A natural nanoclay mineral in-situ foamed polyurea foam and a method of making the same
By wetting and mixing natural nano-clay minerals, the location and process of carbon dioxide gas generation were adjusted, solving the problem of poor matching between the foaming process and the matrix gel in the preparation of polyurea foam. This achieved uniformity and stability of the cell structure and improved the material properties.
Patent Information
- Application Number
- CN202611386385.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-24
AI Technical Summary
During the preparation of polyurea foam, the foaming process is difficult to match with the matrix gelation and curing process, resulting in problems such as large differences in cell size, uneven distribution, local large pores or cell collapse. In addition, traditional physical foaming agents may remain and affect the material properties.
Wetting treatment is performed using natural nano-clay minerals such as halloysite nanotubes, which adsorb water molecules onto their surface and within their pores, forming a mixture of hydrated nano-clay minerals and amino compounds. This mixture regulates the location and process of carbon dioxide gas generation through heterogeneous nucleation sites, forming bubbles and reducing the use of physical foaming agents.
It achieves uniformity and stability of the cell structure, reduces cell merging and collapse, improves the consistency of the material's mechanical properties, and avoids the residue problem of traditional foaming agents.
Smart Images

Figure CN123152158A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer foam material preparation technology, specifically to an in-situ foamed polyurea made from natural nano-clay minerals and its preparation method. Background Technology
[0002] Polyurea materials are typically formed by the addition polymerization of isocyanate components and terminal amino compound components. Their molecular structure usually includes hard and soft segment phases. The hard segment phase provides high strength and rigidity, while the soft segment phase imparts good toughness and elasticity. Therefore, polyurea materials possess good mechanical properties, impact resistance, and environmental adaptability. By forming a certain number of cells within the polyurea matrix, the material density can be further reduced, and it can be endowed with cushioning and energy absorption properties, thus forming polyurea foam materials.
[0003] Currently, polyurea foam is typically prepared using either chemical or physical foaming methods. In chemical foaming, isocyanates react with water to generate carbon dioxide gas, which then forms cells within the polymer matrix. Physical foaming usually involves introducing foaming materials such as low-boiling-point hydrocarbons, fluorocarbons, or expandable microspheres, and forming cells through heating, exothermic reactions, or volume expansion. Furthermore, existing technologies also utilize terminal amino compounds to form adducts with carbon dioxide, releasing carbon dioxide during the polymerization process to achieve in-situ foaming.
[0004] However, the reaction rate between isocyanate and amino groups in polyurea systems is relatively fast. After the isocyanate component and amino compound component are mixed, the viscosity of the system increases rapidly within a short period of time and gradually gels. Therefore, when water is used as a chemical foaming source, if water is added directly to the reaction system in a free state, it is difficult to maintain a consistent spatial distribution of water in the system and the degree of contact with isocyanate. Local areas are prone to water enrichment, leading to the concentrated generation of carbon dioxide in these local areas. At the same time, the rapid gelation of the polyurea matrix restricts the continuous growth of bubbles, making it difficult to stably match the foaming process with the matrix curing process on a time scale.
[0005] In the aforementioned situations, some areas may generate a large amount of gas before the matrix forms sufficient support, leading to rapid bubble growth, merging, and even pore wall rupture. Other areas may fail to form sufficient cells due to insufficient or late-arriving foaming gas. This can easily result in significant differences in cell size, uneven cell distribution, the presence of large pores in certain areas, or cell collapse within the polyurea foam, thereby affecting the structural uniformity and consistency of the foam material's mechanical properties.
[0006] While using physical blowing agents such as low-boiling-point organic compounds can mitigate the problem of uncontrollable reaction rates between isocyanates and free water to some extent, these agents may not completely escape during foam curing. Residual small molecules can plasticize the polyurea matrix and may gradually volatilize over time, altering the internal pressure and structure of the cells. Furthermore, using expandable microspheres to form cells presents challenges related to the interfacial bonding performance between the microsphere shell and the polyurea matrix, as well as raw material costs.
[0007] In addition, there are existing schemes that use carbon dioxide adducts as foaming sources, which require the corresponding terminal amino compounds to form adducts with carbon dioxide in advance, which puts forward corresponding requirements on the raw material processing method and the composition of foaming components, and the preparation system is relatively complex.
[0008] Therefore, under the rapid polymerization and curing reaction characteristics of polyurea, how to adjust the location and process of foaming gas generation so that the foaming process can be adapted to the gelation and curing process of the polyurea matrix, and reduce the problems of uneven cell distribution, insufficient structural stability and foaming agent residue caused by traditional physical foaming agents or direct addition of free water, remains a technical problem to be solved in the preparation of polyurea foam. Summary of the Invention
[0009] In view of this, the purpose of this invention is to provide an in-situ foamed polyurea foam made from natural nano-clay minerals and its preparation method, so as to adjust the generation location and process of foaming gas during the polyurea foaming process, improve the matching between the foaming process and the polyurea matrix gelation and curing process, reduce phenomena such as cell merging, collapse, and uneven distribution, and reduce the use of traditional physical foaming agents. To achieve the above objectives, this invention provides the following technical solution: In one possible implementation, a method for preparing in-situ foamed polyurea from natural nano-clay minerals is provided, comprising: S1. Wetting treatment is applied to the natural nano clay mineral to allow water molecules to be adsorbed onto the surface and / or inside the pores of the natural nano clay mineral, thereby obtaining a natural nano clay mineral containing adsorbed water. S2. The natural nano-clay mineral containing adsorbed water is added to amino compound B component for dispersion to obtain natural nano-clay mineral-B component premix. S3. Mix isocyanate component A with the natural nano-clay mineral-component B premix, so that the isocyanate groups in isocyanate component A react with the amino groups in amino compound component B to form a polyurea matrix, and the adsorbed water reacts with the isocyanate groups to generate carbon dioxide gas. The natural nano-clay minerals provide spatial confinement for the adsorbed water to regulate the release process of the adsorbed water and provide heterogeneous nucleation sites for the carbon dioxide gas, enabling the carbon dioxide gas to nucleate in situ and form pores during the formation of the polyurea matrix, thus obtaining a foamed material. S4. The foaming material is placed in a mold for molding and curing to obtain natural nano-clay mineral in-situ foamed polyurea foam.
[0010] In one possible implementation, the natural nanoclay mineral includes at least one of halloysite nanotubes, sepiolite, and attapulgite.
[0011] In one possible implementation, the natural nano-clay mineral is halloysite nanotubes; S1 includes: laying the halloysite nanotubes flat and placing them in a constant temperature and humidity environment for water vapor wetting treatment. The temperature of the water vapor wetting treatment is 40-60°C, the relative humidity is 75%-80%, and the treatment time is 4-8 hours, so that the water content of the treated halloysite nanotubes is 10%-30% of the mass of the halloysite nanotubes.
[0012] In one possible implementation, the amino compound B component is preheated to 40-80°C before or during S2. Halloysite nanotubes that have been moistened with water vapor are added to the preheated amino compound B component, so that the water adsorbed inside the pores of the halloysite nanotubes is released into the amino compound B component during the premixing process, and the amount and rate of water release are adjusted by the preheating temperature of the amino compound B component.
[0013] In one possible implementation, the amount of halloysite nanotubes added is 1% to 10% of the sum of the mass of the isocyanate A component and the amino compound B component; In step S2, the halloysite nanotubes and the amino compound B component are first mechanically stirred at 500 rpm for 20 min, and then ultrasonically dispersed for 5 to 10 min to obtain the natural nano-clay mineral-B component premix.
[0014] In one possible implementation, the isocyanate A component includes at least one of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, and isophorone diisocyanate. The amino compound component B includes at least one of poly-1,4-butanediol bis(4-aminobenzoate), polyoxypropylene diamine, and polytetrahydrofuran diamine. The equivalent ratio of the isocyanate groups in the isocyanate A component to the amino groups in the amino compound B component is (1-1.1):1.
