Fibrous aerogel and method of making the same
By using fluorinated water glass as raw material, combined with pH adjustment by acid solution and directional cryogenic casting high-temperature heat treatment, high-temperature resistant and high-strength fiber aerogels were prepared, solving the problems of high preparation cost and poor performance, and expanding their application in environmental protection, energy conservation and aerospace fields.
Patent Information
- Application Number
- CN202611556072.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies make it difficult to prepare high-temperature resistant and high-strength fiber aerogels at low cost and high efficiency, and traditional methods have problems such as complex preparation process, high cost and poor thermal insulation performance.
Using fluorinated water glass as raw material, silica sol was prepared by adjusting the pH value with an acid solution. Combined with directional cryogenic casting and high-temperature heat treatment, fiber aerogel was prepared to form a silica network structure and fiber materials were added to improve mechanical properties.
This technology enables the low-cost preparation of high-strength, high-temperature resistant fiber aerogels, which possess excellent mechanical strength and thermal insulation properties, making them suitable for environmental protection, energy conservation, chemical, and aerospace applications.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aerogel technology, and particularly relates to a fiber aerogel and its preparation method. Background Technology
[0002] Aerogels are three-dimensional continuous porous materials with an internal structure composed of interwoven nanoscale pores and a framework. This microstructure endows them with excellent physicochemical properties such as low density, high specific surface area, large porosity, low thermal conductivity, low sound velocity propagation, and low dielectric constant. Furthermore, they can be chemically "tailored," making aerogels promising for a wide range of applications. Fabricating porous aerogel structures from silica materials can combine the advantages of both aerogels and silica, expanding the application range of silica and providing a material foundation for technological innovation in related fields. Silica aerogels have attracted considerable attention due to their nanoporous structure, with porosities exceeding 90%, pore sizes between 1 and 100 nm, and specific surface areas reaching up to 1000 m². 2 / g has a research history of nearly 80 years and has broad application potential in the fields of acoustics, thermodynamics, optics, and mechanics.
[0003] Fiber aerogels possess high strength, flexibility, hydrophobicity, and solvent resistance, overcoming the shortcomings of traditional aerogels in terms of poor mechanical properties and compensating for their application limitations, thus attracting widespread attention in recent years. In recent years, flexible aerogels made of silica, carbonaceous materials, ceramics, and biomass have been successively developed. These aerogel materials have achieved certain results in improving mechanical properties, enhancing mechanical strength, and improving material application performance, demonstrating promising application prospects. Among them, ceramic aerogels, due to their lightweight, porosity, thermal insulation, high temperature resistance, high porosity, and high specific surface area, have broad application value in aerospace, energy conservation and environmental protection, and building insulation fields.
[0004] Sodium silicate (water glass) is a soluble silicate composed of alkali metal oxides and silicon dioxide. Its low price is beneficial for reducing the cost of aerogel preparation, but the lack of a low-cost, short-cycle solution currently limits its application in large-scale ceramic aerogel preparation. Developing a novel, efficient, and economical method that combines the low cost of water glass with the superior performance of ceramic fiber aerogels is of great significance for expanding its application in the field of SiO2 aerogels. Dong et al. (Advanced Composites and Hybrid Materials, 2023, 6(5): 186.) successfully prepared ultra-low density (only 3.4 mg cm⁻¹) aerogels using 3D sol-gel electrospinning technology. -3Al₂O₃ / ZrO₂ fiber aerogel. This material possesses excellent mechanical properties, maintaining good flexibility even at temperatures up to 1300°C, capable of bending 180° and recovering after 90% compressive strain, and remaining structurally stable at 1500°C. However, the preparation process of this material is complex and the production cost is high. Chinese patent CN119841660A uses directional cryogenic casting, chemical vapor deposition, and thermal etching oxidation to prepare a thermally insulating refractory ceramic aerogel. This material exhibits a negative Poisson's ratio effect, retaining 95% of its original height after 100 compression cycles under 50% compressive strain. However, the hot-surface testing temperature of this material is only 900°C, indicating poor thermal insulation performance. Summary of the Invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a high-temperature resistant and high-strength fiber aerogel and its preparation method.
[0006] This invention provides a method for preparing fibrous aerogel, comprising the following steps: S1) Fluorine-containing water glass is mixed with water, and the pH value is adjusted by acid solution to obtain silica sol; S2) The silica sol is dispersed in water, and a binder and fiber material are added sequentially to obtain a precursor solution; S3) The precursor solution is directionally cryogenically cast in a mold, and then freeze-dried and subjected to high-temperature heat treatment in sequence to obtain fiber aerogel.
