A mylar film, a method for preparing the same and a battery
By setting a liquefactive gas-absorbing membrane on the surface of the Mylar membrane, the gas in the battery cell is eliminated through physical adsorption and chemical reaction, which solves the problem of swelling of square aluminum-cased lithium batteries, realizes the control of internal pressure and the extension of battery life, and has the functions of insulation and protection.
Patent Information
- Application Number
- CN202611327618.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing Mylar membranes cannot effectively solve the problems of cell swelling, capacity decay, and safety hazards caused by gas accumulation during the charging and discharging process of square aluminum-cased lithium batteries.
A liquefaction-repellent membrane is formed on the surface of the Mylar membrane, comprising a liquefaction-repellent component and a gas-repellent component. The liquefaction-repellent component includes a fluorinated liquefaction-repellent structure, and the gas-repellent component includes a physical adsorbent and a lithium-based chemical degassing agent. The gas generated by the battery cell is eliminated through physical adsorption and chemical reaction, thereby reducing the internal pressure and stabilizing the electrode interface.
It effectively absorbs the gas generated by the battery cell, reduces internal pressure, inhibits cell swelling, stabilizes the electrode interface, extends battery life, and maintains the insulation, puncture resistance, and dimensional stability of the Mylar film, while being compatible with existing battery mass production processes.
Smart Images

Figure CN123152148A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, specifically to a Mylar membrane, its preparation method, and a battery. Background Technology
[0002] In recent years, the application demand for lithium-ion batteries has increased significantly. Square aluminum-cased lithium batteries have become the mainstream cell form for power batteries and large-scale energy storage power stations due to their advantages of high structural rigidity, uniform heat dissipation, and strong assembly reliability. During the charging, discharging, or storage of the cell, side reactions such as electrolyte decomposition, SEI membrane damage and regeneration, and trace water decomposition will continuously occur inside the cell, stably generating gases (such as CO2, CO, CH4, C2H4, HF, etc.). The square aluminum shell has extremely small deformation, making it easy for the generated gas to accumulate inside the battery cell, triggering a series of vicious chain problems. Common problems include: the internal pressure of the battery cell continuously rises, forcing the electrode assembly to deform under pressure, causing the electrode sheet to separate from the diaphragm interface, and increasing the contact resistance; the tabs are subjected to long-term compressive stress, resulting in microcracks and a surge in internal resistance; uneven distribution of electrolyte inside the battery cell intensifies local side reactions, further accelerating gas production, forming a vicious cycle of "gas production - swelling - deterioration - more gas production", which ultimately manifests as battery cell swelling, rapid capacity drop, and significant reduction in cycle life. In severe cases, it may trigger the premature opening of the explosion-proof valve, causing battery cell leakage and failure, posing a safety hazard.
[0003] Mylar membrane is a standard insulating material for square aluminum-cased battery cells. It features excellent insulation, dimensional stability, electrolyte resistance, and low thermal shrinkage. It is primarily used to isolate the aluminum casing from the cell's electrode assembly, preventing short circuits, punctures, and lithium-intercalation corrosion of the casing. However, currently commercially available Mylar membranes only offer basic physical protection and cannot address the industry-wide pain points of cell gas circulation and swelling.
[0004] Currently, industry solutions for lithium battery gas generation and swelling mainly include: thickening the casing, optimizing the explosion-proof valve structure, and adding electrolyte gas-suppressing additives. However, for the thickening casing solution, the thickened casing can only passively withstand internal pressure and cannot eliminate the generated gas; for the solution of optimizing the explosion-proof valve structure, the pressure relief of the explosion-proof valve will cause electrolyte loss and imbalance of the cell system, and the leaked flammable gas poses a safety risk. For the solution of adding electrolyte gas-suppressing additives, it can only slow down the gas generation rate and cannot consume the existing gas, so the gas accumulation problem still exists after long-term circulation.
[0005] Therefore, providing a Mylar membrane that can both isolate the battery casing from the cell electrode assembly and have the ability to absorb gas generated, thus avoiding the adverse effects of gas generation on the battery, is a technical problem that urgently needs to be solved. Summary of the Invention
[0006] In view of the above-mentioned technical problems existing in the prior art, the purpose of this application is to provide a Mylar membrane, its preparation method and battery.
[0007] To achieve the above objectives, this application adopts the following technical solution: In a first aspect, this application provides a Mylar membrane, the Mylar membrane comprising a base membrane and a liquefactive gas-absorbing membrane disposed on the surface of the base membrane, the liquefactive gas-absorbing membrane comprising a liquefactive component and a gas-absorbing component, the gas-absorbing component being selected from physical adsorbents and / or lithium-based chemical degassing agents.
[0008] In one embodiment, the hydrophobic component includes a fluorinated hydrophobic structure derived from at least one of a fluorosilane coupling agent, a perfluoropolyether, or a perfluoroalkyl acrylate polymer.
[0009] In one embodiment, the lyophobic component coats the getter component to form a lyophobically modified getter component.
[0010] In one embodiment, the lithium-based chemical degassing agent comprises lithium hydroxide and / or lithium carbonate.
[0011] In one embodiment, the lithium-based chemical degassing agent is a nanoparticle.
[0012] In one embodiment, the physical adsorbent includes at least one of molecular sieves, metal-organic framework materials, and mesoporous silica.
[0013] In one embodiment, the molecular sieve includes one of 13X molecular sieve, 4A molecular sieve, or 5A molecular sieve.
[0014] In one embodiment, the specific surface area of the molecular sieve is ≥580 m². 2 / g, preferably 600m 2 / g~700 m 2 / g.
[0015] In one embodiment, the metal-organic framework material comprises a high-rigidity Zr-based insulating MOF.
[0016] In one embodiment, the metal-organic framework material has a specific surface area ≥1200 m². 2 / g, preferably 1400m 2 / g~1800 m 2 / g.
[0017] In one embodiment, the specific surface area of the mesoporous silica is ≥180 m². 2 / g, preferably 200m 2 / g~250m 2 / g.
[0018] In one embodiment, the contact angle of the liquefying getter membrane with the electrolyte is ≥110°.
[0019] In one embodiment, the thickness of the liquefactive getter membrane on one side is 2 μm to 5 μm, preferably 2.5 μm to 3.5 μm.
[0020] In one embodiment, the pore size of the liquefactive getter membrane is in the range of 0.2 μm to 3 μm.
[0021] In one embodiment, the liquefying getter membrane further includes an adhesive.
[0022] In one embodiment, the adhesive comprises polyvinylidene fluoride and polytetrafluoroethylene, and is free of sodium carboxymethyl cellulose, wherein the mass ratio of polyvinylidene fluoride to polytetrafluoroethylene is preferably 7:3 to 8.5:1.5.
[0023] In one embodiment, the total content of the liquid-repellent component and the gas-absorbing component is 75% to 98%, based on the total mass of the liquid-repellent getter membrane as 100%.
[0024] In one embodiment, with the total mass of the liquefying getter membrane as 100%, the mass ratio of the physical adsorbent to the lithium-based chemical degassing agent in the getter component is (40~50):(35~50).
[0025] In one embodiment, the liquid-repellent component accounts for 1% to 2% of the mass of the getter component.
