A process for the preparation of a zeolite molecular sieve hybrid high absorbent resin
By subjecting Na-type ZSM-5 molecular sieves to ammonium ion exchange and calcination, controlling the degree of sodium ion exchange, preparing a surface treatment solution, and spraying it with heat treatment, the problems of fixation stability of zeolite molecular sieves in highly absorbent resins and inhibition of ammonia components were solved, achieving a balance between dry ammonia removal, wet ammonia suppression, centrifugal water retention, and pressurized absorption.
Patent Information
- Application Number
- CN202611299581.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to control the relative ratio of proton sites to Na-type exchangeable sites in zeolite molecular sieves without altering the bulk polymerization process of highly absorbent resins, and to introduce these sites onto the surface of resin particles through surface treatment processes, thereby achieving a balance between dry ammonia removal, wet ammonia suppression, centrifugal water retention, pressurized absorption, and molecular sieve fixation stability.
By subjecting Na-type ZSM-5 molecular sieves to ammonium ion exchange, washing, drying, and calcination, controlling the sodium ion exchange degree to 35%–65%, a surface treatment solution is prepared together with highly absorbent resin matrix particles. During the surface crosslinking stage, spraying and heat treatment are performed to form a zeolite molecular sieve hybrid highly absorbent resin.
It achieves improved ammonia-containing component inhibition and liquid absorption performance without changing the bulk polymerization process of the highly absorbent resin, while also enhancing the fixation stability of the molecular sieve and maintaining centrifugal water retention and pressurized absorption capacity.
Smart Images

Figure CN123152154A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of highly absorbent resin composite materials, and specifically to a method for preparing a zeolite molecular sieve hybrid highly absorbent resin. Background Technology
[0002] Superabsorbent polymers (SAPs) can absorb and retain large amounts of aqueous liquids and are widely used in absorbent products such as diapers, nursing pads, and pet pee pads. SAPs used in these products not only need high centrifugal water retention and pressure absorption capacity, but also need to suppress the generation and release of ammonia odor after absorbing saline urine. In aqueous systems, ammonia components exist in the form of non-ionic ammonia and ammonium ions, and their relative proportions are affected by pH, temperature, and ionic strength. Simply increasing the adsorption capacity of gaseous ammonia or simply increasing the ion exchange capacity is insufficient to simultaneously achieve both wet ammonia suppression and resin absorbency.
[0003] CN104429992A discloses a production process for pet diaper pads with ammonia removal function and high saline absorption capacity. The process involves placing natural zeolite powder with a particle size less than 100 micrometers in 1 mol / L sulfuric acid, treating it at 50-80℃ for 10-60 minutes, filtering and drying to obtain acidified zeolite, and then thoroughly mixing 2-10 parts by weight of the acidified zeolite with 100 parts by weight of highly absorbent resin. This method utilizes acidified zeolite to improve ammonia removal performance; however, the acid treatment simultaneously alters multiple compensating cations and the framework environment, and the coexistence ratio of proton-type sites and exchangeable Na-type sites is not quantitatively controlled using verifiable elemental ratios. Furthermore, the dry mixing of the acidified zeolite and resin makes it difficult to control the uniformity of molecular sieve distribution and binding stability on the resin particle surface.
[0004] WO2001013965A1 discloses a water-absorbing polymer containing silica-rich zeolite and its preparation method. The silica-rich zeolite can be added in suspension form at the latest during the polymer surface crosslinking stage. Example 5 describes applying silica-rich zeolite, ethylene carbonate, and water together to a dried, pulverized, and sieved water-absorbing polymer, followed by heating at 180°C for 30 minutes. This method already discloses a process of introducing zeolite in suspension and then heating it to fix it during the surface crosslinking stage. Therefore, simply changing the zeolite addition stage from bulk polymerization to surface crosslinking is insufficient to solve the balance problem between the ammonia-containing component suppression ability and the liquid absorption performance. This method mainly uses high-silica hydrophobic zeolite to adsorb organic odor substances, without using the ratio of H-type to Na-type sites in the zeolite as a control variable, and without establishing an exchange window for the ammonia / ammonium form conversion in a saline wet system.
[0005] Na-type zeolites retain a large number of exchangeable cation sites, but have a limited number of proton-type acidic sites. While highly protonated zeolites can increase the number of sites that interact with ammonia in acid-base reactions, they may alter the local ionic environment of the superabsorbent resin particle surface and the liquid absorption behavior of the surface cross-linked layer, making it difficult to maintain centrifugal water retention or pressure absorption capacity. Current technology has not yet established a correlation between zeolite ionic forms, surface introduction methods, and dry-state ammonia removal, wet-state ammonia release inhibition, and liquid absorption performance.
[0006] Furthermore, if molecular sieves are added to the bulk polymerization system of highly absorbent resins, the molecular sieves come into contact with monomers, crosslinking components, and the polymer network in formation from the start of the polymerization reaction. The accessibility of their surface and pores may be affected by the coverage of the polymer network. If dry mixing or low-temperature spraying is performed after the crosslinking of the resin surface is completed, the fixation stability of the molecular sieves is insufficient, and they are prone to falling off during transportation, sieving, and use.
[0007] Therefore, the core problem that existing technologies need to solve is: how to control the relative ratio of proton sites and Na-type exchangeable sites in zeolite molecular sieves with detectable parameters without changing the bulk polymerization process of highly absorbent resin, and introduce them to the surface of resin particles through surface treatment processes, so that the resulting material can achieve a balance between dry ammonia removal, wet ammonia suppression, centrifugal water retention, pressure absorption and molecular sieve fixation stability. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing a zeolite molecular sieve hybrid superabsorbent resin. Without altering the bulk polymerization process of the superabsorbent resin, the ionic morphology of the zeolite molecular sieve is detectably controlled, and it is introduced into the superabsorbent resin particles during the surface crosslinking stage, thereby balancing the suppression performance of ammonia components, liquid absorption performance, and molecular sieve fixation stability.
