A biomimetic chiral room-temperature phosphorescent material, a preparation method and application thereof
By preparing a biomimetic chiral room-temperature phosphorescent material containing CNC, quinoline derivatives and polyvinyl alcohol, the problems of complex synthesis and mechanical fragility of CPL materials have been solved, achieving efficient and long-lasting phosphorescence emission and multi-channel information storage, which is suitable for fields such as information encryption and anti-counterfeiting.
Patent Information
- Application Number
- CN202611059128.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-16
- Publication Date
- 2026-11-24
AI Technical Summary
Existing CPL materials have complex synthesis routes, low chiral transfer efficiency, fragile mechanical properties of pure CNC materials, and difficulty in achieving room temperature phosphorescence effects. Traditional organic phosphorescent units have weak spin-orbit coupling effects and fast non-radiative decay.
By employing achiral organic phosphorescent molecules, CNCs, chiral modulators, and hydrophilic long-chain polymers, high asymmetry factor CPL phosphorescent materials are prepared through intermolecular forces such as hydrogen bonds to enhance spin-orbit coupling effects and triple exciton crossing processes. The self-assembly of CNCs and the selective reflection of light in chiral structures are utilized.
It achieves efficient and sustained room-temperature phosphorescence emission, enhances the mechanical properties and flexibility of the material, enables multi-channel information storage and encryption, and possesses environmental friendliness and high security.
Smart Images

Figure CN123152147A_ABST
Abstract
Description
Technical Field
[0001] This application relates to a biomimetic chiral room temperature phosphorescent material, its preparation method and application, and in particular to a method for preparing a flexible circularly polarized organic room temperature phosphorescent thin film of chiral nematic cellulose nanocrystals (CNC) and its application in the fields of information encryption and anti-counterfeiting and chiral catalysis, belonging to the field of functional luminescent material technology. Background Technology
[0002] Circularly polarized light (CPL) can be obtained by emitting left-handed and right-handed polarized light with different rotation directions from a luminescent material system. It can be regarded as the superposition of two planar linearly polarized lights with the same propagation direction and mutually perpendicular vibration direction. It has broad application prospects in 3D display devices, information storage and encryption, biochemical analysis and diagnosis, and chiral asymmetric catalysis.
[0003] Traditional CPL material construction strategies involve connecting luminescent units to chiral units via covalent bonding or supramolecular assembly. However, this approach results in relatively complex and cumbersome synthetic routes, limited chiral transfer efficiency, and a low asymmetry factor in the resulting CPLs. g lum Most of them are too low.
[0004] Chirality is a widely existing property in nature, present in microscopic biomolecules such as amino acids, proteins, and DNA, as well as in the exoskeletons and cuticles of some insects. By learning from nature and introducing luminescent units into chiral helical systems, and utilizing the selective reflection and penetration of light in chiral structures, it is possible to develop chiral circularly polarized light systems.
[0005] Cellulose nanocrystals (CNCs) can be extracted from natural materials via acid hydrolysis, exhibiting excellent environmental friendliness and biocompatibility. Their aqueous dispersions possess colloidal stability at the nanoscale, preventing excessive aggregation, and spontaneously assemble into chiral nematic liquid crystals above a threshold concentration. Therefore, biomimetic chiral structural materials can be obtained by drying CNC suspensions. However, the lack of strong intermolecular forces between CNCs results in relatively brittle mechanical properties in pure CNC-based materials, limiting their widespread adoption.