[0026] In one embodiment, the content of the binder is 5% to 10% based on the total mass of the liquid-repellent getter membrane as 100%.
[0027] In one embodiment, the base film is at least one of polypropylene (PP) film, polyethylene terephthalate (PET) film, or PET / PP composite film.
[0028] In one embodiment, the thickness of the base film is 50 μm to 150 μm.
[0029] Secondly, this application provides a method for preparing a Mylar membrane, the method comprising the following steps: (1) Provide a slurry comprising a liquid-repellent component, a getter component, a binder, and a solvent; The gas-absorbing component is selected from physical adsorbents and / or lithium-based chemical degassing agents; (2) The slurry is coated on the surface of the base film and dried to obtain a Mylar film.
[0030] In one embodiment, step (1) includes: mixing the liquid-repellent component, the air-getting component and a solvent and performing a liquid-repellent modification reaction to obtain a liquid-repellent modified air-getting component, and mixing the liquid-repellent modified air-getting component with a binder to obtain a slurry.
[0031] In one embodiment, the solvent comprises ethanol and N-methylpyrrolidone, wherein the volume ratio of ethanol to N-methylpyrrolidone is preferably 2:8 to 4:6.
[0032] In one embodiment, the solid content of the slurry is 33% to 38%.
[0033] In one embodiment, the viscosity of the slurry was tested using a rotational viscometer at a rotational speed of 12 r / min and using a No. 3 rotor. The viscosity of the slurry was measured to be 8000 mPa·s to 12000 mPa·s.
[0034] In one embodiment, during the preparation of the slurry, the conditions for the hydrophobic modification reaction are: a constant temperature water bath at 45℃~55℃.
[0035] In one embodiment, during the preparation of the slurry, the time for the hydrophobic modification reaction is 90 min to 120 min.
[0036] In one embodiment, the hydrophobic modification reaction is accompanied by stirring at a speed of 300 r / min to 400 r / min.
[0037] In one embodiment, during the preparation of the slurry, after the hydrophobic modification reaction is completed, the resulting reaction product is dried.
[0038] In one embodiment, during the preparation of the slurry, the liquid-repellent modified air-getting component is mixed with the binder and then subjected to high-speed sand milling. The high-speed sand milling speed is 800 r / min to 1200 r / min, and the high-speed sand milling time is 30 min to 60 min.
[0039] In one embodiment, after drying in step (2), the obtained Mylar film is subjected to static aging, and the static aging time is preferably 8h~15h.
[0040] Thirdly, this application provides a battery including a housing and a cell electrode assembly and an electrolyte located inside the housing. The surface of the electrode assembly is covered with the Mylar membrane described in the first aspect, wherein one side of the Mylar membrane, which is hydrophobic and gas-absorbing, faces the cell electrode assembly, and the other side of the Mylar membrane faces the housing.
[0041] In one embodiment, the Mylar membrane fully covers the surface of the cell electrode assembly, leaving only a tab lead-out position.
[0042] In one embodiment, the cell electrode assembly is a square electrode assembly, including a first end face and a second end face arranged opposite each other, a top face and a bottom face arranged opposite each other, and two side faces arranged opposite each other. The Mylar membrane covers all six faces, leaving only the electrode tab lead-out position.
[0043] In one embodiment, a Mylar membrane is provided at the gap between the battery cell electrode assembly and the casing, and at the contact area between the electrode tab and the casing.
[0044] In one embodiment, the housing includes a cell cover plate, and a plurality of plastic strips are disposed on the surface of the cell cover plate near the cell electrode assembly. The Mylar membrane is fixed to the plastic strips on the side near the cell cover plate by heat fusion.
[0045] Compared with existing technologies, this application has the following advantages: (1) This application provides a liquefactive gas-absorbing membrane on the surface of the base membrane. The gas-absorbing components impart gas generation and absorption capabilities to the Mylar membrane through physical adsorption and / or chemical curing. This allows for in-situ consumption and circulation of gas within the battery cell sealing system, reducing the internal pressure of the battery cell, inhibiting battery cell swelling, stabilizing the electrode interface, and slowing down battery cell performance degradation. Simultaneously, the liquefactive components endow the liquefactive gas-absorbing membrane with the properties of being permeable to air but impermeable to liquid. The electrolyte cannot wet the liquefactive gas-absorbing layer, thus fundamentally avoiding the problems of side reactions such as hydrolysis and catalytic decomposition caused by the contact between the components in the liquefactive gas-absorbing membrane and the electrolyte. Moreover, the Mylar membrane of this application retains the excellent insulation, puncture resistance, electrolyte resistance, and dimensional stability of traditional Mylar membranes. The Mylar membrane can fill the gap between the battery cell electrode assembly and the battery casing, and its mechanical strength constrains the deformation of the battery cell electrode assembly, achieving a dual anti-swelling effect of "pressure reduction + positioning".
[0046] (2) The preparation method of the Mylar membrane in this application is simple, fully compatible with the existing battery mass production process, and has strong industrialization potential.
[0047] (3) The electrolyte contact angle of the Mylar membrane of this application is 93° or more, preferably 111° or more; the capacity retention rate after 1000 battery cycles is 93.9% or more, preferably 94.5% or more; the expansion force after 1000 cycles is 1294 kgf or less, preferably 1193 kgf or less; the thickness expansion rate after 1000 cycles is 2.89% or less, preferably 2.30% or less; and the increase in internal resistance after high-temperature storage is 20.9% or less, preferably 14.7% or less. Attached Figure Description
[0048] Figure 1 This is a process flow diagram of the preparation process of Mylar membrane provided in one embodiment of this application.
[0049] Figure 2This is a schematic diagram of the structure of a Mylar membrane provided in one embodiment of this application, wherein 1 is a base membrane; and 2 is a liquid-repellent and air-absorbing membrane. Detailed Implementation
[0050] The technical solution of this application will be further described below through specific implementation methods.
[0051] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments.
[0052] The specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of this application.
[0053] In one embodiment, this application provides a Mylar membrane, which includes a base membrane and a liquefactive gas-absorbing membrane disposed on the surface of the base membrane. The liquefactive gas-absorbing membrane includes a liquefactive component and a gas-absorbing component, wherein the gas-absorbing component is selected from physical adsorbents and / or lithium-based chemical degassing agents.
[0054] One embodiment of this application involves providing a liquefactive getter membrane on the surface of a base membrane. The getter components impart gas generation and absorption capabilities to the Mylar membrane through physical adsorption and / or chemical curing. This allows for in-situ consumption and circulation of gas within the battery cell sealing system, reducing internal cell pressure, inhibiting cell swelling, stabilizing the electrode interface, and slowing down cell performance degradation. Simultaneously, the liquefactive components endow the liquefactive getter membrane with the properties of being permeable to air but impermeable to liquid, preventing the electrolyte from wetting the liquefactive getter layer. This fundamentally avoids side reactions such as hydrolysis and catalytic decomposition caused by contact between the components in the liquefactive getter membrane and the electrolyte. Furthermore, the Mylar membrane of this application retains the excellent insulation, puncture resistance, electrolyte resistance, and dimensional stability of traditional Mylar membranes. The Mylar membrane can fill the gap between the battery cell electrode assembly and the battery casing, relying on its mechanical strength to constrain the deformation of the battery cell electrode assembly, achieving a dual anti-swelling effect of "voltage reduction + limiting".
