PMMA-based recyclable ultra-lightweight material, and preparation method and application thereof
By mixing PMMA-based liquid resin with thermally expanded microspheres and performing a two-stage curing process, the problems of non-recyclability and poor interfacial bonding of thermosetting resins are solved, resulting in the preparation of low-density, recyclable PMMA-based ultralight materials suitable for ship hulls, diving equipment, buoys, and wind turbine blades.
Patent Information
- Application Number
- CN202611482902.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing composite foam materials are non-recyclable due to the use of thermosetting resins, and hollow glass microspheres have high density and poor interfacial bonding with PMMA matrix, making it difficult to meet the application requirements of ultra-lightweight and recyclable materials.
PMMA-based liquid resin was mixed with thermally expandable microspheres, and a two-stage curing process was carried out under closed conditions. The thermoplastic outer shell and internal foaming agent of the thermally expandable microspheres were used to control the exothermic reaction, thus preparing a PMMA-based recyclable ultralight material.
It achieves low density and good interfacial bonding of PMMA-based materials, reducing the material density to 0.10~0.40 g/cm³, and is recyclable, with stable performance, avoiding microcracks and interfacial bonding problems.
Smart Images

Figure CN123152166A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer resin composite material synthesis technology, and in particular to a PMMA-based recyclable ultralight material, its preparation method, and its application. Background Technology
[0002] Foam materials, formed by filling a polymer matrix with lightweight hollow fillers, possess low density and high strength, and are widely used in deep-sea exploration. Commonly used polymer matrix materials for composite foam materials include thermosetting resins such as epoxy resin, unsaturated resin, and phenolic resin, while hollow glass microspheres (HGM) are commonly used as lightweight hollow fillers. However, when the matrix material is a thermosetting resin, the resin cross-linking and curing results in non-recyclable composite foam materials, generating solid waste and causing environmental pollution. Therefore, recyclable thermoplastic resin materials hold promise for wider application. Furthermore, hollow glass microspheres have a minimum density of 0.15 g / cm³. 3 Around 1000 meters, this does not meet the demand for ultralight materials.
[0003] Polymethyl methacrylate (PMMA) is an important transparent engineering plastic, also known as acrylic or plexiglass. PMMA has a density of approximately 1.14~1.20 g / cm³. 3 PMMA possesses good light transmittance, electrical insulation, chemical stability, and mechanical strength. Furthermore, PMMA and its composites can be recycled using MMA monomers as a solvent. Application number 202520274290.2, "An Integrated Recycling Device for Large-Scale PMMA Composite Products," provides an experiment and apparatus for PMMA resin recycling. Therefore, it also has advantages such as recyclability and reusability, making PMMA a viable option for use as a matrix resin in applications requiring lower density.
[0004] Thermally expandable microspheres are polymer microspheres composed of a thermoplastic polymer shell and encapsulated liquid alkane gas. When heated to the vaporization temperature of the internal liquid alkane gas, the microspheres undergo thermal expansion, increasing in diameter to several times their original size. Therefore, when used as a lightweight filler, they significantly reduce the system density.
[0005] Currently, there are no reported studies on the preparation of ultralight materials using PMMA-based liquid resin and thermally expandable microspheres; most studies use hollow glass microspheres to prepare lightweight core materials. Patent application number 201611037872.0 discloses a method for preparing glass microsphere / PMMA composite materials. This patent discloses a method for combining glass microspheres and PMMA using melt extrusion. A certain amount of PMMA, hollow glass microspheres, and functional reagents are mixed and melt-blended using a twin-screw extruder to obtain the PMMA composite material. This invention is simple and easy to operate. However, because glass microspheres are inorganic materials and their surfaces are not organically modified, the interfacial bonding is poor when they are combined with PMMA organic polymers. Furthermore, glass microspheres are prone to cracking when mixed with resin in the extruder, leading to an increase in the overall density of the material and a decrease in other properties such as mechanical properties. Summary of the Invention
[0006] The purpose of this invention is to provide a PMMA-based recyclable ultralight material, its preparation method, and its application, which solves the problems of existing composite foam materials being non-recyclable due to the use of thermosetting resins, and hollow glass microspheres having high density, poor interfacial bonding with the PMMA matrix, and being prone to breakage during processing, making it difficult to meet the application requirements of ultralight and recyclable materials.