[0006] Room-temperature phosphorescent (RTP) materials typically possess long lifetimes ranging from microseconds to several seconds and relatively long afterglow emission, along with advantages such as large Stokes shift, low cost, and low toxicity. However, due to the weak spin-orbit coupling effect and rapid non-radiative decay of organic phosphorescent units, producing noticeable phosphorescence effects under everyday environmental conditions such as room temperature has always been a challenge. Summary of the Invention
[0007] The purpose of this invention is to address the shortcomings of existing technologies by providing a biomimetic chiral room-temperature phosphorescent material, its preparation method, and its applications. This invention utilizes non-chiral organic phosphorescent molecules, CNC (Chiral Coefficient of Motion), chiral modulators, and hydrophilic long-chain polymers to prepare a long-lifetime CPL phosphorescent material with a high asymmetry factor. This method rigidifies the matrix through intermolecular forces such as hydrogen bonds, effectively enhancing the spin-orbit coupling effect (SOC) and the triple exciton in the stable intersystem crossover process (ISC), thereby improving RTP efficiency and lifetime and achieving efficient and sustained RTP emission.
[0008] To achieve the above objectives, this application adopts the following technical solution:
[0009] In a first aspect, this application provides a biomimetic chiral room-temperature phosphorescent thin film material, wherein the material contains chiral units, photoluminescent units, and modulation units. The chiral units are cellulose nanocrystals (CNC), the photoluminescent units are quinoline derivatives containing nitrogen heteroatoms, and the modulation units include α-D-glucose and polyvinyl alcohol. α-D-glucose is used to modulate the reflective structural color of the material and enhance its room-temperature phosphorescence emission performance under ultraviolet excitation; polyvinyl alcohol is used to enhance the material's room-temperature phosphorescence emission performance under ultraviolet excitation and to enhance its mechanical properties.
[0010] Furthermore, the quinoline derivative containing nitrogen heteroatoms includes 4-aminoquinoline. In addition, other quinoline derivatives can be selected to achieve phosphorescence, such as 4-hydroxyquinoline and 4-quinolinecarboxylic acid. Different molecules have different fluorescent phosphorescence emission bands, and the experimental results may vary.
[0011] Furthermore, the thin film material is a composite thin film comprising a base layer and a PVA hydrophilic polymer layer; the base layer is a CNC-based chiral luminescent film prepared from a dispersion of α-D-glucose, CNC, and a quinoline derivative containing nitrogen heteroatoms.
[0012] Secondly, this application provides a method for preparing the thin film material as described in the first aspect, comprising the following steps: Step 1: Disperse α-D-glucose and quinoline derivatives containing nitrogen heteroatoms in CNC aqueous dispersion to prepare a dispersion; Step 2: Take the dispersion obtained in Step 1 and prepare a film to obtain a CNC-based chiral luminescent film; Step 3: PVA aqueous solution is poured onto the obtained CNC-based chiral luminescent film, and after drying, a biomimetic chiral room temperature phosphorescent thin film material is obtained.
[0013] Furthermore, in step 1, the mass ratio of α-D-glucose to CNC is 0-0.5, and the mass ratio of the quinoline derivative containing nitrogen heteroatoms to CNC is 0.5-2:500.
[0014] Furthermore, the film-forming method in step 2 is selected from solvent evaporation film-forming, solution casting film-forming, spin coating film-forming, spray coating film-forming, or dip-coating film-forming.
[0015] Furthermore, the film-forming method in step 2 is selected from solvent evaporation film-forming, which involves placing the container containing the dispersion in a constant temperature environment of 40-60°C (such as a constant temperature drying oven) to allow the solvent to evaporate and form a film.
[0016] Furthermore, in step 3, the mass concentration of the PVA aqueous solution is 2-4%, and the drying temperature is 40-60℃.
[0017] Thirdly, this application provides the application of the film material as described in the first aspect in packaging anti-counterfeiting, information encryption and anti-counterfeiting.
[0018] Fourthly, this application provides a method for information encryption or anti-counterfeiting encryption, comprising: constructing matrices expressing physical optical information using the thin film material and ordinary fluorescent thin film material described in any one of claims 1-3 for the parts to be encrypted; converting the matrices expressing physical optical information into matrix information using computer vision recognition technology; and translating the binary matrix into text information through an encryption / decryption protocol.
[0019] Fifthly, this application provides an anti-counterfeiting label made of the film material described in the first aspect, or made using the information encryption or anti-counterfeiting encryption method described in the fourth aspect.
