An aerogel coating composite thermal insulation sheet and a method of making the same

By forming an interpenetrating polymer network between core-shell aerogel microspheres and a cross-linked acrylate copolymer shell, the interfacial debonding and phonon scattering problems of aerogel-coated composite sheets during bending and service are solved, achieving higher thermal insulation performance and structural stability.

CN123152149APending Publication Date: 2026-11-24山东久强新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611359936.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing aerogel-coated composite sheets are prone to interfacial debonding and phonon scattering mismatch during construction bending and outdoor service, failing to meet long-term service requirements and not fully realizing their thermal insulation performance.

Method used

A core-shell structured aerogel microsphere is formed by an interpenetrating polymer network with a cross-linked acrylate copolymer shell. This network is then chemically bonded to an acrylate binder matrix to form a continuous integral structure, thereby constructing a nanoscale sealed air layer to regulate the heat conduction path.

Benefits of technology

It improves the stability and thermal insulation performance of the coating structure, reduces the thermal conductivity, and enhances the bonding state under external mechanical action and temperature changes, thus meeting the high-performance application requirements of building insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152149A_ABST
    Figure CN123152149A_ABST
Patent Text Reader

Abstract

This invention discloses an aerogel-coated composite thermal insulation sheet and its preparation method, relating to the field of building thermal insulation materials technology. The thermal insulation sheet comprises: a flexible polymer sheet substrate and an acrylic composite coating. This invention utilizes core-shell aerogel microspheres as the thermal insulation functional phase, with a cross-linked acrylic copolymer shell completely encapsulating the silica aerogel core. This ensures that the shell and the acrylic binder matrix have the same characteristic functional groups. During the thermosetting process of the acrylic composite coating, the microsphere shell and the binder matrix undergo a co-crosslinking reaction, forming an interpenetrating polymer network. This allows the core-shell aerogel microspheres and the acrylic binder matrix to form a continuous integral structure through chemical bonding, replacing the particle-filling mode of traditional physical blending. This ensures that the aerogel core is completely encapsulated and fixed by the polymer crosslinking system, guaranteeing the integrity of the coating structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building insulation materials technology, specifically to an aerogel-coated composite insulation sheet and its preparation method. Background Technology

[0002] With the continuous improvement of building energy efficiency standards and the steady advancement of dual-carbon goals, the thermal insulation performance of building envelopes has become one of the core indicators for measuring building energy efficiency. Traditional building insulation materials are gradually failing to meet the development needs of ultra-low energy consumption buildings and near-zero energy consumption buildings in terms of thermal insulation efficiency, service life, and construction adaptability. The industry's demand for lightweight, flexible, and high-performance new thermal insulation materials is becoming increasingly urgent. Aerogel, as a new generation of thermal insulation material, has received widespread attention in the field of building energy conservation. Among them, coated aerogel composite sheets have shown broad market potential in multiple scenarios such as building exterior walls, roofs, and pipe insulation due to their application advantages such as bendability, easy cutting, and adaptability to complex building facades. The research and development and implementation of related products have become a key development direction in the field of building energy conservation materials.

