Composite resin low dielectric material and preparation method thereof, preparation method and application of composite low dielectric microporous material

By combining a composite material of a low-dielectric polymer and an intrinsically low-polarity resin with irradiation crosslinking and gas foaming technology, the problem of balancing the dielectric properties and overall material performance of high-frequency copper-clad laminate substrates has been solved. This results in low dielectric loss and low delay in high-frequency signal transmission, along with excellent thermal dimensional stability and mechanical properties.

CN123152159APending Publication Date: 2026-11-24EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611629934.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing high-frequency copper clad laminate substrates have the problem of not being able to balance dielectric properties and overall material performance in high-frequency signal transmission. In particular, the materials are prone to thermal relaxation and thermal deformation under high-temperature thermal shock, which cannot meet the demanding application requirements of high-end copper clad laminates.

Method used

A composite material of low dielectric polymer and intrinsically low polarity resin is prepared by radiation crosslinking to form a dense three-dimensional crosslinked network, combined with gas foaming technology to improve the heat resistance and foaming performance of the material.

Benefits of technology

It achieves low dielectric loss and low delay in high-frequency signal transmission, possesses excellent thermal dimensional stability and mechanical properties, and can maintain good dielectric and processing properties at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152159A_ABST
    Figure CN123152159A_ABST
Patent Text Reader

Abstract

This invention provides a composite resin low-dielectric material and its preparation method, as well as a method for preparing composite low-dielectric microporous materials and their applications, belonging to the field of polymer composite materials and electronic communication substrates. This invention modifies the dielectric properties, foaming behavior, and heat resistance of polymers by introducing intrinsically low-polarity resins. Simultaneously, the intrinsically low-polarity resin and a crosslinking agent form a dense three-dimensional network structure through radiation crosslinking, which further enhances the foaming and mechanical properties of the system without affecting the original heat resistance of the polymer.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the field of high polymer composite materials and electronic communication substrates, and in particular to a composite resin low dielectric material and a preparation method thereof, a preparation method and application of a composite low dielectric microporous material. BACKGROUND

[0002] With the rapid development of 5G / 6G mobile communication, millimeter wave radar and high-performance computers, modern electronic information technology is moving towards high frequency, high speed and high density integration. Copper clad plate (CCL) as the core basic substrate for manufacturing printed circuit board (PCB), its dielectric properties directly determine the quality and efficiency of the signal transmission process. When the signal operating frequency enters the microwave and radio frequency band (GHz level and above), the dielectric loss and signal delay effect (RC delay) generated by the transmission of electromagnetic waves in the insulating medium will increase exponentially. Traditional copper clad plate substrate (such as standard FR-4 epoxy resin system) has many polar groups, resulting in high dielectric constant (D k ) and dielectric loss (D f ), which will cause serious high-frequency signal distortion, attenuation and heating problems, and cannot meet the stringent requirements of the new generation of communication equipment for "low loss, low delay and high fidelity". Therefore, developing a new type of high-frequency and high-speed copper clad plate resin substrate with ultra-low dielectric properties, high heat resistance and excellent processing performance has become a key technical bottleneck that needs to be broken through in the current electronic material field.

[0003] Air is the best medium with low dielectric properties (dielectric constant D k(≈1, dielectric loss is almost 0). Therefore, introducing air microporous structures into low-polarity polymer matrices is considered the most effective core strategy to break through the intrinsic dielectric limit of existing solid high-frequency substrates. In recent years, a large number of domestic patents have been used to conduct extensive research on the preparation of low-dielectric, high-performance polymer microporous materials. However, in actual industrial preparation and high-frequency copper clad laminate (CCL) applications, these traditional single systems often fall into the technical bottleneck of "dielectric properties and overall material properties being difficult to balance", facing many intractable engineering problems. For example, PPO, type II TLCP, PPS, and PS, which are used to prepare polymer microporous materials, all have inherent defects of severely insufficient heat resistance. When faced with the complex actual production applications of modern high-frequency and high-speed electronic substrates (such as having to withstand the high-temperature thermal shock of lead-free reflow soldering above 260°C), these materials are prone to thermal relaxation, thermal deformation, and insufficient heat resistance, and cannot meet the demanding application requirements of high-end copper clad laminates. In addition, there are some high-performance polymers with heat resistance and dielectric properties that meet the requirements of high-end processing applications, such as polyetheretherketone (PEEK), polybenzimidazole (PBI), and type I thermotropic liquid crystal polymers (type I TLCP). These polymers have extremely high melting points (Tm) or glass transition temperatures (Tg), which leads to excessively high processing temperatures. It is impossible to introduce air microporous structures inside through conventional supercritical fluid foaming processes, making the processing extremely difficult. Summary of the Invention

[0004] This invention provides a composite resin low-dielectric material and its preparation method, a preparation method and application of composite low-dielectric microporous material. The composite resin low-dielectric material prepared by this invention can improve the heat resistance and foaming behavior of foamed materials and reduce the processing difficulty.