[0020] The thin film described in this application possesses a certain degree of flexibility, capable of being bent 180° without structural damage. When irradiated with 254 nm, the film exhibits a fluorescence emission peak at 360 nm, and blue-violet fluorescence is observable to the naked eye. After the UV lamp is turned off, a green phosphorescence afterglow is visible to the naked eye at room temperature, with phosphorescence emission peaks located near 450 and 470 nm. The phosphorescence lifetime can reach up to 1.36 s.
[0021] The thin film exhibits chiral polarized light reflection properties. By adjusting its structure, the reflective structural color of the film can be observed under sunlight, with a reflection peak range of 479nm-653nm. Furthermore, the reflected light possesses chiral polarization, allowing it to pass through a left-handed polarizing filter but not a right-handed polarizing filter.
[0022] The thin film exhibits chiral circular polarization luminescence properties, allowing the chiral emission signal to switch according to the incident direction. Specifically, for thin films with a strong luminescence asymmetry factor, the excited chiral phosphorescence can be directly distinguished by left- or right-handed polarizers to identify emission differences, thereby constructing a multi-channel anti-counterfeiting label.
[0023] The thin film can achieve multi-channel information storage and expression through customized structural color patterns and light-emitting units, using computer image recognition technology.
[0024] Compared with the prior art, this application has the following beneficial effects: (1) This application provides a chiral biomass thin film material with fluorescence / room temperature phosphorescence emission characteristics and its preparation method. The chiral matrix is cellulose nanocrystals (CNC), and the photoluminescent unit is a quinoline derivative. This application uses biomass cellulose nanocrystals as raw materials and water as the selected dispersion solvent, which is green and environmentally friendly. By adding α-D-glucose as a regulator, the pitch of CNC during the self-assembly process is adjusted, and the reflection band is flexibly controlled, thereby obtaining thin films with different reflection structural color wavelengths.
[0025] (2) This application introduces quinoline derivatives containing nitrogen heteroatoms and utilizes the characteristic of heteroatoms to facilitate singlet-triplet intersystem crossing (ISC), enabling it to transform to the T1 state and release energy back to the ground state through phosphorescence emission at room temperature. Furthermore, quinoline derivatives can form hydrogen bonds and other intermolecular interactions with cellulose, glucose, and PVA, thereby restricting the intramolecular movement of quinoline derivatives, which is beneficial for restricting the nonradiative relaxation of its excited state. The polymer matrix reduces its contact with quenching factors in the environment, enhancing the release of energy from the excited state through radiative relaxation, thus enabling the observation of a more obvious luminescence effect. This avoids the use of inorganic materials containing heavy metals as luminescent units and has environmentally friendly characteristics.
[0026] (3) This application utilizes the chiral self-assembly property of CNC to obtain a chiral self-assembled matrix. By utilizing the selective transmission capability of the matrix to polarized light, it achieves the reflection of left-handed polarized light and the transmission of right-handed polarized light. The structural color of the film can still be observed under a left-handed polarization filter, but disappears under a right-handed polarization filter. The propagation path of photoluminescence generated by excitation sources in different directions is different in the film. The spectral overlap between the reflection band gap and the phosphorescence emission band of Q-NH2 is the key factor determining the intensity and asymmetry of CPRTP. When the band gap redshifts away from the emission peak, its CPRTP peak gradually redshifts. Therefore, the CPRTP emission position can be controlled by adjusting the α-D-glu content. Thus, chiral dual-rotation room temperature phosphorescence emission of a single film can be achieved by switching the excitation incident direction.
[0027] (4) This application overcomes the problem of brittle mechanical properties caused by the lack of strong intermolecular interactions between CNC units by casting a layer of water-soluble hydrophilic long-chain polymer onto the CNC film, thereby giving the film a certain degree of flexibility and processability, enabling non-destructive bending. The ease of processability ensures improved stability and weather resistance of the film in chiral optical applications and provides a practical strategy for mass production.
