Mica oriented styrene-butadiene rubber composite, preparation method and flame-retardant conveyor belt
By using ice templates to oriented frozen mica nanosheets and styrene-butadiene rubber latex, a 'brick-mud' layered structure was constructed, which solved the problems of performance degradation and insufficient flame retardancy of styrene-butadiene rubber conveyor belts at high temperatures, and achieved a significant improvement in high-temperature ablation resistance and flame retardancy.
Patent Information
- Application Number
- CN202611539321.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional styrene-butadiene rubber conveyor belts exhibit significant degradation in high-temperature mechanical properties under conditions of high temperature, open flame, and ozone erosion. They also lack sufficient flame retardancy and weather resistance, and the random distribution of mica nanosheets prevents them from forming a continuous thermal barrier and barrier layer.
An ice-template method was used to oriented freeze mica nanosheets and mix them with styrene-butadiene rubber latex to form an oriented frozen body. After removing the ice crystals, the mixture was impregnated with a vulcanization aid and hot-pressed to construct a composite styrene-butadiene rubber material with oriented mica nanosheets, forming a layered ordered structure similar to 'brick-mud'.
It significantly improves the high temperature resistance, flame retardancy and weather resistance of composite materials, and can form a dense ceramic protective layer at an instantaneous high temperature of 800℃, making it suitable for rubber conveyor belts in high temperature instantaneous ablation conditions.
Smart Images

Figure CN123152164A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of rubber composite material technology, specifically relating to a mica oriented styrene-butadiene rubber composite material, its preparation method, and a flame-retardant conveyor belt. Background Technology
[0002] Styrene-butadiene rubber (SBR) is the most produced general-purpose synthetic rubber. It is characterized by wear resistance, aging resistance, and excellent processing performance. It is widely used in rubber products such as tires, conveyor belts, and hoses. However, under complex working conditions such as metallurgy, mining, and building materials, conveyor belts are subjected to long-term corrosion from high-temperature materials, open flames, and ozone. Traditional SBR has defects such as significant degradation of high-temperature mechanical properties and insufficient flame retardancy, making it difficult to meet the service requirements under extreme conditions.
[0003] Mica, a layered silicate, is heat-resistant, flame-retardant, and has a high aspect ratio, making it suitable for rubber reinforcement. However, in traditional mechanical blending, mica flakes are randomly distributed, failing to leverage their anisotropic advantages and making it difficult to form a continuous thermal barrier and separation layer along the working surface of the conveyor belt. The ice template method (directional cryogenic casting) utilizes the "liquid-solid-gas" phase transition that occurs during the directional freezing process of the solvent, using the displacing effect of ice crystals to drive the assembly units to achieve an ordered arrangement.
[0004] Chinese invention patent (publication number: CN114214864A) discloses a method for preparing high thermal conductivity mica paper based on the ice template method. The product matrix of this method is mica paper, not styrene-butadiene rubber (SBR), and it does not involve the vulcanization aid impregnation-hot pressing vulcanization process, making it unsuitable for ablation-resistant and flame-retardant conveyor belts. Chinese invention patent (publication number: CN106810876A) relies on mechanical extrusion to achieve filler orientation, not ice template directional freezing. The matrix is silicone rubber, polyurethane, etc., and does not belong to the SBR latex-mica nanosheet system, thus not addressing the high-temperature, flame-retardant, and weather-resistant requirements of conveyor belts. Chinese invention patent (publication number: CN115181322A) produces a porous sound-absorbing aerogel filled with montmorillonite, not dense vulcanized SBR, and it does not possess the "directional freezing-freeze-vulcanization aid impregnation-hot pressing vulcanization" process route of this invention.
[0005] In existing technologies, when styrene-butadiene rubber (SBR) is used in conveyor belts in metallurgy, mining, and building materials industries, it is subjected to long-term exposure to high-temperature materials, open flames, and ozone erosion. As a result, the material itself suffers from significant degradation of high-temperature mechanical properties, insufficient flame retardancy, ablation resistance, and weather resistance. If mica is used as a modified filler, the mica nanosheets are mostly randomly distributed under traditional processing methods, making it difficult to construct a continuous layered barrier structure. This fails to fully utilize the thermal barrier and barrier functions of the mica sheets, making it difficult to meet the usage requirements of conveyor belts under extreme service conditions. Summary of the Invention
[0006] The purpose of this invention is to provide a mica-oriented styrene-butadiene rubber composite material, its preparation method, and a flame-retardant conveyor belt, in order to solve the problems of irregular mica distribution inside traditional styrene-butadiene rubber conveyor belts, which result in deterioration of high-temperature mechanical properties, poor flame retardancy, ablation resistance, and poor weather resistance.