[0005] This invention provides a method for preparing a composite resin low-dielectric material, comprising the following steps: The matrix resin, crosslinking agent and antioxidant are melt-blended and then crosslinked by radiation to obtain the composite resin low dielectric material. The matrix resin comprises a low-dielectric polymer and an intrinsically low-polarity resin; the dielectric constant of the low-dielectric polymer is below 3.9; the intrinsically low-polarity resin comprises acenaphthene copolymer resin and / or thermosetting polyphenylene ether; the end-capping groups of the thermosetting polyphenylene ether comprise double bonds and / or epoxy groups. The intrinsic low-polarity resin accounts for 10-90% of the mass of the matrix resin. When the end-capping groups of the thermosetting polyphenylene ether include double bonds, the mass of the crosslinking agent is 10-60% of the mass of the intrinsic low-polarity resin; When the end-capping group of the thermosetting polyphenylene ether is an epoxy group, the mass of the crosslinking agent is 0-10% of the mass of the intrinsic low-polarity resin; The temperature T of the melt blend is calculated according to equation (1).cal The T cal The glass transition temperature T is greater than that of intrinsically low polar resins. g : T cal =T D -(W) LPR ×k) Equation (1); T D The processing temperature of the low dielectric polymer is given in °C. W LPR This represents the mass fraction of the intrinsic low-polarity resin in the matrix resin. k=150; When the temperature calculated according to equation (1) is lower than the glass transition temperature T of the intrinsic low polarity resin g When the temperature of the melt blend is T g above; The irradiation dose for the irradiation crosslinking is 1~5 MGy.

[0006] Preferably, the low-dielectric polymer includes one or more of thermoplastic polyphenylene ether, type I thermotropic liquid crystal polymer, type II thermotropic liquid crystal polymer, polystyrene, polyether ether ketone, and polybenzimidazole.

[0007] Preferably, the thermosetting polyphenylene ether comprises one or more of methacrylate-terminated thermosetting polyphenylene ether, vinyl benzyl ether-terminated thermosetting polyphenylene ether, epoxy glycidyl ether-terminated thermosetting polyphenylene ether, and acrylate-terminated thermosetting polyphenylene ether.

[0008] Preferably, the crosslinking agent comprises one or more of 5,5'-(1,4-phenylenebis(methylene))bis(1,3-diallyl-1,3,5-triazine-2,4,6-trione), trimethylallyl isocyanurate, and bismaleimide.

[0009] Preferably, the antioxidant is 1.5% of the mass of the matrix resin; the antioxidant includes antioxidant 1010 and antioxidant 168; the mass ratio of antioxidant 1010 to antioxidant 168 is 1:2.

[0010] The present invention also provides a composite resin low dielectric material prepared by the preparation method described in the above technical solution.

[0011] This invention also provides a method for preparing a composite low-dielectric microporous material, characterized by comprising the following steps: The composite low-dielectric material described in the above technical solution is subjected to saturated adsorption and depressurization foaming in an environment containing a gaseous foaming agent to obtain the composite low-dielectric microporous material. The temperature at which saturation adsorption occurs is the temperature at which the melt blending occurs. The saturation adsorption time is 45~120 min.

[0012] Preferably, the saturation adsorption pressure is 10~20 MPa.

[0013] Preferably, the pressure relief foaming rate is 0.1~200MPa / s.

[0014] The present invention also provides the application of the composite low-dielectric microporous material prepared by the preparation method described above in electronic communication.

[0015] This invention modifies the dielectric properties, foaming behavior, and heat resistance of polymers by introducing intrinsically low-polarity resins. Specifically, the acenaphthene copolymer resin backbone is rich in a large-volume rigid aromatic fused-ring skeleton with an extremely high carbon-hydrogen ratio. Its active double bonds can undergo deep polymerization and crosslinking with a crosslinking agent (during radiation crosslinking), thereby constructing a highly dense, migration-resistant, and extremely low dielectric loss three-dimensional crosslinked network. Similarly, the double bonds in the thermosetting polyphenylene ether end groups can react with the crosslinking agent to construct a highly dense three-dimensional crosslinked network with extremely low dielectric loss. During radiation crosslinking, the epoxy groups in the thermosetting polyphenylene ether end groups undergo radiation-induced cationic ring-opening polymerization (the cation active centers generated by radiation excitation attack the epoxy three-membered ring, causing it to open and bond with other epoxy groups), forming a crosslinked network dominated by ether bonds (COC). The dense cross-linked network formed by the intrinsic low-polarity resin endows the material with a high glass transition temperature (Tg), excellent thermal dimensional stability and heat resistance, and this low-polarity structure enables the material to maintain extremely low dielectric constant and dielectric loss over a very wide frequency range.

