Deep eutectic solvents and their applications, method for devulcanization and recycling of scrap tire rubber powder
By using a low eutectic solvent composed of amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids in a weight ratio of 2-3.5:1-2:1, efficient and green desulfurization of waste tire rubber powder has been achieved, solving the problems of high energy consumption, high pollution, and poor performance of reclaimed rubber in traditional processes. It is suitable for high value-added fields.
Patent Information
- Application Number
- CN202611166950.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-24
AI Technical Summary
Existing waste tire recycling technologies suffer from high energy consumption, high pollution, and poor performance of reclaimed rubber. Traditional desulfurization processes are difficult to achieve low cost, greenness, and high efficiency, and existing eutectic solvent systems have insufficient desulfurization efficiency and selectivity.
A eutectic solvent composed of amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids in a weight ratio of 2-3.5:1-2:1 is used to selectively break sulfur crosslinks while preserving the rubber backbone structure, thereby achieving efficient desulfurization.
It efficiently breaks sulfur crosslinks under mild conditions, reducing production costs, pollution, and improving the mechanical properties and stability of reclaimed rubber. It is suitable for high value-added fields and industrial production.
Smart Images

Figure SMS_1 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of waste rubber resource utilization technology, specifically to eutectic solvents and their applications, and methods for desulfurizing and recovering waste tire rubber powder. Background Technology
[0002] Currently, waste tire recycling mainly focuses on reclaimed rubber, rubber powder, and pyrolysis, with a formal recycling rate of approximately 92%, but the high-value utilization rate is low. Existing desulfurization processes generally suffer from harsh reaction conditions, poor bond-breaking selectivity, and high energy consumption and pollution. Furthermore, desulfurizing agents are expensive, difficult to recycle, have complex process control, and poor batch-to-batch product stability, severely restricting the industrial application of high-value waste rubber. Physical pulverization only processes waste tires into rubber powder without destroying the vulcanization cross-linking network, resulting in rubber powder with low activity and poor interfacial compatibility, making it unsuitable as a direct substitute for virgin rubber and only applicable to low-end filler applications. High-temperature dynamic desulfurization is the current mainstream process, relying on high temperature and pressure to break cross-linking bonds. This method easily damages the rubber backbone while destroying the cross-linking structure, leading to performance degradation of reclaimed rubber. It also suffers from high energy consumption, significant safety hazards, and the production process easily generates odorous waste gas and wastewater, with excessive levels of harmful substances such as polycyclic aromatic hydrocarbons. Chemical desulfurization methods mostly use organic solvents, which, while possessing some desulfurization effect, suffer from high solvent toxicity, low recovery efficiency, high cost, and are prone to secondary pollution, limiting their large-scale application. Therefore, it is urgent to develop safe, efficient, and green waste rubber powder desulfurization technology.
[0003] To address the aforementioned technical challenges, some existing technologies have proposed improvement solutions, but some insurmountable drawbacks remain. For example, CN104387611A discloses a method for desulfurizing and regenerating waste rubber using supercritical CO2 fluid combined with a desulfurizing agent and microwave heating. This method achieves low regeneration temperatures and does not require large amounts of softening oil, but the process is complex, demands strict equipment and operational requirements, and has high energy costs, making low-cost, continuous industrial production difficult. CN104163937A discloses a method for promoting waste rubber desulfurization using ionic liquids, employing a certain amount of rubber softener and desulfurizing agent. However, these softeners and desulfurizers produce toxic and harmful substances, severely polluting the environment and lacking a true green industrialization prospect. Furthermore, the high cost of ionic liquids also limits industrial application.
