A pi aerogel thermal runaway blocking film and a preparation method thereof
By constructing a PI aerogel thermal runaway blocking membrane with a three-dimensional network structure of polyimide nanofibers, the problem of structural failure of lithium battery separators at high temperatures was solved. This membrane maintained the integrity of the solid structure at 300℃, preventing thermal runaway and improving the safety and reliability of lithium batteries.
Patent Information
- Application Number
- CN202611338556.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium battery separator materials lose their structural integrity under extreme high-temperature conditions, leading to the failure of their physical isolation function and making it impossible to effectively prevent thermal runaway chain reactions.
A PI aerogel thermal runaway blocking membrane with a three-dimensional continuous network structure composed of polyimide nanofibers is used. By controlling the fiber diameter, pore size, porosity and thickness, combined with a stepped heating thermal imidization process, the material can maintain its structural integrity and excellent mechanical strength at high temperatures.
Maintaining a solid structure at 300℃ blocks short circuits between the positive and negative electrodes, prevents thermal runaway from spreading, and improves the safety and reliability of lithium batteries under extreme conditions.
Smart Images

Figure CN123152162A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery safety functional materials technology, and in particular to a PI aerogel thermal runaway blocking membrane and its preparation method. Background Technology
[0002] Lithium-ion batteries, as a core component of modern energy storage, are widely used in electric vehicles, consumer electronics, and energy storage power stations. Their safety is directly related to the reliability of end products and the safety of users' lives and property. In the existing lithium-ion battery manufacturing system, the separator is a key component to prevent direct contact and short circuits between the positive and negative electrodes. The mainstream technical solution usually adopts a composite structure of polyolefin-based membrane (such as polyethylene or polypropylene) coated with inorganic ceramic particles. This technical approach utilizes the closed-cell effect of the polyolefin-based membrane at specific temperatures to cut off the ion flow, while relying on the ceramic coating to provide a certain degree of heat resistance support to meet the electrochemical performance and basic safety requirements of the battery under normal operating conditions.
[0003] However, with the continuous improvement of battery energy density and the increasing complexity of application scenarios, existing separator materials face severe challenges in dealing with extreme thermal abuse conditions. When thermal runaway occurs inside the battery, causing a sharp rise in temperature that exceeds the melting point of the polyolefin-based membrane, traditional composite separator structures often fail to maintain their complete physical morphology, leading to the failure of their physical isolation function. This loss of structural integrity under high-temperature conditions makes the battery highly susceptible to large-area short circuits, further exacerbating heat propagation and becoming a long-term technical bottleneck restricting the further improvement of the safety performance of high-energy-density lithium batteries. How to maintain an effective physical isolation barrier under extreme high-temperature conditions and prevent thermal runaway chain reactions is a key problem that urgently needs to be solved in this field. Summary of the Invention
[0004] The purpose of this invention is to provide a PI aerogel thermal runaway blocking membrane and its preparation method, which can solve the technical problem that existing membrane materials lose structural integrity under extreme high temperature conditions, leading to the failure of physical isolation function.
[0005] The first aspect of this application provides a PI aerogel thermal runaway blocking membrane, which is composed of a three-dimensional continuous network structure of polyimide nanofibers; the diameter of the PI nanofibers is 20-50 nm; the average pore size of the blocking membrane is 10-80 nm, the porosity is 70-85%, and the open porosity is greater than 99%; the blocking membrane is an independently formed solid structure with a thickness of 10-25 μm; the thermal shrinkage rate of the blocking membrane is less than 2% after being kept at 300°C for 30 minutes, and the solid structure remains intact under this condition.
[0006] The polyimide nanofibers are generated by polycondensation of pyromellitic dianhydride and diaminodiphenyl ether at a molar ratio of 1:1.00±0.02, and the imidization rate of the polyimide is ≥99.5%.
[0007] Wherein, the volume resistivity of the blocking membrane is >10. 12 Ω·cm, dielectric strength >50kV / mm, electrochemical stability window is 0-4.8V vsLi + / Li.
[0008] The contact angle of the blocking membrane with the 1M LiPF6EC / DMC electrolyte is ≤10°, and the electrolyte absorption rate is ≥300%.
[0009] The barrier membrane has a dry tensile strength ≥50MPa and a wet tensile strength ≥35MPa after immersion in the electrolyte for 24 hours; its dry puncture strength ≥600gf and its wet puncture strength ≥400gf after immersion in the same electrolyte for 24 hours.
[0010] The second aspect of this application provides a method for preparing a PI aerogel thermal runaway blocking membrane, applicable to the preparation of a PI aerogel thermal runaway blocking membrane as described in any one of the above claims, comprising the following steps: S1 Preparation of polyamic acid precursor solution: Under nitrogen protection and with a dew point ≤ -40℃, diaminodiphenyl ether is dissolved in N,N-dimethylacetamide, and pyromellitic dianhydride is added in batches in an equimolar ratio with diaminodiphenyl ether to carry out a polycondensation reaction. The feeding rate is controlled so that the reaction temperature does not exceed 10℃. After the feeding is completed, stirring is continued for 2-6 hours to obtain a polyamic acid solution; S2 wet film casting: After degassing the polyamic acid solution, it is cast onto the surface of a moving steel belt or PET release film through a slit extrusion coating head to form a polyamic acid wet film. S3 Solvent replacement: The polyamic acid wet film is sequentially immersed in ethanol / water solutions with decreasing concentration gradients for replacement until the residual amount of N,N-dimethylacetamide in the film is <0.1%, thus obtaining a polyamic acid hydrogel film; S4 Atmospheric pressure drying: The polyamic acid hydrogel membrane is dried at atmospheric pressure at 20-80℃ with a heating rate of 1-5℃ / min until the water content is <5%, to obtain a polyamic acid aerogel membrane. S5 Thermal imidization: Under nitrogen protection and with an O2 content of <50ppm, the polyamic acid aerogel membrane is subjected to micro-tension and thermal imidization treatment with step-up temperature increase to obtain the PI aerogel thermal runaway blocking membrane.