[0007] Preferably, in step S1), the mass ratio of fluorinated water glass to water is 1:(1~15). The concentration of the acid solution is 0.1~8 mol / L; In step S1), the pH value is adjusted to 1-8; In step S2), the mass ratio of silica sol to water is 1:(1~10). The mass ratio of the silica sol to the binder is 1:(0.1~5). The mass ratio of the silica sol to the fiber material is 1:(0.1~5).
[0008] Preferably, the fluoride ion content in the fluorinated water glass is 0.1% to 5%; The acid solution is selected from one or more of sulfuric acid solution, hydrochloric acid solution, nitric acid solution, acetic acid solution and phosphoric acid solution; The binder is selected from one or more of cellulose nanofibers, chitosan, diatomaceous earth, agarose, polyvinyl alcohol, and polyethylene oxide; The fiber material is selected from one or more of the following: carbon fiber, glass fiber, basalt fiber, aramid staple fiber, polyester staple fiber, silicon oxide fiber, zirconium oxide fiber, titanium oxide fiber, mullite fiber, silicon carbide fiber, boron nitride fiber, silicon nitride fiber, aluminum silicate fiber, and alumina fiber.
[0009] Preferably, the length of the fiber material is 1~150 μm; the aspect ratio of the fiber material is 5~3000.
[0010] Preferably, in step S2), after adding the binder, the mixture is heated and mixed, and then the fiber material is added and the mixture is heated and mixed again to obtain the precursor solution.
[0011] Preferably, the heating and mixing temperature is 60℃~120℃; the heating and mixing time is 5~60 min; The temperature for continued heating and mixing is 60℃~120℃; the time for continued heating and mixing is 5~60 min.
[0012] Preferably, the directional cryogenic casting is a bottom-up gradual freezing process; The freeze-drying temperature is -40℃ to -20℃; the freeze-drying time is 12 to 72 hours; and the freeze-drying pressure is 10 to 50 Pa. The high-temperature heat treatment temperature is 700℃~1000℃; the high-temperature heat treatment time is 0.5~5 h; and the high-temperature heat treatment heating rate is 1~5℃ / min.
[0013] Preferably, after the high-temperature heat treatment, the temperature is reduced to 100℃~300℃ at a rate of 1~5℃ / min, and then cooled in the furnace to obtain fiber aerogel.
[0014] The present invention also provides a fiber aerogel prepared by the above preparation method.
[0015] Preferably, the thermal conductivity of the fiber aerogel is 0.025~0.031 W / (m K); The strength of the fiber aerogel at 10% compression deformation is 0.35~0.45 MPa.
[0016] Compared with the prior art, the preparation method provided by the present invention has the following advantages: (1) This invention uses industrial waste fluorine-containing water glass as raw material to prepare silica sol, and removes fluoride ions from the fluorine-containing water glass efficiently through high-temperature heat treatment, which reduces the cost of raw materials and solves the problem of treating industrial waste fluorine-containing water glass, realizing the high-value utilization of fluorine-containing water glass. (2) The silica sol composite fiber material prepared by industrial waste fluorine-containing water glass as raw material is efficiently prepared into fiber aerogel insulation material by directional freeze casting combined with freeze drying and high temperature heat treatment; the silica sol prepared by water glass will gradually form a silicon oxide network structure during the high temperature heat treatment process, while the fiber material can provide excellent mechanical properties and heat insulation effect. (3) The prepared fiber aerogel exhibits good mechanical strength and excellent thermal stability, which has a positive effect on its application in environmental protection, energy conservation, chemical industry, aviation and other fields. Attached Figure Description
[0017] Figure 1 A photograph of the fiber aerogel prepared in Example 1 of this invention; Figure 2 This is a test image of the fiber aerogel obtained in Example 2 of the present invention using a butane torch. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0019] It should be understood that the expression “one or more of…” individually includes each of the objects described after the expression, as well as various different combinations of two or more of the described objects, unless otherwise understood from the context and usage. The expression “and / or” combined with three or more described objects should be understood to have the same meaning, unless otherwise understood from the context.
[0020] The terms “including,” “having,” or “containing,” including the use of their grammatical synonyms, should generally be understood as open-ended and non-restrictive, for example, not excluding other unstated elements or steps, unless otherwise specifically stated or understood from the context.
[0021] It should be understood that the order of the steps or the order in which certain actions are performed is not important as long as the invention remains operational. Furthermore, two or more steps or actions can be performed simultaneously.
[0022] The use of any and all instances or exemplary language such as “e.g.” or “including” in this document is merely intended to better illustrate the invention and is not intended to limit the scope of the invention unless the claims are made. No language in this specification should be construed as indicating that any unclaimed element is essential to the practice of the invention.
