A method for preparing a hydrolysis-resistant anti-aging PET film through an online coating and synchronous stretching process and a product application thereof

By employing an online coating and synchronous stretching process, combined with a coating formulation containing polyurethane acrylate, nano-SiO₂, and anti-hydrolysis agents, the problem of limited performance of traditional PET films under humid, hot, and ultraviolet environments has been solved, achieving high barrier properties and aging resistance, making it suitable for photovoltaic backsheets and electronic packaging.

CN123152153APending Publication Date: 2026-11-24JIANGSU SHUANGXING COLOR PLASTIC NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510666972.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Traditional PET films exhibit limited aging resistance when exposed to humid, hot, ultraviolet, or oxidizing environments for extended periods. Their hydrolysis and UV resistance are difficult to improve synergistically, resulting in poor process compatibility, interface defects, and high costs, which restricts their large-scale application.

Method used

The process employs online coating and synchronous stretching. After the base film is extruded, a functional polymer solution is coated onto it, and a segmented drying process is combined to enable the coating and the base film to form a synergistic reinforcing structure during the molecular chain orientation process. The coating formulation includes polyurethane acrylate, nano-SiO₂ and hydrolysis inhibitors, while the base film is enriched with carbodiimide anti-hydrolysis agents and composite antioxidants.

Benefits of technology

The prepared PET film exhibits an intrinsic viscosity decrease rate of ≤10% after damp heat aging, a yellowing index ΔYI <2 after UV aging, a tensile strength retention rate of ≥85%, a water vapor transmission rate of ≤1.5g/m²·day, and an oxygen transmission rate of ≤5cm³/m²·day·atm, making it suitable for applications such as photovoltaic backsheets and electronic packaging.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of polymer materials technology, specifically disclosing a hydrolysis-resistant and anti-aging PET film and its online coating and synchronous stretching preparation method. This method involves online coating of a functional polymer solution after base film extrusion and before biaxial stretching, combined with synchronous stretching and segmented drying processes, enabling the coating and base film to form a synergistic reinforcing structure during molecular chain orientation. The coating formulation includes polyurethane acrylate, nano-SiO2, and hydrolysis inhibitors, while the base film contains carbodiimide anti-hydrolysis agents and composite anti-aging agents. The PET film prepared by this invention exhibits excellent resistance to damp heat aging, UV resistance, and high barrier properties, making it suitable for photovoltaic backsheets, electronic packaging, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer material processing technology, and more particularly to a method for preparing hydrolysis-resistant and anti-aging PET film through online coating and synchronous stretching processes, and its product applications. Background Technology

[0002] Polyethylene terephthalate (PET) film is widely used in packaging, electronics, photovoltaics, and other fields due to its excellent mechanical properties, transparency, and processability. However, traditional PET films are prone to performance degradation when exposed to humid, hot, ultraviolet (UV), or oxidizing environments for extended periods. Specifically, this degradation manifests in several ways: limited aging resistance (difficulty in synergistically improving hydrolysis resistance, UV resistance, and barrier properties); poor process compatibility (disjointed processing of functional coatings and base films, leading to interface defects and high costs); and a performance-cost imbalance (high-end functional films rely on expensive processes (such as coating), limiting large-scale applications). Summary of the Invention

[0003] The purpose of this invention is to provide a method for preparing hydrolysis-resistant and anti-aging PET film through online coating and synchronous stretching processes, and its product applications.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] A method for preparing a hydrolysis-resistant and anti-aging PET film, characterized by comprising the following steps:

[0006] (1) Base film preparation: The dried PET resin is melt-blended with anti-hydrolysis agent and antioxidant, and then extruded and cooled to form an amorphous thick sheet;

[0007] (2) Online coating: Coating the thick sheet surface with a coating solution containing polyurethane acrylate, nano-SiO2 and solvent;

[0008] (3) Synchronous stretching and drying: The coated thick film is stretched longitudinally and laterally in sequence, and dried in sections during the stretching process to remove the solvent;

[0009] (4) Heat setting: Heat set at 210-230℃ for 5-15 seconds to obtain hydrolysis resistant and anti-aging PET film.

[0010] The present invention further specifies that the anti-hydrolysis agent is a carbodiimide compound, and the amount added is 0.3-0.5% of the mass of PET resin; the antioxidant is a composite system of phenolic main antioxidant and phosphite auxiliary antioxidant, and the total amount added is 0.2-0.8%.

