Process for degrading an epoxy resin containing ester bonds in combination with a solution composition for degrading an epoxy resin containing ester bonds

By combining organic amine catalysts with water and polar solvents, the problem of epoxy resin's difficulty in degradation under mild conditions has been solved, achieving efficient and low-cost epoxy resin degradation, suitable for large-scale industrial applications at room temperature.

CN123152169APending Publication Date: 2026-11-24TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611552541.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively degrade epoxy resins containing ester bonds under mild conditions, particularly due to the poor compatibility between epoxy resins and water, resulting in demanding reaction conditions and high costs.

Method used

An organic amine catalyst is used in a co-solvent with water as a reactive solvent to treat epoxy resins containing ester bonds. The co-solvent contains a polar solvent, the catalyst is recyclable, and the degradation method is effective over a wide temperature range (including room temperature).

Benefits of technology

It achieves efficient degradation of epoxy resins containing ester bonds at room temperature, exhibits high degradation reactivity, overcomes hydrophobicity barriers with a cosolvent, and is recyclable with a catalyst, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152169A_ABST
    Figure CN123152169A_ABST
Patent Text Reader

Abstract

This invention relates to a method for degrading epoxy resins containing ester bonds and a solution composition for degrading epoxy resins containing ester bonds. The method for degrading epoxy resins containing ester bonds of this invention includes reacting the epoxy resin containing ester bonds with a reactive solvent in a co-solvent, wherein the reactive solvent is water, and the co-solvent comprises a polar solvent that does not react with the epoxy resin containing ester bonds. The solution composition of this invention comprises an organic amine catalyst, the aforementioned reactive solvent, and the aforementioned co-solvent. The method of this invention can efficiently and cost-effectively degrade epoxy resins containing ester bonds over a wide temperature range (especially at room temperature), and the catalyst used can be recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for degrading epoxy resins containing ester bonds and a solution composition for degrading epoxy resins containing ester bonds, belonging to the field of plastic recycling. Background Technology

[0002] Epoxy resin is a traditional polymer material and one of the most important thermosetting resins, accounting for a significant proportion of its usage. Among these, ester-bonded epoxy resins, such as anhydride-cured epoxy resins, are one of the most important subclasses. Due to their excellent mechanical strength, electrical insulation, and thermal and chemical stability, they have become widely used polymer materials in national power systems, wind power generation, and building materials. The rapid growth in usage and demand, coupled with the increase and accumulation of waste plastics, could potentially trigger a global ecological crisis. Therefore, the proper handling and recycling of epoxy resin waste is a global hot topic and a crucial element in achieving sustainable development strategies.

[0003] However, for epoxy resins containing ester bonds, the stable cross-linking structure and high strength make the recycling and disposal of related products and equipment after decommissioning a thorny issue.

[0004] Taking classic anhydride-cured epoxy resin as an example, the crosslinking points in the chemical structure of anhydride-cured epoxy resin are composed of ester bonds. Compared with the carbon chain skeleton in the epoxy and anhydride before curing, the chemical reactivity of the ester bond crosslinking points formed during the epoxy and anhydride curing reaction is relatively more significant. Therefore, the chemical recycling of anhydride-cured epoxy resin usually has obvious selectivity, which is a degradation process based on the breaking of active ester bonds. The ester bond breaking mechanism is divided into several main categories, including alcoholysis, hydrolysis, and aminolysis. Among them, water is the safest, most environmentally friendly, non-toxic, and harmless depolymerization reagent. At the same time, the hydrolysis of ester bonds can produce carboxyl and hydroxyl groups, making the properties and application scenarios of the degradation products predictable and designable, and easy to achieve upgraded recycling. However, the surface of anhydride-cured epoxy resin is extremely hydrophobic, which hinders interfacial mass transfer in the initial stage of the reaction; and the products formed during the degradation process are also highly hydrophobic, which is not conducive to the continuous reaction.

[0005] Research on the hydrolysis of anhydride-cured epoxy resins has a long history. Early methods utilized supercritical water (>374℃, >22.1 MPa) to degrade epoxy resins, but the reaction was too vigorous, and the products were dispersed, making recycling difficult. To address the chemical reactivity of ester bonds in anhydride-cured epoxy resins, milder hydrolysis methods can be designed. However, current feasible strategies for improving interfacial mass transfer in hydrolysis processes are limited to adding amphiphilic molecules or surfactants as catalysts, and even the mildest method still requires a high temperature of 160℃, under which water remains in the form of a high-pressure gas, making the conditions extremely demanding.