[0007] To achieve the above-mentioned technical objectives, the technical solution adopted by the present invention is as follows:
[0008] In a first aspect, the present invention discloses a method for preparing a mica-oriented styrene-butadiene rubber composite material, comprising:
[0009] Mica nanosheets were uniformly dispersed in styrene-butadiene latex to obtain a mica nanosheet / styrene-butadiene latex mixed dispersion.
[0010] The mixed dispersion was placed in a directional freezing device for directional freezing treatment, so that the ice crystals grew in a predetermined direction, and the mica nanosheets were oriented along the ice crystal growth direction under the expulsion of the ice crystals, thus obtaining a directional frozen body.
[0011] The directional cryobody was freeze-dried to remove ice crystals, resulting in an aerogel framework with a directional pore structure composed of mica nanosheets / styrene-butadiene rubber.
[0012] After impregnating the aerogel skeleton with a vulcanization aid, hot pressing and vulcanization are performed to obtain a composite styrene-butadiene rubber material with mica nanosheets oriented filling.
[0013] Further specifying, in the raw material mixing step, the mica nanosheets are dispersed in styrene-butadiene latex by one or more of the following methods: mechanical stirring, ultrasonic dispersion, and high-shear emulsification.
[0014] Further specified, the temperature for directional freezing is -196℃ to -10℃; the freezing method is unidirectional freezing or bidirectional freezing;
[0015] The cold source can be one or more of the following: liquid nitrogen, dry ice-ethanol bath, low temperature circulating bath, or semiconductor refrigeration.
[0016] Further specified, the freeze-drying temperature is -80℃ to -20℃, the vacuum degree is 1 to 100 Pa, and the drying time is 12 to 72 h.
[0017] Further specified, the temperature of the hot pressing and vulcanization treatment is 100℃~200℃, the pressure is 1~30MPa, and the time is 10~120min.
[0018] Further specified, the mica nanosheets have a thickness of 1–50 nm, a lateral dimension of 0.2–10 μm, and an aspect ratio of not less than 50;
[0019] The mica nanosheets account for 1 to 30 wt% of the total mass of the composite styrene-butadiene rubber material.
[0020] Furthermore, the mica nanosheets are modified mica nanosheets, and the modification methods include one or more of the following: silane coupling agent modification, surfactant modification, and polymer linker modification.
[0021] Further specifying, the vulcanization aid includes one or more of vulcanizing agents, accelerators, activators, antioxidants, and reinforcing agents.
[0022] Secondly, this invention discloses a mica-oriented styrene-butadiene rubber composite material, which is prepared by the above-mentioned method for preparing a mica-oriented styrene-butadiene rubber composite material;
[0023] The composite styrene-butadiene rubber material comprises a styrene-butadiene rubber matrix and mica nanosheet fillers oriented therein. The mica nanosheets are oriented along the ice crystal growth direction to form a layered ordered structure similar to a "brick-mud" structure.
[0024] The layered ordered configuration of the "brick-mud" structure refers to the stacking of mica nanosheets as bricks along a specific orientation, with styrene-butadiene rubber matrix as mud phase filling and bonding in the gaps between the mica sheets, forming a masonry-like layered micromorphology.
[0025] Thirdly, the present invention discloses a styrene-butadiene rubber flame-retardant conveyor belt, comprising the above-mentioned composite styrene-butadiene rubber material;
[0026] When preparing the composite styrene-butadiene rubber material, the preset direction of directional freezing is parallel to the direction of the conveyor belt working surface, and the hot pressing direction is perpendicular to the direction of the conveyor belt working surface, so that a layered mica barrier structure parallel to the working surface is formed inside the conveyor belt.
[0027] The invention employing the above technical solution has the following advantages:
[0028] 1. This invention uses the ice template effect to drive the mica nanosheets to be oriented along the ice crystal growth direction, forming a "brick-mud" layered ordered structure inside the rubber matrix. This is different from the random dispersion and mechanical extrusion orientation of traditional mechanical blend fillers, and fully releases the barrier effect of mica nanosheets.