[0009] To achieve the above objectives, the present invention provides the following technical solution:
[0010] A method for preparing a zeolite molecular sieve hybrid superabsorbent resin includes the following steps:
[0011] S1, Na-type ZSM-5 molecular sieve is subjected to ammonium ion exchange with an ammonium salt aqueous solution, followed by washing, drying, and calcination to obtain a partially protonated ZSM-5 molecular sieve that retains both proton-type sites and Na-type exchangeable sites; the sodium ion exchange degree E of the partially protonated ZSM-5 molecular sieve is calculated according to the formula E = [1 - (R1 / R0)] × 100%, where R0 is the Na / Al molar ratio of the Na-type ZSM-5 molecular sieve before ammonium ion exchange, R1 is the Na / Al molar ratio of the partially protonated ZSM-5 molecular sieve obtained after ammonium ion exchange, washing, drying, and calcination, and the sodium ion exchange degree E is 35% to 65%;
[0012] S2 provides highly absorbent resin matrix particles that have undergone bulk polymerization, drying, pulverization and sieving, and combines partially protonated ZSM-5 molecular sieves, water, water-soluble polyols and surface crosslinking agents in the same surface treatment solution.
[0013] S3, the surface treatment liquid is sprayed onto the surface of the highly absorbent resin matrix particles, and the sprayed highly absorbent resin matrix particles are heat-treated to cause cross-linking of the surface layer of the highly absorbent resin matrix particles, and to retain part of the protonated ZSM-5 molecular sieve on the surface layer of the highly absorbent resin matrix particles, thereby obtaining zeolite molecular sieve hybrid highly absorbent resin.
[0014] In a preferred embodiment, in step S1, the sodium ion exchange degree E is 40% to 60%.
[0015] In a preferred embodiment, in step S1, the sodium ion exchange degree E is 45% to 55%.
[0016] In a preferred embodiment, the Na-type ZSM-5 molecular sieve has an MFI topology, a Si / Al molar ratio of 25–60, and a median particle size D50 of 0.5–2.2 μm.
[0017] In a preferred embodiment, in step S1, the ammonium salt is selected from one of ammonium nitrate, ammonium chloride, ammonium sulfate, and ammonium acetate; the concentration of the ammonium salt aqueous solution is 0.20–0.80 mol / L, the solid-liquid mass ratio of Na-type ZSM-5 molecular sieve to the ammonium salt aqueous solution is 1:(8–15), the ammonium ion exchange temperature is 55–75°C, and the ammonium ion exchange time is 45–120 min.
[0018] In a preferred embodiment, in step S1: ammonium ion exchange is performed only once, and after the ammonium ion exchange is completed, solid-liquid separation is performed. The liquid is washed with deionized water until the conductivity of the last washing solution is not higher than 100 μS / cm. Then, it is dried at 100-120°C for 2-6 hours, and heated to 480-550°C at a heating rate of 2-5°C / min, and calcined for 2-4 hours.
[0019] R0 and R1 are the Na / Al molar ratios measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) after the corresponding molecular sieve samples have been completely digested.
[0020] In a preferred embodiment, in step S2: the highly absorbent resin matrix particles are particles containing a partially neutralized polyacrylate crosslinked network, with a particle size of 150–850 μm and a degree of neutralization of 65–80 mol%;
[0021] Based on 100 parts by weight of highly absorbent resin matrix particles, the surface treatment liquid includes 0.8 to 2.2 parts by weight of partially protonated ZSM-5 molecular sieve, 0.05 to 0.25 parts by weight of surface crosslinking agent, 1.5 to 3.5 parts by weight of water, and 0.3 to 1.2 parts by weight of water-soluble polyol.
[0022] In a preferred embodiment, the surface crosslinking agent is ethylene glycol diglycidyl ether, and the water-soluble polyol is 1,2-propanediol. Water and 1,2-propanediol are mixed, and a portion of protonated ZSM-5 molecular sieve is added at 1500–3000 rpm and dispersed for 3–10 min. Then, ethylene glycol diglycidyl ether is added, and the mixture is mixed at 300–800 rpm for 1–3 min to obtain a surface treatment solution. The surface treatment solution is kept circulating or stirred, and spraying is completed within 30 min after preparation.
[0023] In a preferred embodiment, in step S3: the surface treatment liquid is continuously sprayed onto the surface of the highly absorbent resin matrix particles in one go, and after the spraying is completed and mixing continues, a heat treatment is directly performed.
[0024] The feed temperature of the highly absorbent resin matrix particles is 40-70℃. Under the mixing conditions of 500-1200rpm, the spraying is completed within 1-5 minutes, and the mixing continues for 2-8 minutes after spraying.
[0025] The heat treatment temperature is 150-180℃ and the heat treatment time is 20-45 min. After heat treatment, the material is cooled to no higher than 50℃ and particles with a diameter of less than 150μm and greater than 850μm are screened out.
[0026] In a preferred embodiment, in step S2, the surface treatment liquid comprises 1.5 parts by mass of partially protonated ZSM-5 molecular sieve, 2.0 parts by mass of water, 1.0 parts by mass of 1,2-propanediol, and 0.20 parts by mass of ethylene glycol diglycidyl ether, based on 100 parts by mass of highly absorbent resin matrix particles.
[0027] In step S3, after the surface treatment liquid is sprayed onto the surface of the highly absorbent resin matrix particles, it is heat-treated at 165°C for 30 minutes.