[0006] In particular, epoxy resins themselves have poor compatibility with water (especially at lower temperature conditions), which significantly raises the threshold for selecting reaction conditions for hydrolysis strategies.

[0007] Therefore, there is a technological need to develop an efficient method for hydrolyzing and degrading epoxy resins containing ester bonds at room temperature to provide a low-cost solution for the treatment of large quantities of waste equipment and products. Summary of the Invention

[0008] <Problem to be solved by the invention>

[0009] In view of the above, the object of the present invention is to provide a method for degrading epoxy resins containing ester bonds, which can effectively and cost-effectively degrade epoxy resins containing ester bonds based on hydrolysis over a wide temperature range (especially at room temperature), the process is simple, and the catalyst used can be recycled.

[0010] The object of the present invention is to provide a solution composition for degrading epoxy resins containing ester bonds at room temperature, the composition being based on water as a reactive solvent, which can effectively and cost-effectively degrade epoxy resins containing ester bonds over a wide temperature range (especially at room temperature), and the catalyst used can be recycled.

[0011] <Solutions for solving the problem>

[0012] Through in-depth research, the inventors discovered that the following implementation schemes can achieve the above-mentioned objectives of this invention.

[0013] [1]. A method for degrading epoxy resin containing ester bonds, the degradation method comprising: reacting the epoxy resin containing ester bonds with a reactive solvent in a co-solvent in the presence of an organic amine catalyst.

[0014] The reactive solvent is water.

[0015] The cosolvent comprises a polar solvent and does not react with the epoxy resin containing ester bonds.

[0016] [2]. According to the degradation method described in [1], the organic amine catalyst is at least one selected from 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]non-5-ene (DBN), 1,5,7-triazabicyclo[4.4.0]decen-5-ene (TBD), tetramethylguanidine (TMG) or 7-methyl-1,5,7-triazabicyclo[4.4.0]decen-5-ene (MTBD).

[0017] [3]. According to the degradation method described in [1] or [2], wherein the mass ratio of the organic amine catalyst to the epoxy resin containing ester bonds is (0.30~2.00):1;

[0018] The amount of the organic amine catalyst used is in a mass ratio of 1:1 to 1:15 to the total amount of the reactive solvent and the co-solvent.

[0019] [4]. The degradation method according to any one of [1] to [3], wherein the polar solvent is at least one selected from chloroalkane solvents, ketone solvents, nitrile solvents, and ether solvents.

[0020] [5]. The degradation method according to any one of [1] to [4], wherein the volume ratio of the reactive solvent to the co-solvent is 1 / 2 to 1 / 30.

[0021] [6]. The degradation method according to any one of [1] to [5], wherein the amount of the epoxy resin containing ester bonds is 100% to 800% by mass relative to 100% by mass of the reactive solvent.

[0022] [7]. The degradation method according to any one of [1] to [6], wherein the degradation method is carried out at room temperature.

[0023] [8]. A solution composition for degrading epoxy resins containing ester bonds, said solution composition comprising an organic amine catalyst, a reactive solvent, and a co-solvent.

[0024] The reactive solvent is water.

[0025] The cosolvent comprises a polar solvent and does not react with the epoxy resin containing ester bonds.

[0026] <The Effects of the Invention>

[0027] Through the above technical solution, the present invention unexpectedly achieved the following technical effects.

[0028] The degradation method of the present invention follows the principle of hydrolysis.

[0029] In this invention, epoxy resin containing ester bonds is reacted with a specific reactive solvent containing water in a specific co-solvent in the presence of an organic amine catalyst. The degradation reactivity and reaction efficiency of the ester bonds in the epoxy resin containing ester bonds are both high. Furthermore, the introduction of the co-solvent overcomes the significant obstacles to hydrolysis caused by the hydrophobic surface of the epoxy resin and the hydrophobicity of the degradation products. Thus, the molecular chains of epoxy resin containing ester bonds can be effectively degraded over a wide temperature range (above -40°C, for example, above 10°C, or 10°C to 200°C), especially at room temperature (without additional energy input to the reaction system).