[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing a PMMA-based recyclable ultralight material, comprising the following steps: PMMA-based liquid resin was mixed with thermally expanded microspheres to obtain a mixture; Under closed conditions, the mixture is subjected to a first curing and a second curing in sequence to obtain a PMMA-based recyclable ultralight material; The PMMA-based liquid resin includes a liquid resin composed of PMMA and acrylic monomers or a prepolymer mixture of acrylic monomers; When the PMMA-based liquid resin is a liquid resin composed of PMMA and acrylic monomers, an initiator is also added to the mixture; The outer shell of the thermally expandable microspheres is made of thermoplastic material, and the interior of the thermally expandable microspheres is made of foaming agent.
[0008] Furthermore, in the preparation method, in the liquid resin composed of PMMA and acrylic monomers, the acrylic monomers are methyl methacrylate (MMA) or a mixture of MMA and methacrylic acid (MAA), the mass ratio of PMMA to acrylic monomers is 5~50:100, and the relative molecular mass of PMMA is 40,000 to 1,000,000; the mass ratio of the liquid resin composed of PMMA and acrylic monomers to the initiator is 100:0.1~5.
[0009] Furthermore, in the preparation method, the preparation method of the acrylic monomer prepolymer mixture includes the following steps: mixing the acrylic monomer with a prepolymer initiator and performing prepolymerization to obtain the acrylic monomer prepolymer mixture; the acrylic monomer is MMA or a mixture of MMA and MAA; the mass ratio of the acrylic monomer to the prepolymer initiator is 100:0.1~5; the prepolymerization temperature is 20~100℃, and the prepolymerization time is 0.5~5h.
[0010] Furthermore, in the preparation method, the initiator or the prepolymer initiator independently includes azo compound initiators, oxidized initiators, or redox initiators; The azo compound initiator is azobisisobutyronitrile or azobisisoheptanenitrile; The oxidation initiators include tert-butyl peroxyneodecanate, benzoyl peroxide, tert-butyl peroxy(2-ethylhexanoate), tert-butyl peroxyacetate, tetramethylbutyl peroxyneodecanate, dodecyl peroxide, bis(4-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxycarbonate, butyl peroxyneodecanate, dipropyl peroxydicarbonate, diisopropyl peroxydicarbonate, diethoxyethyl peroxydicarbonate, diethoxyhexyl peroxydicarbonate, hexyl peroxydicarbonate, methyl ethyl ketone peroxide, cyclohexanone peroxide, dimethoxybutyl peroxydicarbonate, bis(3-methoxy-3-methoxybutyl) peroxydicarbonate, dibutyl peroxydicarbonate, di(hexadecyl) peroxydicarbonate, ditetradecyl peroxydicarbonate, cumene hydroperoxide, tert-butyl peroxybenzoate, 1,1 One or more of the following: 3,3-tetramethylbutyl peroxypentanoate, hexyl peroxypentanoate, butyl peroxypentanoate, trimethylhexanoyl peroxide, dimethylhydroxybutyl peroxypentanoate, pentyl peroxypentanoate, butyl peroxypentanoate, tert-butyl peroxypentanoate, pentyl peroxypentanoate, tert-butyl peroxypentanoate, tert-amyl peroxy(2-ethyl)hexanoate, didecanoyl peroxide, peracetic acid, and potassium persulfate; The redox initiator comprises a mixture of oxidant and reductant in a molar ratio of 1 to 1.5:1, wherein the oxidant is an oxidizing initiator, and the reductant comprises one or more of N,N'-dimethylaniline, N,N'-dimethyl-p-methylaniline, N,N'-di(2-hydroxypropyl)-p-toluidine, N-methyl-N-2-hydroxyethyl-p-toluidine, N-methyl-N-(2-methacryloyloxyethyl)aniline, and N-methyl-N-(2-methacryloyloxyethyl)-p-toluidine.
[0011] Furthermore, in the preparation method, the thermoplastic material includes one or more of styrene copolymers, polyurethane oligomers, dichloroethylene copolymers, acrylonitrile copolymers, and acrylic copolymers, and the foaming agent includes one or more of ethane, propane, n-pentane, n-hexane, isobutane, and isopentane.