[0055] In one embodiment of this application, the physical adsorbent has a porous structure, which can quickly capture instantaneous gas production and suppress internal pressure rise; the lithium-based chemical degassing agent can undergo an irreversible reaction with the gas in the battery cell, permanently solidifying the gas (e.g., HF, CO2) into a stable solid product.
[0056] In one embodiment, the hydrophobic component includes a fluorinated hydrophobic structure derived from at least one of a fluorosilane coupling agent, a perfluoropolyether, or a perfluoroalkyl acrylate polymer.
[0057] In one embodiment, the fluorosilane coupling agent may be at least one of perfluorooctyltriethoxysilane, perfluorodecyltriethoxysilane, perfluorooctyltrimethoxysilane, and perfluorodecyltrimethoxysilane.
[0058] In one embodiment, the fluorosilane coupling agent undergoes a condensation reaction with the hydroxyl groups on the surface of the getter component to form a chemically bonded surface-modified layer. The final product still contains a fluorinated hydrophobic structure derived from the fluorosilane coupling agent, which is fixed to the surface of the getter component in a coating form.
[0059] In one embodiment, the lyophobic component coats the getter component to form a lyophobically modified getter component.
[0060] In one embodiment, the lithium-based chemical degassing agent comprises lithium hydroxide and / or lithium carbonate.
[0061] By way of example, but not limitation, the equation for the reaction between a lithium-based chemical degassing agent and the gas in the battery cell is as follows: LiOH + HF = LiF↓ + H2O (1) 2LiOH + CO2 = Li2CO3 + H2O (2) Li2CO3+HF=2LiF↓+CO2↑+H2O(3) By using lithium-based chemical degassing agents to react chemically with the gases in the battery cell, gases such as HF and CO2 are removed, which can permanently eliminate HF corrosion and block the continuous decomposition of the electrolyte; CO2 is effectively captured, which can inhibit the swelling of the battery cell and prevent the internal pressure of the battery cell from rising.
[0062] In one embodiment, the liquefaction-gathering membrane includes a physical adsorbent and a lithium-based chemical degassing agent. The advantages of this configuration are twofold: firstly, the synergistic effect of physical and chemical action forms a kinetic synergy mechanism of instantaneous buffer adsorption + long-term permanent curing, resulting in better degassing and preventing high-temperature desorption and secondary gas release; secondly, after the lithium-based chemical degassing agent reacts with the gas in the battery cell, the resulting reaction products (such as LiF, LiCO3, and trace byproduct H2O) are adsorbed and sealed by the physical adsorbent. Therefore, the reaction products are completely confined within the liquefaction-gathering membrane, preventing them from escaping into the electrolyte and thus avoiding increased interfacial impedance or corrosion of the current collector.
[0063] In one embodiment, the lithium-based chemical degassing agent is a nanoparticle. In this application, nanoparticles refer to particles with a volume average particle size (D50) measured by a laser particle size analyzer within the range of 100 nm to 1000 nm (exemplarily, the volume average particle size D50 can be 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, or 1000 nm, etc.), preferably within the range of 200 nm to 500 nm. The advantages of using nanoparticles are: firstly, nanoparticles have a high specific surface area, resulting in a large contact area with HF and CO2 gases, leading to faster chemical reaction kinetics and enabling real-time solidification of gas generation within the battery cell, avoiding short-term gas accumulation that causes internal pressure fluctuations; secondly, the small size of nanoparticles ensures uniform dispersion when mixed with molecular sieves, metal-organic framework materials, and mesoporous silica, preventing clogging of the micropores of the physical adsorption materials and facilitating the synergistic effect of physical adsorption and chemical degassing.
[0064] In one embodiment, the physical adsorbent includes at least one of molecular sieves, metal-organic framework materials, and mesoporous silica.
[0065] In one embodiment, the molecular sieve includes one of 13X molecular sieve, 4A molecular sieve, or 5A molecular sieve.
[0066] In one embodiment, the molecular sieve is a low-sodium molecular sieve (where the soluble sodium content is <10ppm) or a lithium-modified molecular sieve.
[0067] In one embodiment, the specific surface area of the molecular sieve is ≥580 m². 2 / g, for example, could be 580m 2 / g、585m 2 / g、590m 2 / g、595m 2 / g、600m 2 / g、605m 2 / g、610m 2 / g、615m 2 / g、620m 2 / g、625m 2 / g、630m 2 / g、635m 2 / g、640m 2 / g、645m 2 / g、650m 2 / g、660m 2 / g、670m 2 / g、680m 2 / g、690m 2 / g、700m 2 / g、710m2 / g or 720m 2 / g, etc., preferably 600m 2 / g~700m 2 / g.
[0068] In one embodiment, the molecular sieve is a 13X molecular sieve, and the specific surface area of the 13X molecular sieve is 580 m². 2 / g~720m 2 / g, if the specific surface area is higher than 720m² 2 / g, which can easily lead to excessive water and liquid absorption, damaging the hydrophobic layer.
[0069] In one embodiment, the metal-organic framework material comprises a high-rigidity Zr-based insulating MOF.
[0070] Introducing a high-rigidity Zr-based insulating MOF into the liquid-repellent getter membrane helps maintain the integrity of the pores in the long term, ensuring the long-term stability of the getter performance of the liquid-repellent getter membrane.
[0071] In one embodiment, the metal-organic framework material has a specific surface area ≥1200 m². 2 / g, for example, could be 1200m 2 / g、1250m 2 / g、1300m 2 / g, 1350m 2 / g, 1400m 2 / g, 1450m 2 / g, 1500m 2 / g, 1550m 2 / g, 1600m 2 / g、1650m 2 / g、1700m 2 / g、1750m 2 / g or 1800m 2 / g, etc., preferably 1400m 2 / g~1800m 2 / g. If the specific surface area of a metal-organic framework material is too large, the rigidity of the framework decreases, and the material is prone to pore collapse under pressure.
[0072] In one embodiment, the specific surface area of the mesoporous silica is ≥180 m². 2 / g, for example, could be 180m 2 / g、185m 2 / g、190m 2 / g、195m 2 / g、200m 2 / g、205m 2 / g、210m 2 / g、220m 2 / g、225m 2 / g、230m 2 / g、235m 2 / g、240m 2 / g、250m 2 / g、255m 2 / g、260m 2 / g、265m 2 / g、270m 2 / g or 280m 2 / g, etc., preferably 200m 2 / g~250m 2 / g. If the specific surface area of mesoporous silica is too large, it can easily lead to orange peel-like coating.
[0073] In one embodiment, the contact angle of the liquid-repellent getter membrane with the electrolyte is ≥110°, for example, it can be 110°, 112°, 115°, 117°, 120°, 122°, 124°, 127°, 130°, 135°, 138°, 140°, 143°, 146°, 148°, or 150°. This indicates that the liquid-repellent getter membrane has a stable liquid-repellent effect.