[0011] In step S1, triaminobenzene is added to the polyamic acid solution at a concentration of 0.5-1.0 wt% relative to the solid content of polyamic acid as a crosslinking agent.
[0012] In step S3, the concentration gradient of ethanol / water solution is as follows: 100% ethanol, 75% ethanol, 50% ethanol, 25% ethanol and pure water, with each gradient soaking time being 20-40 minutes.
[0013] In step S5, the stepwise heating thermal imidization process is as follows: First stage: heating to 80-120℃ at a heating rate of 5℃ / min and holding for 10-15 minutes; Second stage: heating to 150-200℃ at a heating rate of 2-3℃ / min and holding for 20-30 minutes; Third stage: heating to 250-300℃ at a heating rate of 2℃ / min and holding for 30-45 minutes; Fourth stage: heating to 350℃ at a heating rate of 5℃ / min and holding for 10-15 minutes.
[0014] This application provides a PI aerogel thermal runaway blocking membrane and its preparation method. This method constructs a three-dimensional continuous network structure composed of interwoven polyimide nanofibers within a specific diameter range. The strong charge transfer and recombination between polyimide molecular chains endows the material with extremely high thermal stability, resulting in a microscopically controlled, highly porous, and well-connected open-cell system with controllable average pore size. Furthermore, by precisely controlling the fiber diameter, pore size distribution, and overall thickness, combined with an independently formed solid-state structure design, the risk of melting and collapse at high temperatures, common in traditional base films, is effectively avoided. Through a stepped-heating thermal imidization process and strict control of component molar ratios, the dimensional stability and structural integrity of the material are further ensured during prolonged heating at 300℃, thus achieving the goal of maintaining excellent mechanical strength and electrochemical performance under high-temperature conditions. Therefore, this solution effectively solves the technical problem of the loss of structural integrity of existing separator materials under extreme high temperature conditions, which leads to the failure of physical isolation function. Thus, it avoids the positive and negative large area short circuits and thermal runaway chain diffusion caused by the melting and shrinkage of the separator, and significantly improves the operational safety and reliability of lithium batteries under extreme conditions. Attached Figure Description
[0015] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0016] Figure 1 A flowchart illustrating the preparation method of a PI aerogel thermal runaway blocking membrane provided in this application. Detailed Implementation
[0017] The embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.
[0018] First embodiment: This embodiment provides a PI aerogel thermal runaway blocking membrane, which is composed of a three-dimensional continuous network structure made of polyimide nanofibers. Polyimide (PI), as a special engineering plastic containing imide rings in its main chain, possesses excellent high-temperature resistance and mechanical properties. The nanofibers, prepared through processes such as electrospinning, overlap and entangle with each other, undergoing physical fusion or chemical bonding at the fiber nodes, thereby constructing a self-supporting three-dimensional continuous network framework. This three-dimensional network structure not only provides the necessary mechanical strength for the blocking membrane to withstand the winding pressure during battery assembly but also creates numerous pore spaces, providing channels for lithium ion transport.
[0019] Specifically, the raw materials for this scheme are shown in Table 1: Table 1
[0020] The fiber distribution in this network structure can be either isotropic random arrangement or ordered arrangement with a certain degree of orientation, depending on the fiber collection method during the preparation process. This application does not impose any special limitations on this. The diameter of the PI nanofibers is 20-50 nm; specifically, the diameter of the nanofibers directly affects the specific surface area and pore size distribution of the blocking membrane. When the fiber diameter is within the nanoscale of 20-50 nm, a microscale pore structure can be effectively constructed while maintaining the high flexibility and high strength of the fiber itself. If the diameter is too large, it may lead to a decrease in the porosity of the membrane material or a decrease in flexibility; if the diameter is too small, it may increase the difficulty of preparation and lead to insufficient mechanical properties. In this embodiment, by adjusting parameters such as the viscosity of the spinning solution, the electrospinning voltage, and the receiving distance, the fiber diameter can be controlled to fall within the above range, for example, it can be a specific value such as 30 nm or 40 nm, so as to achieve precise control of the microstructure.
[0021] The average pore size of the blocking membrane is 10-80 nm, the porosity is 70-85%, and the open porosity is greater than 99%, as shown in Table 2. Table 2
[0022] In this structure, the average pore size can refer to the statistical average of the equivalent diameters of the pores within the blocking membrane. Controlling the average pore size within the range of 10-80 nm is to achieve a balance between physically preventing lithium dendrite penetration and allowing electrolyte molecules and lithium ions to pass freely. Porosity is defined as the ratio of pore volume to the total volume of the membrane material, and its calculation formula can be expressed as:
[0023] in, Indicates porosity. It represents the total volume of pores in a membrane material. This refers to the total volume of the membrane material. A high porosity of 70%-85% means that most of the space inside the membrane is vacant, which is beneficial for electrolyte wetting and storage, thereby reducing the battery's internal resistance. Porosity refers to the proportion of interconnected pore volume to the total pore volume. A porosity greater than 99% indicates that the membrane's internal pores are almost entirely open-cell structures, with no or only a very small number of closed pores. This high open-cell characteristic ensures unobstructed ion transport pathways, avoiding ion transport dead zones caused by closed-cell structures, thus guaranteeing the battery's high-rate charge-discharge performance.
[0024] The blocking membrane is an independently formed solid structure with a thickness of 10-25 μm. This independently formed solid structure means that the blocking membrane exists independently of other substrates (such as polyethylene (PE) or polypropylene (PP) microporous membranes), possessing its own complete mechanical morphology and self-supporting properties. This allows it to completely replace the traditional base membrane support layer, fundamentally avoiding structural collapse caused by base membrane melting. The 10-25 μm thickness design balances the requirements of mechanical strength and battery energy density. An excessively thick membrane increases the ineffective volume inside the battery, reducing energy density; while an excessively thin membrane may pose a risk of insufficient mechanical strength. For example, the thickness can be 12 μm, 18 μm, or 22 μm, with the specific value set according to the actual safety redundancy requirements of the battery system.