[0012] Furthermore, in the preparation method, the mass ratio of the PMMA-based liquid resin to the thermally expanded microspheres is 100:1~20.
[0013] Furthermore, in the preparation method, the mixing of the thermally expanded microspheres with the liquid resin includes mechanical stirring and / or ultrasonic treatment.
[0014] Furthermore, in the preparation method, the first curing temperature is 20~100℃, and the first curing time is 0.1~48h; The second curing temperature is 80~120℃, and the second curing time is 1~48h.
[0015] The present invention also provides a PMMA-based recyclable ultralight material, wherein the density of the PMMA-based recyclable ultralight material is 0.10~0.40 g / cm³. 3 .
[0016] This invention also provides an application of PMMA-based recyclable ultralight materials in ship hulls, diving equipment, buoys, or wind turbine blades.
[0017] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects: (1) This invention uses thermally expandable microspheres as lightweight fillers, which greatly reduces the density of PMMA-based lightweight materials. At the same time, since the outer shell of the thermally expandable microspheres is a thermoplastic material, when combined with PMMA resin, the interface bonding between the two is better than that of inorganic hollow glass microspheres. As the resin curing reaction continues to release heat, the alkanes inside the thermally expandable microspheres gradually vaporize, and the thermoplastic material on the surface also softens due to heat. The volume of the thermally expandable microspheres increases to several times its original size, which leads to an increase in the overall volume of the material and a decrease in the density of the composite material.
[0018] (2) In the preparation method of the present invention, the resin is prepolymerized first and then mixed with thermally expandable microspheres or the resin and thermally expandable microspheres are mixed and then cured at low temperature and then cured at high temperature. Both methods can make the reaction polymerization mild and controllable. The prepolymerization reaction releases some heat in advance. The preparation method of resin curing at low temperature and then curing at high temperature controls the heat released by the reaction by slowing down the reaction rate. The method of the present invention effectively controls the problem of excessive heat release caused by rapid polymerization of resin, which leads to premature expansion of microspheres and shell wall rupture. This makes the prepared product foam uniformly and stably, reduces the temperature difference between the inside and outside of the cured blank, and eliminates the original microcracks inside the blank.
[0019] (3) In this invention, the resin undergoes a polymerization reaction under the action of the initiator and releases heat. The large amount of heat released causes the alkane liquid inside the thermal expansion microsphere to vaporize and the thermoplastic shell to soften, thereby causing expansion. Therefore, even at a lower external heating temperature, the thermal expansion microsphere can achieve volume expansion and reduce density. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0021] Figure 1 This is a SEM image of the thermally expanded microspheres in Example 1 before expansion; Figure 2 This is a SEM image of the thermally expanded microspheres in Example 1 after expansion. Detailed Implementation
[0022] This invention provides a method for preparing a PMMA-based recyclable ultralight material, comprising the following steps: PMMA-based liquid resin was mixed with thermally expanded microspheres to obtain a mixture; Under closed conditions, the mixture is subjected to a first curing and a second curing in sequence to obtain a PMMA-based recyclable ultralight material; The PMMA-based liquid resin includes a liquid resin composed of PMMA and acrylic monomers or a prepolymer mixture of acrylic monomers; When the PMMA-based liquid resin is a liquid resin composed of PMMA and acrylic monomers, an initiator is also added to the mixture; The outer shell of the thermally expandable microspheres is made of thermoplastic material, and the interior of the thermally expandable microspheres is made of foaming agent.
[0023] In this invention, the liquid resin composed of PMMA and acrylic monomers preferably contains MMA or a mixture of MMA and MAA, more preferably MMA; the ratio of MMA to MAA is not limited, and a ratio known in the art can be used; specifically, the mass ratio of MMA to MAA is 100:10. The preferred mass ratio of PMMA to acrylic monomers is 20-40:100, and more preferably 30:100; The relative molecular mass of PMMA is preferably 40,000 to 100,000, and more preferably 80,000; the source of PMMA is not limited, and commercially available products well known in the art can be used; The mass ratio of the liquid resin composed of PMMA and acrylic monomers to the initiator is preferably 100:0.5~2, more preferably 100:0.5.