[0074] In one embodiment, the thickness of the liquid-repellent getter membrane on one side is 2μm to 5μm, for example, it can be 2μm, 2.2μm, 2.5μm, 2.8μm, 3μm, 3.3μm, 3.6μm, 4μm, 4.2μm, 4.5μm, 4.8μm or 5μm, preferably 2.5μm to 3.5μm; In one embodiment, the pore size of the liquefactive getter membrane is in the range of 0.2 μm to 3 μm. For example, the pore size can be 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.3 μm, 1.5 μm, 1.8 μm, 2 μm, 2.3 μm, 2.5 μm, 2.7 μm, or 3 μm, etc.
[0075] In one embodiment, the liquefying getter membrane further includes an adhesive.
[0076] In one embodiment, the binder comprises polyvinylidene fluoride and polytetrafluoroethylene, and does not contain sodium carboxymethyl cellulose. This preferred embodiment uses a hydrolysis-resistant and aging-resistant binder, ensuring long-term, firm adhesion of the liquid-repellent getter membrane to the base membrane surface, preventing powder shedding and free impurities during cycling, and mitigating micro-short circuit safety risks.
[0077] In this embodiment, the adhesive does not contain sodium carboxymethyl cellulose because sodium carboxymethyl cellulose is easily hydrolyzed by electrolyte, trace amounts of water inside the battery cell, HF, etc. After hydrolysis, it loses its adhesive strength, causing the liquid-repellent gas-absorbing membrane to pulverize and fall off, thus reducing the gas-absorbing effect.
[0078] In one embodiment, the mass ratio of the polyvinylidene fluoride to the polytetrafluoroethylene is 7:3 to 8.5:1.5, for example, it can be 7:3, 7.5:2.5, 8:2 or 8.5:2.5, etc.
[0079] In one embodiment, based on the total mass of the liquefactive getter membrane as 100%, the total content of the liquefactive component and the getter component is 75% to 98%, for example, it can be 75%, 78%, 80%, 82%, 85%, 88%, 90%, 92%, 95% or 98%, etc.
[0080] In one embodiment, with the total mass of the liquefactive getter membrane as 100%, the mass ratio of the physical adsorbent to the lithium-based chemical degassing agent in the getter component is (40~50):(35~50), wherein the physical adsorbent is selected from the range of "40~50", for example, it can be 40, 42, 43, 45, 46, 48 or 50, etc.; the lithium-based chemical degassing agent is selected from the range of "35~50", for example, it can be 35, 36, 38, 40, 42, 44, 46, 48 or 50, etc.
[0081] In one embodiment, the mass percentage of the lyophobic component relative to the getter component is 1% to 2%, for example, it can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, or 2%.
[0082] In one embodiment, the content of the binder is 5% to 10% based on the total mass of the liquid-repellent getter membrane as 100%, for example, it can be 5%, 6%, 7%, 8%, 9% or 10%, etc.
[0083] In one embodiment, the base film is at least one of polypropylene (PP) film, polyethylene terephthalate (PET) film, or PET / PP composite film.
[0084] In one embodiment, the thickness of the base film is 50 μm to 150 μm, for example, it can be 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm or 150 μm.
[0085] In another embodiment, this application provides a method for preparing the Mylar membrane as described above, comprising the following steps: (1) Provide a slurry comprising a liquid-repellent component, a getter component, a binder, and a solvent; The gas-absorbing component is selected from physical adsorbents and / or lithium-based chemical degassing agents; (2) The slurry is coated on the surface of the base film and dried to obtain a Mylar film.
[0086] The method provided in one embodiment of this application is simple, fully compatible with existing battery mass production processes, and has strong industrial applicability.
[0087] In one embodiment, step (1) includes: mixing the hydrophobic component, the getter component, and a solvent and performing a hydrophobic modification reaction to obtain a hydrophobic modified getter component; and mixing the hydrophobic modified getter component with a binder to obtain a slurry. This technical solution facilitates the formation of a hydrophobic getter membrane with a uniform, hydrophobic inner wall, and a permeable but liquid-impermeable microporous structure, free from localized hydrophilic structures. Gases generated during charging, discharging, or high-temperature storage of the battery cell can freely pass through the hydrophobic permeable membrane, while the electrolyte cannot wet the membrane. This fundamentally avoids side reactions such as hydrolysis and catalytic decomposition caused by contact between the components in the hydrophobic permeable membrane and the electrolyte.
[0088] In one embodiment, the solvent includes ethanol and N-methylpyrrolidone (NMP).
[0089] In one embodiment, the volume ratio of ethanol to N-methylpyrrolidone is 2:8 to 4:6, for example, it can be 2:8, 2.5:7.5, 3:7, 3.5:6.5, or 4:6. Ethanol is used to regulate the hydrolysis rate of fluorosilanes and prevent the self-aggregation of fluorosilane coupling agents; NMP has strong polarity and can penetrate into the micropores of physical adsorbents to achieve global modification of the powder, and NMP is a good solvent for polyvinylidene fluoride (PVDF), which is beneficial for subsequent pulping. The volume ratio of ethanol and NMP within the above-mentioned range ensures a balance between modification and dispersion.
[0090] In one embodiment, the solid content of the slurry is 33% to 38%, for example, it can be 33%, 34%, 35%, 36%, 37% or 38%, etc.
[0091] In one embodiment, a rotational viscometer is used to test the viscosity of the slurry at a rotational speed of 12 r / min. A No. 3 rotor is used, and the viscosity of the slurry is measured to be 8000 mPa·s to 12000 mPa·s, for example, 8000 mPa·s, 8500 mPa·s, 9000 mPa·s, 9500 mPa·s, 10000 mPa·s, 10500 mPa·s, 11000 mPa·s, 11500 mPa·s, or 12000 mPa·s, etc.
[0092] In one embodiment, during the preparation of the slurry, the conditions for the hydrophobic modification reaction are: a constant temperature water bath of 45℃~55℃. For example, the constant temperature can be 45℃, 46℃, 47℃, 48℃, 49℃, 50℃, 51℃, 52℃, 53℃, 54℃, or 55℃, etc.
[0093] In one embodiment, during the preparation of the slurry, the time for the hydrophobic modification reaction is 90 min to 120 min, for example, it can be 90 min, 95 min, 100 min, 105 min, 110 min, 115 min or 120 min, etc.
[0094] In one embodiment, the hydrophobic modification reaction is accompanied by stirring at a speed of 300 r / min to 400 r / min, for example, 300 r / min, 320 r / min, 330 r / min, 340 r / min, 350 r / min, 360 r / min, 370 r / min, 380 r / min, 390 r / min or 400 r / min, etc.
[0095] In one embodiment, during the preparation of the slurry, after the hydrophobic modification reaction is completed, the resulting reaction product is dried.
[0096] One embodiment of this application can improve the uniformity of coating of the liquid-repellent component onto the getter component by adjusting the process parameters of mixing the liquid-repellent component, the getter component and the solvent and carrying out the liquid-repellent modification reaction.
[0097] In one embodiment, the uniformity deviation of the coating of the lyophobic component onto the uptake component is ≤3%, with no localized lyophilic regions.
[0098] In one embodiment, during the preparation of the slurry, the liquid-repellent modified air-getting component is mixed with the binder and then subjected to high-speed milling. The high-speed milling speed is 800 r / min to 1200 r / min, for example, it can be 800 r / min, 850 r / min, 900 r / min, 950 r / min, 1000 r / min, 1050 r / min, 1100 r / min, 1150 r / min or 1200 r / min, etc.
