A polytetrafluoroethylene composite monoweb material and method of making
By introducing hydrophilic sodium carboxylate and triazole groups onto the surface of a polytetrafluoroethylene (PTFE) microporous membrane and activating graft polymerization with ultraviolet irradiation, a unidirectional water vapor migration channel is formed, which solves the problem of water vapor accumulation in PTFE microporous membranes and improves the membrane's high-temperature resistance and moisture resistance.
Patent Information
- Application Number
- CN202611328535.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-24
AI Technical Summary
Polytetrafluoroethylene microporous membrane materials cannot achieve unidirectional permeation of water vapor, which leads to water vapor accumulation at high temperatures, causing the membrane to bulge and crack, and thus failing to meet the requirements for moisture protection.
By introducing hydrophilic sodium carboxylate and triazole groups onto one side of a polytetrafluoroethylene microporous membrane, free radicals are generated through ultraviolet irradiation activation, which initiates the graft polymerization of 1-allyl-triazole-4-carboxylic acid monomers, forming a unidirectional pressure difference channel, thereby enabling water vapor to migrate from the high humidity side to the low humidity side.
This technology enables unidirectional water vapor permeation of polytetrafluoroethylene microporous membranes, improving the membrane's high-temperature resistance and moisture-proof effect, and preventing membrane bulging and cracking.
Smart Images

Figure SMS_2 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of polytetrafluoroethylene (PTFE) technology, specifically to a PTFE composite unidirectional membrane material and its preparation method. Background Technology
[0002] Aluminosilicate fiber is a commonly used inorganic thermal insulation material in high-temperature industrial applications. It possesses advantages such as high temperature resistance, good thermal stability, low thermal conductivity, and excellent fire resistance, and is widely used in industrial kilns, thermal pipelines, and high-temperature equipment cavities. However, the high-porosity, mesh-like porous structure of aluminosilicate fiber provides channels for water vapor diffusion and liquid water wetting. When water vapor enters the pores of the aluminosilicate fiber, the thermal conductivity of water is much higher than that of air, directly causing an increase in the thermal conductivity of the insulation layer and a significant decrease in its thermal insulation performance. Furthermore, when equipment starts and stops, causing temperature differences, the moisture trapped in the insulation layer repeatedly vaporizes and condenses, increasing the interlayer vapor pressure. This can easily lead to bulging and cracking of the insulation structure and accelerate corrosion of the outer wall of the base equipment, shortening the overall service life of the equipment.
[0003] Currently, the main methods for moisture protection of aluminum silicate insulation materials include metal outer shells, hydrophobic modification treatment, and ordinary waterproof membrane wrapping. Among these, waterproof membrane wrapping, such as polytetrafluoroethylene (PTFE), polyethylene, and polyurethane membranes, can effectively block the intrusion of external moisture. However, PTFE and other waterproof membranes can also completely seal the moisture escape channels. Water vapor generated at high internal temperatures cannot be released to the outside, and high-pressure steam accumulates between layers, causing the membrane to bulge, crack, and delaminate the composite structure. This fails to meet the requirement of directional discharge of internal moisture and reverse blocking of external moisture. Summary of the Invention
[0004] This invention solves the problem that polytetrafluoroethylene microporous membrane materials do not have the effect of unidirectional water vapor permeation.
[0005] The technical solution of this invention is: a method for preparing a polytetrafluoroethylene composite unidirectional membrane material. (1) Add water, cuprous iodide catalyst, sodium thiosulfate reducing agent, N,N'-dimethylethylenediamine ligand, cesium carbonate accelerator, propargyl ester, sodium azide, and bromopropylene to dimethyl sulfoxide. Stir the reaction at 25-35℃ for 30-60 min, add water, pour the solution into a separatory funnel, add dichloromethane, shake, and allow to stand for separation. Concentrate the organic layer by rotary evaporation, add it to an alcohol solvent, add a 2.5-3 mol / L sodium hydroxide aqueous solution, heat to 75-85℃, stir the reaction for 2-3 h, reflux, cool, add hydrochloric acid dropwise, adjust the pH to 2-3, precipitate the precipitate, filter, add the precipitate to water, recrystallize and purify to obtain 1-allyl-triazole-4-carboxylic acid monomer. The reaction formula is: .