[0015] In one possible implementation, in step S3, after adding the isocyanate A component to the natural nano-clay mineral-B component premix, the mixture is mechanically stirred at a stirring speed of 300 rpm for 1 min, so that the isocyanate A component and the amino compound B component undergo a polymerization reaction, while the adsorbed water and the isocyanate A component undergo an in-situ foaming reaction.
[0016] In one possible implementation, S4 includes: The foamed material is injected into a mold and placed in a vacuum environment for vacuum degassing to remove air bubbles introduced during the mixing process. The vacuum degree of the vacuum degassing process is -0.08 to -0.1 MPa, and the processing time is 1 to 5 minutes. After completing the vacuum degassing treatment, restore normal pressure and cure at room temperature for 24 hours.
[0017] In one possible implementation, a natural nano-clay mineral in-situ foamed polyurea foam is provided, comprising a polyurea matrix, natural nano-clay minerals dispersed in the polyurea matrix, and a cell structure formed in the polyurea matrix. The natural nano-clay mineral is loaded with adsorbed water before forming the polyurea matrix, and the adsorbed water is constrained by the surface and / or pore structure of the natural nano-clay mineral. The pore structure is formed in situ by carbon dioxide gas generated from the reaction of adsorbed water and isocyanate during the formation of the polyurea matrix, and the natural nano-clay minerals constitute heterogeneous nucleation sites when carbon dioxide gas forms pores.
[0018] In one possible implementation, the natural nano-clay mineral is halloysite nanotubes, the amount of halloysite nanotubes added is 1% to 10% of the sum of the mass of the isocyanate component and the amino compound component forming the polyurea matrix, and the water content of the halloysite nanotubes before participating in the in-situ foaming reaction is 10% to 30% of the mass of the halloysite nanotubes.
[0019] Based on the above technical solution, the present invention relates to an in-situ foamed polyurea foam made from natural nano-clay minerals and its preparation method. This involves wetting the natural nano-clay minerals to adsorb water molecules onto the surface and / or pores of the natural nano-clay minerals. The natural nano-clay minerals containing adsorbed water are then dispersed in amino compound component B and mixed with isocyanate component A. This allows the isocyanate groups to react with the amino groups to form a polyurea matrix, while simultaneously allowing the adsorbed water to react with the isocyanate groups to generate carbon dioxide gas. The natural nano-clay minerals provide spatial constraints on the adsorbed water to regulate its release process, and they also provide heterogeneous nucleation sites for carbon dioxide gas. This allows carbon dioxide gas to nucleate in situ and form pores during the polyurea matrix formation process. This solves the problems of difficulty in adjusting the foaming gas generation process and location under rapid polyurea polymerization and curing conditions, and the difficulty in matching the foaming process with the polyurea matrix gel curing process, which easily leads to pore merging, collapse, and uneven distribution. Furthermore, it reduces the use of traditional physical foaming agents. Attached Figure Description
[0020] Figure 1 A scanning electron microscope image of the polyurea foam prepared using free water in Comparative Example 1; Figure 2 Scanning electron microscope image of polyurea material prepared using dried halloysite nanotubes, as shown in Comparative Example 2; Figure 3 This is a scanning electron microscope image of the polyurea foam prepared using hydrated halloysite nanotubes in Example 1; Figure 4 Fourier transform infrared spectra of halloysite in its original form and halloysite nanotubes after being moistened with water vapor. Figure 5 X-ray diffraction pattern of halloysite nanotubes after water vapor wetting treatment; Figure 6 Thermogravimetric curve of halloysite nanotubes after water vapor wetting treatment; Figure 7 This is a microscopic morphology diagram of the polyurea foam of the present invention; Figure 8 The figure shows the quasi-static compression performance test results of the hydrous halloysite foam obtained in Example 1 and the free water foam obtained in Comparative Example 1 under a strain rate of 0.01 / s. Detailed Implementation
[0021] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can more clearly understand the technical concept, preparation process and mechanism of action of the present invention.
[0022] The core of this invention lies in utilizing the adsorption and spatial confinement of water molecules by natural nano-clay minerals. Water is pre-loaded into the natural nano-clay minerals in an adsorbed state. The hydrated natural nano-clay minerals are then dispersed in amino compound component B and reacted with isocyanate component A. During the reaction, on one hand, isocyanate groups react with amino groups to form a polyurea matrix; on the other hand, the adsorbed water loaded on the natural nano-clay minerals reacts with the isocyanate groups to produce carbon dioxide, and pores are formed in situ within the polyurea matrix using the heterogeneous nucleation sites provided by the natural nano-clay minerals. By adjusting the wetting state of the natural nano-clay minerals, the amount added, the temperature of component B, and subsequent molding conditions, the foaming process is adapted to the gelation and curing process of the polyurea matrix.
[0023] The following describes a preferred embodiment of natural nano-clay minerals using halloysite nanotubes (HNTs), detailing its steam wetting pretreatment, premixing and dispersion with component B, in-situ foaming of components A and B, vacuum degassing, and curing processes. Figures 1 to 8 Examples and comparative examples illustrate the microstructure of the obtained materials and the wetting characterization results of HNTs.
[0024] I. Overall Preparation Method and Principle This embodiment provides a method for preparing in-situ foamed polyurea using natural nano-clay minerals. Isocyanate is used as component A, an amino compound as component B, and natural nano-clay minerals containing adsorbed water as the in-situ foaming functional component. Preferably, the natural nano-clay minerals are HNTs. HNTs have a hollow nanotube structure, with hydrophilic hydroxyl groups on the inner and outer surface defects and at the tube ends. They also possess water-retaining spaces formed by the hollow cavity, the tube wall surface, and the interparticle gaps, enabling them to adsorb water through hydrogen bonding and capillary action.
[0025] In the specific preparation process, the natural nano-clay mineral is first wetted, causing water molecules to adsorb onto the surface and pores of the natural nano-clay mineral, resulting in natural nano-clay mineral containing adsorbed water. Unlike directly adding liquid free water to the reaction system, this embodiment pre-loads water molecules with the natural nano-clay mineral, constraining the water molecules through the surface and pore structure of the natural nano-clay mineral, thereby altering the state and release process of water in the subsequent reaction system.
[0026] Subsequently, the natural nano-clay minerals containing adsorbed water were added to component B of the amino compound for mixing and dispersion, so that the natural nano-clay minerals were uniformly distributed in component B, resulting in a natural nano-clay mineral-component B premix. By pre-dispersing the hydrous natural nano-clay minerals in component B, the water loaded on the natural nano-clay minerals can be dispersed in different regions of the reaction system along with the natural nano-clay minerals, reducing the local water enrichment that occurs when free water is directly added.
[0027] Subsequently, isocyanate component A was added to the premix of natural nano-clay minerals and component B and mixed. During the mixing process, polyurea matrix formation and in-situ foaming reactions occurred simultaneously within the system.
[0028] In the polyurea matrix formation reaction, the isocyanate groups in isocyanate component A react with the amino groups in amino compound component B to generate urea bonds and gradually form a polyurea polymer matrix, causing the viscosity of the reaction system to gradually increase and gel and solidify.
[0029] In the in-situ foaming reaction, the isocyanate groups in isocyanate A react with adsorbed water carried by natural nano-clay minerals to first form unstable carbamic acid, which then decomposes to produce carbon dioxide gas and amines. The generated carbon dioxide gas nucleates within the forming polyurea matrix and gradually forms pores, thus achieving simultaneous formation of the polyurea matrix and the foaming process.
[0030] Natural nano-clay minerals provide a certain degree of physical confinement for adsorbed water. Taking HNTs as an example, some water is adsorbed on the outer surface of the HNTs, while the remaining water enters the hollow cavity and adsorbs onto the inner wall of the cavity. Water on the outer surface can quickly contact the reaction system and participate in the in-situ foaming reaction, while water inside the cavity is constrained by the cavity space and capillary action, requiring diffusion before being gradually released outwards. Therefore, its participation in the in-situ foaming reaction is relatively slow. Consequently, the water in the system does not participate in the reaction simultaneously and centrally after the addition of component A, but rather undergoes a certain release process.