[0099] In one embodiment, the high-speed grinding time is 30 min to 60 min, for example, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, etc.
[0100] Controlling the above process parameters helps to improve the uniformity and stability of the slurry.
[0101] In one embodiment, the slurry remains stable for 8 hours without stratification or sedimentation, making it suitable for high-speed microgravure coating processes.
[0102] In one embodiment, the coating method is a single microgravure coating, without secondary coating, which is simple to operate.
[0103] In one embodiment, the drying process is as follows: the coated Mylar film passes through multiple sequentially connected ovens at a certain speed, and the temperature of the ovens first rises and then falls along the direction of movement of the coated Mylar film.
[0104] In one embodiment, along the direction of movement of the coated Mylar film, the oven temperatures are successively 80°C, 90°C, 100°C, 90°C, and 80°C.
[0105] In one implementation, the speed is 40m / min to 70m / min, for example, it can be 40m / min, 45m / min, 50m / min, 55m / min, 60m / min, 65m / min or 70m / min, etc.
[0106] The above-mentioned preferred technical solution uses a gradient heating and then gradient cooling method for drying, which can fully remove moisture from the Mylar membrane and avoid membrane cracking.
[0107] In one embodiment, after drying in step (2), the resulting Mylar film is subjected to static aging.
[0108] In one embodiment, the static aging time is 8h to 15h, for example, it can be 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, 12.5h, 13h, 13.5h, 14h, 14.5h or 15h.
[0109] By allowing the film to age statically, the internal stress can be released, preventing cracks or film peeling during subsequent die-cutting.
[0110] In one implementation, see Figure 1 The preparation method of the Mylar membrane includes the following steps: S100. Mix the liquefaction component, the getter component and the solvent and carry out a liquefaction modification reaction to obtain the liquefaction-modified getter component. S200: The liquid-repellent modified air-getting component is mixed with the binder and then milled at high speed to obtain a slurry; S300. The slurry is coated on one side of the base film and dried to obtain a Mylar film.
[0111] In another embodiment of this application, a battery is provided, including a housing and a cell electrode assembly and an electrolyte located inside the housing. The surface of the electrode assembly is covered with the Mylar membrane described in the first aspect, wherein one side of the Mylar membrane, which is a hydrophobic and gas-absorbing membrane, faces the cell electrode assembly, and the other side of the Mylar membrane faces the housing.
[0112] In one embodiment, the Mylar membrane completely covers the surface of the cell electrode assembly, leaving only the tab lead-out positions. The advantages of this design are: no blind zone for gas absorption, enabling in-situ elimination of gas generated within the cell, reducing the internal pressure of the cell, and suppressing cell swelling caused by gas generation during charging, discharging, and high-temperature storage. Simultaneously, it also provides insulation protection for the cell electrode assembly and constraint on cell electrode assembly deformation.
[0113] In one embodiment, the cell electrode assembly is a square electrode assembly, including a first end face and a second end face arranged opposite each other, a top face and a bottom face arranged opposite each other, and two side faces arranged opposite each other. The Mylar membrane covers all six faces, leaving only the electrode tab lead-out position.
[0114] In one embodiment, a Mylar membrane is provided at the gap between the battery cell electrode assembly and the outer casing, and at the contact area between the electrode tab and the outer casing, thereby taking into account both electrode tab insulation protection and the function of centralized absorption of local gas generation.
[0115] In one embodiment, the housing includes a cell cover plate. Multiple plastic strips are disposed on the surface of the cell cover plate near the cell electrode assembly. The Mylar membrane near the cell cover plate is fixed to the plastic strips by heat fusion. The heat fusion of the plastic strips inside the cover plate to fix the Mylar membrane side prevents membrane displacement, curling, and detachment during cell assembly and long-term charge-discharge cycles.
[0116] In one embodiment, the cell electrode assembly includes a positive electrode, a negative electrode, and a separator, with the separator located between the positive and negative electrode.
[0117] In one embodiment, the positive electrode sheet includes a positive current collector and a positive electrode material layer disposed on the surface of the positive current collector, wherein the positive electrode material layer includes a positive electrode active material, a conductive agent, and a binder.
[0118] In one embodiment, the positive electrode active material includes at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium manganese oxide, or lithium nickel cobalt manganese oxide.
[0119] In one embodiment, the conductive agent in the positive electrode material layer includes at least one of Super P, acetylene black, Ketjen black, carbon nanotubes, and graphene.
[0120] In one embodiment, the binder in the positive electrode material layer includes polyvinylidene fluoride.
[0121] In one embodiment, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector, wherein the negative electrode material layer includes a negative electrode active material, a conductive agent, and a binder.
[0122] In one embodiment, the negative electrode active material includes at least one of natural graphite, artificial graphite, silicon, silicon-oxygen materials, and silicon-carbon materials.
[0123] In one embodiment, the conductive agent in the negative electrode material layer includes at least one of Super P, acetylene black, Ketjen black, carbon nanotubes, and graphene.
[0124] In one embodiment, the binder in the negative electrode material layer includes polyvinylidene fluoride.
[0125] In one embodiment, the diaphragm includes a diaphragm substrate and a ceramic coating disposed on the surface of the diaphragm substrate.
[0126] In one embodiment, the membrane substrate includes at least one of a polyethylene membrane (PE membrane), a polypropylene membrane (PP membrane), or a polyimide membrane (PI membrane).
[0127] The following are typical but non-limiting embodiments: The battery dimensions in the following examples are 71173-314Ah, which corresponds to the cell size and capacity, with a capacity of 314Ah.
[0128] The information of the raw materials in the embodiments of this application is as follows: Fluorosilane coupling agent: The supplier is Nanjing Nengde New Material Technology Co., Ltd., and the commercial brand name is SCAF13C8M with CAS number 85857-16-5.
[0129] Molecular sieve: The type is battery-grade 13X molecular sieve, supplied by Luoyang Jianlong Micro-Nano New Materials Co., Ltd., commercial grade is JLH013, particle size D50 is 5μm, and specific surface area is 630m². 2 / g.
[0130] Mesoporous silica: Supplier: Nanjing Xianfeng Nanomaterials Technology Co., Ltd., Product No.: 105165, Specific surface area: 237 m² 2 / g.
[0131] High-rigidity Zr-based insulating MOF: Supplier: Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., Product No.: XFF32-1, Specific surface area: 1500 m² 2 / g.
[0132] Nano lithium hydroxide: The supplier is Shanghai Aladdin Biochemical Technology Co., Ltd., the product number is L128662, the CAS number is 1310652, and the particle size D50 is 300nm.
[0133] Nano-lithium carbonate: The supplier is Nangong Fenghui Nanotechnology Co., Ltd., CAS number is 554-13-2, and the particle size D50 is 300nm.
[0134] Polyvinylidene fluoride (PVDF): Supplier is Arkema, commercial brand name is KYNAR® HSV900.
[0135] Polytetrafluoroethylene (PTFE) emulsion: The supplier is Dongyue Future Hydrogen Energy, and the commercial grade is DF3102.