[0006] (2) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and activate it under a mercury lamp for 40-60 minutes.
[0007] (3) The activated microporous membrane is placed in an aqueous solution of 1-allyl-triazole-4-carboxylic acid monomer with a concentration of 0.3-1.2 mol / L, with the side of the release film not attached facing up. It is placed in a quartz glass tube, nitrogen gas is introduced, and the reaction is carried out under a mercury lamp for 60-90 min. The microporous membrane is then removed, the release film is peeled off, and it is added to an aqueous solution of sodium hydroxide. After soaking, it is filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0008] Furthermore, in (1), the molar ratio of cuprous iodide, sodium urea, N,N'-dimethylethylenediamine, cesium carbonate, propynate, sodium azide, and bromopropene is (0.09-0.11):(0.18-0.22):(0.18-0.22):(1-1.1):1:(1.4-1.5):(1.1-1.3).
[0009] Furthermore, in (1), the propynyl ester is methyl propynyl or ethyl propynyl.
[0010] Furthermore, in (1), the alcohol solvent is methanol or ethanol.
[0011] Furthermore, the mercury lamp has a power of 300-600W and a wavelength between 350-450nm.
[0012] The beneficial technical effects of this invention are as follows: One side of the polytetrafluoroethylene (PTFE) microporous membrane is activated by ultraviolet irradiation to generate free radicals. Without an external photoinitiator, this initiates the graft polymerization of 1-allyl-triazole-4-carboxylic acid monomers. Hydrophilic sodium carboxylate and triazole groups are introduced onto one side of the PTFE microporous membrane. Triazole contains multiple nitrogen atoms and can act as hydrogen bond acceptors, further enhancing the hydrophilicity of the microporous membrane surface. The PTFE microporous membrane has a microporous structure, with one side being strongly hydrophobic and the other becoming strongly hydrophilic, forming a unidirectional pressure difference channel. Relying on the difference in hydrophilicity on both sides of the membrane, water vapor can only migrate from the high-humidity side to the low-humidity side. This allows high-temperature water vapor to diffuse from the hydrophilic side along the micropores to the hydrophobic side. Meanwhile, liquid water and moisture outside the hydrophobic side are blocked by surface tension and cannot penetrate the micropores in the reverse direction, thus achieving reverse blocking of water vapor diffusion.
[0013] The polymer grafted onto the surface of the polytetrafluoroethylene microporous membrane of the present invention contains a triazole ring with high thermal stability, which can improve the high temperature resistance of the grafted polymer. After heat treatment, the polymer grafted onto the microporous membrane is not easily thermally decomposed, thereby maintaining a low water contact angle, making it suitable for high-temperature scenarios such as industrial kilns, pipe cavities, and steam equipment shells. Detailed Implementation
[0014] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.
[0015] The wavelength of light emitted by the following mercury lamps is between 350-450 nm.
[0016] Example 1 (1) Add 60 mL of water, 4 mmol of cuprous iodide, 8 mmol of sodium benzoate, 8 mmol of N,N'-dimethylethylenediamine, 40 mmol of cesium carbonate, 40 mmol of ethyl propynate, 60 mmol of sodium azide, and 48 mmol of bromopropene to 140 mL of dimethyl sulfoxide. Stir at 30 °C for 30 min, add water, pour the solution into a separatory funnel, add dichloromethane, shake and let stand to separate the layers, concentrate the organic layer by rotary evaporation, add to 150 mL of ethanol, add 150 mL of 3 mol / L sodium hydroxide aqueous solution, heat to 75 °C, stir and react for 3 h, reflux, cool and add 10% hydrochloric acid dropwise to adjust the pH of the solution to 3, precipitate, filter, add the precipitate to water, recrystallize and purify to obtain 1-allyl-triazole-4-carboxylic acid monomer.
[0017] (2) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 300W mercury lamp for 40 minutes to activate it.