[0028] (5) Through component design and hardware and software collaboration, the biomimetic chiral room temperature phosphorescent thin film based on this application can realize a thin film matrix system to express multiple orthogonal physical optical information, which can be converted into matrix information using computer vision recognition technology, and the binary matrix can be translated into text information through encryption / decryption protocol. It can hide and store multiple string information, enhance security and information capacity; therefore, the materials of this application can be applied to the fields of information encryption and anti-counterfeiting. Attached Figure Description
[0029] Figure 1 A schematic diagram (a) shows the chemical structure and biomimetic strategy of CNC units, Q-NH2 phosphorescent units, and α-D-glucose (α-D-glu) additives, and a schematic diagram (b) shows the preparation process of PVA / CNC films.
[0030] Figure 2 The results show the fluorescence and phosphorescence emission capabilities of CNC-PVA films. Among them, a represents the fluorescence of PVA / CNC-Glu films with different α-D-glu contents under 254 nm UV excitation and the afterglow phenomenon after shutdown; b and c represent the fluorescence / phosphorescence emission spectra of PVA / CNC-Glu films with different α-D-glu contents; and d represents the phosphorescence decay lifetime of PVA / CNC-Glu films with different α-D-glu contents.
[0031] Figure 3 The results show the periodic structure, chiral structural color, and mechanical properties of PVA / CNC-Glu films. Among them, a is a photograph and SEM micrograph of the periodic structure of the structural color film with different α-D-glu contents, b is the ultraviolet-visible reflectance spectrum of the film, and c is the stress-strain curve of the film during the stretching process.
[0032] Figure 4 The results show the chiral optical properties of PVA / CNC-Glu films; where a is the normalized circular dichroism spectrum of the film, and b is a photograph of the film with different α-D-glu contents observed under left-handed and right-handed polarizers.
[0033] Figure 5 The results show the performance of stimulated chiral luminescence of PVA / CNC-Glu films; where a is a schematic diagram of the principle of obtaining circularly polarized light with different chiral directions by excitation from different incident directions; b and c are the transmission circularly polarized spectrum (CPL) and asymmetry factor detected from the top layer, respectively. g lum (c) Wavelength relationship diagram; de represents the transmission CPL detected by bottom-side excitation (d) and g lum(e) - Wavelength relationship diagram.
[0034] Figure 6 The results of the performance testing of chiral circularly polarized phosphorescence of PVA / CNC-Glu-0 thin films show that the chiral difference of phosphorescence under 310nm excitation can be observed by left / right rotating filters, and the observed signal difference is opposite depending on the incident surface.
[0035] Figure 7 This diagram illustrates the application of multi-channel information expression. Thin films with different reflective structural colors and luminescence capabilities are selected. Multi-channel information is expressed through structural color / fluorescence / phosphorescence information. Among them, a represents the thin film used at each point under the optical matrix, b represents the optical matrix observed under a right-handed filter. Since the thin film reflects left-handed polarized light, it cannot penetrate right-handed polarized light, so the structural color of the thin film cannot be observed under the right-handed filter. c represents the optical matrix pattern observed under sunlight, d represents the fluorescence pattern obtained under ultraviolet (254 nm) excitation, and e represents the phosphorescence matrix pattern observed within a few seconds after ultraviolet (254 nm) excitation is turned off. Detailed Implementation
[0036] To make the technical solution of this application clearer and easier to understand, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0037] Inspired by the reflection of light from insect exoskeletons and the emission of circularly polarized light by fireflies—specifically, the selective reflection / transmission of light within chiral periodic structures—this application designs a biomimetic chiral phosphorescent composite film. The chiral matrix is derived from biomass-based green CNC assembly units, and the phosphorescent luminescent units are derived from 4-aminoquinoline (Q-NH2), a quinoline derivative. To impart certain mechanical strength and flexibility to the film, a hydrophilic polymer layer (PVA) is added to the CNC layer.
[0038] The following description, in conjunction with specific embodiments, illustrates this point.