[0024] In this invention, the preparation method of the acrylic monomer prepolymer mixture includes the following steps: mixing acrylic monomers with a prepolymer initiator, performing prepolymerization, and obtaining the acrylic monomer prepolymer mixture; The acrylic monomers are preferably MMA or a mixture of MMA and MAA, and more preferably MMA; the ratio of MMA to MAA is not limited, and a ratio well known in the art can be used; specifically, the mass ratio of MMA to MAA is 100:10; The mass ratio of the acrylic monomer to the prepolymer initiator is preferably 100:0.5~2, more preferably 100:1; The prepolymerization temperature is preferably 50~80℃, more preferably 60℃; the prepolymerization time is preferably 1~2h, more preferably 2h. The preferred endpoint for prepolymerization is a system viscosity > 1000 mP·s; after reaching the endpoint, the polymerization reaction is stopped using a cold water bath.
[0025] In this invention, the initiator or the prepolymer initiator preferably includes an oxidizing initiator or a redox initiator, and more preferably an oxidizing initiator. The preferred azo compound initiator is azobisisobutyronitrile (AIBN); The preferred oxidizing initiator is benzoyl peroxide or dodecyl peroxide; The redox initiator comprises a mixture of oxidant and reductant in a molar ratio preferably of 1.1 to 1.3:1, more preferably 1.2:1; the oxidant is an oxidizing initiator; and the reductant is preferably N,N-dimethylaniline.
[0026] In this invention, the thermoplastic material preferably includes a styrene copolymer, an acrylonitrile copolymer, or an acrylic copolymer, and more preferably an acrylic copolymer. The acrylic copolymer includes acrylate polymers.
[0027] In this invention, the foaming agent preferably includes ethane, propane, n-pentane, n-hexane, isobutane, or isopentane, and more preferably n-hexane.
[0028] In this invention, the thermally expandable microspheres include one or more of polystyrene microspheres, vinyl chloride microspheres, polyurethane microspheres, acrylonitrile microspheres, and acrylate microspheres, preferably polystyrene microspheres, polyurethane microspheres, or acrylate microspheres, and more preferably acrylate microspheres. The names of the substances in the thermally expandable microspheres refer to the type of outer shell material; the internal foaming agent can be selected from one or more of the above-mentioned materials.
[0029] In this invention, the diameter (before expansion) of the thermally expandable microspheres is preferably 2 to 100 μm, the expansion rate of the thermally expandable microspheres is preferably 2 to 50 times, and the thermal expansion temperature of the thermally expandable microspheres is preferably 80 to 130°C.
[0030] In this invention, the source of the thermally expandable microspheres is not limited, and commercially available products well known in the art can be used.
[0031] In this invention, the mass ratio of the PMMA-based liquid resin to the thermally expanded microspheres is preferably 100:5~15, and more preferably 100:10.
[0032] In this invention, the addition of the thermally expanded microspheres is preferably achieved by mechanical stirring or ultrasonic treatment, and more preferably by mechanical stirring.
[0033] In this invention, the conditions for mechanical stirring include: using a kneader or a device with a stirring paddle for mechanical stirring; the stirring speed is preferably 500~5000 r / min, more preferably 600 r / min; the stirring time is preferably 10~30 min, more preferably 20 min; The conditions for ultrasonic treatment include: using an ultrasonic dispersion device, and the ultrasonic treatment time is preferably 10 to 60 minutes, more preferably 10 minutes.
[0034] In this invention, the sealed conditions are preferably carried out in a closed mold cavity.
[0035] In this invention, the first curing temperature is preferably 35~80℃, more preferably 60℃; the first curing time is preferably 2~24h, more preferably 12h.
[0036] In this invention, the second curing temperature is preferably 90~110℃, more preferably 100℃; the second curing time is preferably 3~24h, more preferably 4h. After curing, the material is cooled and removed. During the curing process, the resin solidifies and the microspheres expand completely.
[0037] The present invention also provides a PMMA-based recyclable ultralight material, wherein the density of the PMMA-based recyclable ultralight material is preferably 0.15~0.30 g / cm³. 3 Further preferred is 0.26 g / cm³ 3 .
[0038] This invention also provides an application of PMMA-based recyclable ultralight materials in ship hulls, diving equipment, buoys, or wind turbine blades.
[0039] In this invention, the method of application is not limited, and any solution well known in the art can be used.