[0004] Eutectic solvent desulfurization technology offers a green and innovative direction for the resource utilization of waste rubber. Eutectic solvents, formed by the combination of hydrogen bond donors and acceptors, are characterized by readily available raw materials, simple preparation, low volatility, non-toxicity, biodegradability, and good thermal stability, meeting the requirements of green chemical development. Not only are their desulfurization reaction conditions mild, requiring no high temperature or high pressure, but they can also selectively break sulfur cross-links, preserving the rubber backbone structure to the greatest extent and significantly improving the activity and performance of reclaimed rubber. Furthermore, the solvent is recyclable, effectively reducing production costs and waste emissions, with no risk of secondary pollution. Compared to ionic liquids and traditional chemical desulfurization methods, eutectic solvents combine environmental friendliness and economy, making them suitable for high-value-added fields such as rubber powder-modified asphalt and high-quality reclaimed rubber products, promoting the transformation of waste rubber from low-end disposal to high-value recycling.
[0005] However, most of the existing eutectic solvent desulfurization systems are simple binary (hydrogen bond donor-hydrogen bond acceptor) systems, which can only play a basic role in weakening hydrogen bonds and have limited ability to break bonds in strong sulfur crosslinking networks. Their desulfurization efficiency and selectivity are far from meeting the requirements for industrialization. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of traditional desulfurization processes, such as high energy consumption, high pollution, and poor performance of reclaimed rubber.
[0007] To achieve the above objectives, a first aspect of the present invention provides a eutectic solvent containing an amide substance, an α-hydrogen-containing quaternary ammonium halide, and a reducing carboxylic acid in a weight ratio of 2-3.5:1-2:1.
[0008] The second aspect of the present invention provides the application of the eutectic solvent described in the first aspect in a desulfurization process.
[0009] A third aspect of the present invention provides a method for desulfurizing and recovering waste tire rubber powder, the method comprising: (1) The waste tire rubber powder and the eutectic solvent are subjected to desulfurization treatment to obtain intermediate material; the sulfur content of the waste tire rubber powder is 1.5-2.8 wt%; (2) In the presence of organic additives, the intermediate material is subjected to solid-liquid separation to obtain desulfurized rubber powder with a sol content of 19-25 wt%. In step (1), the eutectic solvent is the eutectic solvent described in the first aspect.
[0010] Through the above technical solution, the present invention has at least the following advantages compared with the prior art: (1) The eutectic solvent used in this invention relies on hydrogen bonding and coordination to selectively break the SS and SC crosslinking bonds at a lower temperature without destroying the CC main chain. This achieves efficient desulfurization while preserving the rubber macromolecular structure, allowing the reclaimed rubber to maintain good mechanical properties and avoiding strength reduction caused by high-temperature cracking.
[0011] (2) The eutectic solvent used in this invention is synthesized from non-toxic and readily available raw materials. When used, there is no organic solvent volatilization or foul odor. The reaction conditions are mild and no toxic byproducts are produced. It can be recycled and reused. It can replace traditional high-temperature, oil-based, and dynamic desulfurization processes, which are highly polluting, to achieve green recycling of waste rubber powder and effectively reduce costs.
[0012] (3) The desulfurization and recycling method of waste tire rubber powder provided by the present invention can reduce the crosslinking density of rubber powder, improve plasticity, and make it easier to mix and process compared with traditional thermal desulfurization or chemical desulfurization. At the same time, polar groups are introduced on the surface to improve the interfacial compatibility with the matrix rubber, asphalt, etc., and improve the mechanical properties and application stability of recycled materials.
[0013] (4) The desulfurization and recycling method of waste tire rubber powder provided by the present invention solves the problems of high energy consumption, large pollution and poor performance of recycled rubber in traditional desulfurization process, and has excellent economic and environmental benefits, suitable for industrial production; and can achieve high desulfurization rate.
[0014] (5) The desulfurization and recycling method for waste tire rubber powder provided by the present invention has mild process conditions, simple operation and low operating cost. Detailed Implementation
[0015] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0016] In this invention, an α-hydrogen-containing quaternary ammonium halide refers to a quaternary ammonium halide in which at least one carbon atom bonded to quaternary nitrogen has at least one hydrogen atom.