[0023] Furthermore, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values in the specific embodiments have been presented as precisely as possible. However, any value inevitably contains standard deviations due to individual test methods. Therefore, unless explicitly stated otherwise, it should be understood that all ranges, quantities, values, and percentages used in this disclosure are modified with the word "approximately". Here, "approximately" generally means that the actual value is within plus or minus 10%, 5%, 1%, or 0.5% of a specific value or range.
[0024] This invention provides a method for preparing fiber aerogel, comprising the following steps: S1) mixing fluorinated water glass with water, adjusting the pH value using an acid solution to obtain silica sol; S2) dispersing the silica sol in water, and sequentially adding a binder and fiber material to obtain a precursor solution; S3) directionally freezing the precursor solution in a mold, and sequentially subjecting it to freeze-drying and high-temperature heat treatment to obtain fiber aerogel.
[0025] In this invention, there are no special restrictions on the source of any raw materials; they can be commercially available.
[0026] In one specific embodiment of the present invention, the fluoride ion content in the fluorinated water glass is preferably 0.1% to 5%; optionally, the fluoride ion content in the fluorinated water glass is 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5% or any two of the above values.
[0027] In one specific embodiment of the present invention, the fluorinated water glass is derived from silicon dioxide, a byproduct of anhydrous hydrogen fluoride produced by the fluorosilicic acid process.
[0028] Fluorinated water glass is mixed with water, and the pH value is adjusted using an acid solution to obtain silica sol. The preferred mass ratio of the fluorinated water glass to water is 1:(1~15). Optionally, the mass ratio of the fluorinated water glass to water is 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, or any two of the above values. The preferred mixing method is stirring. The preferred mixing time is 5~30 min, more preferably 10~20 min, and even more preferably 10~15 min. After mixing, an acid solution is added to adjust the pH value. The preferred concentration of the acid solution is 0.1~8 mol / L. Optionally, the concentration of the acid solution is 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, etc. The pH value is mol / L, 6 mol / L, 7 mol / L, 8 mol / L, or any two of the above values; the acid solution is preferably one or more of sulfuric acid solution, hydrochloric acid solution, nitric acid solution, acetic acid solution, and phosphoric acid solution; in this invention, the pH value is preferably adjusted to 1~8; optionally, the pH value is adjusted to 1, 2, 3, 4, 5, 6, 7, 8, or any two of the above values.
[0029] The silica sol is dispersed in water; the preferred mass ratio of silica sol to water is 1:(1~10); optionally, the mass ratio of silica sol to water is 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10 or any two of the above values; the dispersion method is preferably ultrasonic oscillation; the preferred ultrasonic oscillation time is 10~60 min; optionally, the ultrasonic oscillation time is 10 min, 20 min, 30 min, 40 min, 50 min, 60 min or any two of the above values.
[0030] Then, a binder and fiber material are added to obtain a precursor solution; the binder is preferably one or more of cellulose nanofibers, chitosan, diatomaceous earth, agarose, polyvinyl alcohol, and polyethylene oxide; the mass ratio of silica sol to binder is preferably 1:(0.1~5); optionally, the mass ratio of silica sol to binder is 1:0.1, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, or any two of the above values; the fiber material is preferably one or more of carbon fiber, glass fiber, basalt fiber, aramid staple fiber, polyester staple fiber, silica fiber, zirconium oxide fiber, titanium oxide fiber, mullite fiber, silicon carbide fiber, boron nitride fiber, silicon nitride fiber, aluminosilicate fiber, and alumina fiber; the length of the fiber material is preferably 1~150 μm; optionally, the length of the fiber material is 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, etc. μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm or any two of the above values; the aspect ratio of the fiber material is preferably 5 to 3000; optionally, the aspect ratio of the fiber material is 5, 10, 20, 50, 80, 100, 150, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000 or any two of the above values; the mass ratio of the silica sol to the fiber material is preferably 1:(0.1~5); optionally, the mass ratio of the silica sol to the fiber material is 1:0.1, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5 or any two of the above values.
[0031] In one specific embodiment of the present invention, the degree of polymerization of the cellulose nanofibers is preferably 300 to 1000; optionally, the degree of polymerization of the cellulose nanofibers is 300, 400, 500, 600, 700, 800, 900, 1000 or any two of the above values.
[0032] In one specific embodiment of the present invention, the molecular weight of the chitosan is preferably 50,000 to 300,000; optionally, the molecular weight of the chitosan is 50,000, 80,000, 100,000, 120,000, 150,000, 180,000, 200,000, 220,000, 250,000, 280,000, 300,000 or a range between any two of the above values.