[0025] Thermodynamic properties are shown in Table 3: Table 3
[0026] The barrier membrane exhibits a thermal shrinkage rate of less than 2% after being held at 300°C for 30 minutes, while maintaining its solid structure integrity under these conditions. In this performance indicator, the thermal shrinkage rate reflects the dimensional stability of the material under high-temperature conditions, and its calculation formula can be expressed as:
[0027] in, Indicates the thermal shrinkage rate. This indicates the initial length of the blocking membrane before heating. This indicates the length of the barrier film after heating. A thermal shrinkage rate of less than 2% indicates that the material undergoes almost no dimensional deformation at 300°C. This is because the polyimide molecular chain has extremely high rigidity and thermal stability; its glass transition temperature is typically much higher than 300°C. Therefore, at high temperatures, the movement of the molecular chain is restricted, preventing melting and shrinkage like that of PE separators. Maintaining the integrity of the solid structure means that under these extreme conditions, the barrier film does not soften, melt, or rupture, and can continuously maintain its physical isolation function, effectively blocking direct contact between the positive and negative electrodes, thereby preventing further diffusion of thermal runaway.
[0028] The core innovation of this application lies in the construction of a three-dimensional continuous network aerogel membrane structure entirely composed of self-supporting polyimide nanofibers. This innovation abandons the traditional composite structure of ceramic-coated membranes that rely on an organic base membrane (such as PE / PP) to support inorganic particles. Instead, it utilizes the intrinsic heat resistance of PI material itself, combined with the high specific surface area and high porosity characteristics of nanofibers, to directly form an independent solid membrane layer that does not melt or shrink at high temperatures. By precisely controlling microstructural parameters such as fiber diameter, pore size, porosity, and open porosity, the synergistic optimization of the material's microscopic physical structure and macroscopic thermomechanical properties is achieved, solving the problem of overall structural collapse of existing membranes due to base membrane failure at high temperatures.
[0029] The working process and principle of this application are as follows: Under the normal operating temperature of a lithium battery, the PI aerogel barrier membrane, with its high porosity of 70-85% and open porosity of over 99%, adsorbs and retains a large amount of electrolyte, forming interconnected ion transport channels. This allows lithium ions to migrate freely between the positive and negative electrodes, maintaining the normal electrochemical reaction of the battery. When an abnormal temperature rise occurs inside the battery, reaching or exceeding 300°C and entering the early stage of thermal runaway, traditional PE / PP separators will experience severe thermal shrinkage or even melt due to reaching their melting point, leading to a direct short circuit between the positive and negative electrodes. At this time, the barrier membrane of this application, due to the high rigidity of the polyimide molecular chains and strong intermolecular forces, has a glass transition temperature much higher than the current ambient temperature, preventing significant conformational changes in the molecular chains. Therefore, the barrier membrane can maintain its solid structure integrity at 300°C, with a very small thermal shrinkage rate (less than 2%), and can continue to maintain its three-dimensional network framework physical morphology. This complete three-dimensional network skeleton acts as a robust physical barrier, physically isolating the positive and negative electrodes, blocking the formation of internal short-circuit loops, thereby cutting off the heat and mass transfer chain of the thermal runaway reaction and preventing the spread of thermal runaway.
[0030] Through the above technical solution, this application achieves the following beneficial effects: Due to the adoption of a three-dimensional continuous network structure composed of polyimide nanofibers, and the limitation of the PI nanofiber diameter to 20-50 nm, this microstructure endows the blocking membrane with extremely high specific surface area and porosity, thereby ensuring high electrolyte wettability and high ion mobility, and reducing battery internal resistance. Since the average pore size of the blocking membrane is 10-80 nm, the porosity is 70-85%, and the open porosity is greater than 99%, this highly open-pore interconnected pore structure eliminates resistance to ion transport and effectively blocks the penetration of tiny electrode particles or dendrites, improving the battery's cycle safety. Because the blocking membrane is an independently formed solid structure with a thickness of 10-25 μm, this design completely eliminates the dependence on low-melting-point organic base films, fundamentally eliminating the risk of structural failure caused by base film melting. At the same time, the reasonable thickness design balances the battery's energy density and mechanical strength. Because the thermal shrinkage rate of the barrier film is less than 2% after 30 minutes at 300°C and it maintains the integrity of its solid structure under these conditions, the film can maintain dimensional and structural stability under thermal runaway high-temperature environments without melting or rupture, thanks to the excellent thermal stability of polyimide material. This provides reliable physical isolation at critical moments, effectively prevents short circuits between the positive and negative electrodes, suppresses the chain reaction of thermal runaway, and significantly improves the safety level of lithium-ion batteries under extreme conditions.
[0031] Polyimide is produced by polycondensation of pyromellitic dianhydride and diaminodiphenyl ether at a molar ratio of 1:1.00±0.02, with an imidization rate of ≥99.5%. This precise stoichiometric control aims to ensure sufficient reaction between the dianhydride and diamine monomers during the polymerization process, thereby obtaining a high molecular weight, structurally regular polyamic acid precursor. The purity of pyromellitic dianhydride and diaminodiphenyl ether, as reactant monomers, is crucial to the performance of the final barrier membrane, typically requiring ≥99.9% to avoid molecular chain defects or side reactions caused by impurities. By strictly controlling the molar ratio within the range of 1:1.00±0.02, monomer imbalances caused by weighing errors or trace impurities can be effectively compensated, preventing chain end capping or excessively low molecular weight due to an excess of a single monomer, thus ensuring sufficient length and mechanical strength of the polyimide molecular chain.
[0032] Regarding the imidization rate of polyimide ≥99.5%, the imidization rate refers to the degree of ring closure of the polyamic acid precursor during heat treatment or chemical treatment, and is a key indicator for measuring the thermal and chemical stability of materials. A typical formula for calculating the imidization rate can be expressed as:
[0033] in, Represents 1778 cm⁻¹ in the infrared spectrum -1The intensity of the characteristic absorption peak of the imine ring, Represents 1660cm -1 The intensity of the characteristic absorption peak of the amide group is measured. When the imidization rate reaches or exceeds 99.5%, it indicates that the amyl acid groups on the polyamic acid molecular chain have almost completely undergone dehydration and ring-closure reactions, forming a stable imide ring structure. This high degree of imidization endows the material with excellent heat resistance, significantly increasing its glass transition temperature (Tg) and reducing the content of residual polar carboxyl and amino groups inside the material. This reduces the risk of side reactions with the electrolyte in the battery operating environment, ensuring the electrical insulation performance and structural integrity of the blocking membrane at high temperatures.