[0136] Example 1 This embodiment provides a Mylar membrane, the structural schematic of which can be found in the figure below. Figure 2 The Mylar membrane consists of a base membrane and a liquefactive getter membrane located on one side of its surface. The base membrane is a polypropylene (PP) membrane with a thickness of 100 μm; the liquefactive getter membrane has a thickness of 3 μm and includes a liquefactive component, an getter component, and a binder. The liquefactive component is a fluorosilane coupling agent, and the getter component is a physical adsorbent and a lithium-based chemical degassing agent. The physical adsorbent is a molecular sieve, and the lithium-based chemical degassing agent is nano-lithium hydroxide and nano-lithium carbonate (with a mass ratio of 1:1). The binder is a composite binder of PVDF and PTFE with a mass ratio of 8:2.
[0137] With the total mass of the liquefactive getter membrane as 100%, the total content of the liquefactive component and the getter component is 90%, the mass ratio of the physical adsorbent and the lithium-based chemical degassing agent in the getter component is 50:40, the mass percentage of the liquefactive component relative to the getter component is 1.5%, and the content of the binder is 10%.
[0138] This embodiment also provides a method for preparing the above-mentioned Mylar membrane, including the following steps: A mixed solvent was obtained by mixing S100, anhydrous ethanol, and N-methylpyrrolidone at a volume ratio of 3:7. The liquid-repellent component, the getter component, and the mixed solvent were mixed and reacted in a constant temperature water bath at 50°C and stirred at a speed of 350 r / min for 100 min. The mixture was then vacuum dried at 60°C for 2 h to remove residual solvent, thus obtaining the liquid-repellent modified getter component.
[0139] S200. PVDF and PTFE are mixed to obtain a composite binder. After mixing the liquid-repellent modified getter component with the composite binder, the mixture is subjected to high-speed sand milling at 1000 r / min for 40 min to obtain a slurry. The solid content of the slurry is 35%, and the viscosity of the slurry is 10000 mPa·s under the condition that the rotational viscometer test speed is 10 r / min.
[0140] S300: A single coating is performed using a micro-gravure coating method. The slurry is coated onto one side of the base film at a speed of 60 m / min, and then dried in a multi-section oven connected in sequence at the same speed. Along the direction of movement of the coated Mylar film, the oven temperatures are 80℃, 90℃, 100℃, 90℃ and 80℃ respectively. After drying, the coated Mylar film is allowed to age at room temperature for 12 hours, and then die-cut to obtain the Mylar film.
[0141] Example 2 This embodiment provides a Mylar membrane, which consists of a base membrane and a liquefactive getter membrane located on one side of the base membrane. The base membrane is a polypropylene membrane (PP membrane) with a thickness of 60 μm; the liquefactive getter membrane has a thickness of 2.5 μm and includes a liquefactive component, an getter component, and a binder. The liquefactive component is a fluorosilane coupling agent, and the getter component is a physical adsorbent and a lithium-based chemical degassing agent. The physical adsorbent is mesoporous silica, the lithium-based chemical degassing agent is nano-lithium carbonate, and the binder is a composite binder of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) with a mass ratio of PVDF to PTFE of 7.5:2.5.
[0142] With the total mass of the liquefactive getter membrane as 100%, the total content of the liquefactive component and the getter component is 90%, the mass ratio of the physical adsorbent and the lithium-based chemical degassing agent in the getter component is 45:35, the mass percentage of the liquefactive component relative to the getter component is 1%, and the content of the binder is 10%.
[0143] This embodiment also provides a method for preparing the above-mentioned Mylar membrane, including the following steps: A mixed solvent was obtained by mixing S100, anhydrous ethanol, and N-methylpyrrolidone at a volume ratio of 3.5:6.5. The liquid-repellent component, the getter component, and the mixed solvent were mixed and reacted in a constant temperature water bath at 45°C and stirred at a speed of 300 r / min for 120 min. The mixture was then vacuum dried at 60°C for 2 h to remove residual solvent, thus obtaining the liquid-repellent modified getter component.
[0144] S200. PVDF and PTFE are mixed to obtain a composite binder. After mixing the liquid-repellent modified getter component with the composite binder, the mixture is subjected to high-speed sand milling at 800 r / min for 60 min to obtain a slurry. The solid content of the slurry is 38%, and the viscosity of the slurry is 12000 mPa·s under the condition that the rotational viscometer test speed is 10 r / min.
[0145] S300: A single coating is performed using a micro-gravure coating method. The slurry is coated onto one side of the base film at a speed of 60 m / min, and then dried in a multi-section oven connected in sequence at the same speed. Along the direction of movement of the coated Mylar film, the oven temperatures are 80℃, 90℃, 100℃, 90℃ and 80℃ respectively. After drying, the coated Mylar film is allowed to stand at room temperature for 8 hours for aging, and then die-cut to obtain the Mylar film.
[0146] Example 3 This embodiment provides a Mylar membrane, which consists of a base membrane and a liquefactive getter membrane located on one side of its surface. The base membrane is a polypropylene membrane (PP membrane) with a thickness of 130 μm; the liquefactive getter membrane has a thickness of 3.5 μm and includes a liquefactive component, an getter component, and a binder. The liquefactive component is a fluorosilane coupling agent, and the getter component is a physical adsorbent and a lithium-based chemical degassing agent. The physical adsorbent is a high-rigidity Zr-based insulating MOF, and the lithium-based chemical degassing agent is nano-lithium hydroxide and nano-lithium carbonate (with a mass ratio of 2:1). The binder is a composite binder of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) with a mass ratio of PVDF to PTFE of 8.5:1.5.
[0147] Based on the total mass of the liquefactive getter membrane as 100%, the total content of the liquefactive component and the getter component is 95%, the mass ratio of the physical adsorbent and the lithium-based chemical degassing agent in the getter component is 45:50, the mass percentage of the liquefactive component relative to the getter component is 2%, and the content of the binder is 5%.
[0148] This embodiment also provides a method for preparing the above-mentioned Mylar membrane, including the following steps: S100, anhydrous ethanol, and N-methylpyrrolidone were mixed in a volume ratio of 3:7 to obtain a mixed solvent. The liquid-repellent component, the getter component, and the mixed solvent were mixed and reacted in a constant temperature water bath at 55°C and stirred at a speed of 400 r / min for 90 min. The mixture was then vacuum dried at 60°C for 2 h to remove residual solvent, thus obtaining the liquid-repellent modified getter component.
[0149] S200. PVDF and PTFE are mixed to obtain a composite binder. After mixing the liquid-repellent modified getter component with the composite binder, the mixture is subjected to high-speed sand milling at 1200 r / min for 30 min to obtain a slurry. The solid content of the slurry is 33%, and the viscosity of the slurry is 8000 mPa·s under the condition that the rotational viscometer test speed is 10 r / min.
[0150] S300: A single coating is performed using a micro-gravure coating method. The slurry is coated onto one side of the base film at a speed of 50 m / min, and then dried in a multi-section oven connected in sequence at the same speed. Along the direction of movement of the coated Mylar film, the oven temperatures are 80℃, 90℃, 100℃, 90℃ and 80℃ in sequence. After drying, the coated Mylar film is allowed to age at room temperature for 15 hours, and then die-cut to obtain the Mylar film.