[0031] Meanwhile, the natural nano-clay minerals uniformly dispersed in the reaction system are solid nanoparticles, and their surfaces can serve as heterogeneous nucleation sites during the formation of carbon dioxide bubbles. When carbon dioxide is generated near the natural nano-clay minerals, bubble nuclei can form on their surfaces and grow further, thereby increasing the number of bubble nucleation sites in the reaction system and reducing the likelihood of bubbles coalescing and growing excessively after initial formation.
[0032] Therefore, this embodiment uses the loading and constraint of water by natural nano-clay minerals to regulate the spatial distribution and release process of foaming water in the reaction system on the one hand, and to provide heterogeneous nucleation sites by natural nano-clay minerals on the other hand, so that the generation of carbon dioxide, the nucleation and growth of bubbles are matched with the gradual thickening, gelation and solidification process of polyurea matrix, thereby forming a relatively fine and uniformly distributed cell structure.
[0033] After completing the above polymerization and in-situ foaming, the resulting foamed material is placed in a mold and subjected to vacuum degassing and curing. Vacuum degassing is mainly used to remove large air bubbles introduced during feeding and mechanical stirring. Subsequently, curing continues under normal pressure to fully shape the polyurea matrix, ultimately obtaining in-situ foamed polyurea from natural nano-clay minerals.
[0034] In this embodiment, HNTs are preferably used as the natural nano-clay mineral. The following describes in detail the wetting pretreatment, premixing and dispersion with component B, in-situ foaming of component A and component B, and subsequent degassing and curing process using HNTs as an example.
[0035] II. Step S1: Steam wetting pretreatment of HNTs Step S1: The HNTs are pretreated with steam to make water molecules uniformly adsorbed on the outer surface, hollow cavity and interparticle gaps of the HNTs, so as to obtain water-containing HNTs with a set water content.
[0036] Specifically, select dry HNTs powder without obvious lumps, and spread it evenly on the material tray of the constant temperature and humidity test chamber, with a thickness not exceeding 5 mm. Controlling the HNTs powder to a small spread thickness allows water vapor in the humid air to come into full contact with the powder, reducing the difference in wetting degree between the inside and outside caused by excessive powder layer thickness, and facilitating the diffusion of moisture into the HNTs tube bundles, particle gaps, and hollow cavity.
[0037] Subsequently, the temperature and relative humidity of the constant temperature and humidity test chamber were set to treat the HNTs powder under constant temperature and humidity. The treatment temperature was 40–60℃, the relative humidity was 75%–80%, and the treatment time was 4–8 hours. After treatment, the HNTs powder was removed and its moisture content was tested, ensuring that the moisture content of the treated HNTs was 10%–30% of its own mass.
[0038] The steam wetting treatment temperature is controlled at 40–60℃ primarily to balance the diffusion capacity of water molecules with the adsorption stability of HNTs on water molecules. Within this temperature range, water molecules possess suitable diffusion kinetic energy, enabling them to diffuse into the outer surface of HNTs, the hollow tube cavity, and the gaps between the tube bundles. This allows a certain amount of water to be adsorbed both inside and outside the tubes, while simultaneously maintaining a relatively stable hydrogen bond adsorption state between the hydroxyl groups on the HNT surface and water molecules.
[0039] When the processing temperature is too high, the adsorption equilibrium capacity of water molecules on the silica-alumina hydroxyl surface of HNTs decreases, and the adsorbed water is prone to desorption, making it difficult for HNTs to maintain the required water content. At the same time, excessively high temperature may also affect the stability of hydrophilic sites on the tube wall, which is not conducive to the continuous loading of subsequent water.
[0040] When the processing temperature is too low, the diffusion rate of water vapor molecules decreases, making it difficult for moisture to fully enter the hollow cavity and inter-tube gaps of HNTs, and causing it to tend to concentrate mainly on the surface of the powder. Even if the processing time is extended, uneven distribution of water content inside and outside the tubes may occur, resulting in significant differences in the amount of gas produced at different locations during subsequent in-situ foaming, which in turn affects the cell size and uniformity of distribution.
[0041] The relative humidity is controlled at 75%–80%. Within this range, the gas phase can provide enough water molecules to adsorb onto the surface and pores of HNTs through hydrogen bonding and capillary action, while avoiding the formation of significant liquid free water between particles.
[0042] When the relative humidity is too low, the adsorption driving force of HNTs for water molecules is insufficient, resulting in a low water content. Consequently, the amount of water that can react with isocyanate to produce carbon dioxide is insufficient, affecting the in-situ foaming effect. When the relative humidity is too high, liquid free water is easily condensed in the gaps between HNT particles, causing some water to re-exist in a free water state. At the same time, it may also cause HNT powder to clump, reducing its dispersion uniformity in component B.
[0043] The steam wetting treatment time is set to 4–8 hours to allow sufficient time for water vapor to diffuse within the HNT bundles, hollow cavities, and interparticle spaces, gradually achieving a relatively uniform adsorption state. This treatment time ensures that moisture fully penetrates the HNTs while also considering the processing efficiency in the actual preparation process.
[0044] The water content of the treated HNTs is controlled to be 10%–30% of their own mass. The water adsorbed in the HNTs is the water source for the subsequent in-situ foaming reaction with isocyanate. Therefore, its water content directly affects the amount of carbon dioxide generated and the degree of foaming. When the water content of the HNTs is too low, there is insufficient water to participate in the reaction, resulting in less carbon dioxide generation and making it difficult to achieve the expected foaming effect. When the water content of the HNTs is too high, a large amount of water will participate in the reaction and generate a large amount of carbon dioxide in a short time, which can easily cause excessive cell growth and affect the stability of the cell structure. Therefore, controlling the water content of the HNTs at 10%–30% can maintain a good coordination between the in-situ gas generation process and the formation process of the polyurea matrix.
[0045] After the steam wetting treatment described above, water molecules can be distributed relatively evenly on the surface of HNTs and inside the hollow cavity. Compared with directly adding liquid water to the reaction system, this treatment method allows water to be loaded onto HNTs in an adsorbed state. Among them, the adsorbed water located on the outer surface of HNTs can participate in subsequent reactions more quickly, while the water located inside the hollow cavity is constrained by the cavity space and capillary action, and its migration rate to the external reaction system is relatively slow. This provides a water source with a certain release process for the subsequent in-situ foaming process.
[0046] III. Combination Figures 4-6 Explanation of the wetting characterization results of HNTs To verify the adsorption of moisture by HNTs after steam wetting treatment and the retention of the HNTs' own structure after wetting treatment, Fourier transform infrared spectroscopy, X-ray diffraction and thermogravimetric analysis were used to characterize the treated HNTs in this embodiment.
[0047] Combination Figure 4 , Figure 4 The Fourier transform infrared spectra of halloysite and HNTs after steam wetting are shown. Compared with the original halloysite, the HNTs after steam wetting show a new vibrational peak at 3553 cm⁻¹, which corresponds to the hydroxyl vibration peak of adsorbed water on the halloysite surface. This indicates that after the aforementioned steam wetting treatment, water vapor can be adsorbed by HNTs, thus causing the HNTs to form a state containing adsorbed water.
[0048] Combination Figure 5 , Figure 5 The X-ray diffraction results of HNTs after water vapor wetting treatment are shown. Figure 5 It can be seen that the treated HNTs still have several obvious and relatively sharp diffraction peaks, which correspond to the characteristic peaks of halloysite. This indicates that after the aforementioned steam wetting treatment, halloysite still has a good crystalline state and its crystal structure is well maintained. This demonstrates that the steam wetting treatment used in this embodiment can load moisture onto HNTs without significantly damaging their basic crystal structure.