[0034] The electrical properties are shown in Table 4: Table 4
[0035] The volume resistivity of the blocking membrane is >10. 12 Ω·cm, dielectric strength >50kV / mm, electrochemical stability window is 0-4.8V vsLi + / Li.
[0036] Volume resistivity is an important indicator of a material's insulation capability; a higher value indicates a stronger ability to prevent leakage current from passing through the material. In this embodiment, the blocking film exhibits extremely high volume resistivity, primarily due to the tight packing of imide rings and the highly cross-linked three-dimensional network structure within the polyimide molecular chain, which significantly restricts the migration of free carriers within the material. This superior insulation performance effectively blocks micro-short-circuit channels within the battery, preventing the risk of self-discharge or thermal runaway caused by localized insulation failure.
[0037] Dielectric strength characterizes the maximum electric field strength a material can withstand before it breaks down. The blocking membrane in this embodiment possesses a dielectric strength greater than 50 kV / mm, meaning that even under extremely high voltage gradients, the membrane can maintain its physical and chemical stability and will not be broken down by the electric field. This characteristic is crucial for ensuring the safety of high-voltage power batteries under extreme operating conditions, preventing dielectric collapse of the separator under high electric fields that could lead to a direct short circuit between the positive and negative electrodes.
[0038] The electrochemical stability window reflects the voltage range within which a material does not undergo redox decomposition in an electrolyte environment. The blocking membrane provided in this embodiment has an electrochemical stability window covering 0-4.8 V vs Li + / Li. This wide voltage range covers the operating potential range of current mainstream lithium-ion battery cathode materials (such as high-nickel ternary materials, lithium iron phosphate, etc.). This means that during normal charge and discharge cycles, and even under abnormal voltages such as overcharging, the blocking film itself can maintain electrochemical inertness and will not undergo harmful redox reactions with electrode materials or electrolytes, thereby ensuring the long-term stability of the battery interface and cycle life.
[0039] The wetting properties of the electrolyte are shown in Table 5: Table 5
[0040] The contact angle of the blocking membrane with 1M LiPF6EC / DMC electrolyte is ≤10°, and the electrolyte absorption rate is ≥300%.
[0041] The parameter of a contact angle ≤10° characterizes the spreading and wetting ability of the electrolyte on the surface of the blocking membrane. In this embodiment, when a 1M LiPF6EC / DMC electrolyte is dropped onto the surface of the blocking membrane, the droplet spreads rapidly due to the presence of trace amounts of polar groups (such as incompletely closed-ring carboxyl or amide groups) on the surface of the PI nanofibers and the high-roughness surface structure formed by the nanofibers. The contact angle is extremely small, even close to 0°, exhibiting excellent hydrophilicity. This ultra-low contact angle ensures that the electrolyte can quickly wet the surface and pores of the membrane, eliminating the risk of bubble retention and facilitating the rapid establishment of ion transport channels inside the battery.
[0042] The parameter of electrolyte absorption rate ≥300% reflects the ability of the internal pore structure of the blocking membrane to store electrolyte. Electrolyte absorption rate is usually expressed by the formula... Perform calculations, where Electrolyte absorption rate, This refers to the wet weight after immersion in the electrolyte. The dry weight is before impregnation. Because the blocking membrane of this application has a high porosity of 70-85% and a high open-pore ratio of over 99%, its interconnected three-dimensional network of pores can adsorb and lock in a large amount of electrolyte through capillary action. When the electrolyte absorption rate reaches over 300%, it means that a unit mass of dry membrane can adsorb at least three times its own mass of electrolyte. This high absorption rate not only ensures efficient electrolyte absorption during the battery filling process and shortens the production cycle, but more importantly, it can alleviate the drying phenomenon caused by electrolyte consumption or decomposition during battery cycling, thereby maintaining stable ionic conductivity and extending the battery's cycle life.
[0043] Its mechanical properties are shown in Table 6: Table 6
[0044] The dry tensile strength of the blocking membrane is ≥50MPa, and the wet tensile strength after immersion in 1M LiPF6EC / DMC electrolyte for 24 hours is ≥35MPa; the dry puncture strength is ≥600gf, and the wet puncture strength after immersion in the same electrolyte for 24 hours is ≥400gf.
[0045] Dry tensile strength and wet tensile strength are key indicators characterizing the resistance of separator materials to damage during machining and in the electrolyte environment inside the battery. A dry tensile strength ≥50MPa indicates that the barrier membrane has excellent bulk mechanical strength, meeting the tension requirements of high-speed winding processes for lithium-ion battery separators. It is not prone to breakage or damage during production, ensuring processing yield and production efficiency. When the barrier membrane absorbs electrolyte inside the battery, its microfiber network will swell to a certain extent, which may lead to a decrease in mechanical properties. A wet tensile strength ≥35MPa indicates that the barrier membrane can still maintain high mechanical strength after being immersed in 1M LiPF6EC / DMC electrolyte for 24 hours. The material does not undergo significant degradation or excessive swelling in the electrolyte environment, and can adapt to the service environment inside the battery for a long time, continuously providing stable physical isolation for the positive and negative electrodes and preventing electrode contact short circuits due to insufficient separator strength.