[0029] 2. This invention adopts a process route of directional freezing-freeze drying-post-impregnation with vulcanizing aids-hot pressing vulcanization, which avoids the interference of premixing vulcanizing aids on ice crystal growth, effectively protects the directional layered structure formed by the ice template from being destroyed by the vulcanization molding process, and successfully transforms the porous aerogel skeleton into a dense composite styrene-butadiene rubber material.
[0030] 3. The directional arrangement of mica sheets in this invention constructs a continuous thermal barrier, which significantly improves the high temperature resistance, flame retardancy, ablation resistance and weather resistance of the composite material. When burned at high temperature, a dense ceramic protective layer can be formed on the surface, which can withstand instantaneous high temperature impact of up to 800°C. It is suitable for rubber conveyor belts in harsh working conditions of high temperature and instantaneous ablation, and has good industrial application value. Attached Figure Description
[0031] The present invention can be further illustrated by the non-limiting embodiments given in the accompanying drawings;
[0032] Figure 1 This is a flowchart illustrating the preparation process of styrene-butadiene rubber composite materials provided in an embodiment of the present invention.
[0033] Figure 2 This is a SEM image of the anisotropic composite rubber material of Example 1 of the present invention;
[0034] Figure 3 This is a SEM image of the atomized composite rubber material in Example 1 of the present invention.
[0035] Figure 4 This is a combustion experiment (self-extinguishing after flameout) of the anisotropic composite rubber material in Example 1 of the present invention.
[0036] Figure 5 This is a SEM image of the anisotropic composite rubber material of Example 2 of the present invention;
[0037] Figure 6 This is a SEM image of the anisotropic composite rubber material of Example 3 of the present invention;
[0038] Figure 7 This is a SEM image of the anisotropic composite rubber material in Example 4 of the present invention;
[0039] Figure 8 This is a SEM image of the anisotropic composite rubber material in Example 5 of the present invention;
[0040] Figure 9 This is a SEM image of the isotropic composite rubber material of Comparative Example 1 of the present invention;
[0041] Figure 10 This is a SEM image of the wear marks on the isotropic composite rubber material of Comparative Example 1 of this invention.
[0042] Figure 11 The combustion experiment of the isotropic composite rubber material of Comparative Example 1 of this invention (it cannot self-extinguish after being removed from the flame).
[0043] Figure 12 This is a SEM image of the unfilled composite rubber material in Comparative Example 2 of the present invention. Detailed Implementation
[0044] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that similar or identical parts are referred to by the same reference numerals in the drawings or description. Implementations not shown or described in the drawings are forms known to those skilled in the art.
[0045] A method for preparing mica-oriented styrene-butadiene rubber composite material includes:
[0046] Mica nanosheets were uniformly dispersed in styrene-butadiene latex to obtain a mica nanosheet / styrene-butadiene latex mixed dispersion.
[0047] The mixed dispersion was placed in a directional freezing device for directional freezing treatment, so that the ice crystals grew in a predetermined direction, and the mica nanosheets were oriented along the ice crystal growth direction under the expulsion of the ice crystals, thus obtaining a directional frozen body.
[0048] The directional cryobody was freeze-dried to remove ice crystals, resulting in an aerogel framework with a directional pore structure composed of mica nanosheets / styrene-butadiene rubber.
[0049] After impregnating the aerogel skeleton with a vulcanization aid, hot pressing and vulcanization are performed to obtain a composite styrene-butadiene rubber material with mica nanosheets oriented filling.
[0050] Example 1
[0051] This embodiment describes the first method for preparing mica-oriented styrene-butadiene rubber composite material, including the following steps:
[0052] Take 10g of mica nanosheets modified with silane coupling agent (KH570) (thickness approximately 20nm, side dimension approximately 5μm, aspect ratio approximately 250), add 490g of styrene-butadiene latex containing 100g of dry styrene-butadiene rubber (dry styrene-butadiene rubber model SBR1502), and use a shear dispersion emulsifier with a high-speed shearing speed of 8000rpm for 10min to obtain a mica nanosheet / styrene-butadiene latex mixed dispersion;
[0053] The above-mentioned mica nanosheet / styrene-butadiene latex mixed dispersion was placed in a directional freezing device for directional freezing treatment, so that the ice crystals grew in a predetermined direction. The mica nanosheets and styrene-butadiene raw rubber particles were oriented along the ice crystal growth direction under the extrusion of the ice crystals, thus obtaining a directional frozen body.