[0049] Combination Figure 6 , Figure 6 The thermogravimetric curves of HNTs after water vapor wetting treatment are shown. Figure 6 It can be seen that HNTs lose about 21% of their weight below 100℃. This weight loss corresponds to the interlayer water and surface adsorbed water in halloysite, further indicating that after water vapor wetting treatment, water can be effectively adsorbed by HNTs and retained in their structure.
[0050] In addition, HNTs also exhibit a corresponding weight loss process in the temperature range of 400–600 °C. This stage of weight loss mainly corresponds to the dehydroxylation reaction of halloysite, which is different from the weight loss process caused by interlayer water and surface adsorbed water below 100 °C.
[0051] Therefore, combining Figures 4-6 The characterization results show that after the aforementioned steam wetting treatment, water can be effectively adsorbed by HNTs, while HNTs can still maintain their basic crystal structure. Fourier transform infrared spectroscopy and thermogravimetric analysis results respectively verified the presence of adsorbed water in HNTs from two aspects: characteristic peaks of adsorbed water and low-temperature weight loss. This provides experimental basis for the subsequent reaction of the adsorbed water with isocyanate to produce carbon dioxide.
[0052] IV. Step S2: Premixing and dispersing of aqueous HNTs and component B Step S2: Add the aqueous HNTs obtained in step S1 to amino compound component B, and premix and disperse them by mechanical stirring combined with ultrasonic dispersion to obtain a homogeneous premix of HNTs-component B.
[0053] Specifically, HNTs powder, after being steam-wetted, is weighed according to a predetermined ratio and added to component B. Component B can be a single-terminated amino polyether or a single amino chain extender to suit polyurea foam products with different hardness and toughness requirements. In this embodiment, component B can be poly-1,4-butanediol bis(4-aminobenzoate).
[0054] The amount of HNTs added is 1% to 10% of the sum of the masses of components A and B. Controlling the amount of HNTs within this range allows them to function as nanofillers in the polyurea system, providing a water-containing carrier and heterogeneous nucleation sites for subsequent in-situ foaming. Furthermore, it avoids powder agglomeration and a significant increase in system viscosity due to excessive HNT addition, which would negatively impact the mixing and foaming of components A and B. When the amount of HNTs added is too low, its effect on cell nucleation and material reinforcement is relatively limited; when the amount added is too high, particle agglomeration and dispersion difficulties are likely to occur.
[0055] During premixing and dispersion, the aqueous HNTs and component B were first mechanically stirred using a mechanical mixer at a speed of approximately 500 rpm for approximately 20 minutes. Mechanical stirring ensured that the HNTs powder was fully wetted by component B and that larger HNT agglomerates were initially dispersed within component B.
[0056] After mechanical stirring, the mixture is then ultrasonically dispersed for 5–10 minutes. Ultrasonic dispersion further breaks down the micro-agglomerates remaining after mechanical stirring, allowing HNTs to be more uniformly dispersed in component B. After mechanical stirring and ultrasonic dispersion, a homogeneous premix of HNTs and component B, free of obvious particles and precipitates, is obtained.
[0057] During this premixing process, the HNTs treated in step S1 still carry a certain amount of adsorbed water. Part of this water is adsorbed on the outer surface of the HNTs' tubular structure, while the other part enters the hollow cavity of the HNTs and adsorbs on the hydrophilic sites on the inner wall of the cavity. The adsorbed water on the outer surface has more direct contact with component B and the subsequently added component A, thus it can participate in the subsequent in-situ foaming reaction more quickly. The water inside the cavity, however, is constrained by the space within the nanotube cavity and affected by capillary action, requiring a certain mass transfer process to migrate out of the tube, resulting in a relatively slow release rate.
[0058] Therefore, by pre-dispersing hydrated HNTs uniformly in component B, adsorbed water can be dispersed throughout different regions of component B along with the HNT particles, reducing the concentration of water in localized areas and providing a more uniform water distribution basis for the subsequent in-situ foaming reaction after the addition of component A. Simultaneously, the uniformly dispersed HNT particles can provide dispersed heterogeneous nucleation sites during the subsequent carbon dioxide generation process, which is beneficial for forming a more uniform cell structure.
[0059] V. Regulation of moisture release and foaming process by component B temperature Before or during step S2, the release state of adsorbed water in HNTs and the subsequent in-situ foaming process can be further adjusted by adjusting the preheating temperature of component B.
[0060] Specifically, before adding component A, component B is preheated to 40–80°C, preferably 50–70°C. When steam-wetted HNTs are added to the preheated component B, the adsorbed water at different locations in the HNTs exhibits different release characteristics.
[0061] Of the water, some is adsorbed onto the outer surface of the HNTs via hydrogen bonds. This water is in direct contact with the surrounding component B and can participate relatively quickly in the reaction between isocyanate and water after the subsequent addition of component A. The other portion of water is located inside the hollow cavity of the HNTs and adsorbed onto hydrophilic sites on the inner wall of the cavity. Due to the constraints of the nanoscale cavity space and capillary action, the water inside the cavity needs to overcome certain mass transfer resistance before migrating out, thus its release rate is relatively slow.
[0062] Preheating component B increases the thermal motion of water molecules within the HNTs cavity and weakens some of the hydrogen bond bonds between water molecules and the cavity wall. Simultaneously, as the temperature rises, the water vapor pressure within the cavity increases accordingly, creating a diffusion driving force for the migration of component B from the inside of the cavity to the outside. This allows some water within the cavity to gradually release outwards before component A is added, rather than reacting concentratedly after component A is added.
[0063] Therefore, the migration degree and release timing of adsorbed water inside the HNTs lumen can be controlled by adjusting the preheating temperature of component B. Specifically, within the aforementioned temperature range, as the preheating temperature of component B increases, the thermal motion of water molecules inside the HNTs lumen strengthens, increasing their ability to migrate out of the lumen, allowing more adsorbed water to gradually migrate into component B during the premixing stage. When the preheating temperature of component B is relatively low, more adsorbed water remains inside the HNTs lumen and is gradually released outward during the reaction process after the addition of component A, thus exhibiting a more pronounced slow-release characteristic.
[0064] The preheating temperature of component B not only affects the release process of adsorbed water in HNTs, but also influences the subsequent formation rate of the polyurea matrix. Appropriately increasing the temperature of component B can accelerate the reaction between amino groups and isocyanate groups, allowing the polyurea matrix to quickly establish a certain viscosity and structural strength. When adsorbed water reacts with isocyanate to produce carbon dioxide, the viscoelastic polyurea matrix can encapsulate and fix the formed bubbles, thereby reducing bubble coalescence and cell collapse.
[0065] Therefore, the preheating temperature of component B affects both the adsorbed water release process and the polyurea gelation process. By adjusting the preheating temperature of component B, a better matching relationship can be maintained between the release of adsorbed water, the generation of carbon dioxide, and the gelation and curing process of the polyurea matrix in HNTs, thereby regulating the cell formation process.
[0066] VI. Step S3: Mixing component A and component B and in-situ foaming In step S3, isocyanate component A is mixed with the homogeneous premix of HNTs-B obtained in step S2, so that the polyurea matrix formation reaction and the in-situ foaming reaction of adsorbed water are carried out simultaneously.
[0067] Specifically, isocyanate component A and HNTs-B homogeneous premixes are weighed according to a set ratio, such that the equivalent ratio of isocyanate groups in isocyanate component A to amino groups in component B is (1-1.1):1. Then, isocyanate component A is rapidly added to the HNTs-B homogeneous premix, and the mixture is stirred at approximately 300 rpm for about 1 minute using a mechanical stirrer to rapidly and uniformly mix components A, B, and the aqueous HNTs dispersed in component B, thereby initiating polymerization and in-situ foaming reactions.
[0068] After component A is mixed with the homogeneous premix of HNTs-B, polyurea matrix molding reaction and in-situ foaming reaction occur simultaneously in the system.