[0016] For polymers such as PPO, Type II TLCP, and PS, the addition of intrinsic low-polarity resin to the system through irradiation to form a cross-linked structure can improve the melt strength of the system in the molten state, effectively suppressing cell coalescence and collapse during the foaming process, and improving the foaming performance of the material. The cross-linking of intrinsic low-polarity resin and cross-linking agent further locks the molecular chain segments, improving the mechanical properties of the material while enhancing the heat resistance of the composite system. For high-temperature engineering plastics such as Type I TLCP, PEEK, and PBI, the addition of intrinsic low-polarity resin has excellent melt plasticizing effects on these polymers, and the processing temperature of the mixed system decreases systematically with increasing amounts of both. Simultaneously, the intrinsic low-polarity resin and cross-linking agent form a dense three-dimensional network structure through irradiation cross-linking, which can further improve the foaming and mechanical properties of the system without affecting the original heat resistance of the polymer. Attached Figure Description

[0017] Figure 1 This is a scanning electron microscope image of the low-dielectric composite microporous material from Example 1; Figure 2 This is a scanning electron microscope image of the low-dielectric composite microporous material from Example 12; Figure 3 Here is a scanning electron microscope image of the low-dielectric composite microporous material in Comparative Example 2; Figure 4 Here is a scanning electron microscope image of the low-dielectric composite microporous material in Comparative Example 8; Figure 5 This is a scanning electron microscope image of the low-dielectric composite microporous material in Comparative Example 9. Detailed Implementation

[0018] This invention provides a method for preparing a composite resin low-dielectric material, comprising the following steps: The matrix resin, crosslinking agent and antioxidant are melt-blended and then crosslinked by radiation to obtain the composite resin low dielectric material. The matrix resin comprises a low-dielectric polymer and an intrinsically low-polarity resin; the dielectric constant of the low-dielectric polymer is below 3.9; the intrinsically low-polarity resin comprises acenaphthene copolymer resin and / or thermosetting polyphenylene ether; the end-capping groups of the thermosetting polyphenylene ether comprise double bonds and / or epoxy groups. The intrinsic low-polarity resin accounts for 10-90% of the mass of the matrix resin. When the end-capping groups of the thermosetting polyphenylene ether include double bonds, the mass of the crosslinking agent is 10-60% of the mass of the intrinsic low-polarity resin; When the end-capping group of the thermosetting polyphenylene ether is an epoxy group, the mass of the crosslinking agent is 0-10% of the mass of the intrinsic low-polarity resin; The temperature T of the melt blend is calculated according to equation (1). cal The T cal The glass transition temperature T is greater than that of intrinsically low polar resins. g : T cal =T D -(W) LPR ×k) Equation (1); T D The processing temperature of the low dielectric polymer is given in °C. W LPR This represents the mass fraction of the intrinsic low-polarity resin in the matrix resin. k=150; When the temperature calculated according to equation (1) is lower than the glass transition temperature T of the intrinsic low polarity resin g When the temperature of the melt blend is T g above; The irradiation dose for the irradiation crosslinking is 1~5 MGy.

[0019] In this invention, the intrinsic low-polarity resin has a mass of 10-90% of the matrix resin mass. In specific embodiments of this invention, it can be 12%, 15%, 18%, 20%, 25%, 30%, 32%, 36%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, 78%, 80%, 82%, or 85%.

[0020] In this invention, the low dielectric polymer preferably includes one or more of thermoplastic polyphenylene oxide (PPO), type I thermotropic liquid crystal polymer (type I TLCP), type II thermotropic liquid crystal polymer (type II TLCP), polystyrene (PS), polyether ether ketone (PEEK), and polybenzimidazole (PBI).

[0021] In this invention, the intrinsic low polarity resin includes acenaphthene copolymer resin and / or thermosetting polyphenylene ether; the above two resins can have foaming properties, low dielectric properties and heat resistance properties.