[0040] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0041] Example 1
[0042] This embodiment provides a method for preparing a PMMA-based recyclable ultralight material, including the following steps: PMMA macromolecules with a relative molecular weight of 80,000 (Dongguan Hongxing New Materials Co., Ltd.) were dissolved in MMA monomers (Shanghai Macklin, China), with PMMA accounting for 30% of the total mass of MMA. Then, a binary liquid resin of PMMA+MMA, an initiator (molar ratio of benzoyl peroxide: N,N-dimethylaniline = 1.2:1), and thermally expandable microspheres were mixed at a mass ratio of 100:0.5:5. The thermally expandable microspheres were acrylate microspheres (shell of thermoplastic acrylate polymer, internal foaming agent of low-boiling hydrocarbon n-hexane, expansion rate of 2~50 times, thermal expansion temperature of 80~130℃; Shandong Feipi New Materials Technology Co., Ltd.). The thermally expandable microspheres were added by mechanical stirring at a stirring speed of 600 r / min for 20 min to obtain a liquid mixture. The above mixture is poured into a closed mold cavity, heated to 35°C for curing and kept at that temperature for 12 hours. After the material has set, the temperature is raised to 100°C for post-curing for 4 hours. Finally, the cured material is removed by cooling, thus obtaining the PMMA-based recyclable ultralight material.
[0043] Referring to ASTM D 4052-2011 for the density of composite materials and GB / T 8813-2020 for the compressive strength of composite materials, the density of the PMMA-based recyclable ultralight material prepared in Example 1 was tested to be 0.26 g / cm³. 3 Its compressive strength is 32 MPa.
[0044] The thermally expanded microspheres in Example 1 were observed by SEM before expansion, and the results are as follows: Figure 1 As shown, the particle size range of the thermally expanded microspheres is approximately 15~70μm.
[0045] The thermally expanded microspheres from Example 1 were expanded in the resin and then observed by SEM. The results are as follows: Figure 2 As shown, the particle size range of the thermally expanded microspheres is 35~130μm at this time.
[0046] Example 2
[0047] This embodiment provides a method for preparing a PMMA-based recyclable ultralight material, including the following steps: A certain amount of MMA monomer (Shanghai Maclean, China) was weighed and initiator LPO was added. The mass ratio of MMA monomer to initiator dodecyl peroxide was 100:1. The mixture was heated to 60°C for prepolymerization reaction for 2 hours. When the viscosity of the system increased to 1000 mP·s, heating was stopped and the mixture was cooled to room temperature in an ice-water bath. At this time, thermally expandable microspheres were added to the high-viscosity resin system by kneading and stirring. The thermally expandable microspheres were polystyrene thermally expandable microspheres (shell is styrene copolymer, internal foaming agent is n-hexane, average particle size before expansion is 2~6 μm, expansion rate is 2~50 times, thermal expansion temperature is 80~120°C, Nouryon (USA)). The mass ratio of resin system to thermally expandable microspheres was 100:10. The stirring speed was 600 r / min, and the mixture was stirred for 20 min. After stirring and mixing, the mixture was vacuumed to remove bubbles and obtain the mixture. The mixture is then poured into a sealed mold, heated to 60°C and reacted for 2 hours, then heated to 110°C and kept at that temperature for 3 hours. After cooling to room temperature, PMMA-based recyclable ultralight material is obtained.
[0048] Referring to the test method of Example 1, the density of the PMMA-based recyclable ultralight material prepared in Example 2 is 0.15 g / cm³. 3 The compressive strength is 20 MPa.
[0049] Example 3
[0050] PMMA macromolecules with a relative molecular weight of 50,000 (Dongguan Hongxing New Materials Co., Ltd.) were dissolved in a mixture of MMA monomers (Shanghai Maclean, China) and MAA monomers, with PMMA accounting for 20% of the total mass of MMA+MAA and the mass ratio of MMA to MAA being 100:10. Then, a liquid resin composed of PMMA+MMA+MAA, an initiator (molar ratio of dodecyl peroxide: N,N-dimethylaniline = 1.1:1), and thermally expandable microspheres were mixed at a mass ratio of 100:1:10. The expanded microspheres are acrylonitrile microspheres (the shell is acrylonitrile oligomer, the internal foaming agent is the low-boiling-point hydrocarbon isobutane, the average particle size before expansion is 10~20μm, the expansion rate is 2~50 times, and the thermal expansion temperature is 80~130℃; Nouryon (USA)). The thermally expanded microspheres are first added by mechanical stirring at a speed of 500r / min for 20min, and then dispersed by ultrasonic equipment at room temperature for 10min to obtain a uniform liquid mixture. The above mixture is poured into a closed mold cavity, heated to 40°C for curing and kept at that temperature for 4 hours. After the material has set, the temperature is raised to 120°C for post-curing for 6 hours. Finally, the cured material is removed by cooling, thus obtaining the PMMA-based recyclable ultralight material.