[0017] Sol content refers to the polymer phase portion dissolved by Soxhlet extraction (using organic solvents such as toluene, chloroform, and THF) after the selective cleavage of CS monosulfide / disulfide / polysulfide crosslinking bonds in a eutectic solvent breaks down the network chain into non-crosslinked, freely soluble linear rubber macromolecules.
[0018] As previously stated, a first aspect of the present invention provides a eutectic solvent containing an amide, an α-hydrogen-containing quaternary ammonium halide, and a reducing carboxylic acid in a weight ratio of 2-3.5:1-2:1.
[0019] During their research, the inventors of this invention discovered that a eutectic solvent containing amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids in a weight ratio of 2-3.5:1-2:1 can achieve efficient desulfurization through a triple synergistic mechanism of hydrogen bond polarization, nucleophilic attack, and reduction bond breaking. Specifically, the α-hydrogen atoms in the α-hydrogen-containing quaternary ammonium halides, bonded to nitrogen, can polarize sulfur atoms and form weak hydrogen bonds, effectively weakening the CS and SS crosslinking bonds; the amide groups in the amides undergo nucleophilic attack on activated sulfur bonds at high temperatures, promoting the breaking of crosslinking bonds; and the reducing carboxylic acid further breaks sulfur bonds through reduction and inhibits side reactions. The synergistic effect of these three mechanisms allows for the selective breaking of sulfur crosslinking bonds (SS and CS bonds) in vulcanized rubber under mild conditions, disrupting the three-dimensional network structure while preserving the integrity of the rubber backbone (CC bonds).
[0020] Preferably, the amide is selected from at least one of formamide, acetamide, propionamide, butyramide, hexamethylenetetramine, benzamide, caprolactam, pyrrolidone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide, and more preferably from at least one of formamide, acetamide, hexamethylenetetramine, N-methylpyrrolidone, caprolactam, and N,N-dimethylacetamide.
[0021] Preferably, the α-hydrogen-containing quaternary ammonium halide is an α-hydrogen-containing quaternary ammonium chloride and / or an α-hydrogen-containing quaternary ammonium bromide.
[0022] Preferably, the α-hydrogen-containing quaternary ammonium chloride is selected from choline chloride, tetramethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, tetrabutylammonium chloride, benzyltrimethylammonium chloride, dodecyltrimethylammonium chloride, and hexadecyltrimethylammonium chloride, and more preferably at least one of choline chloride, tetrabutylammonium chloride, and benzyltrimethylammonium chloride.
[0023] In a preferred embodiment, the α-hydrogen-containing quaternary ammonium bromide is tetrabutylammonium bromide and / or choline bromide, preferably tetrabutylammonium bromide.
[0024] Preferably, the reducing carboxylic acid is selected from at least one of formic acid, acetic acid, oxalic acid, lactic acid, malic acid, citric acid, ascorbic acid, thioglycolic acid, gluconic acid, and tartaric acid, and more preferably from at least one of formic acid, oxalic acid, lactic acid, malic acid, and ascorbic acid.
[0025] Preferably, the viscosity of the eutectic solvent at 30°C is 3-200 mPa·s.
[0026] The present invention does not impose any particular limitations on the preparation process of the eutectic solvent, as long as the obtained eutectic solvent system can be completely melted and form a homogeneous and transparent liquid. For example, the eutectic solvent is prepared by a method including the following steps: The eutectic solvent is obtained by contact mixing of amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids at 60-100°C.
[0027] As previously stated, the second aspect of the present invention provides the application of the eutectic solvent described in the first aspect in a desulfurization process.
[0028] In a preferred embodiment, the desulfurization rate of the eutectic solvent is ≥83wt%, more preferably ≥90wt%, and even more preferably ≥92wt%.