[0003] However, most conventional aerogel-coated composite sheets are prepared using a physical blending method, directly mixing aerogel powder with a binder and then coating it onto the substrate surface. While this process facilitates large-scale production, it has significant drawbacks in practical applications. On the one hand, the aerogel particles are exposed in the coating, with only a physical bond to the binder, resulting in poor interfacial compatibility. Under the influence of bending during construction and temperature cycling during long-term outdoor service, interfacial debonding easily occurs between the particles and the binder, leading to powdering and detachment. This not only affects the construction environment but also causes the material performance to gradually decline over time, failing to meet the requirements for long-term service in building engineering. On the other hand, there is an inherent phonon scattering mismatch between the aerogel particles and the binder. Theoretically, this effect can be used to control the thermal insulation performance through interfacial structure design. However, current technologies only adjust macroscopic parameters such as aerogel content and binder type, without actively designing and controlling the interfacial structure between the particles and the substrate. This fails to fully realize the thermal insulation potential of aerogel materials and limits further breakthroughs in product performance. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of existing technologies and provide an aerogel-coated composite thermal insulation sheet and its preparation method. This invention uses core-shell aerogel microspheres as the thermal insulation functional phase, with a cross-linked acrylate copolymer shell completely encapsulating the silica aerogel core. The shell and the acrylate binder matrix have the same characteristic functional groups. During the thermosetting process of the acrylate composite coating, the microsphere shell and the binder matrix undergo a co-crosslinking reaction to form an interpenetrating polymer network. This allows the core-shell aerogel microspheres and the acrylate binder matrix to form a continuous integral structure through chemical bonding, replacing the particle filling mode of traditional physical blending. The aerogel core is completely wrapped and fixed by the polymer crosslinking system. Under external mechanical action and temperature changes, the microspheres and the matrix maintain a stable bonding state, ensuring the integrity of the coating structure.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: On the one hand, an aerogel-coated composite thermal insulation sheet, the thermal insulation sheet comprising: a flexible polymer sheet substrate and an acrylic composite coating;

[0006] The acrylate composite coating is composed of core-shell structured aerogel microspheres and acrylate adhesive matrix, and is bonded to the surface of a flexible polymer sheet substrate.

[0007] The core-shell structured aerogel microspheres have a silica aerogel core and a cross-linked acrylate copolymer shell.

[0008] The core-shell structured aerogel microspheres are uniformly dispersed inside the acrylate binder matrix, and the cross-linked acrylate copolymer shell and the acrylate binder matrix contain the same characteristic functional groups;

[0009] After the acrylate composite coating is thermocured, the cross-linked acrylate copolymer shell and the acrylate adhesive matrix form an interpenetrating polymer network through a co-crosslinking reaction.

[0010] Furthermore, the thickness of the cross-linked acrylate copolymer shell is 50-200 nm, the characteristic functional group is methacryloxy, and the methacryloxy is uniformly distributed in the molecular chain segments of the cross-linked acrylate copolymer shell; the cross-linked acrylate copolymer shell is grafted onto the outer surface of the silica aerogel core by covalent chemical bonding.

[0011] Furthermore, the interpenetrating polymer network is a three-dimensional continuous cross-linked structure, and the core-shell structured aerogel microspheres form a continuous integral structure chemically bonded to the acrylate binder matrix through the interpenetrating polymer network.

[0012] Furthermore, the acrylate composite coating is a uniform cross-linked curing system with a dry film thickness of 100-500 μm, and the core-shell structured aerogel microspheres account for 20%-50% of the mass of the acrylate binder matrix; the core-shell structured aerogel microspheres are distributed in a monodisperse state in the acrylate binder matrix.

[0013] Furthermore, the flexible polymer sheet substrate is selected from polyethylene terephthalate sheet, polyimide sheet or flexible polyvinyl chloride sheet, and the thickness of the flexible polymer sheet substrate is 50-300 μm.

[0014] On the other hand, a method for preparing an aerogel-coated composite thermal insulation sheet includes the following specific steps:

[0015] Core-shell microsphere grafting modification: Using silica wet gel microspheres as reaction templates, silica wet gel microspheres are dispersed in a mixed solvent to form a suspension system. Acrylic ester reactants, crosslinking agents and initiators are added, and crosslinked ester copolymer shells are grafted onto the surface of silica wet gel microspheres through emulsion polymerization to obtain grafted wet gel microspheres.

[0016] Core-shell microsphere drying and shaping: After washing, the grafted wet gel microspheres are sent to a supercritical drying equipment for supercritical drying to obtain core-shell structured aerogel microspheres.

[0017] Preparation of composite coating slurry: Core-shell structured aerogel microspheres are added to a mixture of acrylate binder and solvent, dispersed evenly, and then a curing agent is added. The mixture is then mixed until the system is homogeneous to obtain the composite coating slurry.