[0018] (3) The activated microporous membrane was placed in an aqueous solution of 1-allyl-triazole-4-carboxylic acid monomer with a concentration of 0.3 mol / L, with the side of the release membrane not attached facing up. It was placed in a quartz glass tube, nitrogen gas was introduced, and the reaction was carried out under a 300W mercury lamp for 80 min. The microporous membrane was then removed, the release membrane was peeled off, and it was added to a 2% sodium hydroxide aqueous solution. After soaking, it was filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0019] Example 2 (1) Add 60 mL of water, 4 mmol of cuprous iodide, 8.8 mmol of sodium benzoate, 7.2 mmol of N,N'-dimethylethylenediamine, 40 mmol of cesium carbonate, 40 mmol of methyl propynate, 60 mmol of sodium azide and 44 mmol of bromopropene to 140 mL of dimethyl sulfoxide. Stir at 30 °C for 40 min, add water, pour the solution into a separatory funnel, add dichloromethane, shake and let stand to separate the layers, concentrate the organic layer by rotary evaporation, add to 150 mL of methanol, add 150 mL of 3 mol / L sodium hydroxide aqueous solution, heat to 75 °C, stir and react for 3 h, reflux, cool and add 15% hydrochloric acid dropwise to adjust the pH of the solution to 2, precipitate, filter, add the precipitate to water, recrystallize and purify to obtain 1-allyl-triazole-4-carboxylic acid monomer.
[0020] (2) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 300W mercury lamp for 60 minutes to activate it.
[0021] (3) The activated microporous membrane was placed in an aqueous solution of 1-allyl-triazole-4-carboxylic acid monomer with a concentration of 0.6 mol / L, with the side of the release film not attached facing up. It was placed in a quartz glass tube, nitrogen gas was introduced, and the reaction was carried out under a 300W mercury lamp for 90 min. The microporous membrane was then removed, the release film was peeled off, and it was added to a 3% sodium hydroxide aqueous solution. After soaking, it was filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0022] Example 3 (1) Add 60 mL of water, 4.4 mmol of cuprous iodide, 7.2 mmol of sodium benzoate, 8 mmol of N,N'-dimethylethylenediamine, 40 mmol of cesium carbonate, 40 mmol of ethyl propynate, 56 mmol of sodium azide, and 52 mmol of bromopropene to 140 mL of dimethyl sulfoxide. Stir at 35 °C for 30 min, add water, pour the solution into a separatory funnel, add dichloromethane, shake and let stand to separate the layers, concentrate the organic layer by rotary evaporation, add to 150 mL of ethanol, add 150 mL of 3 mol / L sodium hydroxide aqueous solution, heat to 85 °C, stir and react for 2 h, reflux, cool and add 10% hydrochloric acid dropwise to adjust the pH of the solution to 3, precipitate, filter, add the precipitate to water, recrystallize and purify to obtain 1-allyl-triazole-4-carboxylic acid monomer.
[0023] (2) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 600W mercury lamp for 60 minutes to activate it.
[0024] (3) The activated microporous membrane was placed in an aqueous solution of 1-allyl-triazole-4-carboxylic acid monomer with a concentration of 0.9 mol / L, with the side of the release film not attached facing up. It was placed in a quartz glass tube, nitrogen gas was introduced, and the reaction was carried out under a 600W mercury lamp for 60 min. The microporous membrane was taken out, the release film was peeled off, and it was added to a 3% sodium hydroxide aqueous solution. After soaking, it was filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0025] Example 4 (1) 60 mL of water, 3.6 mmol of cuprous iodide, 8.4 mmol of sodium benzoate, 8.4 mmol of N,N'-dimethylethylenediamine, 44 mmol of cesium carbonate, 40 mmol of ethyl propynate, 60 mmol of sodium azide, and 48 mmol of bromopropylene were added to 140 mL of dimethyl sulfoxide. The mixture was stirred at 25 °C for 60 min. Water was added, and the solution was poured into a separatory funnel. Dichloromethane was added, and the mixture was shaken and allowed to stand for separation. The organic layer was concentrated by rotary evaporation and added to 150 mL of ethanol. 150 mL of 2.5 mol / L sodium hydroxide aqueous solution was added, and the mixture was heated to 80 °C and stirred for 3 h. The mixture was refluxed and cooled. 10% hydrochloric acid was added dropwise to adjust the pH of the solution to 2. A precipitate was precipitated, filtered, and the precipitate was added to water. The mixture was recrystallized and purified to obtain 1-allyl-triazole-4-carboxylic acid monomer.