[0029] As mentioned above, a third aspect of the present invention provides a method for desulfurizing and recovering waste tire rubber powder, the method comprising: (1) The waste tire rubber powder and the eutectic solvent are subjected to desulfurization treatment to obtain intermediate material; the sulfur content of the waste tire rubber powder is 1.5-2.8 wt%; (2) In the presence of organic additives, the intermediate material is subjected to solid-liquid separation to obtain desulfurized rubber powder with a sol content of 19-25 wt%. In step (1), the eutectic solvent is the eutectic solvent described in the first aspect.
[0030] The inventors discovered that by using the above method, the cross-linking network of the desulfurized rubber powder is significantly destroyed, making it suitable for direct use in the processing of recycled rubber. The eutectic solvent used in the raw materials can also be recycled.
[0031] Preferably, in step (1), the average particle diameter of the waste tire rubber powder is 120-180 μm.
[0032] Preferably, in step (1), the rubber hydrocarbon content in the waste tire rubber powder is ≥42wt%, the ash content is ≤10wt%, and the carbon black content is ≥26wt%. It should be noted that the remaining components in the waste tire rubber powder are aromatic softening oil, fatty acids, anti-aging additives, and trace amounts of sulfide salt components.
[0033] Preferably, in step (1), the amount of the eutectic solvent used is 8-25 mL relative to 1 g of the waste tire rubber powder.
[0034] In a preferred embodiment, in step (2), the organic auxiliary is ethanol and / or acetone.
[0035] Preferably, in step (1), the conditions for the desulfurization treatment include: a temperature of 80-100℃, a stirring rate of 300-600rpm, and a time of 1-4h.
[0036] The method provided by this invention also includes post-processing steps such as washing and drying. For example, the filter cake obtained from the solid-liquid separation is washed and dried sequentially to obtain the desulfurized rubber powder; the washing is performed 2-3 times; the drying conditions include a temperature of 60-80℃ and a time of 4-6 hours. Further details are omitted here and should not be construed as limiting the invention by those skilled in the art.
[0037] The present invention will be described in detail below through examples. In the following examples, unless otherwise specified, the pharmaceuticals and reagents used are all conventional commercially available products.
[0038] Waste tire rubber powder: purchased from China Rubber Resources Recycling (Suzhou) Co., Ltd., with an average particle diameter of 120-180μm and a sulfur content of 1.5-2.8wt%; the rubber hydrocarbon content is ≥42wt%, the ash content is ≤10wt%, the carbon black content is ≥26wt%, and the remainder consists of aromatic softening oil, fatty acids, anti-aging additives, and trace amounts of sulfide salt components.
[0039] The following preparation examples illustrate the preparation method of the eutectic solvent provided by the present invention. Preparation Example 1 According to the raw materials and their amounts shown in Table 1, weigh out amide substances, α-hydrogen-containing quaternary ammonium halides and 10g of reducing carboxylic acids, mix and heat to 80℃ for contact mixing, keep warm for 2h, and obtain a eutectic solvent.
[0040] The remaining preparation examples were carried out using a similar method to Preparation Example 1, with the differences shown in Table 1. Each example yielded a eutectic solvent, and its viscosity at 30°C was tested using a rotary digital viscometer.
[0041] Table 1
[0042] Note: "Weight ratio of the three" refers to the weight ratio of amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids; "—" indicates that the substance is not added; "viscosity" refers to the viscosity of the eutectic solvent at 30°C.
[0043] The following examples illustrate the method for desulfurizing and recycling waste tire rubber powder provided by the present invention. Example 1 (1) Mix waste tire rubber powder (3g) with the eutectic solvent (DES-1) prepared above for desulfurization treatment to obtain intermediate material; The amount of eutectic solvent used is 15 mL relative to 1 g of waste tire rubber powder. Desulfurization conditions: temperature 90℃, stirring speed 400rpm, time 3h; (2) In the presence of organic additives, the intermediate material is settled and filtered to separate solid and liquid. The filter cake obtained by solid-liquid separation is washed twice with deionized water and twice with ethanol, and then dried at 70°C for 5 hours to obtain desulfurized rubber powder. The organic additive is ethanol.