[0018] Substrate coating and curing: The composite coating slurry is coated onto the surface of the flexible polymer sheet substrate by roller coating or blade coating process, and after heat curing treatment, an acrylic composite coating is formed, thereby obtaining the aerogel coating composite thermal insulation sheet.

[0019] Furthermore, in the core-shell microsphere grafting modification, the silica wet gel microspheres undergo solvent displacement pretreatment before emulsion polymerization. The solvent used for displacement is a mixed solvent. After 3-5 soaking and displacement cycles, the solvent composition of the internal pores of the silica wet gel microspheres is consistent with that of the mixed solvent. The mixed solvent is a mixture of anhydrous ethanol and deionized water, with a volume ratio of anhydrous ethanol to deionized water of 2-4:1. The emulsion polymerization reaction is carried out under a nitrogen protective atmosphere at a reaction temperature of 60-70℃ for 3-5 hours. The acrylate reactive monomer is an acrylate monomer containing methacryloyloxy group, the crosslinking agent is ethylene glycol dimethacrylate, and the initiator is ammonium persulfate. The mass ratio of acrylate reactive monomer to crosslinking agent is 8-12:1-2, and the mass ratio of acrylate reactive monomer to initiator is 20-30:1.

[0020] Furthermore, in the drying and shaping of the core-shell microspheres, anhydrous ethanol is used to wash the grafted wet gel microspheres 3-5 times to remove acrylate reactants that did not participate in the polymerization reaction, as well as acrylate homopolymers generated during the reaction that were not grafted onto the surface of the silica wet gel microspheres; supercritical drying is carried out using a carbon dioxide supercritical drying process, with a drying pressure of 10-15 MPa, a drying temperature of 40-50℃, and a drying time of 4-8 h, resulting in core-shell structured aerogel microspheres.

[0021] Furthermore, in the preparation of the composite coating slurry, the acrylate binder is dissolved in butyl acetate solvent to form a binder solution with a mass fraction of 25%-35%; then, core-shell structured aerogel microspheres are slowly added and stirred and dispersed at a speed of 150-300 r / min until there is no obvious agglomeration in the system; then, an isocyanate curing agent is added, with a mass ratio of curing agent to acrylate binder solid of 1:8-12; and the mixture is stirred until the system is completely homogeneous to obtain the composite coating slurry.

[0022] Furthermore, in the substrate coating and curing process, the thickness of the wet film of the composite coating slurry is controlled to be 300-800μm during the roller coating or scraping process; the thermal curing adopts a segmented heating curing method, first pre-curing at 70-90℃ for 20-40min, then heating to 100-120℃ and holding for curing for 50-70min, until the acrylic composite coating is completely cross-linked and formed, thus obtaining the aerogel coating composite thermal insulation sheet.

[0023] Compared with existing technologies, this aerogel-coated composite thermal insulation sheet and its preparation method have the following advantages:

[0024] I. This invention employs core-shell structured aerogel microspheres as the thermal insulation functional phase, with a cross-linked acrylate copolymer shell completely encapsulating the silica aerogel core. This ensures that the shell and the acrylate binder matrix share the same characteristic functional groups. During the thermosetting process of the acrylate composite coating, the microsphere shell and the binder matrix undergo a co-crosslinking reaction, forming an interpenetrating polymer network. This allows the core-shell structured aerogel microspheres and the acrylate binder matrix to form a continuous, integral structure through chemical bonding, replacing the particle-filling mode of traditional physical blending. The aerogel core is completely encapsulated and fixed by the polymer crosslinking system. Under external mechanical forces and temperature changes, the microspheres and the matrix maintain a stable bonding state, ensuring the integrity of the coating structure.

[0025] II. This invention constructs a core-shell interface structure on the surface of aerogel particles, forming a nanoscale sealed air layer at the interface between the silica aerogel core and the cross-linked acrylate copolymer shell. This air layer is distributed along the heat conduction path, adding additional interfacial thermal resistance to the heat conduction process. At the same time, the core-shell structure can adjust the phonon scattering matching state between the aerogel phase and the polymer phase, thereby regulating the heat conduction process through the interfacial effect, changing the heat conduction path inside the coating, fully releasing the thermal insulation properties of the aerogel material itself, and allowing the functional phase of the aerogel to play a more complete role.