[0046] Puncture strength refers to the ability of a separator to resist penetration by sharp external objects (such as lithium dendrites or electrode burrs), and is directly related to the risk of internal micro-short circuits in the battery. A dry-state puncture strength ≥600gf means that the barrier membrane has a dense and tough microstructure in its unwetted state, effectively blocking electrode burrs that may be generated during the manufacturing process. During battery cycling, lithium dendrites may grow on the negative electrode surface; these dendrites are sharp and penetrating. A wet-state puncture strength ≥400gf indicates that after the barrier membrane absorbs liquid and becomes wetted, its three-dimensional network framework remains tough, effectively resisting the puncture and growth of lithium dendrites. This significantly reduces the probability of internal short circuits or even thermal runaway caused by dendrites piercing the separator, thereby improving the battery's cycle life and safety performance.
[0047] Second Embodiment Please see Figure 1 This application provides a method for preparing a PI aerogel thermal runaway blocking membrane, comprising the following steps: Step S1: Preparation of polyamic acid precursor solution: Under nitrogen protection and with a dew point ≤ -40℃, diaminodiphenyl ether is dissolved in N,N-dimethylacetamide, and pyromellitic dianhydride in batches in an equimolar ratio with diaminodiphenyl ether is added to carry out a polycondensation reaction. The feeding rate is controlled so that the reaction temperature does not exceed 10℃. After the feeding is completed, stirring is continued for 2-6 hours to obtain a polyamic acid solution.
[0048] This step aims to prepare a polyamic acid precursor solution with a suitable molecular weight through a low-temperature polycondensation reaction, providing a basic raw material for the subsequent construction of a three-dimensional network structure aerogel membrane. In this process, N,N-dimethylacetamide (DMAc) acts as a solvent, not only dissolving the monomers but also promoting the polycondensation reaction between diaminodiphenyl ether (ODA) and pyromellitic dianhydride (PMDA), generating polymer chains containing amic acid groups.
[0049] Given PMDA's high sensitivity to moisture, even trace amounts can lead to hydrolysis, generating byproducts such as phthalic acid, disrupting the equimolar ratio of monomers, and consequently affecting the molecular weight and properties of the final polyimide (PI). Therefore, the reaction must be carried out under nitrogen protection in a strictly anhydrous environment with a dew point ≤ -40°C to ensure the moisture content entering the reaction system remains at an extremely low level. Furthermore, since polycondensation is an exothermic process, excessively high reaction temperatures can easily cause uneven molecular weight distribution or gelation. Controlling the feeding rate to limit the reaction temperature below 10°C, combined with continuous stirring for 2-6 hours after feeding, helps to obtain a polyamic acid solution with uniform molecular weight, regular structure, and suitable intrinsic viscosity.
[0050] Step S2: Casting of wet film: After degassing the polyamic acid solution, it is cast onto the surface of a moving steel belt or PET release film through a slit extrusion coating head to form a polyamic acid wet film.
[0051] The degassed polyamic acid solution is fed into a slot extrusion coating head, which utilizes its precise control over the coating gap and liquid layer thickness to transform the liquid precursor into a wet film layer with a specific geometry. During the casting process, a moving steel belt or polyethylene terephthalate (PET) release film acts as a carrier, providing a flat and continuous support surface to ensure that the polyamic acid solution forms a wet film of uniform thickness.
[0052] By coordinating the movement speed of the carrier and the feed rate of the coating head, the initial thickness of the wet film can be precisely controlled, thereby determining the final thickness specifications of the aerogel film after drying. This continuous casting method not only improves production efficiency but also effectively ensures the consistency of the film layer on a macroscopic scale.
[0053] Step S3 Solvent replacement: The polyamic acid wet film is sequentially immersed in ethanol / water solutions with decreasing concentration gradients for replacement until the residual amount of N,N-dimethylacetamide in the film is <0.1%, thus obtaining a polyamic acid hydrogel film.
[0054] To avoid the collapse of nanopores caused by the enormous capillary pressure resulting from the rapid evaporation of high-boiling-point solvents during direct high-temperature drying, this step employs solvent replacement technology to replace N,N-dimethylacetamide (DMAc) in the wet membrane with a low-boiling-point, low-surface-tension solvent system. The replacement process uses an ethanol / water solution system with a decreasing concentration gradient: first, the wet membrane is immersed in a high-concentration ethanol solution, allowing the ethanol to permeate and replace the DMAc within the membrane; then, the ethanol concentration is gradually decreased while the water content is increased, ultimately transitioning to a pure water system.
[0055] Due to the significant difference in surface tension between DMAc (approximately 32.7 mN / m) and water (approximately 72.8 mN / m), a gradient replacement strategy ensures a smooth transition in the surface tension of the solvent within the membrane, effectively preventing severe pore wall shrinkage or structural collapse caused by abrupt changes in surface tension. Replacement is considered complete when the residual DMAc content within the membrane is detected to be below 0.1%. This low residual standard ensures that residual high-boiling-point solvents will not cause pore wall adhesion or structural shrinkage during subsequent drying, thus obtaining a structurally stable polyamic acid hydrogel membrane.
[0056] Step S4: Drying at ambient pressure: Dry the polyamic acid hydrogel membrane at ambient pressure at 20-80℃ with a heating rate of 1-5℃ / min until the water content is <5%, thus obtaining the polyamic acid aerogel membrane.
[0057] Based on the stable hydrogel structure established in the previous steps, this step removes moisture from the membrane through atmospheric pressure drying while maintaining the integrity of the aerogel nanoporous structure. Compared to supercritical drying, atmospheric pressure drying has the advantages of low cost, simple equipment, and ease of large-scale production, but the risk of pore collapse caused by capillary forces needs to be overcome.
[0058] During the drying process, a slow heating rate of 1-5℃ / min, combined with the smooth transition of the solvent surface tension mentioned above, effectively reduces the vapor pressure gradient during liquid evaporation within the pores, promoting the smooth escape of moisture from the nanopores. Controlling the drying temperature within the range of 20-80℃ prevents structural damage caused by excessively rapid boiling of moisture. As the drying process progresses until the water content within the membrane drops below 5%, the solvent-filled pores transform into air-filled pores, ultimately resulting in a fluffy polyamic acid aerogel membrane with a high specific surface area.
[0059] Step S5 Thermal imidization: Under nitrogen protection and with an O2 content of <50ppm, the polyamic acid aerogel membrane is subjected to micro-tension and thermal imidization treatment with step temperature increase to obtain a PI aerogel thermal runaway blocking membrane.