[0028] By adopting the above technical solution, the beneficial effects of the present invention are as follows:
[0029] This invention does not add zeolite molecular sieves to the bulk polymerization system of highly absorbent resins. Instead, it uses highly absorbent resin matrix particles that have already undergone bulk polymerization, drying, pulverization, and sieving as the treatment object, and introduces zeolite molecular sieves during the surface crosslinking stage. This does not require changes to the existing bulk polymerization process of highly absorbent resins and can be integrated with existing surface treatment production lines for highly absorbent resin particles.
[0030] Furthermore, an incomplete ammonium ion exchange was performed on the Na-type ZSM-5 molecular sieve. After washing, drying, and calcination, an H / Na-ZSM-5 molecular sieve was formed that simultaneously retained proton sites and Na-type exchangeable sites. The sodium ion exchange degree was calculated by using the change in the Na / Al molar ratio before and after the exchange. This transformed the molecular sieve ion morphology from indirect process parameters such as ammonium salt concentration and exchange time into material parameters that can be detected and verified by ICP-OES, which is beneficial to improving the consistency and repeatability of molecular sieve treatment results for different batches.
[0031] Furthermore, controlling the sodium ion exchange ratio (SOr) between 35% and 65% avoids the insufficient proton sites when using only Na-type molecular sieves and also reduces the adverse effects of highly protonated molecular sieves on the liquid absorption network of the highly absorbent resin surface during humid heat surface treatment. Experimental results show that the dry ammonia removal rate generally increases with increasing SOr. The wet ammonia release inhibition rate does not increase linearly with SOr, but reaches a higher level at moderate SOr. Specifically, when the SOr is 50.0%, the wet ammonia release inhibition rate reaches 82%, higher than the 52%, 61%, and 55% when the SOr is 20.0%, 80.0%, and 92.5%, respectively. This indicates that moderately retaining both proton and Na-type exchangeable sites is beneficial for balancing ammonia component inhibition performance under both dry and wet conditions.
[0032] Furthermore, H / Na-ZSM-5 molecular sieve, water, polyol, and surface crosslinking agent are formulated into a single surface treatment solution. This solution allows for simultaneous surface crosslinking of the highly absorbent resin particles and retention of the molecular sieve surface through a single spraying and heat treatment, eliminating the need for separate pre-spraying, pre-fixation, separate drying, or secondary heat treatment of the molecular sieve. Compared to adding the solution during bulk polymerization, surface dry mixing, and step-by-step spraying, this treatment path reduces the likelihood of the molecular sieve being coated by the polymer network or detaching from the resin particle surface, while also reducing the number of process steps.
[0033] Furthermore, within the sodium ion exchange capacity range of 35%–65%, the obtained hybrid superabsorbent resin exhibited a CRC of 31.6–32.0 g / g and an AAP of 26.7–27.1 g / g, reaching 97.5%–98.8% and 97.1%–98.5% respectively, compared to the surface cross-linked sample without added molecular sieves. When the sodium ion exchange capacity increased to 80.0% and 92.5%, the CRC and AAP further decreased. Thus, this invention, through a control path of “partial ion exchange—ion speciation detection—surface spraying—heat treatment,” improves the suppression ability of ammonia components while reducing the adverse effects of introducing molecular sieves on brine absorption performance and pressure absorption performance. Attached Figure Description
[0034] Figure 1This is a flowchart of the method for preparing zeolite molecular sieve hybrid high-absorption resin according to the present invention. Detailed Implementation
[0035] The following embodiments are used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Unless otherwise stated, all "parts" refer to parts by mass, and all water used is deionized water. The examples and comparative examples used the same batch of Na-type ZSM-5 molecular sieve and the same batch of highly absorbent resin matrix. Each performance test used three independent sample batches, and each independent sample batch had three parallel samples. The arithmetic mean of the three parallel samples of the same independent sample batch was calculated first, and then the arithmetic mean of the average values obtained from the three independent sample batches was calculated. Unless otherwise stated, the data listed in Tables 3 to 5 are the arithmetic mean of the test results of three independent sample batches.
[0036] See Figure 1 The preparation method of the present invention includes steps S1, S2, and S3. Step S1 is the preparation step of partially protonated ZSM-5 molecular sieve, which involves ammonium ion exchange, solid-liquid separation, washing, drying, and calcination of Na-type ZSM-5 molecular sieve to obtain a partially protonated ZSM-5 molecular sieve with a sodium ion exchange degree of 35%–65%. Step S2 is the preparation step of surface treatment liquid, which involves preparing a surface treatment liquid by combining partially protonated ZSM-5 molecular sieve, water, water-soluble polyol, and a surface crosslinking agent. Step S3 is the surface treatment step of highly absorbent resin matrix particles, which involves spraying the surface treatment liquid onto the surface of highly absorbent resin matrix particles that have undergone bulk polymerization, drying, pulverization, and sieving, followed by heat treatment, cooling, and sieving to obtain a zeolite molecular sieve hybrid highly absorbent resin.
[0037] The reference Na-type ZSM-5 molecular sieve has an MFI topology, a Si / Al molar ratio of 40.2, a D50 of 1.2 μm, and a D90 of 4.5 μm. Samples before and after exchange were completely acid-digested, and the Na and Al contents were determined by ICP-OES. The sodium ion exchange degree was calculated based on the measured R0 and R1 values for each batch.
[0038] The highly absorbent resin matrix was prepared as follows: Based on 100 parts of acrylic acid, a 48 wt% sodium hydroxide aqueous solution was added under cooling conditions to achieve a neutralization degree of 72 mol%; the solid content of the monomer aqueous solution was adjusted to 40 wt%, and 0.12 parts of polyethylene glycol diacrylate were added as an internal crosslinking agent. Under nitrogen protection, 0.15 parts of sodium persulfate and 0.03 parts of ascorbic acid were added to initiate polymerization. The resulting gel was kept at 80–95 °C for 30 min, crushed, dried at 150 °C for 60 min, pulverized, and sieved to obtain particles of 150–850 micrometers.