[0151] Example 4 The difference from Example 1 is that the getter component does not contain a physical adsorbent, and the total mass of the getter component is the same as that of Example 1.
[0152] Example 5 The difference from Example 1 is that the getter component does not contain a lithium-based chemical degassing agent, and the total mass of the getter component is the same as that of Example 1.
[0153] Example 6 The difference from Example 1 is that the mass ratio of the physical adsorbent to the lithium-based chemical degassing agent is 35:55.
[0154] Example 7 The difference from Example 1 is that the mass ratio of the physical adsorbent to the lithium-based chemical degassing agent is 55:35.
[0155] Example 8 The difference from Example 1 is that the mass ratio of the lyophobic component to the getter component is 0.5%.
[0156] Example 9 The difference from Example 1 is that the mass ratio of the lyophobic component to the getter component is 2.5%.
[0157] Example 10 The difference from Example 1 is that the preparation method of the slurry is different. In this example, the liquid-repellent component is not used to pre-modify the getter component. Instead, the liquid-repellent component, getter component, liquid-repellent component, mixed solvent and composite binder are directly mixed and then subjected to high-speed sand milling at 1000 r / min for 40 min to obtain the slurry.
[0158] In this embodiment, the method and parameters for coating, drying and static aging of the slurry are the same as in Example 1.
[0159] Comparative Example 1 This comparative example uses a traditional Mylar membrane, specifically a PP membrane with a thickness of 100μm.
[0160] Using the Mylar membranes of Examples 1-10 and Comparative Example 1, batteries were prepared according to the following method, including the following steps: (1) Preparing the positive electrode sheet: Lithium iron phosphate, carbon nanotubes, PVDF, and Super P were mixed uniformly in NMP at a mass ratio of 97.5:0.4:1.5:0.6 to obtain a positive electrode slurry. The positive electrode slurry was coated on the surface of a positive electrode current collector aluminum foil (12 μm thick), dried, and cold-pressed to obtain a positive electrode sheet with a thickness of 164 μm.
[0161] (2) Preparation of negative electrode: Natural graphite, Super P, sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed evenly in water at a mass ratio of 96.5:0.6:1.1:1.8 to obtain a negative electrode slurry. The negative electrode slurry was coated on the surface of a copper foil (6 μm thick) for the negative electrode current collector. After drying and cold pressing, a negative electrode sheet with a thickness of 124 μm was obtained.
[0162] (3) Provide a diaphragm: The membrane comprises a PE membrane and an Al2O3 ceramic layer and a PVDF layer disposed on one side of its surface. The thickness of the PE membrane is 7 μm, and the thicknesses of the Al2O3 ceramic layer and the PVDF layer are 3 μm and 2 μm, respectively.
[0163] (4) An aluminum shell is used as the outer shell, and the outer shell also includes a cell cover plate. The outer shell is used to accommodate the cell electrode assembly. The cell electrode assembly is prepared by winding positive electrode sheet, negative electrode sheet and separator. Mylar film is wrapped around the cell electrode assembly. When wrapping, the liquid-repellent and gas-absorbing layer faces the cell electrode assembly. After wrapping, the Mylar film completely covers the surface of the cell electrode assembly, leaving only the tab lead-out position. After the tab is led out, Mylar film is set in the contact area between the tab and the aluminum shell.
[0164] Multiple plastic strips are set on the surface of the cell cover plate near the cell electrode assembly. The Mylar membrane is fixed to the plastic strips by heat fusion. Then the cell electrode assembly is inserted into the shell, welded, injected with electrolyte, formed, and capacity tested to obtain the battery.
[0165] Performance testing: (1) Test the contact angle of the electrolyte. The test method is as follows: use a contact angle measuring instrument, and under the condition of 25℃, drop the electrolyte onto the surface of the hydrophobic absorbent membrane and read the contact angle value of the electrolyte.
[0166] (2) The capacity retention rate of the battery after 1000 cycles was tested. The test method was as follows: under an environment of 25°C, constant current and constant voltage charging at 1C and constant current discharging at 1C, with a charging cutoff voltage of 3.65V and a discharging cutoff voltage of 2.5V, for 1000 cycles, and the discharge capacity C of the 1000th cycle was recorded. 1000 The discharge capacity C1 in the first cycle is used as the basis for calculating the capacity retention rate over 1000 cycles. The formula is: Capacity retention rate over 1000 cycles = C1 / C1. 1000 / C1×100%.
[0167] (3) Test the expansion force of the battery after 1000 cycles. The test method is as follows: use a pressure sensor to clamp the battery cell with an initial preload of 300 kgf, and record the expansion force of the battery cell on the clamp after 1000 cycles.
[0168] (4) Test the thickness expansion rate of the battery after 1000 cycles. The test method is as follows: test the initial thickness h0 of the cell, test the thickness h1 of the cell after 1000 cycles, and calculate the thickness expansion rate accordingly. The calculation formula is: thickness expansion rate = (h1-h0) / h0×100%.
[0169] (5) Test the increase in internal resistance of the battery after high temperature storage. The test method is as follows: place the battery in an environment of 45℃ for 30 days, test the AC internal resistance R0 of the cell before storage and the AC internal resistance R1 of the cell after storage, and calculate the increase in internal resistance accordingly. The calculation formula is: internal resistance increase = (R1-R0) / R0×100%.
[0170] (6) Observe the swelling and rebound phenomenon of the battery after 1000 cycles.
[0171] The results are shown in Table 1. As shown in Table 1, Comparative Example 1 uses a traditional PP Mylar membrane without gas-absorbing function, which lacks the ability to capture and consume gas. Its thickness expansion rate reaches 4.80% after 1000 cycles, and its internal resistance increases by 25.6% at high temperatures, resulting in continuous battery swelling. This application, by setting a hydrophobic gas-absorbing membrane on the surface of the base film, enables the Mylar membrane to have excellent hydrophobic properties, significantly reducing the cell's internal pressure during cycling, suppressing swelling during high-temperature storage and long-cycle cycling, reducing the increase in internal resistance, and greatly improving the cycle life and long-term safety of the square aluminum-cased lithium battery.
[0172] The Mylar membrane of this application has an electrolyte contact angle of 93° or higher, preferably 111° or higher; a capacity retention rate of 93.9% or higher, preferably 94.5% or higher, after 1000 battery cycles; an expansion force of 1294 kgf or less, preferably 1193 kgf or less, after 1000 cycles; a thickness expansion rate of 2.89% or less, preferably 2.30% or less, after 1000 cycles; and an internal resistance increase of 20.9% or less, preferably 14.7% or less, after high-temperature storage.
[0173] Meanwhile, a comparison between Example 1 and Examples 4-7 shows that the combination of physical adsorbent and lithium-based chemical degassing agent in the gas-absorbing component is more conducive to improving battery performance.
[0174] Compared to Example 1, Example 4 removes the physical adsorbent and relies solely on the lithium-based chemical degassing agent. It lacks the porous channels to capture and buffer the instantaneous gas generation, resulting in a significant increase in cell expansion force, thickness expansion rate, and internal resistance. Slight bulging occurs after cycling.
[0175] Compared to Example 1, Example 5 removes the lithium-based chemical degassing agent and relies solely on physical adsorption, which cannot irreversibly neutralize HF or solidify CO2, resulting in a significant increase in internal resistance during high-temperature storage.