[0022] In this invention, the end-capping groups of the thermosetting polyphenylene ether include double bonds and / or epoxy groups. During irradiation crosslinking, the double bonds undergo crosslinking reactions with the crosslinking agent and / or with the epoxy groups themselves. Other active groups usually require thermal curing, which is not suitable for this process, and may lead to problems such as excessively high polarity resulting in an increased dielectric constant. The thermosetting polyphenylene ether preferably includes one or more of the following: methacrylate-terminated thermosetting polyphenylene ether, vinyl benzyl ether-terminated thermosetting polyphenylene ether, epoxy glycidyl ether-terminated thermosetting polyphenylene ether, and acrylate-terminated thermosetting polyphenylene ether. Methacrylate-terminated thermosetting polyphenylene ether (PPE), vinyl benzyl ether-terminated PPE, and acrylate-terminated PPE all have active double bonds at their end caps, allowing them to react with crosslinking agents to form highly dense three-dimensional crosslinked networks with extremely low dielectric loss. When epoxy glycidyl ether-terminated PPE is crosslinked by radiation, under high-energy irradiation, radiation-induced active centers are generated near the epoxy end groups in its molecular chains, promoting ring-opening reactions of the epoxy groups and forming a three-dimensional crosslinked network through free radical coupling and interchain reactions. This crosslinked structure is mainly connected by ether bonds (C–O–C), while also containing a certain proportion of C–C crosslinking bonds. The dense crosslinked network formed by crosslinking endows the material with a high glass transition temperature (Tg), excellent thermal dimensional stability and heat resistance, and this low-polarity structure allows the material to maintain extremely low dielectric constant and dielectric loss over a very wide frequency range.

[0023] If the mass of the intrinsic low-polarity resin is less than 10% of the mass of the low-dielectric polymer, it cannot effectively improve the temperature resistance, mechanical properties, and foaming properties of PS, PPO, and Type II TLCP systems; and it cannot effectively reduce the processing temperature of PBI, PEEK, and Type I TLCP systems, making processing too difficult. If it is higher than 90%, it will reduce the toughness of PS, PPO, and Type II TLCP systems, significantly reducing mechanical and foaming properties; and it will reduce the excellent heat resistance provided by high-temperature engineering plastics to the system, as well as the toughness, mechanical properties, and foaming properties.

[0024] In this invention, when the end-capping groups of the thermosetting polyphenylene ether include double bonds, the mass of the crosslinking agent is 10-60% of the mass of the intrinsic low-polarity resin; the mass of the crosslinking agent being 10-60% of the mass of the intrinsic low-polarity resin can be 12%, 15%, 18%, 20%, 25%, 30%, 32%, 36%, 40%, 42%, 45%, 48%, 50%, 52%, or 55% in specific embodiments of this invention; when the end-capping groups of the thermosetting polyphenylene ether are epoxy groups... When the crosslinking agent is used, the mass of the crosslinking agent is 0-10% of the intrinsic low polarity resin mass, and in specific embodiments of the present invention, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%; the crosslinking agent preferably includes one or more of 5,5'-(1,4-phenylenebis(methylene))bis(1,3-diallyl-1,3,5-triazine-2,4,6-trione) (JN891), trimethylallyl isocyanurate (TMAIC) and bismaleimide (BMI).

[0025] If the mass of the crosslinking agent is less than 10% of the mass of the intrinsic low-polarity resin, the crosslinking density of the system will be insufficient, and a dense three-dimensional network cannot be constructed to effectively improve the mechanical strength, heat resistance and thermal dimensional stability of the material. If it is higher than 60%, it will not only lead to excessive local crosslinking and reduce the toughness of the substrate, but also introduce polar defects due to the unreacted residual crosslinking agent monomers, thereby increasing the dielectric properties of the system.

[0026] In this invention, the antioxidant is preferably 1.5% of the mass of the matrix resin; the antioxidant preferably includes antioxidant 1010 and antioxidant 168; the mass ratio of antioxidant 1010 to antioxidant 168 is preferably 1:2.

[0027] The present invention calculates the melt blending temperature T according to formula (1). cal The T cal The glass transition temperature T is greater than that of intrinsically low polar resins. g : Tcal =T D -(W) LPR ×k) Equation (1); T D The processing temperature of the low dielectric polymer is given in °C (based on the processing temperatures commonly used for each resin in practical applications, PPO is 280~310 °C, PEEK is 360~400 °C, PBI is 440~460 °C, Type I TLCP is 370~410 °C, and Type II TLCP is 290~340 °C. When the amount of intrinsic low polarity resin added is 50 wt%, it is calculated according to formula (1): when the low dielectric polymer is PPO, the melt blending temperature is 205~235 °C; when the low dielectric polymer is PEEK, the melt blending temperature is 285~325 °C; when the low dielectric polymer is PBI, the melt blending temperature is 365~385 °C; when the low dielectric polymer is Type I TLCP, the melt blending temperature is 295~335 °C; and when the low dielectric polymer is Type II TLCP, the melt blending temperature is 215~265 °C). W LPR This represents the mass fraction of the intrinsic low-polarity resin in the matrix resin. k=150; k is a specific plasticizing efficiency coefficient limited by the temperature difference between the two phase transition temperatures.