[0026] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.

[0028] Figure 1 A flowchart illustrating a method for preparing an aerogel-coated composite thermal insulation sheet;

[0029] Figure 2 This is a framework diagram of a method for preparing an aerogel-coated composite thermal insulation sheet;

[0030] Figure 3 This is a framework diagram of the preparation of composite coating slurry in a method for preparing an aerogel-coated composite thermal insulation sheet. Detailed Implementation

[0031] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.

[0032] Example 1:

[0033] This embodiment prepares an aerogel-coated composite thermal insulation sheet. The specific preparation process is as follows:

[0034] Core-shell microsphere grafting modification: 50g of wet-based silica wet gel microspheres were weighed as the reaction template. First, a solvent displacement pretreatment was performed using a mixed solvent of anhydrous ethanol and deionized water at a volume ratio of 3:1. Each time, 200mL of the mixed solvent was added, and the mixture was stirred for 20min, then filtered and separated. This displacement process was repeated three times to ensure that the solvent composition of the internal pores of the silica wet gel microspheres was consistent with the mixed solvent. The pretreated silica wet gel microspheres were then added to a mixed solvent of 300mL anhydrous ethanol and 100mL deionized water and stirred. A uniform suspension system was formed; the suspension system was transferred to a reactor, and nitrogen gas was continuously introduced for 30 minutes to remove oxygen from the suspension system. Stirring was started and the temperature was raised to 65°C; 40g of methacryloyloxy-containing acrylate monomer and 4g of ethylene glycol dimethacrylate crosslinking agent were added to the suspension system, and after stirring and dispersing for 10 minutes, 1.6g of ammonium persulfate initiator was added. The reaction was maintained at this temperature for 4 hours. A crosslinked acrylate copolymer shell was grafted onto the surface of the silica wet gel microspheres via emulsion polymerization. After the reaction, grafted wet gel microspheres were obtained, such as... Figure 1 As shown.

[0035] Core-shell microsphere drying and shaping: The grafted wet gel microspheres were removed and filtered for separation. They were then washed four times with anhydrous ethanol, with 200 mL of anhydrous ethanol added for each wash. After soaking and stirring for 15 minutes, the microspheres were filtered to remove unreacted methacryloyloxy-containing acrylate monomers and ungrafted acrylate homopolymers formed during the reaction. After washing, the material was fed into a supercritical drying device and dried using a supercritical carbon dioxide drying process. The drying pressure was controlled at 12 MPa, the drying temperature at 45℃, and the drying time at 6 hours. After drying, core-shell structured aerogel microspheres were obtained, such as... Figure 2 As shown, transmission electron microscopy revealed that the cross-linked acrylate copolymer shell is uniformly coated on the surface of the silica aerogel core through covalent chemical bonding. The shell layer is continuous without any breaks and has a thickness of approximately 120 nm. The nanoporous structure of the core remains intact without any collapse or damage.

[0036] Preparation of composite coating slurry: Weigh 30g of solid acrylate binder and add it to 70g of butyl acetate solvent. Stir until the binder is completely dissolved, forming a 30% (w / w) binder solution. Slowly add 15g of core-shell structured aerogel microspheres to the binder solution and stir continuously at 200r / min for 30min until there is no obvious agglomeration. Then add 3g of isocyanate curing agent and continue stirring for 15min until the system is completely homogeneous, obtaining the composite coating slurry. Figure 3 As shown, the slurry system is in a stable dispersion state, and there is no obvious sedimentation or stratification after standing for 2 hours.