[0030] In addition, the degradation method of the present invention uses simple raw materials, recyclable catalysts, flexible equipment, simple process, low cost, and energy saving, making it suitable for large-scale industrial production.

[0031] Furthermore, the degradation system in the degradation method of the present invention can be either heterogeneous or homogeneous. Therefore, the degradation method of the present invention has excellent versatility.

[0032] The solution composition of the present invention can make the degradation reactivity and degradation efficiency of ester bonds in epoxy resins containing ester bonds both high. Furthermore, the introduction of a co-solvent overcomes the huge obstacles to hydrolysis caused by the hydrophobic surface of epoxy resin and the hydrophobicity of degradation products. Thus, the molecular chains of epoxy resins containing ester bonds can be effectively degraded in a wide temperature range (above -40°C, for example above 10°C, or 10°C to 200°C), especially at room temperature (without additional energy input to the reaction system). Attached Figure Description

[0033] Figure 1 An exemplary chemical equation for the degradation method of the present invention (room temperature chemical recovery of anhydride-cured epoxy resin) is shown.

[0034] Figure 2 The infrared spectrum of the anhydride-cured epoxy resin in Example 1 is shown.

[0035] Figure 3 Digital photographs of the hydrolysis process of anhydride-cured epoxy resin in water-THF mixed solvent in Example 1 are shown (showing the initial state (0 hours), 3 hours, and 12 hours respectively).

[0036] Figure 4 The accompanying diagram shows a comparison of the residual solid mass monitoring curve and digital photographs during the hydrolysis process of the anhydride-cured epoxy resin in a water-THF mixed solvent in Example 1.

[0037] Figure 5 The infrared spectra of the hydrolysis products in Example 1 under acidic and alkaline conditions are shown.

[0038] Figure 6 The infrared spectra of the degradation products of the anhydride-cured epoxy resin in Example 3 and the infrared spectra of the degradation products of the anhydride-cured epoxy resin in the reference example are shown.

[0039] Figure 7 The image shows the recovered catalyst in Example 4 and the comparison of its 1H NMR spectrum with that of the original catalyst (DMSO-d6). Detailed Implementation

[0040] Various exemplary embodiments, features, and aspects of the present invention will be described in detail below. The term "exemplary" as used herein means "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as superior to or better than other embodiments.

[0041] Furthermore, to better illustrate the present invention, numerous specific details are set forth in the following detailed embodiments. Those skilled in the art should understand that the present invention can be practiced without certain specific details. In other instances, methods, means, apparatus, and steps well known to those skilled in the art have not been described in detail in order to highlight the spirit of the present invention.

[0042] Unless otherwise stated, all units used in this specification are international standard units, and all numerical values ​​and ranges appearing in this invention should be understood to include systematic errors that are unavoidable in industrial production.

[0043] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.

[0044] In this specification, references to "some specific / preferred embodiments," "other specific / preferred embodiments," "implementation," etc., refer to specific elements (e.g., features, structures, properties, and / or characteristics) related to that embodiment, which are included in at least one of the embodiments described herein and may or may not be present in other embodiments. Furthermore, it should be understood that these elements may be combined in any suitable manner in various embodiments.

[0045] In this specification, the numerical range referred to as "value A to value B" refers to the range including endpoint values ​​A and B. The numerical range referred to as "above" and "below" refers to the range including endpoint values. The numerical range referred to as "greater than" and "less than" refers to the range excluding endpoint values.

[0046] In this specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes both the scenario in which the event occurs and the scenario in which the event does not occur.

[0047] In this manual, "room temperature" refers to the ambient temperature, which is usually between -40°C and 40°C.

[0048] <Degradation methods for epoxy resins containing ester bonds>

[0049] The degradation method of the epoxy resin containing ester bonds of the present invention includes: reacting the epoxy resin containing ester bonds with a reactive solvent in a co-solvent in the presence of an organic amine catalyst, wherein the reactive solvent is water, and the co-solvent contains a polar solvent that does not react with the epoxy resin containing ester bonds.