[0039] The preparation conditions for molecular sieves with different sodium ion exchange degrees are shown in Table 1. After one ammonium exchange cycle, each sample underwent solid-liquid separation, was washed with deionized water until the conductivity of the final wash solution did not exceed 100 μSiemens / cm, dried at 110°C for 4 hours, and then heated to 520°C at a rate of 3°C / min and held at that temperature for 3 hours. The high-degree protonated molecular sieve of Comparative Example 5 was prepared using the repeated ammonium exchange method described in Comparative Example 5 below. The calcination equipment was equipped with ammonia and nitrogen oxide tail gas treatment units. The cooled molecular sieves were sealed and stored, and their moisture content was measured before spraying.
[0040] Table 1: Preparation conditions of molecular sieves with different sodium ion exchange degrees
[0041]
[0042] Example 1:
[0043] Take 1.5 parts of Z35 molecular sieve with a sodium ion exchange capacity of 35.0%. Mix 2.0 parts of water with 1.0 part of 1,2-propanediol, slowly add Z35 at 2000 rpm and continue dispersing for 5 min; add 0.20 parts of ethylene glycol diglycidyl ether, mix at 500 rpm for 3 min to obtain the surface treatment solution. Keep the treatment solution stirred slowly at 200 rpm and use it within 30 min after preparation.
[0044] 100 parts of highly absorbent resin matrix particles were preheated to 55 degrees Celsius, and surface treatment liquid was sprayed into them within 3 minutes under mixing conditions of 800 rpm, and mixing was continued for 5 minutes; then heated at 165 degrees Celsius for 30 minutes, cooled to 45 degrees Celsius, and particles smaller than 150 micrometers and larger than 850 micrometers were sieved out to obtain Example 1.
[0045] Examples 2-5:
[0046] Examples 2-5 replace Z35 in Example 1 with equal masses of Z42.5, Z50, Z57.5, and Z65, respectively, while the remaining raw material amounts, spraying conditions, and heat treatment conditions are the same as in Example 1. Examples 1-5 only change the sodium ion exchange degree of the molecular sieve to evaluate the effect of exchange degree on performance.
[0047] Example 6: Molecular sieve dosage
[0048] Both Examples 6-1 and 6-2 used Z50, with the molecular sieve dosage adjusted to 0.8 parts and 2.2 parts respectively, and the other conditions were the same as in Example 3.
[0049] Examples 7-10: Si / Al and particle size endpoints
[0050] Example 7 used 1.5 parts of H / Na-ZSM-5 molecular sieve with a Si / Al molar ratio of 25, a D50 of 1.2 μm, and a sodium ion exchange capacity of 50.0%; Example 8 used 1.5 parts of H / Na-ZSM-5 molecular sieve with a Si / Al molar ratio of 60, a D50 of 1.2 μm, and a sodium ion exchange capacity of 50.0%; Example 9 used 1.5 parts of H / Na-ZSM-5 molecular sieve with a Si / Al molar ratio of 40, a D50 of 0.5 μm, and a sodium ion exchange capacity of 50.0%; Example 10 used 1.5 parts of H / Na-ZSM-5 molecular sieve with a Si / Al molar ratio of 40, a D50 of 2.2 μm, and a sodium ion exchange capacity of 50.0%. All other conditions were the same as in Example 3.
[0051] Comparative Examples 1-5: Cross-commutation Boundary Control
[0052] Comparative Example 1 did not include molecular sieves; the composition of the remaining surface treatment solution, as well as the spraying and heat treatment conditions, were the same as in Example 3. The missing 1.5 parts of molecular sieve were not made up with other solids. Comparative Example 2 used 1.5 parts of Na-type ZSM-5 molecular sieve that had not undergone ammonium exchange and calcination. Comparative Examples 3 and 4 used Z20 with a sodium ion exchange capacity of 20.0% and Z80 with a sodium ion exchange capacity of 80.0%, respectively, with all other conditions being the same as in Example 3.
[0053] Comparative Example 5 used a highly protonated ZSM-5 molecular sieve. The Na-type ZSM-5 molecular sieve was placed in a 1.0 mol / L ammonium nitrate solution and exchanged at 60°C for 6 hours at a solid-liquid mass ratio of 1:10. This exchange was repeated twice. After washing and drying, the sieve was calcined at 520°C for 3 hours to obtain a molecular sieve with a sodium ion exchange rate of 92.5%. 1.5 parts of a surface treatment solution were added, and the remaining conditions were the same as in Example 3.
[0054] Comparative Example 6: Addition of Ontology Aggregation
[0055] In the monomer aqueous solution for preparing the superabsorbent resin matrix, 1.5 parts of Z50 relative to 100 parts of dry resin solids were added. The internal crosslinking agent, monomer neutralization degree, solid content, initiator dosage, and polymerization, gel breaking, drying, pulverizing, and sieving conditions were the same as those for the preparation of the superabsorbent resin matrix. For surface treatment, only a treatment solution consisting of 2.0 parts of water, 1.0 part of 1,2-propanediol, and 0.20 parts of ethylene glycol diglycidyl ether was sprayed, and the mixture was heated according to the conditions of Example 3.
[0056] Comparative Example 7: Dry Mixing After Surface Crosslinking
[0057] First, complete the surface crosslinking treatment without molecular sieve according to Comparative Example 1. After cooling, add 1.5 parts of Z50 and dry mix at 500 rpm for 10 min. Do not spray or heat again.
[0058] Comparative Example 8: Acidified Natural Zeolite Dry Mix
[0059] Natural zeolite powder with a particle size of less than 100 micrometers was placed in 1.0 mol / L sulfuric acid and treated at 70°C for 30 min. It was then vacuum filtered and washed with deionized water until the pH of the final washing solution was not lower than 5.5. The solution was dried at 105°C to constant weight to obtain acidified natural zeolite. First, a surface cross-linking treatment without molecular sieves was performed according to Comparative Example 1. After cooling, 1.5 parts of acidified natural zeolite were added, and the mixture was dry-mixed at 500 rpm for 10 min without further heat treatment.