[0011] The present invention further specifies that the solid content of polyurethane acrylate in the coating solution is 20-30%, the amount of nano-SiO2 added is 1-3% of the total mass of the coating solution, and the solvent is a mixture of acetone and ethyl acetate with a boiling point range of 50-80℃.

[0012] The present invention further specifies that the preheating temperature for longitudinal stretching is 90-100℃, the stretching ratio is 3.0-4.0 times, and the stretching rate is 100-200% / s; the preheating temperature for transverse stretching is 110-130℃, and the stretching ratio is 3.5-4.5 times.

[0013] The present invention further provides that the segmented drying includes:

[0014] (a) During the longitudinal stretching stage, hot air drying at 60-80℃ is used to ensure that the solvent evaporation rate is ≥90%;

[0015] (b) The transverse stretching stage is dried with high-temperature hot air at 100-120℃ to completely remove residual solvent.

[0016] The present invention further specifies that the coating solution is applied by microgravure coating or slot extrusion coating, the wet film thickness is 5-10 μm, and the coating speed is 10-30 m / min.

[0017] The present invention also provides a hydrolysis-resistant and anti-aging PET film prepared according to the above preparation method, characterized in that its layer structure includes:

[0018] (a) PET base film layer, with a thickness of 10-50 μm;

[0019] (b) A functional coating with a thickness of 0.5-2 μm, the coating comprising a composite network of polyurethane acrylate and nano-SiO2.

[0020] The present invention further provides that the PET film obtained has the following properties:

[0021] (a) After 1000 hours of damp heat aging, the intrinsic viscosity decreases by ≤10%;

[0022] (b) After 500 hours of UV aging, the yellowing index ΔYI < 2, and the tensile strength retention rate ≥ 85%;

[0023] (c) Water vapor transmission rate ≤ 1.5 g / m 2 • day, oxygen permeability ≤ 5cm 3 / m 2 ·day·atm.

[0024] This invention also provides an equipment system for the online coating process in the preparation method of hydrolysis-resistant and anti-aging PET film, characterized in that it comprises:

[0025] (a) Coating unit: Equipped with micro-gravure rollers or slit dies, seamlessly connected to the base film extrusion line;

[0026] (b) Drying module: integrated into the longitudinal stretching roller group and the transverse tenter frame to achieve segmented temperature control; (c) Solvent recovery device: recovers volatile acetone and ethyl acetate through condensation and activated carbon adsorption, with a recovery rate of ≥80%.

[0027] The present invention also provides an application of the PET film described above in photovoltaic backsheets, flexible electronic packaging, or high-barrier food packaging.

[0028] The beneficial effects of this invention are:

[0029] This invention involves online coating of a functional polymer solution after base film extrusion and before biaxial stretching, combined with simultaneous stretching and segmented drying processes, enabling the coating and base film to form a synergistic reinforcing structure during molecular chain orientation. The coating formulation includes polyurethane acrylate, nano-SiO2, and hydrolysis inhibitors, while the base film contains carbodiimide anti-hydrolysis agents and composite anti-aging agents. The PET film prepared by this invention exhibits excellent resistance to damp heat aging, UV resistance, and high barrier properties, making it suitable for applications such as photovoltaic backsheets and electronic packaging. Detailed Implementation

[0030] The following will describe the implementation of this application in detail with reference to the embodiments, so that the implementation process of how this application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.

[0031] A method for preparing a hydrolysis-resistant and anti-aging PET film, characterized by comprising the following steps:

[0032] (1) Base film preparation: The dried PET resin is melt-blended with anti-hydrolysis agent and antioxidant, and then extruded and cooled to form an amorphous thick sheet;

[0033] (2) Online coating: Coating the thick sheet surface with a coating solution containing polyurethane acrylate, nano-SiO2 and solvent;

[0034] (3) Synchronous stretching and drying: The coated thick film is stretched longitudinally and laterally in sequence, and dried in sections during the stretching process to remove the solvent;

[0035] (4) Heat setting: Heat set at 210-230℃ for 5-15 seconds to obtain hydrolysis resistant and anti-aging PET film.

