerical increase, indicating that the high-temperature toughening method described in this invention can be used to regulate the mechanical properties of starch-based gels from different plant sources.

[0094] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for toughening starch gel, characterized in that, Includes the following steps: Starch-based raw materials are gelatinized and shaped to obtain pre-shaped starch gels; After adjusting the water content of the pre-formed starch gel to 20%~55% by volume, the pre-formed starch gel with adjusted water content is sealed, heat-treated at 80~110 ℃ for 10~50 min, and then cooled to obtain toughened starch gel.

2. The toughening method according to claim 1, characterized in that, The moisture content is controlled by pre-drying or water absorption. The pre-drying includes any one of the following: natural drying, hot air drying, constant temperature and humidity drying, or vacuum drying; The water absorption includes any one of the following: soaking, spraying, and constant humidity balance.

3. The toughening method according to claim 1, characterized in that, The heat treatment method includes any one of the following: water bath heating, steam heating, high-pressure steam treatment, and electromagnetic induction heating.

4. The toughening method according to claim 1, characterized in that, The cooling method includes any one of the following: cryogenic medium cooling, natural cooling, and forced air cooling.

5. The toughening method according to claim 1, characterized in that, The cooling process also includes rehydration, which involves placing the toughened starch gel in boiling water until there is no visible unhydrated core in the cross-section of the gel.

6. The toughening method according to claim 1, characterized in that, The starch-based raw material includes at least one of the following: cereal starch, legume starch, potato starch, and starch-containing cereal powder, potato powder, or legume powder.

7. The application of the toughening method according to claims 1 to 6 in improving the mechanical properties and / or structural properties of starch gels.

8. The application according to claim 7, characterized in that, The mechanical properties include at least one of the following: Tensile properties, stress relaxation stability, shear properties, and textural properties; The textural properties include at least one of hardness, elasticity, and chewiness.

9. The application according to claim 7, characterized in that, The structural performance includes at least one of the following: Water retention, stability, and network density.

10. The starch gel prepared by the toughening method according to claims 1 to 6.

Citation Information

Patent Citations

  • A starch double crosslinked network hydrogel and its preparation method

    CN109354719B