[0039] Unless otherwise stated, all experimental materials (including but not limited to reagents and test kits) involved in the following examples are commercially available standards or reagents.
[0040] Example 1 This embodiment provides a method for preparing a CNC-PVA-based thin film with phosphorescent properties, including the following steps: Step 1: Preparation of CNC chiral aggregates: Dissolve 4.0 mg of Q-NH2 molecules in 5.0 ml of deionized water and heat to 60-80℃. Take a certain amount of CNC aqueous dispersion with a solid content (approximately 3 wt%) and add a certain amount of the above Q-NH2 solution to make the mass ratio of Q-NH2 to CNC 1:500. Then add deionized water to dilute the above CNC dispersion to 3.0 wt%. Add α-D-glucose to the dispersion in a certain proportion, with the mass ratio of α-D-glucose to CNC ranging from 0-50%. After ultrasonically dispersing and dissolving the resulting solution, evaporate and dry at 50℃ for 12-24 hours to obtain a CNC chiral film.
[0041] Step 2: Dissolve a certain amount of PVA-1799 (average degree of polymerization ≈ 1700, degree of alcoholysis 99 mol%) in deionized water by heating and stirring at 90-100℃ to prepare a 3.0 wt% PVA aqueous solution. Pour 3.0 ml of the above PVA solution onto the CNC film. The addition of the PVA solution will cause the CNC matrix to swell again, and some PVA molecular chains will penetrate into the interface. The system will be evaporated and dried at 50℃ for 12-24 hours to obtain the composite modified film. The prepared sample is numbered PVA / CNC-Glu-X, where X represents the mass percentage of α-D-glucose and CNC.
[0042] The pouring of PVA aqueous solution causes the CNC aggregates to swell, and the heating and volatilization process promotes the upward diffusion of Q-NH2 molecules. The introduction of PVA also forms hydrogen bonds with Q-NH2 and can further restrict its intramolecular movement through the confinement space of the polymer network, thereby enhancing the room temperature phosphorescence emission of Q-NH2 in the CNC, glucose and PVA polymer environment.
[0043] The photoluminescence properties of the thin film were detected by fluorescence phosphorescence spectroscopy, and the results are as follows: Figure 2 As shown in ad. By Figure 2 As can be seen from a, under 254nm excitation, obvious fluorescence can be observed, and at room temperature, room-temperature phosphorescence afterglow emission of the film can still be observed for a few seconds after the ultraviolet excitation source is turned off. Figure 2 As shown in bc, by scanning the emission spectrum with a fluorescence-phosphorescence spectrometer, a fluorescence emission peak at 360 nm and phosphorescence emission peaks at 450 nm / 470 nm can be observed. Figure 2 d is the phosphorescence decay lifetime diagram. As can be seen from the figure, the phosphorescence lifetime at room temperature increases synchronously with the increase of glucose content, and the phosphorescence lifetime is ≥1.0s and can reach up to 1.36s.
[0044] Example 2 This embodiment provides the performance characterization or test results of the PVA / CNC-based thin film with chiral optical capabilities prepared in Example 1: The CNC assembly possesses a chiral helical periodic structure, which, according to Bragg's equation, can reflect light in a specific wavelength band. The thin film from Example 1 was selected, and its cross-sectional periodic spacing structure was observed under a scanning electron microscope. The spacing was positively correlated with the glucose content, ranging from 392 nm to 605 nm. Furthermore, the reflective structural color of the film gradually shifted from green to red and then to red. Figure 3 As shown in Figure a, the reflectance spectrum of the thin film was collected using a UV-Vis-NIR spectrometer, demonstrating that the reflectance band gradually red-shifts with increasing glucose content, as shown in Figure a. Figure 3 As shown in b. The mechanical properties of the film were tested using a universal testing machine. The results showed that the film exhibited a certain mechanical strength under tensile stress. Compared to pure CNC-based films, where the inter-unit forces are weak and the film is brittle, the introduction of PVA allows energy to be dissipated through the movement of PVA macromolecular chains under external tensile stress, effectively improving the material's durability and processability. Figure 3 As shown in c.