[0069] In the polyurea matrix molding reaction, the isocyanate groups in isocyanate component A react with the amino groups in component B to form urea bonds, gradually forming a polyurea polymer matrix. As the reaction continues, the reaction system gradually thickens and undergoes cross-linking and curing, providing a coating and shaping basis for the subsequent formation of cells.
[0070] Meanwhile, in the in-situ foaming reaction, the isocyanate groups in isocyanate A react with the adsorbed water carried by HNTs to first generate unstable carbamic acid, which then decomposes to produce carbon dioxide gas and amines. The generated carbon dioxide gas nucleates and expands in the gradually thickening polyurea matrix to form cells, thus completing in-situ foaming simultaneously with the formation of the polyurea matrix.
[0071] Since HNTs are uniformly dispersed within component B in step S2, the water adsorbed on the surface of HNTs and inside the tubes is also dispersed in different regions of the reaction system along with the HNTs. After the addition of component A, the adsorbed water on the outer surface of HNTs can quickly contact the isocyanate and participate in the gas generation reaction, while the water inside the HNTs tubes is constrained by the nanoscale tube space and capillary action, and its migration to the outside of the tube and participation in the reaction is relatively slow. This makes the carbon dioxide generation process somewhat continuous, rather than all the water participating in the reaction at the same time.
[0072] Furthermore, HNTs, which are uniformly dispersed in the reaction system, are nanoscale solid particles, and their surfaces can serve as heterogeneous nucleation sites during the formation of carbon dioxide bubbles. When carbon dioxide is generated near HNTs, bubble nuclei can form on the surface of the HNT particles and grow further, thereby increasing the number of bubble nucleation sites in the system and reducing the possibility of bubble aggregation, merging, or excessive growth, which is conducive to the formation of a finer and more uniformly distributed pore structure.
[0073] Therefore, in this step, the polymerization reaction between isocyanate and amino compounds, as well as the gas generation reaction between isocyanate and water adsorbed by HNTs, occur simultaneously. This allows carbon dioxide to be continuously generated and bubbles to form as the polyurea matrix gradually forms, achieving simultaneous polymerization, foaming, and shaping. Through the aforementioned water loading and release effects of HNTs, combined with the heterogeneous nucleation sites provided by HNTs, the generation of carbon dioxide, bubble nucleation, and growth processes can be coordinated with the gelation and curing process of the polyurea matrix, providing a foundation for the subsequent formation of a polyurea foam with a more uniform structure.
[0074] VII. Step S4: Vacuum degassing and curing Step S4: The foamed material obtained in step S3 is subjected to vacuum degassing treatment, and then cured under normal pressure after vacuum degassing to obtain natural nano-clay mineral in-situ foamed polyurea foam.
[0075] Specifically, after step S3 completes the mixing of component A and the homogeneous premix of HNTs-B components, the foaming material still retains a certain degree of fluidity. The foaming material is then quickly poured into a polytetrafluoroethylene mold, and the mold containing the foaming material is rapidly moved into a vacuum degassing chamber. After sealing the vacuum degassing chamber, the vacuum system is activated to achieve a vacuum level of -0.08 to -0.1 MPa, which is maintained for 1 to 5 minutes. Preferably, the vacuum treatment time is 2 to 3 minutes.
[0076] During the feeding and mechanical mixing of components A and B, outside air may be entrained into the reactants, forming relatively large air bubbles. These air bubbles are not formed by the in-situ foaming reaction between HNTs-adsorbed water and isocyanates. If retained in the final polyurea foam, they can easily form large, non-uniform pores. Therefore, vacuum degassing is used to allow the large air bubbles entrained during mechanical mixing and feeding to escape from the foamed material, thereby reducing pore defects caused by outside air.
[0077] Meanwhile, the vacuum treatment time is controlled within 1–5 minutes, preferably 2–3 minutes, to balance the removal of large-sized air bubbles with the preservation of the in-situ pore structure. By controlling the vacuum level and vacuum treatment time, the impact on the microporous structure formed by the in-situ reaction of HNTs adsorbing water can be reduced while removing non-target air bubbles, thereby preserving the micron-sized pores formed by carbon dioxide.
[0078] After vacuum treatment is completed and the foam is initially formed, the vacuum system is shut down, and the vacuum degassing chamber is restored to normal pressure. Subsequently, the formed polyurea foam is placed at room temperature for 24 hours to allow the isocyanate groups and amino groups to continue reacting and to further solidify and shape the polyurea matrix, ultimately obtaining in-situ foamed polyurea from natural nano-clay minerals.
[0079] Through the above-mentioned vacuum degassing and curing treatment, large air bubbles formed during feeding and mixing can be distinguished from target cells formed by in-situ foaming. This reduces large-sized air pore defects while preserving the microporous structure formed in-situ, thereby improving the uniformity of the internal structure of polyurea foam.
[0080] VIII. Methods for Adjusting the Cell Structure In this embodiment, the cell size, number of cells, cell distribution, and foam density of polyurea foam can be adjusted by adjusting the water content of HNTs, the amount of HNTs added, the preheating temperature of component B, as well as the mold size and material filling amount.
[0081] Specifically, the water content of HNTs can be changed by adjusting the degree of vapor wetting. Within the aforementioned allowable range, the higher the water content of HNTs, the more water can participate in the isocyanate-water reaction, resulting in a greater amount of carbon dioxide gas produced, thus increasing the degree of cell expansion. Conversely, when the water content of HNTs decreases, the amount of water that can participate in the in-situ foaming reaction decreases accordingly, reducing the amount of carbon dioxide generated. Therefore, the degree of foaming and cell size can be adjusted by regulating the water content of HNTs.
[0082] The pore structure can also be altered by adjusting the amount of HNTs added. Within the aforementioned allowable range, increasing the amount of HNTs added can, on the one hand, increase the total amount of adsorbed water introduced into the reaction system with the HNTs, thereby increasing the amount of carbon dioxide generated during in-situ foaming; on the other hand, HNTs, as solid nanoparticles, can provide heterogeneous nucleation sites. As the amount of HNTs added increases, the number of bubble nucleation sites in the system increases accordingly, which is beneficial for increasing the number of pores and making the pores smaller and more uniform. Therefore, the pore density, pore size, and their distribution can be adjusted by regulating the amount of HNTs added.
[0083] Furthermore, the release state of adsorbed water in HNTs can be altered by adjusting the preheating temperature of component B. As mentioned earlier, when the temperature of component B increases, the migration ability of water molecules inside the HNT cavity is enhanced, allowing water inside the cavity to be released more fully. This alters the amount of water participating in the gas-generating reaction and the release process during subsequent in-situ foaming, and also affects the foaming ratio. When the temperature of component B is relatively low, more water remains inside the HNT cavity and is gradually released after the addition of component A, resulting in more pronounced slow-release foaming characteristics, which is beneficial for forming a finer and more uniform cell structure.
[0084] Furthermore, the cell structure and foam density can be adjusted by modifying the mold size and the amount of material filled. Under the same mold conditions, changing the volume of foaming material added to the mold alters the expansion space of the foaming material within the mold. When the amount of material filled is small, the proportion of foaming material in the mold volume decreases, and the space available for carbon dioxide bubble expansion increases accordingly, which facilitates further expansion of the material and reduces the density of the resulting foam. Accordingly, the mold size and the amount of material filled can be adjusted according to the target foam density and degree of foaming.
[0085] Therefore, this embodiment adjusts the carbon dioxide generation, the number of bubble nucleation, the moisture release process, and the cell expansion space by using one or more parameters among HNTs moisture content, HNTs addition amount, component B preheating temperature, mold size, and material filling amount, thereby achieving the adjustment of polyurea foam cell structure and foam density.
[0086] IX. Example 1 This embodiment provides a method for preparing polyurea foam using in-situ foaming with water-containing HNTs.
[0087] In this embodiment, a mold with dimensions of φ80mm×120mm is used, and the mold volume is approximately 603cm³. Component A of isocyanate is liquefied MDI, with a dosage of 89g; component B of amino compound is poly-1,4-butanediol bis(4-aminobenzoate), with a dosage of 101g; and HNTs are used in a dosage of 10g.