[0036] The present invention further specifies that the anti-hydrolysis agent is a carbodiimide compound, and the amount added is 0.3-0.5% of the mass of PET resin; the antioxidant is a composite system of phenolic main antioxidant and phosphite auxiliary antioxidant, and the total amount added is 0.2-0.8%.

[0037] The present invention further specifies that the solid content of polyurethane acrylate in the coating solution is 20-30%, the amount of nano-SiO2 added is 1-3% of the total mass of the coating solution, and the solvent is a mixture of acetone and ethyl acetate with a boiling point range of 50-80℃.

[0038] The present invention further specifies that the preheating temperature for longitudinal stretching is 90-100℃, the stretching ratio is 3.0-4.0 times, and the stretching rate is 100-200% / s; the preheating temperature for transverse stretching is 110-130℃, and the stretching ratio is 3.5-4.5 times.

[0039] The present invention further provides that the segmented drying includes:

[0040] (a) During the longitudinal stretching stage, hot air drying at 60-80℃ is used to ensure that the solvent evaporation rate is ≥90%;

[0041] (b) The transverse stretching stage is dried with high-temperature hot air at 100-120℃ to completely remove residual solvent.

[0042] The present invention further specifies that the coating solution is applied by microgravure coating or slot extrusion coating, the wet film thickness is 5-10 μm, and the coating speed is 10-30 m / min.

[0043] The present invention also provides a hydrolysis-resistant and anti-aging PET film prepared according to the above preparation method, characterized in that its layer structure includes:

[0044] (a) PET base film layer, with a thickness of 10-50 μm;

[0045] (b) A functional coating with a thickness of 0.5-2 μm, the coating comprising a composite network of polyurethane acrylate and nano-SiO2.

[0046] The present invention further provides that the PET film obtained has the following properties:

[0047] (a) After 1000 hours of damp heat aging, the intrinsic viscosity decreases by ≤10%;

[0048] (b) After 500 hours of UV aging, the yellowing index ΔYI < 2, and the tensile strength retention rate ≥ 85%;

[0049] (c) Water vapor transmission rate ≤ 1.5 g / m 2 • day, oxygen permeability ≤ 5cm3 / m 2 ·day·atm.

[0050] This invention also provides an equipment system for the online coating process in the preparation method of hydrolysis-resistant and anti-aging PET film, characterized in that it comprises:

[0051] (a) Coating unit: Equipped with micro-gravure rollers or slit dies, seamlessly connected to the base film extrusion line;

[0052] (b) Drying module: integrated into the longitudinal stretching roller group and the transverse tenter frame to achieve segmented temperature control; (c) Solvent recovery device: recovers volatile acetone and ethyl acetate through condensation and activated carbon adsorption, with a recovery rate of ≥80%.

[0053] The present invention also provides an application of the PET film described above in photovoltaic backsheets, flexible electronic packaging, or high-barrier food packaging.

[0054] This invention involves online coating of a functional polymer solution after base film extrusion and before biaxial stretching, combined with simultaneous stretching and segmented drying processes, enabling the coating and base film to form a synergistic reinforcing structure during molecular chain orientation. The coating formulation includes polyurethane acrylate, nano-SiO2, and hydrolysis inhibitors, while the base film contains carbodiimide anti-hydrolysis agents and composite anti-aging agents. The PET film prepared by this invention exhibits excellent resistance to damp heat aging, UV resistance, and high barrier properties, making it suitable for applications such as photovoltaic backsheets and electronic packaging.

[0055] Example 1:

[0056] Objective: Basic formulation and process validation

[0057] step:

[0058] Base film preparation:

[0059] Raw materials: PET resin (IV = 0.8 dL / g) after drying is mixed with 0.4% carbodiimide (Stabaxol P), 0.3% Irganox 1010 (phenolic antioxidant), and 0.2% Irgafos 168 (phosphite).

[0060] Extrusion: Extruded into 1.0mm thick sheets using a single screw extruder (280℃), with a cooling roller temperature of 20℃.

[0061] Online coating:

[0062] Coating solution: 25% polyurethane acrylate (PUA), 2% nano-SiO2 (modified with KH550), 73% acetone / ethyl acetate (7:3).

[0063] Coating method: slot extrusion, wet film thickness 8μm, coating speed 15m / min.