[0033] In a specific embodiment of the present invention, the molecular weight of the polyvinyl alcohol is preferably 50,000 to 100,000; optionally, the molecular weight of the polyvinyl alcohol is 50,000, 60,000, 70,000, 80,000, 90,000, 100,000 or any two of the above values; the degree of hydrolysis of the polyvinyl alcohol is preferably 87% to 90%; optionally, the degree of hydrolysis of the polyvinyl alcohol is 87%, 88%, 89%, 90% or any two of the above values.
[0034] In one specific embodiment of the present invention, the molecular weight of the polyethylene oxide is preferably 600,000 to 1,000,000; optionally, the molecular weight of the polyethylene oxide is 600,000, 700,000, 800,000, 900,000, 1,000,000 or any two of the above values.
[0035] In one specific embodiment of the present invention, the fiber material is preferably an inorganic fiber material.
[0036] In a specific embodiment of the present invention, in step S2), after adding the binder, it is preferable to heat and mix, and then add the fiber material and continue heating and mixing to obtain a precursor solution; the heating and mixing temperature is preferably 60℃~120℃; optionally, the heating and mixing temperature is 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃ or any two of the above values; the heating and mixing time is preferably 5~60 min; optionally, the heating and mixing time is 5 min, 10 min, 15 min, 20 min, 30 min, 40 min, 50 min, 60 min or any two of the above values; the temperature for continued heating and mixing is preferably 60℃~120℃; optionally, the temperature for continued heating and mixing is 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃ or any two of the above values; the temperature for continued heating and mixing is preferably 5~60 min; optionally, the temperature for continued heating and mixing is 5 min, 10 min, 15 min, 60 min or any two of the above values. min, 20 min, 30 min, 40 min, 50 min, 60 min, or any two of the above values.
[0037] The precursor solution is directionally cryogenically cast in a mold. Directional cryogenic casting can construct a directional porous structure, enhance mechanical flexibility, reduce drying shrinkage, control pore structure, and is a simple and environmentally friendly process suitable for preparing high-performance thermally insulating, flexible, and compressible aerogel materials. The directional cryogenic casting is preferably a bottom-up gradual freezing process. More specifically, liquid nitrogen temperature is transferred vertically through a copper column, causing the precursor solution to freeze gradually from bottom to top. The directional cryogenic casting time is preferably 10-60 min, more preferably 20-40 min, even more preferably 25-35 min, and most preferably 30 min.
[0038] Finally, the fiber aerogel is obtained by freeze-drying and high-temperature heat treatment; the freeze-drying temperature is preferably -40℃ to -20℃; optionally, the freeze-drying temperature is -40℃, -35℃, -30℃, -25℃, -20℃ or any two of the above values; the freeze-drying time is preferably 12 to 72 h; optionally, the freeze-drying time is 12 h, 24 h, 36 h, 48 h, 60 h, 72 h or any two of the above values; the freeze-drying pressure is preferably 10 to 50 Pa; optionally, the freeze-drying pressure is 10 Pa, 20 Pa, 30 Pa, 40 Pa, 50 Pa. Pa or any two of the above values; the heating rate of the high-temperature heat treatment is preferably 1~5℃ / min; optionally, the heating rate of the high-temperature heat treatment is 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min or any two of the above values; the temperature of the high-temperature heat treatment is preferably 700℃~1000℃; optionally, the temperature of the high-temperature heat treatment is 700℃, 800℃, 850℃, 900℃, 1000℃ or any two of the above values; the time of the high-temperature heat treatment, i.e., the holding time, is preferably 0.5~5 h; optionally, the time of the high-temperature heat treatment, i.e., the holding time, is 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h or any two of the above values. During the high-temperature heat treatment, not only can fluoride ions be removed (vaporizing into the gas phase), but the silica sol will also gradually form a silicon oxide network structure.
[0039] In a specific embodiment of the present invention, after the high-temperature heat treatment, the temperature is preferably reduced to 100°C to 300°C at a rate of 1 to 5°C / min, and then cooled in the furnace to obtain a fiber aerogel; optionally, the cooling rate is 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min or any two of the above values; optionally, the temperature is reduced to 100°C, 150°C, 200°C, 250°C, 300°C or any two of the above values.