[0054] The directional cryobody was placed in a freeze dryer at -60℃ and 10Pa pressure for 24h to remove ice crystals and obtain a mica nanosheet / styrene-butadiene rubber aerogel skeleton with directional pore structure.
[0055] The above-mentioned mica nanosheet / styrene-butadiene rubber aerogel skeleton was impregnated in a vulcanizing aid solution containing 2.5g of vulcanizing agent (sulfur), 2.5g of accelerator (2-thiol benzothiazole), 5g of activator (zinc oxide), and 0.5g of antioxidant (N-phenyl-N′-cyclohexyl-p-phenylenediamine). The impregnation was repeatedly squeezed until uniform, and then hot-pressed at 150℃ and 10MPa for 30min, with the hot-pressing direction perpendicular to the working surface of the conveyor belt, to obtain a composite styrene-butadiene rubber material with oriented mica nanosheets (e.g., Figure 1 , Figure 2 and Figure 3 (as shown);
[0056] The mica nanosheets obtained in this embodiment exhibit a layered, ordered "brick-and-mortar" configuration. The composite material has a Shore A hardness of 68, a tensile strength of 18.5 MPa, and an Akron wear volume of 0.70 cm³. 3 / 1.61km, flame retardant rating reaches UL-94 / V-0 (as shown in Table 1), has self-extinguishing effect, and the material surface can form a continuous and dense barrier protective layer when burned at high temperature (as shown in Table 1). Figure 4 (As shown).
[0057] Example 2
[0058] The difference between this embodiment and Example 1 is that 5g of stearic acid-modified mica nanosheets (thickness about 10nm, side dimension about 1μm, aspect ratio about 100) are added in the raw material mixing step.
[0059] In this embodiment, mica nanosheets account for approximately 4.3 wt% of the total mass of the vulcanized composite styrene-butadiene rubber material (e.g., ...). Figure 5 (as shown);
[0060] In this embodiment, the filler content is reduced, resulting in a composite material with a Shore A hardness of 62, a tensile strength of 16.0 MPa, and an Akron wear volume of 0.78 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-1 (as shown in Table 1), still has good high temperature barrier ability, and mechanical properties are slightly lower than those of Example 1.
[0061] Example 3
[0062] The difference between this embodiment and Example 1 is that 25g of sodium carboxymethyl cellulose modified mica nanosheets (thickness about 50nm, side dimension about 10μm, aspect ratio about 200) are added in the raw material mixing step.
[0063] In this embodiment, mica nanosheets account for approximately 18.5 wt% of the total mass of the vulcanized composite styrene-butadiene rubber material (e.g., ...). Figure 1 , Figure 2 and Figure 6 (as shown);
[0064] In this embodiment, the increased mica filler content further enhances the layered barrier effect. The composite material has a Shore A hardness of 78, a tensile strength of 21.0 MPa, and an Akron wear volume of 0.65 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-0 (as shown in Table 1), with the best wear resistance, high temperature resistance and ablation resistance.
[0065] Example 4
[0066] The difference between this embodiment and Embodiment 1 is that 490g of styrene-butadiene latex is added in the raw material mixing step. This styrene-butadiene latex contains 50g of dry styrene-butadiene rubber (dry styrene-butadiene rubber type SBR1502), with the remaining component being water. In this embodiment, mica nanosheets account for approximately 14.2wt% of the total mass of the vulcanized composite styrene-butadiene rubber material (e.g., ...). Figure 7 (as shown);
[0067] In this embodiment, the proportion of rubber matrix is reduced, while the relative proportion of filler is increased. The composite material has a Shore A hardness of 75, a tensile strength of 15.5 MPa, and an Akron wear volume of 0.72 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-0 (as shown in Table 1); the reduction in rubber phase leads to a slight decrease in material flexibility, but the flame retardant performance remains at a high level.