[0028] When the temperature calculated according to equation (1) is lower than the glass transition temperature T of the intrinsic low polarity resin g When the temperature of the melt blend is T g The above. Specifically, the processing temperature of PS is 100~120℃. When the amount of intrinsic low polarity resin added is 50 wt%, according to formula (1), the processing temperature of melt blending is 25~45℃, which is less than the glass transition temperature Tg of PS. Therefore, the temperature of melt blending is above the glass transition temperature Tg.

[0029] Acenamel copolymer resins or thermosetting PPOs can significantly plasticize thermoplastic PPO, PEEK, PBI, Type I TLCP, and Type II TLCP, thereby greatly reducing their processing temperature. As the content of acenamel copolymer resins or thermosetting PPO gradually increases, the processing temperature of this blend system shows a regular decreasing trend.

[0030] After melt blending and before radiation crosslinking, the present invention preferably compresses the resulting blend; the compressing temperature is preferably the melt blending temperature.

[0031] In this invention, the irradiation dose for crosslinking is 1-5 MGy, and in specific embodiments, it can be 2 MGy, 3 MGy, or 4 MGy. During the irradiation crosslinking process, the matrix resin segments are further excited to form a three-dimensional crosslinked network structure. During the irradiation crosslinking process, low-dielectric polymers do not undergo crosslinking reactions; only intrinsically low-polarity resins undergo crosslinking reactions. If the irradiation dose is too low, the crosslinking density is insufficient, and the melt strength is insufficient to support pore nucleation; if the irradiation dose is too high, the polymer backbone undergoes irreversible radiation degradation and chain breakage, the mechanical properties of the matrix are degraded, and the foaming effect is severely deteriorated.

[0032] This invention also provides a method for preparing a composite low-dielectric microporous material, comprising the following steps: The composite resin low-dielectric material prepared by the preparation method described above is subjected to saturated adsorption and depressurization foaming in an environment containing a gaseous foaming agent to obtain the composite low-dielectric microporous material. The temperature at which saturation adsorption occurs is the temperature at which the melt blending occurs. The saturation adsorption time is 45~120 min.

[0033] In this invention, the gaseous foaming agent preferably includes one or more of CO2, N2, methanol and butane.

[0034] In this invention, the saturation adsorption temperature is the melt blending temperature, and the saturation adsorption pressure is preferably 10-20 MPa, which can be 11 MPa, 12 MPa, 13 MPa, 14 MPa, 15 MPa, 16 MPa, 17 MPa, 18 MPa or 19 MPa in specific embodiments of this invention; the saturation adsorption time is preferably 45-120 min, which can be 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min, 100 min, 105 min, 110 min or 115 min in specific embodiments of this invention.

[0035] In this invention, the pressure relief foaming rate is preferably 0.1~200 MPa / s, and in specific embodiments of this invention, it can be 10MPa / s, 20MPa / s, 30MPa / s, 40MPa / s, 50MPa / s, 60MPa / s, 70MPa / s, 80MPa / s, 90MPa / s, 100MPa / s, 110MPa / s, 120MPa / s, 130MPa / s, 140MPa / s, 150MPa / s, 160MPa / s, 170MPa / s, 180MPa / s, or 190MPa / s.

[0036] After the pressure relief foaming, the present invention preferably involves placing the reaction vessel used for saturated adsorption and pressure relief foaming in water for cooling until the foam cells are fixed.

[0037] This invention also provides the application of the composite low-dielectric microporous material prepared by the preparation method described above in electronic communications. Specifically, the composite low-dielectric microporous material is used in high-frequency, high-speed copper-clad laminates.

[0038] The following detailed description, in conjunction with embodiments, illustrates the composite resin low-dielectric material and its preparation method, the preparation method of the composite low-dielectric microporous material, and their applications. However, these descriptions should not be construed as limiting the scope of protection of this invention.

[0039] The intrinsic glass transition temperature T of the acenaphthene copolymer resin (EXP-Y60) used in the examples and comparative examples g The intrinsic glass transition temperature T of methacrylate-terminated thermosetting PPO (SABIC NORYL™ SA9000) is 150℃. g The intrinsic glass transition temperature T of vinyl benzyl ether-terminated thermosetting PPO (OPE-2St 2200) is approximately 160℃. g The intrinsic glass transition temperature T of epoxy glycidyl ether-terminated thermosetting PPO (OPE-2GE) is approximately 145 °C. g The intrinsic glass transition temperature T of acrylate-terminated thermosetting PPO (OPE-2EA) is approximately 140 °C. g The glass transition temperature T of PPO (LXN040) is approximately 150 °C. g The melting point T of type I TLCP (PRET Z370) is 210 °C. m The melting point T of type II TLCP (PRET K280G) is 370 °C. m The glass transition temperature T of PBI (KM-PBI U60) is 280℃. g The melting point T of PEEK (VIctrex 450G) is 425 °C. m The glass transition temperature T of PS (PG-383) is 343 °C. g The temperature is 100℃.