[0040] This invention innovatively uses fluorinated water glass as a silicon precursor, significantly reducing raw material costs while improving the utilization rate of industrial fluorinated water glass. During high-temperature heat treatment, fluoride ions are efficiently removed from the fluorinated water glass, and the silica sol prepared from the water glass gradually forms a stable silica network structure. The fiber material imparts excellent mechanical strength and thermal insulation properties to the material. This preparation method is characterized by low cost and high efficiency. The prepared fiber aerogel exhibits good mechanical strength and excellent thermal stability, showing broad application prospects in environmental protection, energy conservation, chemical industry, aerospace, and other fields. It has significant practical implications for promoting the industrialization of aerogel materials.
[0041] The present invention also provides a fiber aerogel prepared by the above preparation method.
[0042] In one specific embodiment of the present invention, the thermal conductivity of the fiber aerogel is preferably 0.025~0.031 W / (m K); optionally, the thermal conductivity of the fiber aerogel is 0.025 W / (m K), 0.026 W / (m K), 0.027 W / (m K), 0.028 W / (m K), 0.029 W / (m K), 0.030 W / (m K), 0.031 W / (m K) or a range between any two of the above values.
[0043] In a specific embodiment of the present invention, the strength of the fiber aerogel at 10% compression deformation is preferably 0.35~0.45 MPa; optionally, the strength of the fiber aerogel at 10% compression deformation is 0.35 MPa, 0.36 MPa, 0.37 MPa, 0.38 MPa, 0.39 MPa, 0.40 MPa, 0.41 MPa, 0.42 MPa, 0.43 MPa, 0.44 MPa, 0.45 MPa, or a range between any two of the above values.
[0044] To further illustrate the present invention, the following describes in detail a fiber aerogel and its preparation method provided by the present invention with reference to embodiments.
[0045] All reagents used in the following examples are commercially available; the fluorinated water glass used in the examples is derived from silica, a byproduct of anhydrous hydrogen fluoride produced by the fluorosilicic acid process; the molecular weight of chitosan is 50,000-100,000; the molecular weight of polyvinyl alcohol is 70,000-100,000, and the degree of alcoholysis is 87%-90%; the molecular weight of polyethylene oxide is 800,000-1,000,000; the degree of polymerization of cellulose nanofibers is 500-1,000; and the glass fiber is glass fiber needle-punched felt conforming to the national standard "Glass Fiber Filter Materials" (GB / T 25041-2016) and other specifications.
[0046] The standard for testing the thermal conductivity of the fiber aerogel in the examples is GB / T 10295-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Thermal Insulation Materials"; the standard for testing the strength of the fiber aerogel at 10% compression deformation is GB / T8813-2008 "Determination of Compression Properties of Rigid Foamed Plastics".
[0047] Example 1
[0048] 1.1 Fluoride-containing water glass with a fluoride ion content of 0.1% and deionized water were stirred at a mass ratio of 1:1 for 10 min to make them uniformly mixed. The pH of the mixture was adjusted to 2 using 0.1 M dilute sulfuric acid to obtain silica sol.
[0049] 1.2 Mix water and silica sol at a mass ratio of 10:1 and ultrasonically vibrate for 60 min to disperse them evenly.
[0050] 1.3 Weigh chitosan according to a chitosan to silica sol mass ratio of 0.1:1 and add it to the above uniformly dispersed solution, and stir at 80℃ for 60 min.
[0051] 1.4 Weigh mullite fibers (150 μm in length, aspect ratio 100) and silica sol in a 1:1 mass ratio and add them to the resulting solution. Stir at 80°C for 30 min.
[0052] 1.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). Then, it was freeze-dried at a pressure of 10 Pa and a temperature of -40 °C for 48 h. Finally, the temperature was increased to 900 °C at a heating rate of 2 °C / min and held at 900 °C for 2 h. Then, the temperature was decreased to 200 °C at a heating rate of 2 °C / min and cooled in the furnace to obtain a fiber aerogel with a thickness of 20 mm.
[0053] Figure 1 This is a photograph of the fiber aerogel prepared in Example 1.
[0054] The thermal conductivity of the fiber aerogel obtained in Example 1 was tested to be 0.0281 W / (m K), the strength at 10% compression deformation was 0.371 MPa, and no combustion was observed during 180 s of butane torch testing at 1200℃ (normal contact range, outer flame contact surface), with the back surface temperature being only 336.3℃. After the test, there was no dimensional shrinkage, demonstrating good thermal insulation performance and high-temperature structural stability.
[0055] Example 2
[0056] 2.1 Fluoride-containing water glass with a fluoride ion content of 3% and deionized water were stirred at a mass ratio of 1:3 for 30 min to make them uniformly mixed. The pH of the mixture was adjusted to 1 using 2.5 M dilute hydrochloric acid to obtain silica sol.