[0068] Example 5
[0069] The difference between this embodiment and Embodiment 1 is that 490g of styrene-butadiene latex is added in the raw material mixing step. This styrene-butadiene latex contains 150g of dry styrene-butadiene rubber (dry styrene-butadiene rubber type SBR1502), with the remaining component being water. In this embodiment, mica nanosheets account for approximately 5.9wt% of the total mass of the vulcanized composite styrene-butadiene rubber material (e.g., ...). Figure 8 (as shown);
[0070] In this embodiment, the rubber matrix content is relatively high, the composite material has a Shore A hardness of 65, a tensile strength of 19.0 MPa, and an Akron wear volume of 0.68 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-0 (as shown in Table 1); the material retains the high elasticity of rubber, has excellent mechanical properties, and also has good flame retardant and high temperature resistance properties.
[0071] Example 6
[0072] The difference between this embodiment and Example 1 is that the dosage of mica nanosheets was adjusted and the feeding ratio was controlled so that the mica nanosheets accounted for 1 wt% of the total mass of the composite styrene-butadiene rubber material after vulcanization. 11g of mica nanosheets modified with silane coupling agent KH570 (thickness approximately 20nm, lateral dimension approximately 5μm, aspect ratio approximately 250) were added to 490g of styrene-butadiene latex, which contained 100g of dry styrene-butadiene rubber (dry styrene-butadiene rubber model SBR1502). The remaining raw material ratios, dispersion processes, and impregnation vulcanization aid formulations were consistent with Example 1. The directional freezing temperature was -10℃, and a low-temperature circulating bath was used as the cold source. The freeze-drying temperature was -20℃, the vacuum degree was 100Pa, and the drying time was 12h. Ice crystal sublimation removal was completed under the condition of appropriate sample thickness. The hot pressing molding and vulcanization treatment temperature was 100℃, the pressure was 1MPa, and the vulcanization was carried out for 120min.
[0073] In this embodiment, the mica filler is added at the minimum amount, the matrix rubber has a high proportion, the material has good flexibility, but the number of layered barrier phases is relatively small; the composite material has a Shore A hardness of 60, a tensile strength of 13.2 MPa, and an Akron wear volume of 0.84 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-2 (as shown in Table 1), has a certain high temperature barrier capability, but the flame retardant and mechanical properties are significantly reduced compared to Example 1.
[0074] Example 7
[0075] The difference between this embodiment and Embodiment 1 is that the dosage of mica nanosheets was adjusted and the feeding ratio was controlled so that the mica nanosheets accounted for 30wt% of the total mass of the composite styrene-butadiene rubber material after vulcanization. 42.5g of mica nanosheets modified with silane coupling agent KH570 (thickness approximately 20nm, lateral dimension approximately 5μm, aspect ratio approximately 250) were added to 490g of styrene-butadiene latex, which contained 100g of dry styrene-butadiene rubber (dry styrene-butadiene rubber model SBR1502).
[0076] The proportions of other raw materials, dispersion process, and impregnation vulcanization aid formulation are consistent with those in Example 1; the directional freezing temperature is -196℃, and liquid nitrogen is used as the cold source.
[0077] Freeze-drying temperature -80℃, vacuum degree 1Pa, drying time 72h; hot pressing molding and vulcanization treatment temperature 200℃, pressure 30MPa, heat preservation vulcanization 10min; the high temperature and high pressure short time vulcanization conditions require strict control of time to avoid thermal degradation of rubber matrix.
[0078] In this embodiment, the mica filler achieves a tensile strength of 22.3 MPa and an Akron wear volume of 0.61 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-0 (as shown in Table 1), high temperature burning can form a dense and complete filler, the relative proportion of matrix rubber is reduced, the oriented mica sheets form a large number of continuous layered barriers, the high temperature resistance and ablation resistance barrier effect is significantly improved, but the excessive filler causes the material flexibility to decrease; the composite material Shore A hardness is 83, which is a complete ceramic protective layer.
[0079] Example 8
[0080] The difference between this embodiment and Example 1 is that the lower limit combination of the process range is used. 10g of mica nanosheets modified with silane coupling agent KH570 (thickness approximately 20nm, lateral dimension approximately 5μm, aspect ratio approximately 250) are added to 490g of styrene-butadiene latex, which contains 100g of dry styrene-butadiene rubber (dry styrene-butadiene rubber model SBR1502). The mica nanosheets account for approximately 8wt% of the total mass of the vulcanized composite styrene-butadiene rubber material. The directional freezing temperature is -10℃, the cold source is a low-temperature circulating bath, and unidirectional freezing is used. The freeze-drying temperature is -20℃, the vacuum degree is 100Pa, and the drying time is 12h. The hot-pressing molding-vulcanization temperature is 100℃, the pressure is 1MPa, and the vulcanization time is 120min. The remaining steps are the same as in Example 1.