[0026] (2) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 600W mercury lamp for 40 minutes to activate it.
[0027] (3) The activated microporous membrane was placed in an aqueous solution of 1-allyl-triazole-4-carboxylic acid monomer with a concentration of 1.2 mol / L, with the side of the release film not attached facing up. It was placed in a quartz glass tube, nitrogen gas was introduced, and the reaction was carried out under a 600W mercury lamp for 70 min. The microporous membrane was taken out, the release film was peeled off, and it was added to a 4% sodium hydroxide aqueous solution. After soaking, it was filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0028] Comparative Example 1 differs from Example 1 in that acrylic acid is used instead of the 1-allyl-triazole-4-carboxylic acid monomer.
[0029] (1) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 300W mercury lamp for 40 minutes to activate it.
[0030] (2) The activated microporous membrane was placed in an aqueous solution of 0.3 mol / L acrylic acid with the side of the release film facing up. It was placed in a quartz glass tube, nitrogen gas was introduced, and the reaction was carried out under a 300W mercury lamp for 80 min. The microporous membrane was then removed, the release film was peeled off, and it was added to an aqueous solution of 2% sodium hydroxide by mass. After soaking, it was filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0031] Comparative Example 2 differs from Example 1 in that 1-vinyl-1H-1,2,4-triazole (CAS No. 2764-83-2) is used instead of the 1-allyl-triazole-4-carboxylic acid monomer.
[0032] (1) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 300W mercury lamp for 40 minutes to activate it.
[0033] (2) The activated microporous membrane was placed in an aqueous solution of 1-vinyl-1H-1,2,4-triazole with a concentration of 0.3 mol / L, with the side of the release film not attached facing up. It was placed in a quartz glass tube, nitrogen gas was introduced, and the reaction was carried out under a 300W mercury lamp for 80 min. The microporous membrane was then removed, the release film was peeled off, and it was added to an aqueous solution of sodium hydroxide with a mass fraction of 2%. After soaking, it was filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material.
[0034] Comparative Example 3 differs from Example 1 in that acrylic acid and 1-vinyl-1H-1,2,4-triazole are used instead of the 1-allyl-triazole-4-carboxylic acid monomer.
[0035] (1) Attach the release film to one side of the polytetrafluoroethylene microporous membrane, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing up, introduce nitrogen gas, and irradiate it under a 300W mercury lamp for 40 minutes to activate it.
[0036] (2) The activated microporous membrane was placed in an aqueous solution containing acrylic acid and 1-vinyl-1H-1,2,4-triazole (the concentration of acrylic acid in the solution was 0.15 mol / L and the concentration of 1-vinyl-1H-1,2,4-triazole was 0.15 mol / L). The side of the release film that was not attached was facing up. The membrane was placed in a quartz glass tube, nitrogen gas was introduced, and the membrane was irradiated under a 300W mercury lamp for 80 min. The microporous membrane was then removed, the release film was peeled off, and the membrane was added to a 2% sodium hydroxide aqueous solution. After soaking, the membrane was filtered, washed with deionized water, and dried to obtain a polytetrafluoroethylene composite unidirectional membrane material.
[0037] The water contact angle Q0 of the membrane material shall be tested in accordance with GB / T 30693-2014.
[0038] The membrane material was placed in an oven and heated to 250℃ for 1 hour, then left at room temperature for 3 hours. The water contact angle Q1 was then measured. The water contact angle retention rate W before and after heat treatment was calculated. W = Q0 / Q1 = 100%.
[0039]
[0040] In each embodiment, one side of the polytetrafluoroethylene (PTFE) microporous membrane is activated by ultraviolet irradiation to generate free radicals, which initiate the graft polymerization of 1-allyl-triazole-4-carboxylic acid monomer. Hydrophilic sodium carboxylate and triazole groups are introduced onto one side of the PTFE microporous membrane. Triazole contains multiple nitrogen atoms, which can act as hydrogen bond acceptors, further enhancing the hydrophilicity of the microporous membrane surface and improving water vapor permeability. Simultaneously, the grafted polymer contains a highly thermally stable triazole ring, which improves the high-temperature resistance of the grafted polymer. After heat treatment, the grafted polymer on the microporous membrane is not easily thermally decomposed, thus maintaining a low water contact angle, making it suitable for high-temperature applications such as industrial kilns, pipe cavities, and steam equipment shells.