[0057] 2.2 Mix water and silica sol at a mass ratio of 3:1 and ultrasonically vibrate for 30 min to disperse them evenly.
[0058] 2.3 Weigh polyvinyl alcohol according to a mass ratio of 2:1 to silica sol and add it to the above uniformly dispersed solution. Stir at 60°C for 30 min.
[0059] 2.4 Weigh silicon carbide fibers (1 μm in length, aspect ratio 3000) and silica sol in a mass ratio of 0.1:1 and add them to the resulting solution. Stir at 60°C for 60 min.
[0060] 2.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). It was freeze-dried for 72 h at a pressure of 25 Pa and a temperature of -20 °C. Finally, the temperature was increased to 900 °C at a rate of 1 °C / min and held at 900 °C for 3 h. The temperature was then decreased to 200 °C at a rate of 1 °C / min and cooled in the furnace to obtain a fiber aerogel with a thickness of 20 mm.
[0061] Testing revealed that the fiber aerogel obtained in Example 2 had a thermal conductivity of 0.0292 W / (m K), a strength of 0.383 MPa at 10% compression deformation, and could rebound within a 5.0% compression ratio. Furthermore, it showed no combustion during a 180-second butane torch test at 1200°C, with a back surface temperature of only 296.4°C, and no dimensional shrinkage after the test, demonstrating excellent thermal insulation performance and high-temperature structural stability. (See also...) Figure 2 , Figure 2 The image shows a test pattern of the fiber aerogel obtained in Example 2 using a butane torch.
[0062] Example 3
[0063] 3.1 Fluoride-containing water glass with a fluoride ion content of 5% and deionized water were stirred at a mass ratio of 1:15 for 60 min to ensure uniform mixing. The pH of the mixture was adjusted to 5 using 8 M dilute nitric acid to obtain silica sol.
[0064] 3.2 Mix water and silica sol at a mass ratio of 1:1 and ultrasonically vibrate for 10 min to disperse them evenly.
[0065] 3.3 Weigh out polyethylene oxide at a mass ratio of 5:1 to silica sol fiber and add it to the above-mentioned uniformly dispersed solution. Stir at 120°C for 5 min.
[0066] 3.4 Weigh glass fiber (15 μm in length, aspect ratio 5) and silica sol in a mass ratio of 5:1 and add it to the resulting solution. Stir at 120°C for 5 min.
[0067] 3.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). Then, it was freeze-dried for 12 h under a pressure of 50 Pa and a temperature of -30 °C. Finally, the temperature was increased to 900 °C at a heating rate of 5 °C / min and held at 900 °C for 5 h. Then, the temperature was decreased to 200 °C at a heating rate of 5 °C / min and cooled in the furnace to obtain a fiber aerogel with a thickness of 20 mm.
[0068] The aerogel obtained in Example 3 was tested and found to have a thermal conductivity of 0.0275 W / (m K), a strength of 0.412 MPa at 10% compression deformation, and the ability to rebound within a 5.0% compression ratio. Furthermore, it showed no combustion during a 180-second test under a butane torch at 1200°C, with a back surface temperature of only 341.2°C, and no dimensional shrinkage after the test, demonstrating excellent thermal insulation performance and high-temperature structural stability.
[0069] Example 4
[0070] 4.1 Fluoride-containing water glass with a fluoride ion content of 2% and deionized water were stirred at a mass ratio of 3:10 for 50 min to ensure uniform mixing. The pH of the mixture was adjusted to 4 using 4 M dilute phosphoric acid to obtain silica sol.
[0071] 4.2 Mix water and silica sol at a mass ratio of 2:1 and ultrasonically vibrate for 35 min to disperse them evenly.
[0072] 4.3 Weigh the binder according to the mass ratio of agarose to silica sol of 3:1 and add it to the above uniformly dispersed solution. Stir at 90°C for 25 min.
[0073] 4.4 Weigh glass fiber (100 μm in length, aspect ratio 1000) and silica sol in a mass ratio of 3:1 and add it to the resulting solution. Stir at 90°C for 35 min.
[0074] 4.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). Then, it was freeze-dried at a pressure of 30 Pa and a temperature of -35 °C for 36 h. Finally, the temperature was increased to 900 °C at a heating rate of 3 °C / min, held at 900 °C for 0.5 h, and then cooled to 200 °C at a heating rate of 3 °C / min and then cooled in the furnace to obtain a fiber aerogel with a thickness of 20 mm.