[0040] Processing temperature: 280~310℃ for PPO (LXN040), 360~400℃ for PEEK, 440~460℃ for PBI, 370~410℃ for Type I TLCP, 290~340℃ for Type II TLCP, and 100~120℃ for PS.

[0041] In the examples and comparative systems, when the low-dielectric polymers are PPO, PEEK, PBI, type II TLCP, and type II TLCP, the blending and hot-pressing temperatures, and the saturation adsorption temperature are determined by the formula (1) mentioned above. When the low-dielectric polymer in the system is PS, due to its glass transition temperature T... g Lower, with intrinsically low polarity resins having a lower T g The system's blending and hot-pressing temperatures and saturated adsorption temperatures were determined based on this benchmark.

[0042] Example 1 A torque rheometer was used to mix acenaphthene copolymer resin (50 wt%) and PPO (50 wt%) as matrix resins, with the addition of 10 wt% JN891, 0.5 wt% antioxidant 1010, and 1 wt% antioxidant 168, respectively. The program settings were fixed at 220 °C, 5 min, and 60 rpm to obtain an acenaphthene copolymer resin / PPO / JN891 composite material. This material was then pressed into 50 mm × 10 mm × 4 mm strips using a hot press at 220 °C. The samples were irradiated with 2 MGy and used in subsequent foaming processes.

[0043] After heating the high-pressure foaming equipment to the foaming temperature, the sample to be foamed is placed in the high-pressure foaming equipment, and the air in the equipment is replaced by CO2 purging. CO2 is added to the reactor to a pressure of 15 MPa through a pressurizing device, and saturation adsorption is carried out in a CO2 atmosphere at 220 °C for 1 h.

[0044] The pressure was rapidly released at a rate of 200 MPa / s, and the reactor was placed in water to cool until the cells were fixed, thus obtaining a microporous acenaphthene copolymer resin composite material.

[0045] Examples 2-24 The differences from Example 1 are shown in Table 1; all other aspects are the same as in Example 1. (The amount of crosslinking agent added is based on the intrinsic low-polarity resin content; the amount of low-dielectric polymer is: 100% - the mass content of the intrinsic low-polarity resin.) Table 1. Differences between Examples 2-24 and Example 1

[0046] The following comparative examples are all used for comparison with Example 1. Comparative Example 1 A torque rheometer was used to mix acenaphthene copolymer resin (50 wt%) and PPO (50 wt%) as matrix resins, with the addition of 10 wt% JN891, 0.5 wt% antioxidant 1010, and 1 wt% antioxidant 168, respectively. The program settings were fixed at 220 °C, 5 min, and 60 rpm to obtain an acenaphthene copolymer resin / PPO / JN891 composite material. This material was then pressed into 50 mm × 10 mm × 4 mm strips using a hot press at 220 °C. The samples were irradiated with 2 MGy and used in subsequent foaming processes.

[0047] After heating the high-pressure foaming equipment to the foaming temperature, the sample to be foamed is placed in the high-pressure foaming equipment, and the air in the equipment is replaced by CO2 purging. CO2 is added to the reactor to a pressure of 15 MPa through a pressurizing device, and saturation adsorption is carried out in a CO2 atmosphere at 260 °C for 1 hour.

[0048] The pressure was rapidly released at a rate of 200 MPa / s, and the reactor was placed in water to cool until the cells were fixed, thus obtaining a microporous acenaphthene copolymer resin composite material.

[0049] Comparative Examples 2-15 The differences from Comparative Example 1 are shown in Table 2; all other aspects are the same as Comparative Example 1. (Crosslinking agent addition amount / wt% (based on additive content)) Table 2. Differences between Comparative Examples 2-15 and Comparative Example 1

[0050] Heat distortion temperature tests were performed on the samples from Examples 1-23 and Comparative Examples 1-15 before foaming treatment, and mechanical tests were performed on the samples after foaming treatment. A universal testing machine was used to test the compression modulus at a compression rate of 2 mm / min. The apparent density of the intrinsic low-polarity resin composite material was determined using an analytical balance with an attached density component, and the foaming ratio was calculated. The foamed product was quenched using liquid nitrogen, gold was sprayed onto the cross section, and the cell structure was measured and analyzed using a scanning electron microscope. The dielectric constant and dielectric loss of intrinsic low-polarity resin composite materials before and after foaming were tested using a network analyzer and a resonant cavity. The experimental results are recorded in Table 3.