[0044] Example 2 The procedure was carried out in a similar manner to Example 1, except that the reaction reagents and reaction conditions were different, specifically: In step (1), the eutectic solvent is DES-2; The amount of eutectic solvent used is 19 mL relative to 1 g of waste tire rubber powder; Desulfurization conditions: temperature 85℃, stirring speed 400rpm, time 4h; In step (2), the organic auxiliary is acetone.
[0045] Example 3 The procedure was carried out in a similar manner to Example 1, except that the reaction reagents and reaction conditions were different, specifically: In step (1), the eutectic solvent is DES-3; The amount of eutectic solvent used is 17 mL relative to 1 g of waste tire rubber powder; The desulfurization treatment conditions were: temperature 100℃, stirring speed 500rpm, and time 3.5h.
[0046] Example 4 The procedure was carried out in a similar manner to Example 1, except that the reaction reagents and reaction conditions were different, specifically: In step (1), the eutectic solvent is DES-4; The amount of eutectic solvent used is 18 mL relative to 1 g of waste tire rubber powder; The desulfurization treatment conditions were: temperature 90℃, stirring speed 450rpm, and time 3h.
[0047] Example 5 The procedure was carried out in a similar manner to Example 1, except that the reaction reagents and reaction conditions were different, specifically: In step (1), the eutectic solvent is DES-5; The amount of eutectic solvent used is 22 mL relative to 1 g of waste tire rubber powder; The desulfurization treatment conditions were: temperature 95℃, stirring speed 550rpm, and time 3.5h.
[0048] Example 6 The procedure was carried out in a similar manner to Example 1, except that the reaction reagents and reaction conditions were different, specifically: In step (1), the eutectic solvent is DES-6; The amount of eutectic solvent used is 13 mL relative to 1 g of waste tire rubber powder; The desulfurization treatment conditions were: temperature 92℃, stirring speed 400rpm, and time 4h.
[0049] Examples 7 to 9 The method is similar to that in Example 1, except that: Implement the reverse 7 method by replacing DES-1 with DES-7 of the same weight; Implement the reverse 8 method by replacing DES-1 with DES-8 of the same weight; Implement the reverse 9 method by replacing DES-1 with DES-9 of the same weight; The remaining steps are the same as in Example 1, and desulfurized rubber powder is prepared accordingly.
[0050] Comparative Examples 1 to 4 The method is similar to that in Example 1, except that: Comparative Example 1 replaces DES-1 with DES-D1 of the same weight; Comparative Example 2 replaces DES-1 with DES-D2 of the same weight; Comparative Example 3 replaces DES-1 with DES-D3 of the same weight; Comparative Example 4 replaces DES-1 with DES-D4 of the same weight; The remaining steps are the same as in Example 1, and desulfurized rubber powder is prepared accordingly.
[0051] Test case The sol content and desulfurization rate of the desulfurized rubber powder prepared in the above examples were tested, and the results are shown in Table 2.
[0052] The testing method is as follows: Sol content determination: Soxhlet extraction method was used. A certain mass of sample was weighed, wrapped in filter paper, and extracted with acetone for 12 hours using a Soxhlet extractor. The sample was then dried in a vacuum drying oven at 60°C until constant weight, and the mass m0 was obtained. The sample was then submerged in toluene and extracted for 14 hours. The sample was then dried in a vacuum drying oven at 60°C until constant weight, and the mass m1 was obtained. Finally, the sol content was calculated according to the following formula (1): Sol content (wt%) = [(m0) m1) / m1]×100% formula (1).