[0075] The aerogel obtained in Example 4 was tested and found to have a thermal conductivity of 0.0253 W / (m K), a strength of 0.431 MPa at 10% compression deformation, and the ability to rebound within a 5.0% compression ratio. Furthermore, it showed no combustion during a 180-second butane torch test at 1200°C, with a back surface temperature of only 283.9°C, and no dimensional shrinkage after the test, demonstrating excellent thermal insulation performance and high-temperature structural stability.
[0076] Example 5
[0077] 5.1 Fluoride-containing water glass with a fluoride ion content of 4% and deionized water were stirred at a mass ratio of 5:12 for 40 min to make them uniformly mixed. The pH of the mixture was adjusted to 8 using 6 M dilute acetic acid to obtain silica sol.
[0078] 5.2 Mix water and silica sol at a mass ratio of 5:1 and ultrasonically vibrate for 45 min to disperse them evenly.
[0079] 5.3 Weigh out cellulose nanofibers at a mass ratio of 2:1 to silica sol and add them to the above uniformly dispersed solution. Stir at 80°C for 30 min.
[0080] 5.4 Weigh glass fiber (50 μm in length, aspect ratio 50) and silica sol in a mass ratio of 4:1 and add it to the resulting solution. Stir at 80°C for 50 min.
[0081] 5.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). Then, it was freeze-dried at a pressure of 40 Pa and a temperature of -35 °C for 48 h. Finally, the temperature was increased to 900 °C at a heating rate of 2 °C / min and held at 900 °C for 3 h. Then, the temperature was decreased to 200 °C at a heating rate of 2 °C / min and cooled in the furnace to obtain a fiber aerogel with a thickness of 20 mm.
[0082] Testing revealed that the fibrous aerogel obtained in Example 5 had a thermal conductivity of 0.0301 W / (m K) and a strength of 0.392 MPa at 10% compression deformation, exhibiting resilience within a 5.0% compression ratio. Furthermore, it showed no combustion during a 180-second butane torch test at 1200°C, with a back surface temperature of only 304.5°C, and no dimensional shrinkage after the test, demonstrating excellent thermal insulation performance and high-temperature structural stability.
[0083] Comparative Example 1
[0084] 1.1 Fluoride-containing water glass with a fluoride ion content of 0.1% and deionized water were stirred at a mass ratio of 1:1 for 10 min to make them uniformly mixed. The pH of the mixture was adjusted to 2 using 0.1 M dilute sulfuric acid to obtain silica sol.
[0085] 1.2 Mix water and silica sol at a mass ratio of 10:1 and ultrasonically vibrate for 60 min to disperse them evenly.
[0086] 1.3 Weigh chitosan according to a chitosan to silica sol mass ratio of 0.1:1 and add it to the above uniformly dispersed solution, and stir at 80℃ for 60 min.
[0087] 1.4 Weigh mullite fibers (150 μm in length, aspect ratio 100) and silica sol in a 1:1 mass ratio and add them to the resulting solution. Stir at 80°C for 30 min.
[0088] 1.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). After being completely frozen at -40℃, it was directly heated to 900℃ at a heating rate of 2℃ / min without freeze drying. It was held at 900℃ for 2 h, and then cooled to 200℃ at a heating rate of 2℃ / min before being cooled in the furnace.
[0089] Results: During the high-temperature heat treatment, the samples experienced severe cracking and structural collapse due to the rapid melting of ice crystals and the violent escape of water vapor. Intact aerogel blocks could not be obtained; only fragmented, irregular blocks or dense fragments were produced. Because the porous framework was essentially destroyed, the thermal conductivity increased significantly to over 0.12 W / (m·K), making compressive strength impossible to test normally. Furthermore, significant shrinkage and localized ablation were observed during the 1200℃ butane torch test.
[0090] The results show that after directional freezing, ice crystals must be removed by freeze-drying to maintain the skeletal structure, while direct high-temperature heat treatment will cause structural damage due to the violent evaporation of liquid water.
[0091] Comparative Example 2
[0092] The high-temperature heat treatment temperature was changed from 900℃ to 600℃.
[0093] 2.1 Fluoride-containing water glass with a fluoride ion content of 0.1% and deionized water were stirred at a mass ratio of 1:1 for 10 min to make them uniformly mixed. The pH of the mixture was adjusted to 2 using 0.1 M dilute sulfuric acid to obtain silica sol.
[0094] 2.2 Mix water and silica sol at a mass ratio of 10:1 and ultrasonically vibrate for 60 min to disperse them evenly.
[0095] 2.3 Weigh chitosan according to a chitosan to silica sol mass ratio of 0.1:1 and add it to the above uniformly dispersed solution, and stir at 80℃ for 60 min.