[0037] Substrate Coating and Curing: A 100μm thick polyethylene terephthalate sheet was selected as the flexible polymer sheet substrate, cut into 200mm×200mm sample sizes, and the surface dust and impurities were cleaned. The composite coating slurry was uniformly coated onto the surface of the flexible polymer sheet substrate using a scraping process, and the thickness of the wet film of the composite coating slurry was controlled to be 500μm. The coated sample was sent into a forced-air drying oven and cured in stages. First, it was pre-cured at 80℃ for 30 minutes to allow the solvent to evaporate slowly, and then the temperature was raised to 110℃ and held for 60 minutes until the acrylic composite coating was completely cross-linked and formed, thus obtaining the aerogel-coated composite thermal insulation sheet. The dry film thickness of the finished acrylic composite coating was about 250μm, and the coating was firmly bonded to the substrate without any surface defects such as peeling, pinholes, or craters.

[0038] Finished product testing: The thermal conductivity of the sample in the vertical direction was tested using a thermal conductivity meter with heat flow method at a room temperature of 25℃. The aerogel-coated composite insulation sheet was cut into 100mm×50mm samples and repeatedly bent 180° along a 10mm diameter stainless steel rod 100 times. The mass before and after bending was weighed and the mass loss rate was calculated. The surface morphology of the coating was observed. The sample was placed in a high and low temperature cycling test chamber and subjected to cold and hot cycling tests in the temperature range of -20℃ to 80℃. The duration of each cycle was 4 hours. After a total of 100 cycles, the thermal conductivity was retested and the change rate was calculated. The test results showed that the thermal conductivity of the sample in this embodiment was 0.018W / (m・K). After the bending test, there was no visible powder shedding on the coating surface, and the mass loss rate was 0.08%. After cold and hot cycling, there was no cracking or delamination of the coating, and the thermal conductivity increase rate was 2.9%.

[0039] Example 2:

[0040] This embodiment prepares an aerogel-coated composite thermal insulation sheet. The specific preparation process is as follows:

[0041] Core-shell microsphere grafting modification: 50g of wet silica wet gel microspheres were weighed as reaction templates. Solvent replacement pretreatment was performed using a mixed solvent of anhydrous ethanol and deionized water at a volume ratio of 2:1. Each time, 200mL of the mixed solvent was added, and the mixture was stirred for 20min before filtration and separation. This replacement process was repeated three times to ensure the solvent composition of the internal pores of the silica wet gel microspheres was consistent with the mixed solvent. The pretreated silica wet gel microspheres were then added to a mixed solvent of 250mL anhydrous ethanol and 125mL deionized water, and stirred to form a homogeneous suspension. After purging with nitrogen for 30min to remove oxygen, the temperature was raised to 62℃. 28g of methacryloyloxy acrylate monomer and 3.2g of ethylene glycol dimethacrylate crosslinking agent were added and dispersed evenly. 1.2g of ammonium persulfate initiator was then added, and the reaction was maintained at this temperature for 3.5h to obtain the grafted wet gel microspheres.

[0042] Core-shell microsphere drying and shaping: The grafted wet gel microspheres were washed three times with anhydrous ethanol to remove residual acrylate monomers containing methacryloyloxy groups and acrylate homopolymers. Then, they were sent to a supercritical drying equipment and a supercritical carbon dioxide drying process was adopted. The drying pressure was controlled at 11 MPa, the drying temperature at 42℃, and the drying time at 5h. After drying, core-shell structured aerogel microspheres were obtained, and the thickness of the cross-linked acrylate copolymer shell was about 80 nm.

[0043] Preparation of composite coating slurry: Dissolve acrylate binder in butyl acetate solvent to form a binder solution with a mass fraction of 28%; add core-shell structured aerogel microspheres, controlling the filling mass ratio of core-shell structured aerogel microspheres in the acrylate binder matrix to be 25%, stir and disperse at 180 r / min until there is no obvious agglomeration, then add isocyanate curing agent, the mass ratio of curing agent to acrylate binder solid is 1:9, stir until the system is homogeneous, and obtain composite coating slurry.

[0044] Substrate coating and curing: A 150μm thick polyimide sheet was selected as the flexible polymer sheet substrate. A composite coating slurry was applied using a roller coating process, and the wet film thickness was controlled to be 400μm. A segmented temperature curing method was adopted, first pre-curing at 75℃ for 25min, and then heating to 105℃ and holding for 55min until the acrylate composite coating was completely cross-linked and formed, thus obtaining the aerogel-coated composite thermal insulation sheet.