[0081] This embodiment uses the lower limit of process parameters, resulting in a slow ice crystal growth rate, yet mica nanosheets can still achieve directional arrangement; low-temperature, low-pressure, long-term vulcanization ensures sufficient rubber crosslinking; the composite material has a Shore A hardness of 64, a tensile strength of 14.6 MPa, and an Akron wear volume of 0.81 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-1 (as shown in Table 1), can achieve self-extinguishing upon removal of flame, and its overall performance is better than the comparative example, but slightly lower than Example 1.
[0082] Example 9
[0083] The difference between this embodiment and Example 1 is that the upper limit combination of the process range is used: 10g of mica nanosheets modified with silane coupling agent KH570 (thickness about 20nm, lateral dimension about 5μm, aspect ratio about 250) are added to 490g of styrene-butadiene latex, which contains 100g of dry styrene-butadiene rubber (dry styrene-butadiene rubber model SBR1502). The mica nanosheets account for about 8wt% of the total mass of the composite styrene-butadiene rubber material after vulcanization; the directional freezing temperature is -196℃, the cold source is liquid nitrogen, and the freezing is bidirectional; the freeze-drying temperature is -80℃, the vacuum degree is 1Pa, and the drying time is 72h; the hot pressing molding-vulcanization temperature is 200℃, the pressure is 30MPa, and the vulcanization time is 10min; the remaining steps are the same as in Example 1.
[0084] This embodiment employs the upper limit of process parameters, rapid freezing to induce rapid nucleation and growth of ice crystals, and rapid displacement of mica nanosheets to achieve highly oriented alignment; high temperature and high pressure are used to complete vulcanization molding in a short time; the composite material has a Shore A hardness of 77, a tensile strength of 20.2 MPa, and an Akron wear volume of 0.66 cm³. 3 / 1.61km, flame retardant rating UL-94 / V-0 (as shown in Table 1), excellent wear resistance, high temperature resistance and ablation resistance.
[0085] Comparative Example 1
[0086] The difference between this comparative example and Example 1 is that the anisotropic composite rubber was not prepared using the ice template method; instead, the mica nanosheet / styrene-butadiene latex mixed dispersion obtained from the raw material mixing step was directly frozen in a refrigerator (e.g., Figure 9 (as shown);
[0087] The comparative formulation was identical to that of Example 1, but lacked the ice-template directional freezing process. The mica nanosheets were randomly distributed within the rubber matrix, failing to form a continuous layered "brick-and-mortar" barrier structure. The composite material had a Shore A hardness of 66, a tensile strength of 15.0 MPa, and an Akron wear volume of 0.90 cm³. 3 / 1.61km, no UL-94 flame retardant rating (as shown in Table 1), cannot self-extinguish upon removal of flame, and its high-temperature resistance and ablation resistance are significantly inferior to Example 1, proving that directional freezing of ice templates is a necessary process condition for obtaining high-performance composite materials (e.g. Figure 11 (As shown).
[0088] Comparative Example 2
[0089] The difference between this comparative example and Example 1 is that mica nanosheets (such as...) were not added. Figure 12 (as shown);
[0090] This comparative example does not introduce mica nanosheet functional fillers, and the pure styrene-butadiene rubber matrix does not contain a lamellar barrier phase. The composite material has a Shore A hardness of 58, a tensile strength of 12.0 MPa, and an Akron wear volume of 1.00 cm³. 3 / 1.61km, no UL-94 flame retardant rating (as shown in Table 1), fast burning speed, and the lowest wear resistance and high temperature flame retardant performance among all groups, indicating that mica nanosheets play a key role in improving the overall performance of the material.
[0091] Comparative Example 3
[0092] The difference between this comparative example and Example 1 is that styrene-butadiene latex was not used, the material was not formed, and relevant tests and characterization could not be carried out.
[0093] The comparative example lacks a continuous phase of styrene-butadiene latex rubber, and the system cannot form a complete rubber matrix, so a composite material that can be used for conveyor belts cannot be obtained (as shown in Table 1). This confirms that styrene-butadiene latex is an indispensable matrix raw material for this system.
[0094] The core differences between the embodiments and the comparative examples are the amount and modification method of mica nanosheets, the grade and raw rubber content of styrene-butadiene latex, the freezing method, and whether mica was added or styrene-butadiene latex was used.