[0050] The degradation method of this invention is based on hydrolysis. In this invention, the co-solvent significantly swells and relaxes the epoxy resin network, thereby improving the mass transfer between the reactive components in the solution and the solid cross-linked network of the epoxy resin, allowing the reactive reagent and the polymer network to come into full contact and react smoothly. Based on this, in the presence of an organic amine catalyst, the ester bonds in the epoxy resin containing ester bonds react with the reactive solvent (i.e., hydrolysis occurs), causing the ester bonds to open (i.e., depolymerization), thereby achieving the degradation of the molecular chains of the epoxy resin containing ester bonds. Specifically, Figure 1 A specific example of this reaction is shown in the figure.

[0051] There are no particular restrictions on the type of organic amine catalyst, as long as it can catalyze the depolymerization reaction of ester bonds in epoxy resins containing ester bonds.

[0052] In some preferred embodiments, the organic amine catalyst is preferably at least one selected from 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]non-5-ene (DBN), 1,5,7-triazabicyclo[4.4.0]decen-5-ene (TBD), 7-methyl-1,5,7-triazabicyclo[4.4.0]decen-5-ene (MTBD), and tetramethylguanidine (TMG).

[0053] In some preferred embodiments, from the viewpoint of better utilizing the catalytic effect of the present invention, the organic amine catalyst is preferably dissolved in a reactive solvent and / or a co-solvent.

[0054] In some preferred embodiments, from the viewpoint of being more conducive to the occurrence of hydrolysis-based degradation reactions, the organic amine catalyst more preferably includes at least 1,5,7-triazabicyclo[4.4.0]decene-5-ene (TBD), and more preferably TBD.

[0055] There are no particular restrictions on the amount of organic amine catalyst used, and it can be adjusted appropriately according to actual needs. In some preferred embodiments, the mass ratio of the organic amine catalyst to the epoxy resin containing ester bonds is preferably (0.30~2.00):1, more preferably (0.40~0.80):1.

[0056] In some more preferred embodiments, the molar ratio of the ester bond in the epoxy resin containing the ester bond to the organic amine catalyst is preferably 1:(0.1~5), more preferably 1:(0.3~3), and even more preferably 1:(0.5~1).

[0057] In some other preferred embodiments, the amount of the organic amine catalyst and the total amount of the reactive solvent and the co-solvent are preferably in a mass ratio of 1:1 to 1:15, for example 1:12, 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, etc.

[0058] In this invention, the reactive solvent is water. There are no particular limitations on the type of water; it can be water directly from nature, tap water, distilled water, deionized water, etc.

[0059] In this invention, there are no particular limitations on the specific composition of the cosolvent, as long as it contains a polar solvent and does not react with epoxy resins containing ester bonds. In this invention, the cosolvent is used to assist in the dissolution of the degraded molecular chains in the solvent system and to promote the reaction by swelling, relaxing, and dispersing the stacked and entangled structures of the polymer molecular chains.

[0060] In some preferred embodiments, the polarity index of the polar solvent is preferably 3 to 6.

[0061] Additionally, preferably, the polar solvent comprises an organic solvent. In some preferred embodiments, the polar solvent is preferably at least one selected from chlorinated alkanes, ketones, nitriles, and ethers, and more preferably at least chlorinated alkanes.

[0062] Examples of chlorinated alkane solvents include, but are not limited to, dichloromethane, trichloromethane, and dichloroethane. They can be used alone or in combination of two or more. Dichloromethane is preferred.

[0063] Examples of ketone solvents include, but are not limited to, acetone, butanone, cyclohexanone, methyl ethyl ketone, etc. They can be used alone or in combination of two or more. Among them, acetone is preferred.

[0064] Examples of nitrile solvents include, but are not limited to, acetonitrile and propionitrile. They can be used alone or in combination of two or more. Acetonitrile is preferred.

[0065] Examples of ether solvents include, but are not limited to, tetrahydrofuran, diethyl ether, ethylene glycol dimethyl ether, and dioxane. They can be used alone or in combination of two or more. Tetrahydrofuran is preferred.

[0066] In some preferred embodiments, the amount of polar solvent is preferably 50% or more, more preferably 60% or more, further preferably 80% or more, even more preferably 90% or more, and particularly preferably 100% or more, relative to the total volume of the cosolvent (100% volume).

[0067] In this invention, there are no particular limitations on the ratio between the reactive solvent and the co-solvent, which can be appropriately adjusted according to factors such as the type of epoxy resin containing ester bonds used. In some preferred embodiments, the volume ratio of the reactive solvent to the co-solvent is preferably 1 / 2 to 1 / 30, more preferably 1 / 3 to 1 / 10.