[0060] Comparative Example 9: Step-by-step spraying
[0061] Disperse 1.5 parts of Z50 in 2.0 parts of water and 1.0 parts of 1,2-propanediol, spray it onto the surface of 100 parts of highly absorbent resin matrix particles and dry it at 80 degrees Celsius for 20 min; then spray it with a surface crosslinking liquid containing 0.20 parts of ethylene glycol diglycidyl ether and 1.0 parts of water and heat treat it at 165 degrees Celsius for 30 min.
[0062] Comparative Example 10: Uncalcined ammonium molecular sieve
[0063] The Na-type ZSM-5 molecular sieve was treated under the Z50 ammonium exchange, washing, and drying conditions, but without calcination at 520°C. A surface treatment solution was prepared at 1.5 parts of the obtained ammonium-type molecular sieve and sprayed and heat-treated at 165°C according to the conditions of Example 3. The Na / Al ratio and residual ammonium content of the molecular sieve were measured before and after surface treatment to confirm that the sample obtained at 165°C was different from the H / Na-ZSM-5 calcined at 520°C.
[0064] Comparative Example 11: Surface crosslinking of silica-rich zeolite added
[0065] Commercially available high-silica hydrophobic zeolite with a SiO2 / Al2O3 molar ratio of approximately 500 and a D50 of 1.2 micrometers after grinding was used. A suspension was prepared by mixing 1.5 parts of high-silica zeolite, 0.5 parts of ethylene carbonate, and 3.0 parts of water per 100 parts of highly absorbent resin matrix particles. This mixture was applied to the surface of the matrix particles and heated at 180°C for 30 minutes to replicate the process of adding silica-rich zeolite during the surface crosslinking stage.
[0066] Performance testing and structural characterization:
[0067] The sodium ion exchange capacity was determined according to the aforementioned method for calculating the change in the Na / Al molar ratio. 0.1000 g of the molecular sieve sample was weighed and placed in a polytetrafluoroethylene microwave digestion vessel. 6.0 mL of nitric acid and 2.0 mL of hydrofluoric acid were added, and the mixture was allowed to stand for a pre-reaction of 10 min before being sealed for digestion. The temperature was raised to 190 °C within 15 min and maintained at 190 ± 5 °C for 30 min. After digestion and cooling, 20 mL of a 4% (w / w) boric acid aqueous solution was added, and the mixture was maintained at 120 °C for 20 min to complex residual fluoride ions. After cooling, the mixture was transferred to a polypropylene volumetric container and brought to a final volume of 100 mL with deionized water.
[0068] The Na and Al contents in the digestion solution were determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). The analytical wavelengths for Na and Al were 589.592 nm and 396.152 nm, respectively. Standard working solutions with concentrations of 0 mg / L, 1 mg / L, 2 mg / L, 5 mg / L, 10 mg / L, and 20 mg / L were prepared using Na and Al standard solutions, respectively. The correlation coefficients of the obtained standard curves were all no less than 0.9995. Each sample was digested twice independently. When the relative deviation of the Na / Al molar ratio measured twice was no greater than 5%, the average of the two measurements was taken as the Na / Al molar ratio of the corresponding sample.
[0069] The centrifugal water retention capacity (CRC) was determined according to the bag method of NWSP 241.0.R2. 0.2000 g of sample was weighed and placed in a nonwoven bag, then immersed in a 0.9 wt% sodium chloride aqueous solution at 23±2℃ for 30 min. After removal, the sample was centrifuged at 1400 rpm for 3 min using a 23 cm diameter centrifuge, with a blank nonwoven bag provided. The CRC was calculated as the ratio of the net mass of liquid absorbed by the sample after centrifugation to the dry sample mass.
[0070] The absorbance under pressure (AAP) was determined according to NWSP 242.0.R2. 0.9000 g of sample was weighed and evenly spread inside a cylinder with a sieve bottom. A load of 0.3 psi was applied, and the cylinder was placed on a 0.9 wt% sodium chloride aqueous solution with the liquid surface level with the upper surface of the glass filter plate for absorption for 60 min. AAP was calculated as the ratio of the net mass of the absorbed liquid to the dry sample mass.
[0071] The dry-state ammonia removal rate and dynamic wet-state ammonia release inhibition rate were measured using the same gas-phase ammonia detection method. The gas-phase ammonia concentration was determined using a pump-suction electrochemical ammonia detector with a range of 0–100 ppm, a resolution of 0.1 ppm, and a limit of quantitation of 0.5 ppm. Zero-point calibration was performed using ammonia-free zero gas before each test, and range calibration was performed using a 50 ppm ammonia standard gas.
[0072] Before measurement, the sample gas bag was repeatedly squeezed and mixed 5 times, or the sealed container was horizontally shaken for 30 seconds to ensure uniform mixing of the internal gas. Then, the gas to be tested was introduced into the detector at a flow rate of 300 mL / min, and readings were taken continuously for 60 seconds. The arithmetic mean of the readings in the last 30 seconds was taken as the gaseous ammonia concentration of the corresponding sample. The same sampling flow rate, sampling time, gas path length, and instrument calibration conditions were used for all examples, comparative examples, and blank samples.
[0073] The dry ammonia removal rate was determined as follows: 1.00 g of dry sample was placed in a 5 L gas bag, filled with 3.00 L of air with an ammonia concentration of 50 ppm, and placed at 25±2℃ and 50%±5% relative humidity for 2 hours. Following the aforementioned gas phase ammonia detection method, the initial ammonia concentration C0 within 1 minute after filling the sample gas bag and the final ammonia concentration Ct after 2 hours were measured. Simultaneously, a blank gas bag without the sample was set up, and C0b and Ctb were measured. The blank-corrected dry ammonia removal rate Rdry was calculated as Rdry={1-[(Ct / C0) / (Ctb / C0b)]}×100%.