[0095] Example 1 uses 10g of KH570 modified mica nanosheets and 100g of dry styrene-butadiene rubber (dry styrene-butadiene rubber model SBR1500) as the base. After directional freezing, impregnation with vulcanizing aids and hot pressing vulcanization, a directional layered structure is obtained, which is self-extinguishing after being removed from the fire and has low wear.
[0096] Table 1 shows the Shore hardness, tensile strength, Akron wear volume, and flame retardancy rating obtained from the embodiments and comparative examples of the present invention.
[0097]
[0098] The foregoing has provided a detailed description of a mica-oriented styrene-butadiene rubber composite material, its preparation method, and a flame-retardant conveyor belt provided by the present invention. The specific embodiments described are merely for the purpose of helping to understand the method and core ideas of the present invention. It should be noted that those skilled in the art can make various improvements and modifications to the present invention without departing from its principles, and these improvements and modifications also fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing mica-oriented styrene-butadiene rubber composite material, characterized in that, include: Mica nanosheets were uniformly dispersed in styrene-butadiene latex to obtain a mixed dispersion of mica nanosheets and styrene-butadiene latex. The mixed dispersion was placed in a directional freezing device for directional freezing treatment, so that the ice crystals grew in a predetermined direction, and the mica nanosheets were oriented along the ice crystal growth direction under the expulsion of the ice crystals, thus obtaining a directional frozen body. The directional cryobody was freeze-dried to remove ice crystals, resulting in an aerogel framework with a directional pore structure composed of mica nanosheets and styrene-butadiene rubber. After impregnating the aerogel skeleton with a vulcanization aid, hot pressing and vulcanization are performed to obtain a styrene-butadiene rubber composite material with mica nanosheets oriented filling.
2. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The dispersion of mica nanosheets in styrene-butadiene latex can be achieved through one or more of the following methods: mechanical stirring, ultrasonic dispersion, and high-shear emulsification.
3. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The directional freezing temperature is -196℃ to -10℃; the freezing method is unidirectional freezing or bidirectional freezing. The cold source for directional freezing can be one or more of the following: liquid nitrogen, dry ice-ethanol bath, low-temperature circulating bath, or semiconductor refrigeration.
4. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The freeze-drying temperature is -80℃ to -20℃, the vacuum degree is 1 to 100 Pa, and the drying time is 12 to 72 hours.
5. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The hot pressing and vulcanization process is carried out at a temperature of 100℃ to 200℃, a pressure of 1 to 30 MPa, and a time of 10 to 120 min.
6. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The mica nanosheets have a thickness of 1–50 nm, a lateral dimension of 0.2–10 μm, and an aspect ratio of not less than 50. The mica nanosheets account for 1 to 30 wt% of the total mass of the composite styrene-butadiene rubber material.
7. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The mica nanosheets are modified mica nanosheets, and the modification methods include one or more of the following: silane coupling agent modification, surfactant modification, and polymer linker modification.
8. The method for preparing a mica-oriented styrene-butadiene rubber composite material according to claim 1, characterized in that: The vulcanization aid includes one or more of the following: vulcanizing agent, accelerator, activator, antioxidant, and reinforcing agent.
9. A mica-oriented styrene-butadiene rubber composite material, prepared by the method for preparing the mica-oriented styrene-butadiene rubber composite material according to any one of claims 1-8; The composite styrene-butadiene rubber material comprises a styrene-butadiene rubber matrix and mica nanosheet fillers oriented therein, wherein the mica nanosheets are oriented along the ice crystal growth direction to form a layered ordered configuration.
10. A styrene-butadiene rubber flame-retardant conveyor belt, comprising the styrene-butadiene rubber composite material as described in claim 9; When preparing the composite styrene-butadiene rubber material, the preset direction of directional freezing is parallel to the direction of the conveyor belt working surface, and the hot pressing direction is perpendicular to the direction of the conveyor belt working surface, so that a layered mica barrier structure parallel to the working surface is formed inside the conveyor belt.
Citation Information
Patent Citations
Composite material with packing in orientated arrangement and preparation method of composite material
CN106810876A
Method for preparing high-thermal-conductivity mica paper based on ice template method
CN114214864A
Sodium alginate / montmorillonite / natural latex aerogel as well as preparation method and application thereof
CN115181322A