[0064] Stretching and drying:

[0065] Longitudinal stretching: Preheat to 100℃, stretching ratio 3.5 times, and simultaneously dry with 80℃ hot air;

[0066] Transverse stretching: preheating at 130℃, stretching ratio 4.0 times, secondary drying at 110℃;

[0067] Heat setting: 225℃ / 10 seconds.

[0068] Test results:

[0069] Water vapor transmission rate (WVTR): 1.2 g / m 2 ·day;

[0070] The intrinsic viscosity decreased by 8.7% after damp heat aging (85℃ / 85%RH, 1000h).

[0071] After QUV aging for 500 hours, ΔYI = 1.5, and the tensile strength retention rate is 89%.

[0072] Example 2:

[0073] Objective: Optimization of coatings with high nanofiller content

[0074] Adjustment points:

[0075] The amount of nano-SiO2 added to the coating was increased to 3.5%, the PUA solid content was 30%, and the solvent ratio was adjusted to acetone / ethyl acetate (6:4).

[0076] Process parameters:

[0077] Coating method: micro-gravure coating (150 lines / inch anilox roller), wet film thickness 10μm;

[0078] The transverse stretch ratio is increased to 4.2 times, and the heat setting temperature is 230℃.

[0079] Test results:

[0080] WVTR decreased to 0.9 g / m 2 ·day;

[0081] Oxygen permeability (OTR): 3.8 cm 3 / m 2 ·day·atm;

[0082] After UV aging, ΔYI = 1.2, and the tensile retention rate is 92%.

[0083] Example 3:

[0084] Objective: Flexible films with low stretch ratios

[0085] Adjustment points:

[0086] The longitudinal / transverse stretch ratio is set to 3.0 times, and the heat setting temperature is 210℃;

[0087] Coating formulation: Add 1% polyether-modified silicone oil (to improve flexibility).

[0088] Test results:

[0089] The elongation at break was increased to 135% (compared to 110% in Example 1);

[0090] WVTR = 1.8g / m 2 ·day, OTR=5.2cm 3 / m 2 ·day·atm;

[0091] Applicable scenarios: Flexible electronic packaging substrates.

[0092] Example 4

[0093] Objective: Composite anti-hydrolysis agent system

[0094] Adjustment points:

[0095] The base film contains 0.3% carbodiimide and an additional 0.2% epoxy hydrolysis inhibitor (ADR-4370).

[0096] Test results:

[0097] The intrinsic viscosity decreased by only 6.5% after damp heat aging;

[0098] Improved coating adhesion (reaching 4B grade in cross-cut adhesion test).

[0099] Example 5

[0100] Objective: UV-cured coating process

[0101] Adjustment points:

[0102] Coating solution: Add 3% photoinitiator (Irgacure 819), and after coating, expose to a UV lamp (365nm, 400mJ / cm). 2 Curing;

[0103] The secondary drying stage of the transverse stretching process is eliminated.

[0104] Test results:

[0105] The coating hardness has been increased to 3H (pencil hardness);

[0106] Solvent residue <50ppm, which meets food packaging standards.

[0107] Comparative Example 1

[0108] Traditional offline coating process:

[0109] The base film is first biaxially stretched, and then coated offline with the same coating solution;

[0110] Drying conditions: 80℃ oven for 10 minutes.

[0111] defect:

[0112] Poor adhesion between the coating and the base film (2B grade in cross-cut adhesion test);

[0113] WVTR = 2.5g / m 2 • day (compared to 1.2 of Example 1)

[0114] Comparative Example 2

[0115] Hydrolysis-resistant base film:

[0116] No carbodiimide is added to the base film; only antioxidants are retained.

[0117] Test results:

[0118] The intrinsic viscosity decreased by as much as 22% after damp heat aging;

[0119] Cracks appeared on the surface of the thin film.

[0120] Comparative Example 3

[0121] No nano-SiO2 coating:

[0122] The coating contains only PUA resin and no nanofillers.

[0123] defect:

[0124] WVTR = 3.0 g / m 2 ·day, OTR = 9.5cm 3 / m 2 ·day·atm;

[0125] After UV aging, ΔYI = 4.8, and it turned yellow significantly.