[0074] The dynamic wet ammonia release inhibition rate was determined as follows: A simulated urine solution containing 0.90 wt% sodium chloride, 2.0 wt% urea, and 0.002 wt% ammonium chloride was prepared. The pH of the simulated urine solution was adjusted to 8.50 ± 0.05 using a 0.10 mol / L sodium hydroxide aqueous solution, and the pH was measured at 23 ± 2 °C. 1.00 g of sample was used to absorb 20.0 g of simulated urine, followed by the addition of 0.20 mL of freshly prepared urease aqueous solution with an activity concentration of 0.10 U / mL, ensuring a total urease activity of 0.02 U in each test container. The absorbed sample was placed in a 2 L sealed container and incubated at 37 ± 1 °C for 4 h. The headspace ammonia concentration was then determined according to the aforementioned gas phase ammonia detection method.
[0075] Based on the headspace ammonia concentration Cblank of Comparative Example 1, the dynamic wet ammonia release inhibition rate was calculated according to Rwet = (Cblank - Csample) / Cblank × 100%, where Csample is the headspace ammonia concentration of the corresponding example or comparative example.
[0076] In this embodiment, 1U of urease activity refers to the amount of enzyme required to catalyze the release of 1 μmol of ammonia per minute from urea under conditions of pH 7.0 and temperature 25°C. A urease aqueous solution with an activity concentration of 0.10 U / mL was prepared according to the nominal specific activity of the urease used. The urease aqueous solution was prepared fresh before use and used within 2 hours of preparation. The urease activity was pre-confirmed using Comparative Example 1, ensuring that the headphase ammonia concentration after 4 hours of reaction was within 20%–80% of the instrument's range. All embodiments and comparative examples used the same batch of simulated urine, the same batch of urease, and the same reaction time; a control of simulated urine without added urease was also provided to distinguish the contribution of initial ammonium chloride release to the dynamic conversion of urea.
[0077] The molecular sieve fixation rate was determined as follows: 50.0g of the finished product was placed in an electromagnetic test sieve with a sieve mesh size of 106μm. After adding the sieve cover, the sieve was vibrated for 15 minutes at a vibration frequency of 50Hz and a vertical amplitude of 1.0mm. After vibration, the mass of the particles on the sieve and the fine powder under the sieve were weighed, and the Si and Al contents in the finished product and the fine powder under the sieve before vibration were determined. The amount of detached molecular sieve was calculated based on the mass of the fine powder under the sieve and the Si and Al contents in the fine powder under the sieve. The molecular sieve fixation rate was calculated as follows: Molecular sieve fixation rate = (Initial molecular sieve amount - Detached molecular sieve amount) / Initial molecular sieve amount × 100%. Each sample was tested using three independent batches, and each independent batch had three parallel samples.
[0078] Test Results and Analysis:
[0079] The ICP-OES determination results of molecular sieves with different exchange degrees are shown in Table 2, and the performance test results of each example and comparative example are shown in Tables 3, 4 and 5.
[0080] Table 2: Results of Ion Speciation Determination of Molecular Sieves with Different Exchange Degrees
[0081]
[0082] Table 3: Performance test results of samples with exchangeability window
[0083]
[0084] Table 4: Performance test results of different introduction and surface treatment routes
[0085]
[0086] Table 5: Performance test results of samples with different molecular sieve dosages, Si / Al molar ratios, and particle size variations.
[0087]
[0088] Table 2 shows that as the degree of ammonium exchange increases, the R1 of the molecular sieve decreases from 0.94 for Na-type raw materials to 0.07, while the Si / Al molar ratio of each group remains between 40.1 and 40.2, indicating that the change in Na content is not caused by the change in the skeleton Al content. The degree of exchange calculated by E=[1-(R1 / R0)]×100% is consistent with the grouping of each sample, and the Na / Al molar ratio can be used to quantitatively distinguish the mixed ion forms of H / Na.
[0089] Table 3 shows that the dry-state ammonia removal rate generally increases with the sodium ion exchange degree, rising from 18% for the Na-type molecular sieve sample to 62% for the sample with a 92.5% exchange degree, indicating that increasing the number of proton sites is beneficial for the removal of ammonia components under dry conditions. The dynamic wet-state ammonia release inhibition rate does not increase monotonically with the exchange degree, but reaches 82% at a 50.0% exchange degree, which is 30 and 21 percentage points higher than the samples with 20.0% and 80.0% exchange degrees, respectively. When the exchange degree is further increased to 92.5%, the dynamic wet-state inhibition rate decreases to 55%.
[0090] Compared to Comparative Example 1, which did not contain molecular sieves but used the same surface crosslinking conditions, the CRC retention rate of Examples 1-5 was 97.5%-98.8%, and the AAP retention rate was 97.1%-98.5%. The AAP retention rate of Comparative Example 4 decreased to 93.8%, and the CRC and AAP retention rates of Comparative Example 5 decreased to 92.0% and 90.5%, respectively. This shows that an exchange rate range of 35%–65% can maintain high liquid absorption performance while achieving high dynamic wet ammonia suppression performance, while excessively high exchange rates will increase the loss of liquid absorption performance.
[0091] Based on the combined results of dry-state deammoniation, dynamic wet-state ammonia suppression, CRC, and AAP, a comprehensive performance window is formed when the exchangeability is between 35% and 65%, with samples exhibiting an exchangeability of 50.0%-57.5% achieving a dynamic wet-state inhibition rate exceeding 80%. These results indicate that the exchangeability range defined in this invention is not arbitrarily chosen within the linear trend of dry-state deammoniation rate increasing with exchangeability, but rather determined jointly by the wet-state ammonia suppression peak and the liquid absorption performance boundary.