[0051] Table 3. Experimental results of the foamed products obtained in Examples 1-24 and Comparative Examples 1-15

[0052] SEM analysis was performed on the intrinsic low-polarity resin composite microporous materials prepared in Examples 1, 12, 2, 8, and 9. The results are as follows: Figures 1-5 As shown.

[0053] in: Figure 1 This is a scanning electron microscope image of the low-dielectric composite microporous material from Example 1; Figure 2 This is a scanning electron microscope image of the low-dielectric composite microporous material from Example 12; Figure 3 Here is a scanning electron microscope image of the low-dielectric composite microporous material in Comparative Example 2; Figure 4 Here is a scanning electron microscope image of the low-dielectric composite microporous material in Comparative Example 8; Figure 5 This is a scanning electron microscope image of the low-dielectric composite microporous material in Comparative Example 9.

[0054] From Table 3 and Figures 1-5 It can be seen that the intrinsic low-polarity resin composite microporous materials prepared using Examples 1-23 of the present invention not only have controllable foaming ratio and uniform cell structure, but also excellent mechanical and dielectric properties. Example 1 controlled the optimal modified formulation ratio and modification process, determined the optimal foaming conditions, and the resulting intrinsic low-polarity resin composite material and corresponding intrinsic low-polarity resin composite microporous material have the best comprehensive performance. In Comparative Example 1, the saturation adsorption temperature was too high, causing cell merging and collapse, which affected the foaming ratio. Comparative Example 2 was not irradiated, and the acenaphthene copolymer resin did not undergo deep cross-linking between chain segments, resulting in a decrease in heat resistance. This led to insufficient strength of the melt during foaming, and severe cell coalescence and collapse. Comparative Example 3 did not add low dielectric polymers such as PPO and PEEK to the matrix resin system. The cross-linking network of the pure acenaphthene copolymer resin had excessive hardness and reduced toughness, lacking buffer toughness. The sample could not withstand the stress of high-pressure gas expansion, resulting in sample pulverization and failure to foam successfully. In Comparative Example 4, no crosslinking agent was added. Deep crosslinking did not occur between the segments of the acenaphthene copolymer resin, resulting in decreased heat resistance and insufficient melt viscoelastic strength to support cell growth. This led to a significant decrease in the foaming ratio, and the material failed to achieve the expected lightweighting. Furthermore, the dielectric constant was too high after foaming. The irradiation dose of Comparative Example 5 was too high, and the proportion of broken chains in the system structure was greater than the degree of crosslinking, which weakened the mechanical strength and heat resistance of the matrix and deteriorated the foaming effect. The irradiation dose of Comparative Example 6 was too low, the cross-linking of the system was insufficient, the heat resistance decreased, the cells ruptured and collapsed, the foaming ratio was too small, and the cell size was too large. The amount of crosslinking agent added in Comparative Example 7 was too high, resulting in excessive local crosslinking, which weakened the intrinsic low dielectric properties of the system and limited the growth of the foam cells, causing the dielectric constant to increase after foaming and the expansion ratio to be too small. The amount of crosslinking agent added in Comparative Example 8 was too low, resulting in low crosslinking density of the system, insufficient melt strength and heat resistance, which led to cell rupture and collapse, reduced foaming ratio, and larger cell size. The blending and hot-pressing temperature of Comparative Example 9 was too high. This caused premature thermal polymerization of the double bonds in the crosslinking agent (scorching phenomenon), resulting in excessive crosslinking in some parts of the system. The melt viscosity increased sharply and even partially solidified. The melt toughness was extremely low, causing it to lose its elastic deformation ability. As a result, the melt could not support the expansion stress of the pores during depressurization, leading to severe rupture and collapse of the cells and an extremely low foaming ratio. The blending and hot-pressing temperature of Comparative Example 10 was too low, and PPO could not fully enter the viscous flow state, resulting in insufficient mixing of the two-phase resins and uneven dispersion of the crosslinking agent. This led to local over-crosslinking, which reduced the mechanical properties and heat resistance of the system, and the foaming ratio was extremely low, failing to form a good microporous network structure. The saturation adsorption temperature of Comparative Example 11 was too low, the matrix was not sufficiently softened, the growth of the foam cells was restricted, resulting in a low foaming ratio. The saturation adsorption time of Comparative Example 12 was too short. This resulted in insufficient dissolution and penetration of CO2 into the matrix, insufficient driving force for nucleation and growth, leading to inadequate foaming, a low foaming ratio, and a high dielectric constant after foaming. The excessive addition of intrinsically low-polarity resin (acenaphthene copolymer resin) in Comparative Example 13 led to a phase inversion in the system. The lack of viscoelastic framework support from the low-dielectric polymer (PPO) backbone resulted in decreased material toughness. During the foaming and depressurization stage, the system lost the elastic deformation capacity required to buffer the expansion stress of high-pressure gas, causing the cells to easily rupture and collapse, resulting in a significant decrease in the foaming ratio and the inability to form a uniform and complete microporous structure. The amount of intrinsic low polarity resin added in Comparative Example 14 was too low, which resulted in the system being unable to form a sufficiently dense three-dimensional cross-linking network with the cross-linking agent during the irradiation cross-linking stage. The improvement in heat resistance was not significant, the improvement in melt strength was limited, and it could not effectively support the expansion stress of the pores during foaming and depressurization, which in turn caused the pores to rupture and collapse, and the foaming ratio to drop significantly. Comparative Example 15 did not contain the intrinsic low-polarity resin. The matrix resin lacked the plasticizing, viscosity-reducing, and cross-linking modification effects brought by this additive, resulting in an insignificant reduction in the processing temperature of the system, unsatisfactory mixing effect, uneven blending, decreased heat resistance, and easy cell rupture and collapse during foaming, leading to a low foaming ratio.