[0051] Referring to the test method of Example 1, the density of the PMMA-based recyclable ultralight material prepared in Example 3 is 0.13 g / cm³. 3 The compressive strength is 35 MPa.
[0052] Comparative Example 1
[0053] The difference from Example 1 is that the thermally expandable microspheres were replaced with hollow glass microspheres (Zhengzhou Shenglete Hollow Glass Microsphere New Material Co., Ltd., HL20), with a particle size of 110 μm and a density of 0.20 g / cm³. 3 With all other conditions unchanged, the above mixture is poured into a closed mold cavity, heated to 35°C for curing and kept at that temperature for 12 hours, then heated to 100°C for post-curing for 4 hours, and finally cooled down to remove the cured material, thus obtaining the PMMA-based recyclable lightweight material.
[0054] Referring to the test method of Example 1, the density of the PMMA-based recyclable lightweight material prepared in Comparative Example 1 was 0.94 g / cm³. 3 The compressive strength is 90 MPa. Comparative analysis revealed that the PMMA composite lightweight material obtained using thermally expandable microspheres as a lightweight filler has a lower density and better interfacial bonding. Although the compressive strength is not as high as when hollow glass microspheres are used as filler, the density is reduced by about three times.
[0055] Comparative Example 2
[0056] Unlike Example 2, in this comparative example, the resin, initiator, and thermally expanded microspheres were mixed directly at room temperature, and after being mixed evenly, they were heated and cured. The curing conditions remained unchanged: 60°C for 4 hours, and then 110°C for 3 hours.
[0057] Experiments revealed that the concentrated release of heat from the resin in Comparative Example 2 caused the shell walls of the thermally expanded microspheres to rupture prematurely. Before the shells had fully softened, the internal gas burst out due to excessive pressure. At this point, the expansion ratio of the microspheres decreased significantly, and the density of the composite material decreased only slightly. When many microsphere shells ruptured, the released internal gas could even inhibit the polymerization reaction of the resin, preventing the resin from curing and ultimately causing the product to fail to be molded.
[0058] Recovery Experiment: A small piece of the PMMA ultralight material prepared in Example 1 was placed in a sample vial containing MMA monomers. The vial was then placed in a shaker to accelerate the dissolution of the PMMA-based ultralight material. The shaker speed was set to 200 rpm, and the temperature was room temperature. Observation showed that as the dissolution time increased, the volume of the sample continuously decreased, and the matrix resin was gradually dissolved into the MMA monomer solution. The thermally expanded microspheres detached and dispersed in the MMA monomers. After several hours of dissolution, the sample was completely decomposed by the MMA monomers, and the matrix resin was completely dissolved.
[0059] In summary, the method of this invention uses thermally expandable microspheres as a lightweight filler, which greatly reduces the density of the resin. Furthermore, because the outer shell of the thermally expandable microspheres is a thermoplastic material, the interfacial bonding between them and PMMA resin is better compared to inorganic hollow glass microspheres when combined.
[0060] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a PMMA-based recyclable ultralight material, characterized in that, Includes the following steps: PMMA-based liquid resin was mixed with thermally expanded microspheres to obtain a mixture; Under closed conditions, the mixture is subjected to a first curing and a second curing in sequence to obtain a PMMA-based recyclable ultralight material; The PMMA-based liquid resin includes a liquid resin composed of PMMA and acrylic monomers or a prepolymer mixture of acrylic monomers; When the PMMA-based liquid resin is a liquid resin composed of PMMA and acrylic monomers, an initiator is also added to the mixture; The outer shell of the thermally expandable microspheres is made of thermoplastic material, and the interior of the thermally expandable microspheres is made of foaming agent.