[0096] 2.4 Weigh mullite fibers (150 μm in length, aspect ratio 100) and silica sol in a 1:1 mass ratio and add them to the resulting solution. Stir at 80°C for 30 min.
[0097] 2.5 The prepared solution was quickly poured into a polytetrafluoroethylene mold and cryogenically cast for 30 min (the liquid nitrogen temperature was transferred vertically through a copper column, so that the solution was gradually frozen from bottom to top). Then, it was freeze-dried at a pressure of 10 Pa and a temperature of -40℃ for 48 h. Finally, the temperature was increased to 600℃ at a heating rate of 2℃ / min, held at 600℃ for 2 h, and then cooled to 200℃ at a heating rate of 2℃ / min before being cooled in the furnace.
[0098] Results: Due to the incomplete pyrolysis and removal of chitosan at 600℃, organic components remained in the aerogel framework, leading to decreased porosity and increased solid-phase thermal conductivity. The comparative example fiber aerogel was found to have a thermal conductivity of 0.045 W / (m·K) and a strength of 0.28 MPa at 10% compression set. However, it exhibited significant smoke and carbonization after only 60 seconds of testing with a butane torch at 1200℃, with the back side temperature rising to 452℃. After the test, the sample size shrank by approximately 8%, and the surface turned black.
[0099] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing fibrous aerogel, characterized in that, Includes the following steps: S1) Fluorine-containing water glass is mixed with water, and the pH value is adjusted by acid solution to obtain silica sol; S2) The silica sol is dispersed in water, and a binder and fiber material are added sequentially to obtain a precursor solution; S3) The precursor solution is directionally cryogenically cast in a mold, and then freeze-dried and subjected to high-temperature heat treatment in sequence to obtain fiber aerogel.
2. The preparation method according to claim 1, characterized in that, In step S1), the mass ratio of fluorinated water glass to water is 1:(1~15). The concentration of the acid solution is 0.1~8 mol / L; In step S1), the pH value is adjusted to 1-8; In step S2), the mass ratio of silica sol to water is 1:(1~10). The mass ratio of the silica sol to the binder is 1:(0.1~5). The mass ratio of the silica sol to the fiber material is 1:(0.1~5).
3. The preparation method according to claim 2, characterized in that, The fluoride ion content in the fluorinated water glass is 0.1%~5%; The acid solution is selected from one or more of sulfuric acid solution, hydrochloric acid solution, nitric acid solution, acetic acid solution and phosphoric acid solution; The binder is selected from one or more of cellulose nanofibers, chitosan, diatomaceous earth, agarose, polyvinyl alcohol, and polyethylene oxide; The fiber material is selected from one or more of the following: carbon fiber, glass fiber, basalt fiber, aramid staple fiber, polyester staple fiber, silicon oxide fiber, zirconium oxide fiber, titanium oxide fiber, mullite fiber, silicon carbide fiber, boron nitride fiber, silicon nitride fiber, aluminum silicate fiber, and alumina fiber.
4. The preparation method according to claim 1, characterized in that, The length of the fiber material is 1~150 μm; the aspect ratio of the fiber material is 5~3000.
5. The preparation method according to claim 1, characterized in that, In step S2), after adding the binder, the mixture is heated and mixed, and then the fiber material is added and the mixture is heated and mixed again to obtain the precursor solution.
6. The preparation method according to claim 5, characterized in that, The heating and mixing temperature is 60℃~120℃; the heating and mixing time is 5~60 min; The temperature for continued heating and mixing is 60℃~120℃; the time for continued heating and mixing is 5~60 min.
7. The preparation method according to claim 1, characterized in that, The directional cryogenic casting process involves gradual freezing from bottom to top. The freeze-drying temperature is -40℃ to -20℃; the freeze-drying time is 12 to 72 hours; and the freeze-drying pressure is 10 to 50 Pa. The high-temperature heat treatment temperature is 700℃~1000℃; the high-temperature heat treatment time is 0.5~5 h; and the high-temperature heat treatment heating rate is 1~5℃ / min.
8. The preparation method according to claim 7, characterized in that, After high-temperature heat treatment, the temperature is reduced to 100℃~300℃ at a rate of 1~5℃ / min, and then cooled in the furnace to obtain fiber aerogel.
9. The fiber aerogel prepared by the preparation method according to any one of claims 1 to 8.
10. The fiber aerogel according to claim 9, characterized in that, The thermal conductivity of the fiber aerogel is 0.025~0.031 W / (m K); The strength of the fiber aerogel at 10% compression deformation is 0.35~0.45 MPa.
Citation Information
Patent Citations
Heat-insulating fire-resistant elastic ceramic aerogel and preparation method thereof
CN119841660A