[0068] In addition to reactive solvents and co-solvents, a third solvent that does not affect the composition / structure of the degradation products may also be present in the degradation method.

[0069] Particularly preferred is the use of a third solvent when the cosolvent contains at least a chlorinated alkane solvent, thereby improving the compatibility of water with the chlorinated alkane solvent.

[0070] There are no particular restrictions on the type of third solvent. From the viewpoint of better improving compatibility, the third solvent is preferably an alcohol solvent containing a primary alcohol group. It should be noted that although ester bonds can undergo alcoholysis, in this invention, the alcohol solvent only functions as a third solvent and does not affect the composition / structure of the degradation products.

[0071] In some preferred embodiments, the amount of water can be 20% or more, preferably 25% or more, and more preferably 30% or more, relative to 100% of the total volume of water and the third solvent; or it can be 90% or less, preferably 70% or less, and more preferably 45% or less. Within the above preferred ranges, the compatibility between water and the co-solvent can be better improved.

[0072] The term "primary alcohol group" refers to a structure in which a hydroxyl group (-OH) is directly attached to a primary carbon atom, i.e., a structure with -CH2OH.

[0073] Examples of alcohol solvents, without limitation, include monohydric alcohols such as methanol, ethanol, n-propanol, n-butanol, n-pentanol, n-hexanol, n-heptanol, benzyl alcohol, and phenethyl alcohol; dihydric alcohols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 1,5-pentanediol; and polyhydric alcohols such as glycerol having three or more primary alcohol groups. These alcohol solvents can be used alone or in combination of two or more.

[0074] In some preferred embodiments, from the viewpoint of more easily achieving the desired technical effects of the present invention and being easy to operate, the alcohol solvent is preferably a monohydric alcohol, and more preferably methanol.

[0075] In addition to organic amine catalysts, reactive solvents, and co-solvents, other components, such as bases, phosphates, diesters, or other additives, may be optionally used in the degradation method. These other components may exist either dissolved in the solvent system or insoluble in the solvent system.

[0076] Examples of alkalis include ammonia, hydroxides, alkoxides, and hydrides of alkali metals such as lithium, sodium, and potassium.

[0077] As phosphate salts, various salts of phosphoric acid can be listed, such as phosphoric acid, diphosphoric acid, phosphorous acid, pyrophosphoric acid, trimetaphosphoric acid, tetrametaphosphoric acid, and pyrophosphorous acid.

[0078] Examples of carbonate diesters include dialkyl carbonates and diaryl carbonates.

[0079] In some preferred embodiments, from the viewpoint of saving costs and making it easier to recover the catalyst, bases, phosphates, or carbonates are not used.

[0080] In some preferred embodiments, no components other than organic amine catalysts, reactive solvents, and co-solvents are used.

[0081] In this invention, the epoxy resin containing ester bonds is a cured epoxy resin.

[0082] Epoxy systems used for epoxy resins containing ester bonds include, but are not limited to: epoxy-acid systems, epoxy-mercapto systems, epoxy-anhydride systems, etc.

[0083] Typical examples of epoxy resins used as raw materials include, but are not limited to, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenolic epoxy resin, aliphatic polyol glycidyl ether epoxy resin, alicyclic epoxy resin, etc.

[0084] As an example, anhydride-cured epoxy resins can typically be obtained by curing epoxy resin and anhydride via a curing reaction.

[0085] Examples of acid anhydrides include, but are not limited to, one or more of aliphatic acid anhydrides, alicyclic acid anhydrides, and aromatic acid anhydrides. Preferably, the acid anhydride is selected from phthalic anhydrides (phthalic anhydride, terephthalic anhydride, isophthalic anhydride), trimellitic anhydride, pyromellitic dianhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, maleic anhydride, dodecenylsuccinic anhydride, (methyl)nadic anhydride, chlorine anhydride, etc.

[0086] In addition, there is no particular limitation on the amount of epoxy resin containing ester bonds in this invention, and it can be adjusted appropriately according to actual needs.

[0087] In some preferred embodiments, the amount of epoxy resin containing ester bonds is preferably 10% to 800% by mass relative to 100% by mass of the total mass of the reactive solvent, more preferably 50% to 600% by mass.