[0060] This step converts polyamic acid, which has low thermal stability, into polyimide, which has high thermal stability, through a thermochemical reaction. During the thermal imidization process, the amic acid groups on the polyamic acid molecular chain undergo a cyclization and dehydration reaction to form an imide ring, thereby endowing the material with excellent heat resistance and mechanical strength.
[0061] To prevent oxidative degradation of the polyimide molecular chains at high temperatures, the treatment process must be carried out in an inert atmosphere with nitrogen protection and an oxygen content below 50 ppm. A stepped heating strategy typically covers multiple temperature stages (e.g., 80-120℃, 150-200℃, 250-300℃, and 350℃), corresponding to different requirements for residual solvent removal, molecular chain rearrangement, and imidization reactions. By precisely controlling the heating rate and holding time at each stage, the cyclization reaction rate can be controlled, avoiding the formation of excessive water vapor due to overly rapid reactions, which could lead to film blistering or pinhole defects.
[0062] Simultaneously, micro-tension is applied to the polyamic acid aerogel membrane to limit its thermal shrinkage under high-temperature conditions, ensuring that the final PI aerogel blocking membrane has a smooth appearance and uniform thickness. Through the above treatment, a PI aerogel thermal runaway blocking membrane with a three-dimensional continuous network structure and excellent high-temperature resistance is finally obtained.
[0063] The above steps, through specific process parameter control and synergistic effects, achieve a complete preparation process from monomer polymerization to membrane forming, solvent replacement, drying, and imidization. The combination of gradient solvent replacement and slow atmospheric pressure drying successfully solves the technical challenge of aerogel collapse under atmospheric pressure drying, enabling the preparation of aerogel membranes with nanoscale pore structures and high porosity without relying on expensive supercritical equipment. Stepped heating thermal imidization and micro-tension control ensure the complete transformation of polymer chains and the dimensional stability of the membrane structure. Verification shows that this process can stably produce PI aerogel thermal runaway-blocking membranes that meet the expected structural characteristics and performance indicators in actual production, providing a reliable material guarantee for improving the safety performance of lithium batteries.
[0064] Triaminobenzene is added to the polyamic acid solution at a concentration of 0.5-1.0 wt% relative to the solid content of polyamic acid as a crosslinking agent.
[0065] In the preparation stage of the polyamic acid precursor solution, triaminobenzene is introduced to enhance the strength of the wet gel skeleton formed after the precursor solution forms a film, preventing severe structural collapse due to capillary pressure during subsequent solvent replacement and drying processes. The triaminobenzene molecule contains three active amino groups, which undergo cross-linking reactions with the carboxyl functional groups on the polyamic acid molecular chains in the polycondensation reaction system. This leads to the formation of chemical bond connections between the polyamic acid molecular chains, resulting in a denser and more stable three-dimensional network structure.
[0066] To ensure uniform dispersion and effective participation of triaminobenzene in the construction of the polymerization network, it is typically added after complete dissolution in N,N-dimethylacetamide (DMAc) and before or simultaneously with the addition of pyromellitic dianhydride. The amount of triaminobenzene added is limited to 0.5-1.0 wt% relative to the polyamic acid solid content; this range is an experimentally verified equilibrium range. If the addition amount is less than 0.5 wt%, the crosslinking density is insufficient, making it difficult to effectively resist the capillary pressure during the subsequent drying process and failing to completely prevent the shrinkage and collapse of the nanopores. If the addition amount is greater than 1.0 wt%, it will lead to excessive crosslinking, resulting in an overly rigid polyamic acid network. This not only affects the surface smoothness of the cast film but may also increase the brittleness and decrease the flexibility of the final polyimide aerogel film, thus failing to meet the requirements of the battery winding process. For example, in some embodiments, the amount of triaminobenzene added can be set to 0.6 wt%, 0.8 wt%, or 0.9 wt%, etc.
[0067] By introducing triaminobenzene for chemical crosslinking, the fibrous skeleton of the polyamic acid wet membrane maintains sufficient geometric stiffness during subsequent solvent replacement (from N,N-dimethylacetamide to water) and atmospheric pressure drying. This enhanced skeleton structure can withstand the enormous capillary tension generated by solvent evaporation within the nanopores, thereby effectively maintaining the pore size distribution, porosity, and permeability of the aerogel membrane, ensuring that the final PI aerogel thermal runaway blocking membrane has the expected microstructure and thermal insulation performance. Furthermore, triaminobenzene participates in the reaction during the subsequent high-temperature thermal imidization process and transforms into a stable crosslinked structure, avoiding the presence of unstable low-molecular-weight compounds in the final membrane material, thus ensuring the electrochemical stability and safety of the blocking membrane at high temperatures.
[0068] The concentration gradients of ethanol / water solution were as follows: 100% ethanol, 75% ethanol, 50% ethanol, 25% ethanol and pure water, with each gradient requiring a soaking time of 20-40 minutes.
[0069] The specific ethanol / water solution concentration gradient described above aims to optimize the interfacial surface tension variation between the solvent inside the polyamic acid wet membrane and the external replacement medium, thereby minimizing the damage to the nanoporous structure caused by sudden changes in capillary pressure. The polyamic acid wet membrane contains a large amount of N,N-dimethylacetamide (DMAc), with a surface tension of approximately 32.7 mN / m, while the surface tension of pure water is as high as 72.8 mN / m. If the wet membrane is directly immersed in pure water, the huge surface tension difference (approximately 40 mN / m) will cause a severe capillary pressure difference when the liquid evaporates or is replaced within the nanopores. This instantaneous pressure can easily cause the delicate polyamic acid nanofiber skeleton to shrink or even collapse, thereby destroying the three-dimensional continuous network structure of the aerogel.