[0088] First, the HNTs undergo steam wetting pretreatment. The HNTs are placed in a constant temperature and humidity environment at 50°C, resulting in a water content of 20% of their mass. After wetting, the water is adsorbed onto the outer surface and inside the hollow tubes of the HNTs, forming an adsorbed water source for subsequent in-situ foaming reactions.
[0089] Subsequently, component B was preheated to 60°C, and 10g of moistened HNTs was added to component B for premixing and dispersion. Following the method described in step S2 above, HNTs were first initially dispersed in component B by mechanical stirring, and then the degree of HNT aggregation was further reduced by ultrasonic dispersion to obtain a homogeneous premix of HNTs and component B.
[0090] After component B is preheated to 60°C, the molecular motion of adsorbed water inside the HNTs cavity increases, and some of the water inside the cavity is gradually released into the component B medium. At the same time, some water remains inside the hollow cavity of the HNTs and is gradually released after the subsequent addition of component A, thus giving the adsorbed water in the HNTs a certain release process.
[0091] After completing the premixing and dispersion of HNTs and component B, 89g of MDI was weighed as component A, and component A was quickly added to the homogeneous premix of HNTs and component B for mechanical stirring to ensure that component A, component B and water-containing HNTs were fully mixed.
[0092] After mixing, the isocyanate groups in component A react with the amino groups in component B to form a polyurea matrix. Simultaneously, the isocyanate groups react with adsorbed water carried by HNTs to produce carbon dioxide gas. The generated carbon dioxide nucleates and expands within the gradually forming polyurea matrix, thus forming bubbles. The HNT particles also serve as heterogeneous nucleation sites, enabling carbon dioxide to form bubble nuclei on the HNT surface, achieving simultaneous polymerization and in-situ foaming reactions.
[0093] After mixing, the resulting foamed material is quickly poured into the φ80mm×120mm mold, and vacuum degassing is performed according to step S4 above to remove large air bubbles introduced during feeding and mechanical stirring. After vacuum degassing, the pressure is restored to normal and the material is allowed to continue curing at room temperature to allow the polyurea matrix to set.
[0094] After the above treatment, in-situ expanded polyurea foam containing HNTs was finally obtained. The density of the polyurea foam obtained in this example is approximately 0.3–0.4 g / cm³.
[0095] Combined with the following discussion Figure 3 The microstructure of the polyurea foam obtained in this embodiment can be further observed. Its cells are mainly near-spherical closed cells with relatively complete cell morphology, continuous cell walls, and relatively small fluctuations in cell size. Overall, it presents a relatively fine and uniformly distributed cell structure.
[0096] 10. Combination Figure 1 Explanation of Comparative Example 1 To illustrate the difference between using aqueous HNTs as the in-situ foaming water source and directly adding free water for foaming, Comparative Example 1 was set up. Comparative Example 1 used MDI, component B, and free water to prepare polyurea foam, wherein water was added directly to the reaction system in the form of free water without being pre-adsorbed into the HNTs.
[0097] Combination Figure 1 The scanning electron microscope images shown reveal significant variations in the pore size of the polyurea foam obtained in Comparative Example 1. Large, medium, and small pores coexist within the same sample, exhibiting a wide pore size distribution and relatively poor pore sphericity. Some pore walls show signs of rupture, with interconnections and merging between adjacent pores. Larger pore structures, pore collapse, and fusion are also observed in some areas. Overall, the density and uniformity of the pore structure are poor.
[0098] The reason for this phenomenon is that when free water is directly added to the reaction system, it lacks the constraint of the HNTs' surface and tubular structure. Upon contact with isocyanate, the water reacts rapidly to produce carbon dioxide. When water is relatively concentrated in a localized area, a large amount of carbon dioxide is generated in that area within a short time, causing the already formed bubbles to continue expanding and easily coalesce. Before the polyurea matrix has formed sufficient structural support, some bubbles undergo excessive growth, pore wall rupture, or pore fusion, resulting in significant differences in the final pore size.
[0099] Therefore, Comparative Example 1 shows that although free water can react with isocyanate to produce carbon dioxide and achieve polyurea foaming, the foaming reaction is more vigorous when free water is added directly, and the bubbles tend to coalesce and grow, making it difficult to obtain a fine and uniformly distributed cell structure. This comparative example can serve as the basis for subsequent comparisons with in-situ foaming examples of aqueous HNTs.
[0100] XI. Combination Figure 2 Explanation of Comparative Example 2 To illustrate the role of HNTs themselves and the adsorbed water they support in the in-situ foaming process, Comparative Example 2 was set up. Comparative Example 2 used MDI, component B, and dried HNTs to prepare polyurea material, wherein the HNTs were not steam-wetted and did not have adsorbed water for in-situ foaming.
[0101] Combination Figure 2 As shown in the scanning electron microscope images, the sample obtained in Comparative Example 2 basically did not form a complete pore structure, and the cross-section mainly showed a dense matrix fracture morphology. Due to the addition of HNTs to the system, some grooves and wrinkles could be observed on the sample surface, but a large number of independent and complete closed-cell bubbles were not observed.
[0102] The main reason for the above phenomenon is that the dried HNTs lack endogenous moisture that can react with isocyanates to produce carbon dioxide. Although HNTs are dispersed as solid nanoparticles in the polyurea system, in the absence of a foaming water source, it is difficult for the system to continuously generate carbon dioxide gas for forming pores, so a distinct pore structure cannot be formed.
[0103] Therefore, simply adding dried HNTs to the polyurea system cannot achieve the in-situ foaming effect described in this invention. Comparative Example 1 further illustrates that the technical effect of this invention does not solely originate from the addition of HNT particles, nor solely from the foaming reaction between water and isocyanate, but is related to the water loading of the HNTs and the release of the adsorbed water during the reaction process.
[0104] In other words, while dry HNTs can exist as nano-solid particles in a polyurea matrix, they lack adsorbed water and therefore cannot provide the gas source required for in-situ foaming. However, when HNTs are loaded with adsorbed water, the adsorbed water can gradually react with isocyanate during the reaction process to produce carbon dioxide. Simultaneously, the HNT particles can provide heterogeneous nucleation sites, thus forming the foam structure shown in Example 1 described later. The comparison results of the three groups of samples show that the dry HNT system, lacking adsorbed water to participate in the in-situ foaming reaction, basically does not form obvious foam pores. In contrast, in the aqueous HNT system, the adsorbed water loaded on the HNTs can participate in the isocyanate-water reaction to generate carbon dioxide, and the HNT particles can provide heterogeneous nucleation sites, thus forming a relatively fine and uniformly sized polyurea foam structure.
[0105] 12. Combination Figure 3 Description of the microstructure of Example 1 Combination Figure 3 As shown in the scanning electron microscope images, the polyurea foam prepared using aqueous HNTs in Example 1 formed a relatively obvious and complete cell structure. The cells were mainly near-spherical closed cells with relatively complete cell outlines and continuous pore walls between adjacent cells. The large-area pore wall rupture and cell fusion phenomena that were more obvious in Comparative Example 1 were not observed.
[0106] From the perspective of cell size and spatial distribution, the size fluctuations between different cells in Example 1 are relatively small, the cell arrangement is relatively dense, and the overall microstructure presents a relatively fine and uniform distribution. Figure 1 Compared to polyurea foam formed by directly adding free water, the large-sized cells and obvious cell collapse and merging phenomena in Example 1 are reduced, indicating that using water-containing HNTs as the in-situ foaming water source can improve the cell formation process.
[0107] Combination Figures 1-3 The comparison shows that when free water is added directly in Comparative Example 1, the reaction between water and isocyanate is more concentrated, and the formed bubbles are prone to coalescence and excessive growth, resulting in a large difference in cell size. When dry HNTs are used in Comparative Example 2, the system lacks a water source that can participate in the in-situ foaming reaction, so a complete cell structure cannot be formed. However, when aqueous HNTs are used in Example 1, a relatively fine and uniformly distributed cell structure can be formed.