2. The preparation method according to claim 1, characterized in that, In the liquid resin composed of PMMA and acrylic monomers, the acrylic monomers are MMA or a mixture of MMA and MAA, the mass ratio of PMMA to acrylic monomers is 5~50:100, and the relative molecular mass of PMMA is 40,000 to 1,000,000; the mass ratio of the liquid resin composed of PMMA and acrylic monomers to the initiator is 100:0.1~5.
3. The preparation method according to claim 1, characterized in that, The preparation method of the acrylic monomer prepolymer mixture includes the following steps: mixing acrylic monomers with a prepolymer initiator and performing prepolymerization to obtain an acrylic monomer prepolymer mixture; the acrylic monomer is MMA or a mixture of MMA and MAA; the mass ratio of the acrylic monomer to the prepolymer initiator is 100:0.1~5; the prepolymerization temperature is 20~100℃, and the prepolymerization time is 0.5~5h.
4. The preparation method according to claim 2 or 3, characterized in that, The initiator or the prepolymer initiator independently includes azo compound initiators, oxidative initiators, or redox initiators; The azo compound initiator is azobisisobutyronitrile or azobisisoheptanenitrile; The oxidation initiators include tert-butyl peroxyneodecanate, benzoyl peroxide, tert-butyl peroxy(2-ethylhexanoate), tert-butyl peroxyacetate, tetramethylbutyl peroxyneodecanate, dodecyl peroxide, bis(4-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, butyl peroxyneodecanate, dipropyl peroxydicarbonate, diisopropyl peroxydicarbonate, diethoxyethyl peroxydicarbonate, diethoxyhexyl peroxydicarbonate, hexyl peroxydicarbonate, methyl ethyl ketone peroxide, cyclohexanone peroxide, dimethoxybutyl peroxydicarbonate, and bis(3-methoxy-3-methoxybutyl) peroxydicarbonate. Dicarbonate, dibutyl peroxydicarbonate, di(hexadecyl)dicarbonate peroxide, ditetradecyl peroxydicarbonate, cumene hydroperoxide, tert-butyl peroxybenzoate, 1,1,3,3-tetramethylbutyl peroxypentanoate, hexyl peroxypentanoate, butyl peroxypentanoate, trimethylhexanoyl peroxide, dimethylhydroxybutyl peroxydecanoate, pentyl peroxydecanoate, butyl peroxydecanoate, tert-butyl peroxyheptanoate, pentyl peroxypentanoate, tert-butyl peroxypentanoate, tert-amyl peroxy(2-ethyl)hexanoate, didecyl peroxide, peracetic acid, potassium persulfate; The redox initiator comprises a mixture of oxidant and reductant in a molar ratio of 1 to 1.5:1, wherein the oxidant is an oxidizing initiator, and the reductant comprises one or more of N,N'-dimethylaniline, N,N'-dimethyl-p-methylaniline, N,N'-di(2-hydroxypropyl)-p-toluidine, N-methyl-N-2-hydroxyethyl-p-toluidine, N-methyl-N-(2-methacryloyloxyethyl)aniline, and N-methyl-N-(2-methacryloyloxyethyl)-p-toluidine.
5. The preparation method according to claim 1, characterized in that, The thermoplastic material includes one or more of styrene copolymers, polyurethane oligomers, dichloroethylene copolymers, acrylonitrile copolymers, and acrylic copolymers, and the foaming agent includes one or more of ethane, propane, n-pentane, n-hexane, isobutane, and isopentane.
6. The preparation method according to claim 1, characterized in that, The mass ratio of the PMMA-based liquid resin to the thermally expandable microspheres is 100:1~20.
7. The preparation method according to claim 1, characterized in that, The thermally expanded microspheres are added by mechanical stirring and / or ultrasonic treatment.
8. The preparation method according to claim 1, characterized in that, The first curing temperature is 20~100℃, and the first curing time is 0.1~48h; The second curing temperature is 80~120℃, and the second curing time is 1~48h.
9. A PMMA-based recyclable ultralight material prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The density of the PMMA-based recyclable ultralight material is 0.10~0.40 g / cm³. 3 .
10. The application of the PMMA-based recyclable ultralight material of claim 9 in ship hulls, diving equipment, buoys or wind turbine blades.
Citation Information
Patent Citations
Preparation method of glass bead / PMMA composite material
CN106700373A