[0045] The chiral properties of the thin films were detected using a circular dichroism spectroscopy (CDS) instrument. The results showed that the normalized CDS spectra of PVA / CNC composite films with different α-D-glu contents all exhibited positive peak signals, and the peak positions followed the same trend as the UV-Vis reflectance spectra (479 nm-653 nm), confirming that the material has a left-handed chiral structure. Figure 4 As shown in Figure a, the reflected structural colors of the thin film under circularly polarized filters of different polarization directions were captured by a camera. The results show that the reflected structural colors of the thin film can still be observed through a left-handed polarized filter that only allows left-handed light to pass through; however, when a right-handed polarized filter that only allows right-handed light to pass through is placed above the thin film, the reflected structural colors of the thin film cannot be observed. This proves that when natural light shines on a material with a left-handed periodic structure, it can selectively reflect left-handed polarized light, such as... Figure 4 As shown in b.
[0046] Figure 5 This demonstrates the chiral luminescence properties of the thin film after UV excitation. Utilizing the selective transmission and reflection of light with specific rotational directions by CNC chiral aggregates, this embodiment achieves chiral luminescence by UV excitation of the Q-NH2 phosphorescent units contained in the thin film. Figure 5 As shown in the left figure, when the ultraviolet excitation source is incident from the top, the left-handed emission light emitted by the excited Q-NH2 molecules cannot penetrate the CNC and is reflected, while the laser-induced emission light that passes through the thin film is right-handed (…). Figure 5 bc). In contrast, such as Figure 5As shown in the right figure, when the ultraviolet excitation source is incident from the bottom layer, Q-NH2 emits photoluminescence in both the incident and outgoing directions. However, the left-handed component of the polarized light emitted back in the incident direction is blocked and reflected to the outgoing direction by the CNC layer, resulting in more left-handed component of light emission in the direction of transmission film. Figure 5 (de). This phenomenon may be due to the gradual migration of Q-NH2 molecules to the top of the film during the two evaporation-drying processes, resulting in uneven distribution of the actual light-emitting units within the film. The material exhibits g lum The value can reach up to 10^ It is on the order of 1, significantly better than most existing circularly polarized phosphorescent materials, fully demonstrating its unique chiral luminescence properties.
[0047] Example 3 This embodiment provides the application of the thin film prepared in Example 1 in the fields of anti-counterfeiting, multi-channel information integration and storage: This embodiment selects a PVA / CNC-Glu-0 thin film with a high emission asymmetry factor in the phosphorescence emission band. With a label underneath, it is excited from the top and bottom using a 310nm excitation source, and the chirality of the phosphorescence reflected in the direction of reflection is observed through left-hand and right-hand circularly polarized filters. Based on previous CPL experimental results, when irradiated from the top, right-hand circularly polarized light passes through the system more easily, while left-hand circularly polarized light is emitted. Therefore, the circularly polarized phosphorescence reflected in the observation direction exhibits a strong left-hand characteristic, passing well through a left-hand circularly polarized filter but not well through a right-hand circularly polarized filter. Similarly, when irradiated from the bottom, the chirality of the phosphorescence signal reflected in the incident direction is reversed, achieving switchable chirality of room-temperature circularly polarized phosphorescence (CPRTP) of the same material. Figure 6 As shown, it is expected to be used in fields such as high-end packaging anti-counterfeiting.