[0126] If certain terms are used in the specification and claims to refer to specific components, those skilled in the art will understand that hardware manufacturers may use different names to refer to the same component. This specification and claims do not distinguish components based on differences in name, but rather on differences in function. The term "comprising" as used throughout the specification and claims is an open-ended term and should be interpreted as "comprising but not limited to." "Approximately" means that within an acceptable margin of error, those skilled in the art can solve the technical problem and substantially achieve the technical effect within a certain margin of error.

[0127] It should be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a product or system comprising a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a product or system. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the product or system that includes that element.

[0128] The foregoing description illustrates and describes several preferred embodiments of the present invention. However, as previously stated, it should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the inventive concept by means of the foregoing teachings or techniques or knowledge in related fields. Any modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A method for preparing a hydrolysis-resistant and anti-aging PET film, characterized in that, Includes the following steps: (1) Base film preparation: The dried PET resin is melt-blended with anti-hydrolysis agent and antioxidant, and then extruded and cooled to form an amorphous thick sheet; (2) Online coating: Coating the thick sheet surface with a coating solution containing polyurethane acrylate, nano-SiO2 and solvent; (3) Synchronous stretching and drying: The coated thick film is stretched longitudinally and laterally in sequence, and dried in sections during the stretching process to remove the solvent; (4) Heat setting: Heat set at 210-230℃ for 5-15 seconds to obtain hydrolysis resistant and anti-aging PET film.

2. The method for preparing a hydrolysis-resistant and anti-aging PET film according to claim 1, characterized in that, The anti-hydrolysis agent is a carbodiimide compound, and the addition amount is 0.3-0.5% of the PET resin mass; the antioxidant is a composite system of phenolic main antioxidant and phosphite auxiliary antioxidant, and the total addition amount is 0.2-0.8%.

3. The method for preparing a hydrolysis-resistant and anti-aging PET film according to claim 1, characterized in that, The coating solution contains 20-30% polyurethane acrylate solids, and the amount of nano-SiO2 added is 1-3% of the total mass of the coating solution. The solvent is a mixture of acetone and ethyl acetate with a boiling point range of 50-80℃.

4. The method for preparing a hydrolysis-resistant and anti-aging PET film according to claim 1, characterized in that, The preheating temperature for longitudinal stretching is 90-100℃, the stretching ratio is 3.0-4.0 times, and the stretching rate is 100-200% / s; the preheating temperature for transverse stretching is 110-130℃, and the stretching ratio is 3.5-4.5 times.

5. The method for preparing a hydrolysis-resistant and anti-aging PET film according to claim 1, characterized in that, The segmented drying includes: (a) During the longitudinal stretching stage, hot air drying at 60-80℃ is used to ensure that the solvent evaporation rate is ≥90%; (b) The transverse stretching stage is dried with high-temperature hot air at 100-120℃ to completely remove residual solvent.

6. The method for preparing a hydrolysis-resistant and anti-aging PET film according to claim 1, characterized in that, The coating solution is applied by microgravure coating or slot extrusion coating, with a wet film thickness of 5-10 μm and a coating speed of 10-30 m / min.

7. A hydrolysis-resistant and anti-aging PET film prepared according to any one of claims 1-6, characterized in that, Its layered structure includes: (a) PET base film layer, with a thickness of 10-50 μm; (b) A functional coating with a thickness of 0.5-2 μm, the coating comprising a composite network of polyurethane acrylate and nano-SiO2.

8. The hydrolysis-resistant and anti-aging PET film according to claim 7, characterized in that, Its performance meets the following requirements: (a) After 1000 hours of damp heat aging, the intrinsic viscosity decreases by ≤10%; (b) After 500 hours of UV aging, the yellowing index ΔYI < 2, and the tensile strength retention rate ≥ 85%; (c) Water vapor transmission rate ≤ 1.5 g / m 2 • day, oxygen permeability ≤ 5cm 3 / m 2 ·day·atm.

9. An equipment system for the online coating process in the preparation method of the hydrolysis-resistant and anti-aging PET film according to claim 1, characterized in that, include: (a) Coating unit: Equipped with micro-gravure rollers or slit dies, seamlessly connected to the base film extrusion line; (b) Drying module: integrated into the longitudinal stretching roller group and the transverse tenter frame to achieve segmented temperature control; (c) Solvent recovery unit: Acetone and ethyl acetate volatilized by condensation and activated carbon adsorption are recovered with a recovery rate of ≥80%.