[0108] The reason for the above differences lies in the fact that the hydrated HNTs in this embodiment simultaneously possess both water loading and heterogeneous nucleation functions. On the one hand, water is pre-loaded on the outer surface and inside the hollow cavity of the HNTs, and is constrained by the surface structure of the HNTs and the cavity space, allowing the water to be released gradually during the reaction process, reducing the situation where free water concentrates in the reaction and causes rapid carbon dioxide concentration. On the other hand, the uniformly dispersed HNT nanoparticles can serve as heterogeneous nucleation sites during the bubble formation process, increasing the number of bubble formation sites and facilitating the formation of more numerous and uniformly sized pores. This allows the generated carbon dioxide to disperse and form more pores, thereby inhibiting the excessive growth of individual pores and the merging of adjacent pores. The above comparison results show that the slow-release effect of hydrated HNTs on adsorbed water and its heterogeneous nucleation function work together to improve the pore formation process and the final microstructure.
[0109] Therefore, combining Figure 3 and Figure 1 , Figure 2 The comparative results show that preloading water into HNTs before participating in polyurea in situ foaming can change the state of water participating in the isocyanate reaction and utilize the heterogeneous nucleation sites provided by HNT particles to make the formation and growth process of the foam cells more uniform, thereby obtaining polyurea foam with relatively fine pores and relatively uniform pore size distribution.
[0110] Thirteen, Combining Figure 7 Description of the overall microstructure of polyurea foam Combination Figure 7 The overall microstructure of the polyurea foam shown shows that the polyurea foam prepared by using water-containing HNTs as the in-situ foaming component has a relatively obvious cell structure. The cells are distributed inside the polyurea matrix, and the overall shape is mainly near-spherical. The cell outline is relatively complete, and the continuity of the cell walls between adjacent cells is good. There are no large-scale obvious cell wall ruptures or large-scale cell penetrations.
[0111] As can be seen from the preparation process in this embodiment, while isocyanate component A reacts with amino compound component B to form a polyurea matrix, adsorbed water pre-loaded on the surface of HNTs and in the hollow cavity reacts with isocyanate groups to generate carbon dioxide gas. The generated carbon dioxide gas nucleates and grows in the gradually forming polyurea matrix, thereby simultaneously constructing a cell structure during the polyurea matrix formation process. On the one hand, HNTs act as a carrier for adsorbed water, allowing the water to exist in a constrained state, distinct from the free water directly added to the system; on the other hand, the HNT particles dispersed in the polyurea reaction system can also provide heterogeneous nucleation sites for bubble formation, thereby affecting the nucleation of carbon dioxide gas and the cell growth process.
[0112] Further analysis of the scanning electron microscopy results and pore size statistics of the aforementioned different samples reveals that the average pore size of the polyurea foam obtained by direct foaming with free water in Comparative Example 1 is 0.51±0.08 mm. The pore size distribution is relatively wide, and there are obvious large-sized pores, pore wall ruptures, and interconnection and merging of adjacent pores. The average pore size of the polyurea foam obtained by in-situ foaming with water-containing HNTs in Example 1 is 0.15±0.03 mm. The pores are mainly nearly spherical, with relatively intact pore walls, and the overall pore size is relatively small and the arrangement is relatively dense.
[0113] The above-mentioned microstructure and pore size statistics show that, compared with directly adding free water for foaming, preloading water onto HNTs before participating in the in-situ foaming of polyurea reduces the average cell size of the resulting polyurea foam from approximately 0.51 mm to approximately 0.15 mm, and reduces phenomena such as large-sized cells, cell fusion, and pore wall rupture. This result indicates that hydrated HNTs can not only serve as a water source for in-situ foaming, but their loading and constraint effects on water can also regulate the process of water participation in the foaming reaction. Simultaneously, HNT particles can provide heterogeneous nucleation sites for bubble formation, thereby jointly improving the cell formation and growth process, resulting in a polyurea foam with a relatively fine, intact, and uniformly distributed porous structure.
[0114] XIV. Combination Figure 8 Explain the quasi-static compressive mechanical properties of polyurea foam To further evaluate the mechanical properties of polyurea foam obtained by in-situ foaming with hydrated HNTs and to illustrate the effect of the aforementioned improvement in cell structure on the macroscopic load-bearing capacity of the material, quasi-static compression tests were performed on the hydrated halloysite foam obtained in Example 1 and the free water foam obtained in Comparative Example 1.
[0115] In this test, the strain rate was 0.01 s⁻¹. -1 The mechanical responses of the two types of polyurea foam during compression were obtained, and their yield stress, elastic modulus, and compressive strength under 50% strain conditions were compared. The test results are as follows: Figure 8 As shown.
[0116] The hydrous halloysite foam obtained in Example 1 had a yield stress of 1.41 MPa, an elastic modulus of 58.75 MPa, and a compressive strength of 10.00 MPa under 50% strain conditions; the free water foam obtained in Comparative Example 1 had a yield stress of 0.38 MPa, an elastic modulus of 27.14 MPa, and a compressive strength of 4.00 MPa under 50% strain conditions.
[0117] The test results above show that, under the same quasi-static compression test conditions, the yield stress, elastic modulus, and compressive strength under 50% strain conditions of the hydrated halloysite foam obtained in Example 1 are all higher than those of the free water foam obtained in Comparative Example 1. Specifically, the yield stress of the hydrated halloysite foam is approximately 3.71 times that of the free water foam, the elastic modulus is approximately 2.16 times that of the free water foam, and the compressive strength under 50% strain conditions is approximately 2.50 times that of the free water foam. This indicates that the polyurea foam obtained after in-situ foaming with hydrated HNTs has higher initial compressive deformation resistance, overall stiffness, and load-bearing capacity under greater compressive deformation conditions.
[0118] In combination with the above Figure 1 and Figure 3 Analysis of the microstructure revealed that when free water is directly added to the polyurea reaction system, the lack of constraint from the surface and tubular structure of HNTs (hydrocarbon nitrates) allows the water to react rapidly with isocyanate in localized areas, generating concentrated carbon dioxide. This leads to rapid bubble growth and aggregation, resulting in cells with significant size variations, accompanied by structural defects such as localized pore wall rupture, pore fusion, and pore collapse. These uneven pore structures and localized pore wall defects easily create stress concentration points. Under compressive loads, these localized pore walls are more prone to bending, yielding, or failure, thus reducing the overall compressive load-bearing capacity of the foam material.
[0119] In contrast, in Example 1, water is preloaded onto the outer surface and inside the hollow cavity of the HNTs and constrained by the surface structure of the HNTs, the cavity space, and capillary action. This allows the adsorbed water to gradually participate in the isocyanate-water reaction during polyurea formation. Simultaneously, the HNTs dispersed in the polyurea system provide multiple heterogeneous nucleation sites, enabling the generated carbon dioxide to form bubble nuclei at more locations, thereby reducing the likelihood of carbon dioxide concentrating into a single large-sized bubble. The resulting bubble size fluctuations are relatively small, the pore wall continuity is better, and large-sized pores and significant bubble fusion and collapse phenomena are reduced.
[0120] Under compressive loads, the relatively fine and uniformly distributed cell structure allows for a more even distribution of external loads among multiple cells and their walls, reducing stress concentration caused by localized large pores, weak pore walls, and cell fusion regions. Simultaneously, the presence of HNTs dispersed within the polyurea matrix also contributes to maintaining the structural stability of the polyurea foam. The combined effect of these factors results in the polyurea foam obtained in Example 1 exhibiting high overall stiffness and compressive load-bearing capacity.
[0121] therefore, Figure 8 The quasi-static compression test results shown are consistent with Figures 1-3The microstructure results shown corroborate each other, indicating that the present invention can not only enable polyurea systems to form cells, but also, through the loading, constraint and release of water by hydrated HNTs, combined with the heterogeneous nucleation effect provided by HNTs, make the formed cell structure more compact and more uniformly distributed. This reduces cell merging, cell wall rupture and local collapse, while improving the yield stress, elastic modulus and compressive bearing capacity under large compressive deformation conditions of the obtained polyurea foam.