[0055] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a composite resin low-dielectric material, characterized in that, Includes the following steps: The matrix resin, crosslinking agent and antioxidant are melt-blended and then crosslinked by radiation to obtain the composite resin low dielectric material. The matrix resin comprises a low-dielectric polymer and an intrinsically low-polarity resin; the dielectric constant of the low-dielectric polymer is below 3.9; the intrinsically low-polarity resin comprises acenaphthene copolymer resin and / or thermosetting polyphenylene ether; the end-capping groups of the thermosetting polyphenylene ether comprise double bonds and / or epoxy groups. The intrinsic low-polarity resin accounts for 10-90% of the mass of the matrix resin. When the end-capping groups of the thermosetting polyphenylene ether include double bonds, the mass of the crosslinking agent is 10-60% of the mass of the intrinsic low-polarity resin; When the end-capping group of the thermosetting polyphenylene ether is an epoxy group, the mass of the crosslinking agent is 0-10% of the mass of the intrinsic low polarity resin; The temperature T of the melt blend is calculated according to equation (1). cal The T cal The glass transition temperature T is greater than that of intrinsically low polar resins. g : T cal =T D -(W) LPR ×k) Equation (1); T D The processing temperature of the low dielectric polymer is given in °C. W LPR This represents the mass fraction of the intrinsic low-polarity resin in the matrix resin. k=150; When the temperature calculated according to equation (1) is lower than the glass transition temperature T of the intrinsic low polarity resin g When the temperature of the melt blend is T g above; The irradiation dose for the irradiation crosslinking is 1~5 MGy.

2. The preparation method according to claim 1, characterized in that, The low-dielectric polymer includes one or more of thermoplastic polyphenylene ether, type I thermotropic liquid crystal polymer, type II thermotropic liquid crystal polymer, polystyrene, polyether ether ketone, and polybenzimidazole.

3. The preparation method according to claim 1, characterized in that, The thermosetting polyphenylene ether includes one or more of the following: methacrylate-terminated thermosetting polyphenylene ether, vinyl benzyl ether-terminated thermosetting polyphenylene ether, epoxy glycidyl ether-terminated thermosetting polyphenylene ether, and acrylate-terminated thermosetting polyphenylene ether.

4. The preparation method according to claim 1, characterized in that, The crosslinking agent includes one or more of 5,5'-(1,4-phenylenebis(methylene))bis(1,3-diallyl-1,3,5-triazine-2,4,6-trione), trimethylallyl isocyanurate, and bismaleimide.

5. The preparation method according to claim 1, characterized in that, The antioxidant is 1.5% of the matrix resin by mass; the antioxidant includes antioxidant 1010 and antioxidant 168; the mass ratio of antioxidant 1010 to antioxidant 168 is 1:

2.

6. The composite resin low-dielectric material prepared by the preparation method according to any one of claims 1 to 5.

7. A method for preparing a composite low-dielectric microporous material, characterized in that, Includes the following steps: The composite resin low dielectric material of claim 6 is subjected to saturated adsorption and depressurization foaming in an environment containing a gaseous foaming agent to obtain the composite low dielectric microporous material. The temperature at which saturation adsorption occurs is the temperature at which the melt blending occurs. The saturation adsorption time is 45~120 min.

8. The preparation method according to claim 7, characterized in that, The pressure for saturated adsorption is 10~20 MPa.

9. The preparation method according to claim 7, characterized in that, The pressure relief foaming rate is 0.1~200MPa / s.

10. The application of the composite low-dielectric microporous material prepared by the preparation method according to any one of claims 7 to 9 in electronic communication.