[0053] Desulfurization rate determination: The sulfur content before and after desulfurization treatment was determined by infrared spectroscopy, and then the desulfurization rate was calculated according to the following formula (2); the higher the desulfurization rate, the more thoroughly the sulfur element was removed. Desulfurization rate (wt%) = [(sulfur content before desulfurization)] Formula (2): [(sulfur content after desulfurization) / sulfur content before desulfurization) × 100%
[0054] Table 2
[0055] As can be seen from the results in Table 2, the eutectic solvents prepared in Examples 1 to 9 can achieve efficient desulfurization of waste tire rubber powder under low temperature conditions, with sufficient destruction of the crosslinking network and excellent decrosslinking effect of the rubber chain.
[0056] The data from Comparative Examples 1 to 3 show that amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids are all indispensable. Only when the three work synergistically can a high sol content and desulfurization rate be obtained.
[0057] Therefore, the eutectic solvent provided by this invention can gently and efficiently break SS and CS crosslinking bonds through a triple mechanism of hydrogen bonding, nucleophilic bond breaking, and reduction synergy, achieving gentle, efficient, and green desulfurization and recycling of waste tire rubber powder. This eutectic solvent can be recycled, reducing production costs and solving the problems of high energy consumption, high pollution, and poor regeneration effect of traditional processes. It is suitable for the industrial production of high-quality reclaimed rubber and has good economic and environmental benefits.
[0058] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A eutectic solvent, characterized in that, The eutectic solvent contains amides, α-hydrogen-containing quaternary ammonium halides, and reducing carboxylic acids in a weight ratio of 2-3.5:1-2:
1.
2. The eutectic solvent according to claim 1, characterized in that, The amides are selected from at least one of formamide, acetamide, propionamide, butyramide, hexamamide, benzamide, caprolactam, pyrrolidone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
3. The eutectic solvent according to claim 1 or 2, characterized in that, The α-hydrogen-containing quaternary ammonium halide is an α-hydrogen-containing quaternary ammonium chloride and / or an α-hydrogen-containing quaternary ammonium bromide.
4. The eutectic solvent according to claim 3, characterized in that, The α-hydrogen-containing quaternary ammonium chloride salt is selected from choline chloride, tetramethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, tetrabutylammonium chloride, benzyltrimethylammonium chloride, dodecyltrimethylammonium chloride, and hexadecyltrimethylammonium chloride; And / or, the α-hydrogen-containing quaternary ammonium bromide is tetrabutylammonium bromide and / or choline bromide.
5. The eutectic solvent according to claim 1 or 2, characterized in that, The reducing carboxylic acid is selected from at least one of formic acid, acetic acid, oxalic acid, lactic acid, malic acid, citric acid, ascorbic acid, thioglycolic acid, gluconic acid, and tartaric acid.
6. The application of the eutectic solvent according to any one of claims 1-5 in the desulfurization process.
7. The application according to claim 6, characterized in that, The desulfurization rate of the eutectic solvent is ≥83wt%.
8. A method for desulfurizing and recycling waste tire rubber powder, characterized in that, The method includes: (1) The waste tire rubber powder and the eutectic solvent are subjected to desulfurization treatment to obtain intermediate material; the sulfur content of the waste tire rubber powder is 1.5-2.8 wt%; (2) In the presence of organic additives, the intermediate material is subjected to solid-liquid separation to obtain desulfurized rubber powder with a sol content of 19-25 wt%. In step (1), the eutectic solvent is the eutectic solvent described in any one of claims 1-5.
9. The method according to claim 8, characterized in that, In step (1), the amount of the eutectic solvent used is 8-25 mL relative to 1 g of the waste tire rubber powder; And / or, in step (2), the organic auxiliary is ethanol and / or acetone.
10. The method according to claim 8 or 9, characterized in that, In step (1), the conditions for the desulfurization treatment include: a temperature of 80-100℃, a stirring rate of 300-600rpm, and a time of 1-4h.
Citation Information
Patent Citations
Preparation method for promoting waste rubber reclaiming by using ionic liquid
CN104163937A
Environment-friendly method for regenerating waste rubber
CN104387611A