[0122] XV. Optional Raw Materials and Alternative Solutions In the above embodiments, component A is MDI, component B is poly-1,4-butanediol bis(4-aminobenzoate), and the natural nano-clay mineral is HNTs. In other embodiments, the specific types of components A, B, and natural nano-clay minerals can be replaced according to the preparation requirements of polyurea foam.
[0123] Specifically, component A can also be selected from toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, or isophorone diisocyanate. All of the above isocyanates can act as isocyanate components, reacting with the amino groups in component B to form a polyurea matrix, and reacting with adsorbed water carried by natural nano-clay minerals to produce carbon dioxide.
[0124] Component B can also be polypropylene diamine or polytetrahydrofuran diamine, or it can continue to use the aforementioned poly-1,4-butanediol bis(4-aminobenzoate). By selecting different amino compounds, different polyurea foam preparation requirements can be met.
[0125] In addition to HNTs, natural nano-clay minerals can also be sepiolite or attapulgite. When using sepiolite or attapulgite, the same general preparation method as described above can be followed: first, load the natural nano-clay minerals with water, then premix and disperse them with component B, and then mix them with component A. The loaded water reacts with isocyanate to produce carbon dioxide, thereby achieving in-situ foaming.
[0126] Furthermore, the mold size, the water content of the natural nano-clay minerals, and the addition ratio of the natural nano-clay minerals can be adjusted according to actual preparation requirements. Specifically, the water content of the natural nano-clay minerals affects the amount of carbon dioxide generated during in-situ foaming, while the addition ratio affects the number of water-containing carriers and heterogeneous nucleation sites in the system. The mold size and material filling amount affect the expansion space of the foamed material. Therefore, the degree of foaming, cell structure, and foam density of the final polyurea foam can be adjusted.
[0127] Therefore, the present invention is not limited to the specific combination of MDI, poly-1,4-butanediol bis(4-aminobenzoate) and HNTs used in the above embodiments. While maintaining the technical concept of using hydrous natural nano-clay minerals as in-situ foaming components, the isocyanate components, amino compound components, types of natural nano-clay minerals and corresponding process parameters can be adjusted.
[0128] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that, without departing from the technical concept of the present invention, the types of isocyanate component A, amino compound component B, natural nano clay minerals, and corresponding preparation process parameters can be adjusted according to actual preparation needs.
[0129] For example, component A can be one or more of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, or isophorone diisocyanate; component B can be one or more of poly-1,4-butanediol bis(4-aminobenzoate), polypropylene oxide diamine, or polytetrahydrofuran diamine; in addition to HNTs, natural nano-clay minerals can also be sepiolite, attapulgite, etc. Meanwhile, the mold size, water content of the natural nano-clay minerals, and their addition ratio can be adjusted according to the foaming degree, cell structure, and density requirements of the target polyurea foam.
[0130] Any equivalent substitutions, simple transformations, or other improvements that do not substantially differ from the above embodiments made based on the technical concept and basic principles of this invention shall fall within the protection scope of this invention.
Claims
1. A process for the preparation of a natural nanoclay mineral in-situ foamed polyurea foam, characterized in that, include: S1. Wetting treatment is applied to the natural nano clay mineral to allow water molecules to be adsorbed onto the surface and / or inside the pores of the natural nano clay mineral, thereby obtaining a natural nano clay mineral containing adsorbed water. S2. The natural nano-clay mineral containing adsorbed water is added to amino compound B component for dispersion to obtain natural nano-clay mineral-B component premix. S3. Mix isocyanate component A with the natural nano-clay mineral-component B premix, so that the isocyanate groups in isocyanate component A react with the amino groups in amino compound component B to form a polyurea matrix, and the adsorbed water reacts with the isocyanate groups to generate carbon dioxide gas. The natural nano-clay minerals provide spatial confinement for the adsorbed water to regulate the release process of the adsorbed water and provide heterogeneous nucleation sites for the carbon dioxide gas, enabling the carbon dioxide gas to nucleate in situ and form pores during the formation of the polyurea matrix, thus obtaining a foamed material. S4. The foaming material is placed in a mold for molding and curing to obtain natural nano-clay mineral in-situ foamed polyurea foam.
2. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 1, characterized in that: The natural nano-clay minerals include at least one of halloysite nanotubes, sepiolite, and attapulgite.
3. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 2, characterized in that: The natural nano-clay mineral is halloysite nanotubes; S1 includes: laying the halloysite nanotubes flat and placing them in a constant temperature and humidity environment for water vapor wetting treatment. The temperature of the water vapor wetting treatment is 40-60°C, the relative humidity is 75%-80%, and the treatment time is 4-8 hours, so that the water content of the treated halloysite nanotubes is 10%-30% of the mass of the halloysite nanotubes.
4. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 3, characterized in that: Before or during step S2, the amino compound component B is preheated to 40–80°C. Halloysite nanotubes that have been moistened with water vapor are added to the preheated amino compound B component, so that the water adsorbed inside the pores of the halloysite nanotubes is released into the amino compound B component during the premixing process, and the amount and rate of water release are adjusted by the preheating temperature of the amino compound B component.
5. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 3, characterized in that: The amount of halloysite nanotubes added is 1% to 10% of the sum of the mass of the isocyanate component A and the amino compound component B; In step S2, the halloysite nanotubes and the amino compound B component are first mechanically stirred at 500 rpm for 20 min, and then ultrasonically dispersed for 5 to 10 min to obtain the natural nano-clay mineral-B component premix.
6. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 1, characterized in that: The isocyanate A component includes at least one of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, and isophorone diisocyanate; The amino compound component B includes at least one of poly-1,4-butanediol bis(4-aminobenzoate), polyoxypropylene diamine, and polytetrahydrofuran diamine. The equivalent ratio of the isocyanate group in component A to the amino group in component B of the amino compound is (1 to 1.1):
1.
7. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 1, characterized in that: In step S3, after adding the isocyanate A component to the natural nano-clay mineral-B component premix, the mixture is mechanically stirred at a stirring speed of 300 rpm for 1 min, so that the isocyanate A component and the amino compound B component undergo a polymerization reaction, while the adsorbed water and the isocyanate A component undergo an in-situ foaming reaction.
8. The method for preparing in-situ foamed polyurea from natural nano-clay minerals according to claim 1, characterized in that: S4 includes: The foamed material is injected into a mold and placed in a vacuum environment for vacuum degassing to remove air bubbles introduced during the mixing process. The vacuum degree of the vacuum degassing process is -0.08 to -0.1 MPa, and the processing time is 1 to 5 minutes. After completing the vacuum degassing treatment, restore normal pressure and cure at room temperature for 24 hours.
9. A natural nanoclay mineral in-situ foamed polyurea foam, characterized in that, It includes a polyurea matrix, natural nano-clay minerals dispersed in the polyurea matrix, and a pore structure formed in the polyurea matrix; The natural nano-clay mineral is loaded with adsorbed water before forming the polyurea matrix, and the adsorbed water is constrained by the surface and / or pore structure of the natural nano-clay mineral. The pore structure is formed in situ by carbon dioxide gas generated from the reaction of adsorbed water and isocyanate during the formation of the polyurea matrix, and the natural nano-clay minerals constitute heterogeneous nucleation sites when carbon dioxide gas forms pores.
10. The in-situ foamed polyurea from natural nano-clay minerals according to claim 9, characterized in that: The natural nano-clay mineral is halloysite nanotubes, and the amount of halloysite nanotubes added is 1% to 10% of the sum of the mass of the isocyanate component and the amino compound component that form the polyurea matrix, and the water content of the halloysite nanotubes before participating in the in-situ foaming reaction is 10% to 30% of the mass of the halloysite nanotubes.