[0045] Finished product testing: The same testing methods and conditions as in Example 1 were used for testing; the test results showed that the thermal conductivity of the sample in this example was 0.020 W / (m·K); after the bending test, there was no obvious powder shedding on the coating surface, and the mass loss rate was 0.12%; after the hot and cold cycle, the thermal conductivity increased by 3.5%, and there was no debonding or cracking.

[0046] Example 3:

[0047] This embodiment prepares an aerogel-coated composite thermal insulation sheet. The specific preparation process is as follows:

[0048] Core-shell microsphere grafting modification: 50g of wet silica wet gel microspheres were weighed as reaction templates. Solvent replacement pretreatment was performed using a mixed solvent of anhydrous ethanol and deionized water at a volume ratio of 4:1. Each time, 200mL of the mixed solvent was added, and the mixture was stirred for 20min before filtration and separation. This process was repeated three times to ensure the solvent composition of the internal pores of the silica wet gel microspheres was consistent with the mixed solvent. The pretreated silica wet gel microspheres were then added to a mixed solvent of 360mL anhydrous ethanol and 90mL deionized water, and stirred to form a homogeneous suspension. After purging with nitrogen for 30min to remove oxygen, the temperature was raised to 68℃. 55g of methacryloyloxy acrylate monomer and 6g of ethylene glycol dimethacrylate crosslinking agent were added and dispersed evenly. 2.2g of ammonium persulfate initiator was then added, and the reaction was maintained at this temperature for 4.5h to obtain the grafted wet gel microspheres.

[0049] Core-shell microsphere drying and shaping: The grafted wet gel microspheres were washed five times with anhydrous ethanol to remove residual monomers and acrylate homopolymers, and then sent to a supercritical drying equipment. The supercritical carbon dioxide drying process was used, with the drying pressure controlled at 14 MPa, the drying temperature at 48℃, and the drying time at 7 h. After drying, core-shell structured aerogel microspheres were obtained, with the thickness of the cross-linked acrylate copolymer shell being approximately 180 nm.

[0050] Preparation of composite coating slurry: Dissolve acrylate binder in butyl acetate solvent to form a binder solution with a mass fraction of 32%; add core-shell structured aerogel microspheres to the solution, controlling the filling mass ratio of core-shell structured aerogel microspheres in the acrylate binder matrix to be 40%, stir and disperse at 250 r / min until there is no obvious agglomeration, then add isocyanate curing agent, the mass ratio of curing agent to acrylate binder solid is 1:11, stir until the system is homogeneous, and obtain composite coating slurry.

[0051] Substrate coating and curing: A flexible polyvinyl chloride sheet with a thickness of 200μm was selected as the flexible polymer sheet substrate. The composite coating slurry was coated by a scraping process, and the wet film thickness was controlled to be 700μm. A segmented temperature-curing method was adopted, first pre-curing at 85℃ for 35min, and then heating to 115℃ and holding for 65min until the acrylic composite coating was completely cross-linked and formed, thus obtaining the aerogel-coated composite thermal insulation sheet.

[0052] Finished product testing: The same testing methods and conditions as in Example 1 were used for testing; the test results showed that the thermal conductivity of the sample in this example was 0.016 W / (m·K); after the bending test, there was no visible powder falling off the coating surface, and the mass loss rate was 0.07%; after the hot and cold cycle, the thermal conductivity increased by 2.7%, and the coating structure remained intact.

[0053] Comparative example:

[0054] This comparative example uses a physical blending process commonly used in the field of building insulation materials to prepare aerogel-coated insulation sheets, which is a conventional existing technical solution. No particle interface modification or co-crosslinking structure design was carried out. The specific preparation process is as follows:

[0055] Weigh out a commercially available general-purpose acrylic emulsion as the adhesive substrate, add deionized water to adjust the solid content of the system to 40%, and add alcohol ester twelve film-forming aid and polyether modified silicone oil defoamer in sequence under low-speed stirring. After mixing evenly, the basic adhesive system is obtained.