[0092] As shown in Table 4, the dry ammonia removal rate and dynamic wet inhibition rate of Example 3 were 18 and 24 percentage points higher than those of Comparative Example 6, respectively. Although Comparative Example 6 had a higher fixation rate, the ability of the molecular sieve to act on ammonia components decreased significantly after entering the bulk polymerization, indicating that placing the molecular sieve on the surface of the preformed resin particles, avoiding the bulk polymerization, is beneficial to maintaining the accessibility of its sites.
[0093] Compared to Comparative Example 7 (dry-mixed after surface crosslinking), Comparative Example 8 (dry-mixed with acidified natural zeolite), and Comparative Example 9 (step-by-step spraying), Example 3 showed that the dynamic wet-state inhibition rate was increased by 21, 22, and 13 percentage points, respectively, and the fixation rate was increased by 40, 42, and 18 percentage points, respectively. These results indicate that preparing H / Na-ZSM-5 and the surface crosslinking agent in the same treatment solution and performing a single spraying and heat treatment can improve the molecular sieve fixation stability and wet-state ammonia suppression effect while reducing the need for separate pre-spraying and pre-drying steps.
[0094] Compared to Comparative Example 10, which used uncalcined ammonium molecular sieves, Example 3 showed an increase of 29 and 38 percentage points in dry-state ammonia removal rate and dynamic wet-state inhibition rate, respectively; compared to Comparative Example 11, which used silica-rich hydrophobic zeolite added via a surface crosslinking route, the increases were 27 and 35 percentage points, respectively. These results indicate that calcination after ammonium exchange and controlling the coexistence of H-type and Na-type sites through the Na / Al molar ratio are crucial conditions for achieving ammonia-containing component inhibition. Adding zeolite with uncontrolled ionic forms only during the surface crosslinking stage cannot achieve the same effect.
[0095] Table 5 shows that increasing the Z50 molecular sieve dosage within the range of 0.8–2.2 parts increases the dry ammonia removal rate and dynamic wet inhibition rate, while CRC and AAP only decrease slowly. A dosage of 1.5 parts achieves a good balance between ammonia component inhibition and liquid absorption performance. Samples with Si / Al ratios of 25 and 60 maintain the effects of this invention, with the Si / Al 25 sample exhibiting higher ammonia removal and wet inhibition performance, and the Si / Al 60 sample exhibiting higher CRC and AAP. Samples with a D50 of 0.5 micrometers exhibit higher ammonia inhibition performance, and samples with a D50 of 2.2 micrometers exhibit higher fixation rate, indicating that the 0.5–2.2 micrometer particle size range can be selected according to performance priorities.
[0096] For Na-ZSM-5 with a Si / Al molar ratio of approximately 40, the total exchange site capacity, estimated using the approximate structural unit NaAlSi40O82, is approximately 0.40 mmol / g. Assuming 1.5 parts of molecular sieve are added to 100 parts of resin, 1.00 g of the finished product contains approximately 0.015 g of molecular sieve, corresponding to a total exchange site capacity of approximately 0.0060 mmol; the total ammonia content in the dry-state test is approximately 0.0061 mmol. This material balance is consistent with the results shown in Table 3, where samples with moderate exchange rates did not show near-complete removal.
[0097] In the wet test, 20.0 g of simulated urine contained approximately 0.0075 mmol of ammonium chloride (0.002 wt%); the maximum ammonia content generated by 0.02 U urease, calculated based on nominal activity, was approximately 0.0048 mmol within 4 hours, totaling approximately 0.0123 mmol. This loading is higher than the total exchange sites of the molecular sieve but within the same order of magnitude. This avoids the very low ammonia loading being masked by the resin matrix, and also reduces the impact of excessively high loading causing different molecular sieves to rapidly reach the same saturation state.
[0098] The number of protons carried by approximately 1.5 wt% molecular sieve is insufficient to significantly protonate the overall carboxylate of the resin. Combined with the results in Table 3 showing a slow decrease in CRC and a more pronounced decrease in AAP at high exchange rates, the change in liquid absorption performance is mainly manifested in the pressure absorption process, which is more sensitive to the surface state of the particles. This result is consistent with the fact that the molecular sieve is located in the surface cross-linking layer, and the local ionic environment changes with the exchange rate, but this invention is not limited to a specific microscopic reaction mechanism.
[0099] The ammonium exchange, filtration and washing, drying and calcination, slurry dispersion, one-time spraying, and surface thermal cross-linking employed in this invention are all unit operations that can be implemented in the molecular sieve and superabsorbent resin industries. By determining the degree of exchange using the Na / Al molar ratio, limiting the molecular sieve particle size and the residence time of the surface treatment solution, and incorporating calcination exhaust gas treatment, a clear, repeatable production path can be formed that conforms to the principles of ion exchange, acid-base interaction, and polymer surface cross-linking. The resulting material can be used in absorbent products such as diapers, nursing pads, and pet pee pads.
[0100] The above embodiments are used to illustrate the technical concept and implementation path of the present invention. Without departing from the technical concept of the present invention, those skilled in the art can make adaptive adjustments to the spraying flow rate of the treatment liquid, the mixing intensity of the materials, and the heat treatment residence time based on the particle size distribution of the highly absorbent resin matrix, the type of surface treatment equipment, and the processing capacity.