[0070] To construct a smooth transition path from the organic phase to the aqueous phase, the concentration gradient of ethanol / water solution was sequentially set as follows: 100% ethanol, 75% ethanol, 50% ethanol, 25% ethanol, and pure water. The surface tension of ethanol is approximately 22.1 mN / m, which is close to that of DMAc. By controlling the concentration gradient, the change in surface tension during each replacement step was kept to around 10 mN / m. For example, when the membrane transitions from a 100% ethanol environment to a 75% ethanol environment, the surface tension of the solvent system experiences only minor fluctuations, allowing the capillary pressure on the liquid inside the membrane to be released smoothly. This gradual solvent replacement method allows DMAc molecules inside the membrane to be gradually diluted and carried out, while external water molecules can gently enter the membrane, avoiding uneven stress on the pore walls caused by drastic changes in surface tension at the two-phase interface.
[0071] The immersion time for each gradient is limited to 20-40 minutes. This time range is set based on a comprehensive consideration of the diffusion kinetics balance of the solvent in the porous medium and production efficiency. If the immersion time is less than 20 minutes, it may result in insufficient solvent replacement, leaving a high concentration of DMAc in the membrane or forming local surface tension extremes, affecting the subsequent drying effect. On the other hand, if the immersion time is longer than 40 minutes, although it can ensure complete replacement, it will reduce the overall production line efficiency in industrial production without any additional gain. Within the 20-40 minute time window, the immersion time can be dynamically adjusted according to the membrane thickness: for thinner membranes (e.g., close to 10 μm), the immersion time can be set to 20-25 minutes; for thicker membranes (e.g., close to 25 μm), the immersion time can be set to 35-40 minutes to ensure that the solvent at all depths within the membrane is fully replaced.
[0072] In step S5, a segmented temperature-controlled strategy is used to perform thermal imidization treatment on the polyamic acid aerogel membrane to convert the polyamic acid molecular chains into a polyimide structure with high thermal stability. This step-heating thermal imidization process specifically includes the following stages: First stage: Heat to 80-120℃ at a heating rate of 5℃ / min, and hold for 10-15 minutes.
[0073] The heating equipment raises the ambient temperature at a constant rate of 5°C / min until a preset target value between 80°C and 120°C is reached, and then maintains this temperature for 10 to 15 minutes. This stage aims to remove residual trace amounts of moisture and low-boiling-point solvents from the polyamic acid aerogel membrane through gentle heating. Although the moisture content of the membrane material has been reduced to a low level in the previous drying step, physically bound water or a small amount of residual solvent may still be adsorbed within its internal nanopores. If the high-temperature heating stage is directly initiated, the instantaneous vaporization of the residual liquid will generate huge vapor pressure, which can easily lead to the formation of bubbles inside the membrane material or even cause structural rupture. Controlling the initial treatment within the 80-120°C range, combined with appropriate heat preservation, allows the residual components to volatilize smoothly under low surface tension, avoiding damage to the nanoporous framework of the aerogel due to sudden and violent volume expansion. At the same time, the heating rate of 5°C / min balances heating efficiency and thermal stress control, effectively preventing stress concentration caused by excessive temperature differences between the membrane surface and interior.
[0074] Second stage: Increase the temperature to 150-200℃ at a heating rate of 2-3℃ / min, and hold for 20-30 minutes.
[0075] After low-temperature pretreatment, the critical initial stage of thermal imidization begins. At this point, the heating rate is adjusted to 2-3℃ / min, allowing the temperature to slowly rise to the target range of 150℃ to 200℃, and then held at this temperature for 20-30 minutes. Within this temperature range, the amide groups on the polyamic acid molecular chain begin to undergo cyclization and dehydration reactions, releasing small-molecule byproduct water, marking the initiation of the transformation to a polyimide structure. Given that this stage of the chemical reaction is exothermic, excessively rapid heating can easily lead to heat accumulation inside the membrane, resulting in localized overheating or uncontrolled reaction. Limiting the heating rate to a lower level of 2-3℃ / min effectively delays the appearance of the exothermic peak, providing sufficient thermal equilibrium time for the system. Furthermore, the 20-30 minute holding time ensures uniform temperature distribution along the membrane thickness, promoting a synchronous and stable initiation of the chemical reaction across the entire cross-section, avoiding the defect of surface overheating and insufficient internal reaction, and laying a good molecular structural foundation for subsequent deep imidization.
[0076] The third stage: Heat to 250-300℃ at a heating rate of 2℃ / min, and hold for 30-45 minutes.
[0077] Building upon the second-stage reaction, the temperature is further increased to a high-temperature range of 250°C to 300°C and maintained at this temperature for 30 to 45 minutes. This stage constitutes the main reaction phase for completing the thermal imidization reaction. During this period, a slow heating rate of 2°C / min is maintained to accelerate the cyclization and dehydration reaction of the polyamic acid, enabling most of the molecular chains to transform from a linear structure to an imide cyclic structure, thereby significantly improving the mechanical properties and thermal stability of the material. Due to the deep reaction and large heat release in this stage, the slow heating rate helps release the internal stress accumulated in the previous stages and prevents the film from curling or cracking due to severe chemical shrinkage. The longer holding time ensures sufficient reaction kinetics, allowing the polyamic acid molecular chains to obtain enough energy to overcome the reaction energy barrier and achieve a high degree of cyclic closure. This stage of treatment directly determines whether the imidization rate of the final polyimide aerogel film can reach the requirement of ≥99.5%, and plays a decisive role in eliminating microscopic defects inside the material. Fourth stage: Heat to 350℃ at a heating rate of 5℃ / min and hold for 10-15 minutes.
[0078] After the main reaction stage is completed, a high-temperature setting treatment is performed. The heating rate is restored to 5℃ / min, and the temperature is rapidly increased to the final target temperature of 350℃ and held for 10 to 15 minutes. This stage aims to eliminate residual unreacted groups, complete further rearrangement and densification of the molecular chains, and finalize the microstructure of the polyimide aerogel membrane. At the high temperature of 350℃, any active groups that have not yet participated in the cyclization reaction are forcibly converted, thereby maximizing the degree of crosslinking and crystallinity of the material and ensuring its dimensional stability under extreme high-temperature conditions. Given that sufficient imidization has been performed previously, there are no large amounts of volatile components remaining inside the membrane material, so a faster heating rate can be used to improve production efficiency. A short holding time of 10-15 minutes is sufficient to complete the relaxation of the molecular chains and stress relief, while avoiding thermal degradation or oxidative decomposition of the material due to prolonged high temperatures. After this stage of treatment, the polyimide aerogel membrane possesses the final required excellent heat resistance and mechanical strength.