[0048] As attached Figure 7 As shown, the film from Example 1, the film without phosphorescent unit Q-NH2 (n-PVA / CNC-Glu-0, except that Q-NH2 solution was not added, the other steps were the same as in Example 1), and the film without Q-NH2 but with the same mass content of fluorescent unit Naph-NH2 ((2-aminoethyl)naphthalimide, CAS: 162265-51-2) (Naph-PVA / CNC-Glu-0, without Q-NH2 solution added during preparation, but with the same mass of Naph-NH2 introduced, the other steps were the same as in Example 1) were selected. Small holes were obtained using a punch, and the films were arranged to form a lattice, as shown. Figure 7 As shown in Figure a. The matrix system erases information by covering the chiral structural color information with a right-handed polarizing film, thus preventing the observation of the information. Figure 7As shown in b. By observing the pattern under sunlight / UV illumination / UV off instants, matrix encoding information of reflected structural colors, fluorescence, and phosphorescence can be obtained, such as... Figure 7 As shown in ce. Figure 7 d represents the fluorescence pattern of the thin film matrix under 254nm ultraviolet light irradiation. Thin films containing Q-NH2 and Naph-NH2 exhibit obvious blue fluorescence. Figure 7 e indicates that when the ultraviolet excitation source is turned off, only the thin film containing Q-NH2 can achieve phosphorescent afterglow emission. The detected physical optical signals are converted into an information encoding matrix using technologies such as computer vision, and then converted into text information through specific computing protocols and text translation protocols (such as Morse code), thereby realizing the integration and encryption of multi-channel information. This allows it to be used as an optical functional element in fields such as flexible display devices, anti-counterfeiting labels, and data encryption systems.
[0049] The above description is merely a preferred embodiment of this application and is not intended to limit this application in any form or substance. It should be noted that those skilled in the art can make several improvements and additions without departing from this application, and these improvements and additions should also be considered within the scope of protection of this application.
Claims
1. A biomimetic chiral room-temperature phosphorescent thin film material, characterized in that, The material contains a chiral unit, a photoluminescent unit, and a regulating unit. The chiral unit is a cellulose nanocrystal (CNC), the photoluminescent unit is a quinoline derivative containing nitrogen heteroatoms, and the regulating unit includes α-D-glucose and polyvinyl alcohol.
2. The thin film material according to claim 1, characterized in that, The quinoline derivative containing nitrogen heteroatoms is 4-aminoquinoline.
3. The thin film material according to claim 1, characterized in that, The film material is a composite film comprising a base layer and a PVA hydrophilic polymer layer; the base layer is a CNC-based chiral luminescent film prepared from a dispersion of α-D-glucose, CNC, and a quinoline derivative containing nitrogen heteroatoms.
4. A method for preparing the thin film material according to any one of claims 1-3, characterized in that, Includes the following steps: Step 1: Disperse α-D-glucose and quinoline derivatives containing nitrogen heteroatoms in CNC aqueous dispersion to prepare a dispersion; Step 2: Take the dispersion obtained in Step 1 and prepare a film to obtain a CNC-based chiral luminescent film; Step 3: PVA aqueous solution is poured onto the obtained CNC-based chiral luminescent film, and after drying, a biomimetic chiral room temperature phosphorescent thin film material is obtained.
5. The preparation method according to claim 4, characterized in that, In step 1, the mass ratio of α-D-glucose to CNC is 0-0.5:1, and the mass ratio of quinoline derivatives containing nitrogen heteroatoms to CNC is 0.5-2:
500.
6. The preparation method according to claim 4, characterized in that, The film-forming method in step 2 is selected from solvent evaporation film-forming, solution casting film-forming, spin coating film-forming, spray coating film-forming, or dip-coating film-forming.
7. The preparation method according to claim 4, characterized in that, In step 3, the mass concentration of the PVA aqueous solution is 2-4%, and the drying temperature is 40-60℃.
8. The application of the film material according to any one of claims 1-3 in packaging anti-counterfeiting, information encryption and anti-counterfeiting.
9. A method for information encryption or anti-counterfeiting encryption, characterized in that, include: The parts that need to be encrypted are constructed using the thin film material described in any one of claims 1-3 and ordinary fluorescent thin film material to form matrices expressing physical optical information. The matrices expressing physical optical information are converted into matrix information using computer vision recognition technology, and the binary matrix is translated into text information through an encryption / decryption protocol.
10. An anti-counterfeiting label, characterized in that, It is made using the thin film material as described in claim 1, or using the information encryption or anti-counterfeiting encryption method as described in claim 9.