[0176] In Examples 6-7, the mass ratio of physical adsorbent to lithium-based chemical degassing agent did not meet the requirement of (40~50):(35~50), resulting in varying degrees of performance degradation of the battery cell compared to Example 1. The overall performance of the battery cell, which combines instantaneous gas generation buffering and long-term chemical solidification, decreased.
[0177] A comparison of Examples 1 and Examples 8-9 shows that there is an optimal range for the content of the hydrophobic component. If the content of the hydrophobic component is too low (Example 8), the hydrophobic coating on the surface of the gas-absorbing component is not complete, and the electrolyte is easy to penetrate into the interior of the coating, causing the gas-absorbing site to fail. If the content of the hydrophobic component is too high (Example 9), the excessive hydrophobic component will block the powder pores and reduce the gas transmission efficiency.
[0178] A comparison between Example 1 and Example 10 shows that modifying the getter component with a liphophore component beforehand, and then mixing it with a binder to prepare a slurry, achieves a complete and uniform liphophore coating on the surface of the getter particles. However, direct blending results in uneven dispersion of the liphophore component, with localized liphophilic regions, leading to a decrease in both liphophore and getter / degassing performance.
[0179] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.
Claims
1. A Mylar membrane, characterized in that, The Mylar membrane includes a base membrane and a liquefactive getter membrane disposed on the surface of the base membrane. The liquefactive getter membrane includes a liquefactive component and an getter component, wherein the getter component is selected from physical adsorbents and / or lithium-based chemical degassing agents.
2. The Mylar membrane according to claim 1, characterized in that, The hydrophobic component includes a fluorinated hydrophobic structure, wherein the fluorinated hydrophobic structure is derived from at least one of a fluorosilane coupling agent, a perfluoropolyether, or a perfluoroalkyl acrylate polymer; and / or The lyophobic component coats the getter component to form a lyophobically modified getter component; and / or, The lithium-based chemical degassing agent includes lithium hydroxide and / or lithium carbonate; and / or, The lithium-based chemical degassing agent is a nanoparticle; and / or, The physical adsorbent includes at least one of molecular sieves, metal-organic framework materials, and mesoporous silica.
3. The Mylar membrane according to claim 2, characterized in that, The molecular sieve includes one of 13X molecular sieve, 4A molecular sieve, or 5A molecular sieve; and / or, The specific surface area of the molecular sieve is ≥580m². 2 / g, preferably 600m 2 / g~700 m 2 / g; and / or, The metal-organic framework material includes a high-rigidity Zr-based insulating MOF; and / or, The specific surface area of the metal-organic framework material is ≥1200 m². 2 / g, preferably 1400 m 2 / g~1800 m 2 / g; and / or, The specific surface area of the mesoporous silica is ≥180m². 2 / g, preferably 200m 2 / g~250m 2 / g.
4. The Mylar membrane according to any one of claims 1-3, characterized in that, The contact angle of the liquefying getter membrane with the electrolyte is ≥110°; and / or, The thickness of the liquefactive getter membrane on one side is 2 μm to 5 μm, preferably 2.5 μm to 3.5 μm; and / or, The pore size of the liquephobic getter membrane is in the range of 0.2 μm to 3 μm; and / or, The liquid-repellent getter membrane also includes an adhesive.
5. The Mylar membrane according to claim 4, characterized in that, The adhesive comprises polyvinylidene fluoride and polytetrafluoroethylene, and does not contain sodium carboxymethyl cellulose. The preferred mass ratio of polyvinylidene fluoride to polytetrafluoroethylene is 7:3 to 8.5:1.
5.
6. The method for preparing the Mylar membrane according to any one of claims 1-5, characterized in that, Based on the total mass of the liquid-repellent getter membrane as 100%, the total content of the liquid-repellent component and the getter component is 75%~98%; and / or, Based on the total mass of the liquefying getter membrane as 100%, the mass ratio of the physical adsorbent to the lithium-based chemical degassing agent in the getter component is (40~50):(35~50); and / or, The liquid-repellent component accounts for 1% to 2% of the mass of the getter component; and / or, Based on the total mass of the liquid-repellent getter membrane as 100%, the content of the binder is 5% to 10%.
7. A method for preparing a Mylar membrane, characterized in that, The preparation method includes the following steps: (1) Provide a slurry comprising a liquid-repellent component, a getter component, a binder, and a solvent; The gas-absorbing component is selected from physical adsorbents and / or lithium-based chemical degassing agents; (2) The slurry is coated on the surface of the base film and dried to obtain a Mylar film.
8. The method for preparing the Mylar membrane according to claim 7, characterized in that, Step (1) includes: mixing the liquid-repellent component, the getter component, and a solvent and performing a liquid-repellent modification reaction to obtain a liquid-repellent modified getter component; mixing the liquid-repellent modified getter component with a binder to obtain a slurry; and / or, The solvent comprises ethanol and N-methylpyrrolidone, wherein the volume ratio of ethanol to N-methylpyrrolidone is preferably 2:8 to 4:6; and / or, Preferably, the solid content of the slurry is 33%~38%; and / or, The viscosity of the slurry was tested using a rotational viscometer at a speed of 12 r / min. A rotor of type 3 was used, and the viscosity of the slurry was measured to be 8000 mPa·s to 12000 mPa·s.
9. The method for preparing the Mylar membrane according to claim 8, characterized in that, In the preparation of the slurry, the conditions for the hydrophobic modification reaction are: a constant temperature water bath at 45℃~55℃; and / or, During the preparation of the slurry, the hydrophobic modification reaction takes 90-120 minutes; and / or, The hydrophobic modification reaction is accompanied by stirring at a speed of 300 r / min to 400 r / min; and / or, During the preparation of the slurry, after the hydrophobic modification reaction is completed, the resulting reaction product is dried. And / or, In the preparation process of the slurry, the liquid-repellent modified air-getting component is mixed with the binder and then subjected to high-speed sand milling. The high-speed sand milling speed is 800 r / min to 1200 r / min, and the high-speed sand milling time is 30 min to 60 min.
10. The method for preparing the Mylar membrane according to any one of claims 7-9, characterized in that, After drying in step (2), the obtained Mylar film is subjected to static aging, and the static aging time is preferably 8h~15h.
11. A battery, characterized in that, The battery includes a housing and a cell electrode assembly and an electrolyte located inside the housing. The surface of the electrode assembly is covered with a Mylar membrane as described in any one of claims 1-6, wherein the liquid-repellent and gas-absorbing side of the Mylar membrane faces the cell electrode assembly, and the other side of the Mylar membrane faces the housing.
12. The battery according to claim 11, characterized in that, The Mylar membrane completely covers the surface of the battery cell electrode assembly, leaving only the tab lead-out position; and / or Mylar membranes are installed at the gaps between the cell electrode assembly and the casing, and at the contact areas between the electrode tabs and the casing.
13. The battery according to claim 11 or 12, characterized in that, The housing includes a cell cover plate, and a plurality of plastic strips are provided on the surface of the cell cover plate near the cell electrode assembly. The Mylar membrane is fixed to the plastic strips on the side near the cell cover plate by heat fusion.