[0079] The aforementioned stepped heating thermal imidization process, through segmented control of the heating rate and holding time, achieves precise control over the entire process from solvent evaporation and reaction initiation to deep imidization and final shaping. The mild preheating in the low-temperature stage eliminates the risk of structural damage caused by abrupt changes in physical state; the slow heating and long holding time in the medium-temperature stage ensure the smooth and uniform chemical reaction; and the deep treatment in the high-temperature stage guarantees the integrity of the molecular structure. This process path, while ensuring an imidization rate of ≥99.5%, effectively alleviates the internal stress caused by volume shrinkage and molecular chain rearrangement during the conversion of polyamic acid to polyimide, preventing the collapse of the aerogel pore structure or distortion of macroscopic dimensions, thereby producing a structurally intact and uniformly performing PI aerogel thermal runaway blocking membrane.
[0080] The above-disclosed embodiments are merely one or more preferred embodiments of this application and should not be construed as limiting the scope of this application. Those skilled in the art can understand that all or part of the processes for implementing the above embodiments and equivalent changes made in accordance with the claims of this application still fall within the scope of this application.
Claims
1. A PI aerogel thermal runaway blocking membrane, characterized in that, The membrane is composed of a three-dimensional continuous network structure made of polyimide nanofibers; the diameter of the PI nanofibers is 20-50 nm; the average pore size of the blocking membrane is 10-80 nm, the porosity is 70-85%, and the open porosity is greater than 99%; the blocking membrane is an independently formed solid structure with a thickness of 10-25 μm; the thermal shrinkage rate of the blocking membrane after being kept at 300°C for 30 minutes is less than 2%.
2. The PI aerogel thermal runaway blocking membrane and its preparation method as described in claim 1, characterized in that, The polyimide nanofibers are generated by polycondensation of pyromellitic dianhydride and diaminodiphenyl ether at a molar ratio of 1:1.00±0.02, and the imidization rate of the polyimide is ≥99.5%.
3. The PI aerogel thermal runaway blocking membrane and its preparation method as described in claim 2, characterized in that, The volume resistivity of the blocking membrane is >10. 12 Ω·cm, dielectric strength >50kV / mm, electrochemical stability window is 0-4.8V vsLi + / Li.
4. The PI aerogel thermal runaway blocking membrane and its preparation method as described in claim 3, characterized in that, The contact angle of the blocking membrane with 1M LiPF6EC / DMC electrolyte is ≤10°, and the electrolyte absorption rate is ≥300%.
5. The PI aerogel thermal runaway blocking membrane and its preparation method as described in claim 4, characterized in that, The blocking membrane has a dry tensile strength ≥50MPa and a wet tensile strength ≥35MPa after immersion in the electrolyte for 24 hours; its dry puncture strength ≥600gf and its wet puncture strength ≥400gf after immersion in the same electrolyte for 24 hours.
6. A method for preparing a PI aerogel thermal runaway blocking membrane, applied to the preparation of a PI aerogel thermal runaway blocking membrane according to any one of claims 1-5, characterized in that, Includes the following steps: Preparation of S1 polyamic acid precursor solution: Under nitrogen protection and with a dew point ≤ -40℃, diaminodiphenyl ether is dissolved in N,N-dimethylacetamide, and pyromellitic dianhydride in batches in an equimolar ratio with diaminodiphenyl ether is added to carry out polycondensation reaction. The feeding rate is controlled so that the reaction temperature does not exceed 10℃. After the feeding is completed, stirring is continued for 2-6 hours to obtain polyamic acid solution. S2 wet film casting: After degassing the polyamic acid solution, it is cast onto the surface of a moving steel belt or PET release film through a slit extrusion coating head to form a polyamic acid wet film. S3 Solvent replacement: The polyamic acid wet film is sequentially immersed in ethanol / water solutions with decreasing concentration gradients for replacement until the residual amount of N,N-dimethylacetamide in the film is <0.1%, thus obtaining a polyamic acid hydrogel film; S4 Atmospheric pressure drying: The polyamic acid hydrogel membrane is dried at atmospheric pressure at 20-80℃ with a heating rate of 1-5℃ / min until the water content is <5%, thus obtaining a polyamic acid aerogel membrane. S5 Thermal imidization: Under nitrogen protection and with an O2 content of <50ppm, the polyamic acid aerogel membrane is subjected to micro-tension and thermal imidization treatment with step-up temperature increase to obtain the PI aerogel thermal runaway blocking membrane.
7. The method for preparing a PI aerogel thermal runaway blocking membrane as described in claim 6, characterized in that, In step S1, triaminobenzene is added to the polyamic acid solution at a concentration of 0.5-1.0 wt% relative to the polyamic acid solid content as a crosslinking agent.
8. The method for preparing a PI aerogel thermal runaway blocking membrane as described in claim 7, characterized in that, In step S3, the concentration gradient of the ethanol / water solution is as follows: 100% ethanol, 75% ethanol, 50% ethanol, 25% ethanol and pure water, and the soaking time for each gradient is 20-40 minutes.
9. The method for preparing a PI aerogel thermal runaway blocking membrane as described in claim 8, characterized in that, In step S5, the step-heating thermal imidization process specifically involves: First stage: Heat to 80-120℃ at a heating rate of 5℃ / min, and hold for 10-15 minutes; Second stage: Increase the temperature to 150-200℃ at a heating rate of 2-3℃ / min, and hold for 20-30 minutes; The third stage: Heat to 250-300℃ at a heating rate of 2℃ / min, and hold for 30-45 minutes; Fourth stage: Increase the temperature to 350℃ at a rate of 5℃ / min and hold for 10-15 minutes.