Claims
1. A method for preparing a zeolite molecular sieve hybrid superabsorbent resin, characterized in that, Includes the following steps: S1, Na-type ZSM-5 molecular sieve is subjected to ammonium ion exchange with an ammonium salt aqueous solution, followed by washing, drying, and calcination to obtain a partially protonated ZSM-5 molecular sieve that retains both proton-type sites and Na-type exchangeable sites; the sodium ion exchange degree E of the partially protonated ZSM-5 molecular sieve is calculated according to the formula E = [1 - (R1 / R0)] × 100%, where R0 is the Na / Al molar ratio of the Na-type ZSM-5 molecular sieve before ammonium ion exchange, R1 is the Na / Al molar ratio of the partially protonated ZSM-5 molecular sieve obtained after ammonium ion exchange, washing, drying, and calcination, and the sodium ion exchange degree E is 35% to 65%; S2 provides highly absorbent resin matrix particles that have undergone bulk polymerization, drying, pulverization and sieving, and combines partially protonated ZSM-5 molecular sieves, water, water-soluble polyols and surface crosslinking agents in the same surface treatment solution. S3, the surface treatment liquid is sprayed onto the surface of the highly absorbent resin matrix particles, and the sprayed highly absorbent resin matrix particles are heat-treated to cause cross-linking of the surface layer of the highly absorbent resin matrix particles, and to retain part of the protonated ZSM-5 molecular sieve on the surface layer of the highly absorbent resin matrix particles, thereby obtaining zeolite molecular sieve hybrid highly absorbent resin.
2. The method for preparing the zeolite molecular sieve hybrid superabsorbent resin according to claim 1, characterized in that, In step S1, the sodium ion exchange degree E is 40% to 60%.
3. The method for preparing the zeolite molecular sieve hybrid high-absorbency resin according to claim 2, characterized in that, In step S1, the sodium ion exchange degree E is 45% to 55%.
4. The method for preparing the zeolite molecular sieve hybrid high-absorbency resin according to claim 1, characterized in that, The Na-type ZSM-5 molecular sieve has an MFI topology, a Si / Al molar ratio of 25–60, and a median particle size D50 of 0.5–2.2 μm.
5. The method for preparing the zeolite molecular sieve hybrid high-absorbency resin according to claim 1, characterized in that, In step S1, the ammonium salt is selected from one of ammonium nitrate, ammonium chloride, ammonium sulfate and ammonium acetate; the concentration of the ammonium salt aqueous solution is 0.20-0.80 mol / L, the solid-liquid mass ratio of Na-type ZSM-5 molecular sieve to ammonium salt aqueous solution is 1:(8-15), the ammonium ion exchange temperature is 55-75℃, and the ammonium ion exchange time is 45-120 min.
6. The method for preparing the zeolite molecular sieve hybrid superabsorbent resin according to claim 1, characterized in that, In step S1: ammonium ion exchange is performed only once. After the ammonium ion exchange is completed, solid-liquid separation is performed. The liquid is washed with deionized water until the conductivity of the last washing liquid is not higher than 100 μS / cm. Then it is dried at 100-120℃ for 2-6 hours and heated to 480-550℃ at a heating rate of 2-5℃ / min for calcination for 2-4 hours. R0 and R1 are the Na / Al molar ratios measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) after the corresponding molecular sieve samples have been completely digested.
7. The method for preparing the zeolite molecular sieve hybrid high-absorbency resin according to claim 1, characterized in that, In step S2: the highly absorbent resin matrix particles are particles containing a partially neutralized polyacrylate crosslinked network, with a particle size of 150–850 μm and a neutralization degree of 65–80 mol%; Based on 100 parts by weight of highly absorbent resin matrix particles, the surface treatment liquid includes 0.8 to 2.2 parts by weight of partially protonated ZSM-5 molecular sieve, 0.05 to 0.25 parts by weight of surface crosslinking agent, 1.5 to 3.5 parts by weight of water, and 0.3 to 1.2 parts by weight of water-soluble polyol.
8. The method for preparing the zeolite molecular sieve hybrid high-absorbency resin according to claim 7, characterized in that, The surface crosslinking agent is ethylene glycol diglycidyl ether, and the water-soluble polyol is 1,2-propanediol. Water and 1,2-propanediol are mixed, and a portion of protonated ZSM-5 molecular sieve is added at 1500-3000 rpm and dispersed for 3-10 min. Then, ethylene glycol diglycidyl ether is added, and the mixture is mixed at 300-800 rpm for 1-3 min to obtain a surface treatment solution. The surface treatment solution is kept circulating or stirred, and spraying is completed within 30 min after preparation.
9. The method for preparing the zeolite molecular sieve hybrid superabsorbent resin according to claim 1, characterized in that, In step S3: the surface treatment liquid is continuously sprayed onto the surface of the highly absorbent resin matrix particles in one go, and after the spraying is completed and mixing is continued, a heat treatment is directly performed. The feed temperature of the highly absorbent resin matrix particles is 40-70℃. Under the mixing conditions of 500-1200rpm, the spraying is completed within 1-5 minutes, and the mixing continues for 2-8 minutes after spraying. The heat treatment temperature is 150-180℃ and the heat treatment time is 20-45 min. After heat treatment, the material is cooled to no higher than 50℃ and particles with a diameter of less than 150μm and greater than 850μm are screened out.
10. The method for preparing the zeolite molecular sieve hybrid high-absorbency resin according to claim 3, characterized in that: In step S2, based on 100 parts by weight of highly absorbent resin matrix particles, the surface treatment liquid includes 1.5 parts by weight of partially protonated ZSM-5 molecular sieve, 2.0 parts by weight of water, 1.0 parts by weight of 1,2-propanediol, and 0.20 parts by weight of ethylene glycol diglycidyl ether. In step S3, after the surface treatment liquid is sprayed onto the surface of the highly absorbent resin matrix particles, it is heat-treated at 165°C for 30 minutes.
Citation Information
Patent Citations
Production technique for pet urinal pad with deammoniation function and high saline water absorption capacity
CN104429992A
Water-absorbent polymers with compounds having a hollow space
WO2001013965A1