[0056] Commercially available ordinary silica aerogel powder was weighed as the thermal insulation filler, with a particle size range of 10-50μm. It was slowly added to the base binder system, with a mass ratio of aerogel powder to binder solid of 3:7. The mixture was first stirred at high speed of 800r / min for 20min until the powder was initially dispersed. Then it was transferred to a sand mill and ground and dispersed for 10min with zirconium beads as the grinding medium to obtain a uniform blended coating slurry.

[0057] Polyethylene terephthalate sheet of the same specifications as in Example 1 was selected as the substrate. After cleaning the surface dust, the blended coating slurry was applied to the substrate surface using a scraping process, and the wet film thickness was controlled to be consistent with that in Example 1. The coated sample was placed in a forced-air drying oven and dried at 80°C for 45 minutes. After the moisture was completely evaporated and the coating was naturally formed and shaped, it was taken out to obtain the comparative aerogel coating heat insulation sheet.

[0058] Finished product testing: The same testing methods and conditions as in Example 1 were used for testing; the test results showed that the thermal conductivity of this comparative sample was 0.028 W / (m·K); after the bending test, obvious white dust fell off the coating surface, and fine cracks were visible at the edges, with a mass loss rate of 4.3%; after the hot and cold cycle, the coating showed signs of local interface debonding, and the thermal conductivity increased by 13.1%.

[0059] In summary, all three embodiments are based on the technical route of core-shell structured aerogel microspheres and co-crosslinked interpenetrating networks, which can stably prepare aerogel-coated composite thermal insulation sheets. By adjusting the shell thickness, aerogel filling ratio, and process parameters, they can be adapted to different application scenarios with varying thermal insulation and mechanical properties. Compared with existing technologies, this technical solution can effectively reduce the thermal conductivity of the coating, while significantly improving the interfacial bonding between the aerogel and the substrate, enhancing structural stability under bending and thermal cycling, and meeting the high-performance application requirements of building insulation materials.

[0060] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. An aerogel coating composite thermal insulation sheet, characterized by, The thermal insulation sheet comprises: a flexible polymer sheet substrate and an acrylic composite coating; The acrylate composite coating is composed of core-shell structured aerogel microspheres and acrylate adhesive matrix, and is bonded to the surface of a flexible polymer sheet substrate. The core-shell structured aerogel microspheres have a silica aerogel core and a cross-linked acrylate copolymer shell. The core-shell structured aerogel microspheres are uniformly dispersed inside the acrylate binder matrix, and the cross-linked acrylate copolymer shell and the acrylate binder matrix contain the same characteristic functional groups; After the acrylate composite coating is thermocured, the cross-linked acrylate copolymer shell and the acrylate adhesive matrix form an interpenetrating polymer network through a co-crosslinking reaction.

2. The aerogel-coated composite thermal insulation sheet according to claim 1, characterized in that, The thickness of the cross-linked acrylate copolymer shell is 50-200 nm, the characteristic functional group is methacryloxy, and the methacryloxy group is uniformly distributed in the molecular chain segments of the cross-linked acrylate copolymer shell; the cross-linked acrylate copolymer shell is grafted onto the outer surface of the silica aerogel core by covalent chemical bonding.

3. The aerogel-coated composite thermal insulation sheet according to claim 1, characterized in that, The interpenetrating polymer network is a three-dimensional continuous cross-linked structure, and the core-shell structured aerogel microspheres form a continuous integral structure chemically bonded to the acrylate binder matrix through the interpenetrating polymer network.

4. The aerogel-coated composite thermal insulation sheet according to claim 1, characterized in that, The acrylate composite coating is a uniform cross-linked curing system with a dry film thickness of 100-500 μm. The core-shell structured aerogel microspheres account for 20%-50% of the mass of the acrylate binder matrix. The core-shell structured aerogel microspheres are distributed in a monodisperse state in the acrylate binder matrix.