[0041] Comparative Example 1 uses an acrylic-grafted polytetrafluoroethylene microporous membrane. The polymer grafted onto the surface of the microporous membrane does not contain triazole groups, resulting in a higher water contact angle than in Example 1. Furthermore, the water contact angle increases after heat treatment, indicating poor high-temperature resistance.
[0042] Comparative Example 2 uses a polytetrafluoroethylene microporous membrane grafted with 1-vinyl-1H-1,2,4-triazole. The polymer grafted onto the surface of the microporous membrane does not contain sodium carboxylate groups, and the water contact angle is significantly larger than that in Example 1, indicating poor hydrophilicity.
[0043] Comparative Example 3 utilizes acrylic acid and 1-vinyl-1H-1,2,4-triazole to co-graft polymer onto a polytetrafluoroethylene microporous membrane. The water contact angle is greater than that in Example 1. After heat treatment, the water contact angle also increases significantly, but the high-temperature resistance is poor.
Claims
1. A method for preparing a polytetrafluoroethylene composite unidirectional membrane material, characterized in that, The preparation method is as follows: S1. Attach one side of the polytetrafluoroethylene microporous membrane to the release film, place it in a quartz glass tube with the side of the polytetrafluoroethylene microporous membrane not attached to the release film facing upwards, introduce nitrogen gas, and activate it under a mercury lamp. S2. The activated microporous membrane is placed in an aqueous solution containing 1-allyl-triazole-4-carboxylic acid monomer, with the side without the release film facing up. It is placed in a quartz glass tube, nitrogen gas is introduced, and the reaction is carried out under a mercury lamp. The microporous membrane is then removed, the release film is peeled off, and it is added to an aqueous solution of sodium hydroxide. After soaking, it is filtered, washed with deionized water, and dried to obtain polytetrafluoroethylene composite unidirectional membrane material. The structural formula of the 1-allyl-triazole-4-carboxylic acid monomer is as follows: .
2. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 1, characterized in that, The mercury lamp has a power of 300-600W and a wavelength between 350-450nm.
3. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 1, characterized in that, The irradiation activation time in S1 is 40-60 min.
4. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 1, characterized in that, The irradiation reaction time in S2 is 60-90 min.
5. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 1, characterized in that, The concentration of the aqueous solution of 1-allyl-triazole-4-carboxylic acid monomer in S2 is 0.3-1.2 mol / L.
6. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 1, characterized in that, The method for preparing the 1-allyl-triazole-4-carboxylic acid monomer is as follows: water, cuprous iodide, sodium benzoate, N,N'-dimethylethylenediamine, cesium carbonate, propargyl ester, sodium azide, and bromopropylene are added to dimethyl sulfoxide. The mixture is stirred at 25-35°C for 30-60 min. Water is then added, and the solution is poured into a separatory funnel. Dichloromethane is added, and the mixture is shaken and allowed to stand for separation. The organic layer is concentrated by rotary evaporation and added to an alcohol solvent. A 2.5-3 mol / L sodium hydroxide aqueous solution is added, and the mixture is heated to 75-85°C and stirred for 2-3 h. The mixture is then refluxed, cooled, and hydrochloric acid is added dropwise to adjust the pH to 2-3. A precipitate is formed, filtered, and the precipitate is added to water for recrystallization and purification to obtain the 1-allyl-triazole-4-carboxylic acid monomer.
7. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 6, characterized in that, The alcohol solvent is methanol or ethanol.
8. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 6, characterized in that, The molar ratio of cuprous iodide, sodium urea, N,N'-dimethylethylenediamine, cesium carbonate, propargyl ester, sodium azide, and bromopropylene is (0.09-0.11):(0.18-0.22):(0.18-0.22):(1-1.1):1:(1.4-1.5):(1.1-1.3).
9. The method for preparing the polytetrafluoroethylene composite unidirectional membrane material according to claim 8, characterized in that, The propynyl ester is methyl propynate or ethyl propynate.
10. A polytetrafluoroethylene composite unidirectional membrane material obtained by the preparation method according to any one of claims 1-9.