5. The aerogel-coated composite thermal insulation sheet according to claim 1, characterized in that, The flexible polymer sheet substrate is selected from polyethylene terephthalate sheet, polyimide sheet or flexible polyvinyl chloride sheet, and the thickness of the flexible polymer sheet substrate is 50-300 μm.

6. A method for preparing an aerogel-coated composite thermal insulation sheet, the method being applicable to the aerogel-coated composite thermal insulation sheet according to any one of claims 1-5, characterized in that, The specific steps of this preparation method are as follows: Core-shell microsphere grafting modification: Using silica wet gel microspheres as reaction templates, silica wet gel microspheres are dispersed in a mixed solvent to form a suspension system. Acrylic ester reactants, crosslinking agents and initiators are added, and crosslinked ester copolymer shells are grafted onto the surface of silica wet gel microspheres through emulsion polymerization to obtain grafted wet gel microspheres. Core-shell microsphere drying and shaping: After washing, the grafted wet gel microspheres are sent to a supercritical drying equipment for supercritical drying to obtain core-shell structured aerogel microspheres. Preparation of composite coating slurry: Core-shell structured aerogel microspheres are added to a mixture of acrylate binder and solvent, dispersed evenly, and then a curing agent is added. The mixture is then mixed until the system is homogeneous to obtain the composite coating slurry. Substrate coating and curing: The composite coating slurry is coated onto the surface of the flexible polymer sheet substrate by roller coating or blade coating process, and after heat curing treatment, an acrylic composite coating is formed, thereby obtaining the aerogel coating composite thermal insulation sheet.

7. The method for preparing an aerogel-coated composite thermal insulation sheet according to claim 6, characterized in that, In the core-shell microsphere grafting modification, the mixed solvent is a mixture of anhydrous ethanol and deionized water, with a volume ratio of anhydrous ethanol to deionized water of 2-4:1; the emulsion polymerization reaction is carried out under a nitrogen protective atmosphere, at a reaction temperature of 60-70℃, and for a reaction time of 3-5 hours; the acrylate reactive monomer is an acrylate monomer containing methacryloyloxy group, the crosslinking agent is ethylene glycol dimethacrylate, the initiator is ammonium persulfate, the mass ratio of acrylate reactive monomer to crosslinking agent is 8-12:1-2, and the mass ratio of acrylate reactive monomer to initiator is 20-30:

1.

8. The method for preparing an aerogel-coated composite thermal insulation sheet according to claim 6, characterized in that, In the drying and shaping of the core-shell microspheres, the grafted wet gel microspheres are washed 3-5 times with anhydrous ethanol to remove acrylate reactants that did not participate in the polymerization reaction, as well as acrylate homopolymers that were not grafted onto the surface of the silica wet gel microspheres during the reaction. Supercritical drying is carried out using a carbon dioxide supercritical drying process with a drying pressure of 10-15 MPa, a drying temperature of 40-50℃, and a drying time of 4-8 h, resulting in core-shell structured aerogel microspheres.

9. The method for preparing an aerogel-coated composite thermal insulation sheet according to claim 6, characterized in that, In the preparation of the composite coating slurry, the acrylate binder is dissolved in butyl acetate solvent to form a binder solution with a mass fraction of 25%-35%; then, core-shell structured aerogel microspheres are slowly added and stirred at a speed of 150-300 r / min until there is no obvious agglomeration in the system. Then, an isocyanate curing agent is added, with a mass ratio of curing agent to acrylate binder solid of 1:8-12. The mixture is stirred until the system is completely homogeneous to obtain the composite coating slurry.

10. The method for preparing an aerogel-coated composite thermal insulation sheet according to claim 6, characterized in that, In the substrate coating and curing process, the thickness of the composite coating slurry wet film is controlled to be 300-800μm during the roller coating or scraping process; the thermal curing adopts a segmented temperature rise curing method, first pre-curing at 70-90℃ for 20-40min, then raising the temperature to 100-120℃ and holding for curing for 50-70min, until the acrylic composite coating is completely cross-linked and formed, thus obtaining the aerogel coating composite thermal insulation sheet.