[0088] Furthermore, in this invention, there are no particular restrictions on the presence of epoxy resins containing ester bonds in the degradation method; they can be dissolved in the solvent system, partially dissolved in the solvent system, or insoluble in the solvent system. In other words, in the degradation method of this invention, the degradation system can be homogeneous or heterogeneous.

[0089] There are no particular restrictions on the form of the epoxy resin containing ester bonds used in the degradation method. For example, the epoxy resin containing ester bonds can be crushed into small pieces as needed. However, there are no particular restrictions on the size of the fragments.

[0090] Machines used for crushing include: impact crushers, shear crushers, compression crushers, pulverizers, ball mills, etc.

[0091] In this invention, the epoxy resin containing ester bonds can be a single epoxy resin containing ester bonds or a mixture of multiple epoxy resins containing ester bonds.

[0092] In addition, in this invention, the epoxy resin containing ester bonds can be in a state of blending with other substances, or it can be an epoxy resin containing ester bonds that is closely bonded to other components (e.g., embedded, bonded together, etc.).

[0093] As other substances or components, they can be the following materials: metals or alloys such as aluminum, iron, copper, zinc, and tin; non-metallic materials such as alumina, glass, ceramics, sand, and silicon; and polymers such as polyethylene, polypropylene, polyvinyl chloride, polyamide, acrylic resin, polystyrene, ABS resin, polymethyl methacrylate, phenolic resin, polyimide, polybutadiene, and SBS. They can exist alone or in combination of two or more.

[0094] Therefore, the degradation method of the present invention is particularly suitable for current commercial room temperature chemical recycling methods for waste plastics.

[0095] In this invention, there are no particular restrictions on the reaction conditions between epoxy resins containing ester bonds and reactive solvents, which can be appropriately adjusted according to actual needs.

[0096] In some specific implementations, the reaction temperature can be above -40°C, for example, above 10°C or above 20°C. Furthermore, from an energy-saving perspective, the upper limit of the reaction temperature can be 200°C, 100°C, or 50°C. In some particularly preferred implementations, the reaction temperature can be ambient temperature (sometimes referred to as room temperature in this invention), generally understood as -40 to 40°C.

[0097] In some specific implementation schemes, the reaction time can be 20 minutes to 30 hours, preferably 30 minutes to 20 hours, for example, 40 minutes, 1 hour, 5 hours, 10 hours, 15 hours, etc.

[0098] In this invention, the degradation method also includes other steps, such as a catalyst recovery step and a degradation product recovery step.

[0099] In this invention, the catalyst recovery efficiency can be very high, for example, above 80% by mass (or above 85% by mass for TBD). In this invention, the catalyst recovery rate is calculated as the percentage between the mass of the recovered catalyst and the mass of the catalyst added in the degradation reaction.

[0100] Solution compositions for degrading epoxy resins containing ester bonds

[0101] A solution composition for degrading epoxy resins containing ester bonds, characterized in that the solution composition comprises an organic amine catalyst, a reactive solvent, and a co-solvent, wherein the reactive solvent comprises water in an amount of 100% by volume relative to the total volume of the reactive solvent, the amount of water being 25% by volume or more, and the co-solvent comprises a polar solvent that does not react with the epoxy resin containing ester bonds.

[0102] Details of this composition are the same as those described above in <Degradation Method of Epoxy Resins Containing Ester Bonds>. They will not be repeated here.

[0103] Particularly preferably, the solution composition of the present invention consists only of an organic amine catalyst, a reactive solvent, and a co-solvent.

[0104] Furthermore, details regarding epoxy resins containing ester bonds are the same as those described in the section on "Degradation Methods for Epoxy Resins Containing Ester Bonds" above. They will not be repeated here.

[0105] The solution composition of the present invention can be widely used in homogeneous or heterogeneous degradation systems.

[0106] The solution compositions of the present invention are particularly suitable for degradation at room temperature.

[0107] Example

[0108] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0109] <Example 1: Room Temperature Homogeneous Hydrolysis Method for Anhydride-Curing Epoxy Resin>

[0110] Preparation of cured epoxy resin: Bisphenol A diglycidyl ether (DGEBA, 85%, 20g, 99.9mmol epoxy groups) and methyltetrahydrophthalic anhydride (MeTHPA, 95%, 17.5g, 99.9mmol) were preheated at 60℃ and stirred until clear and transparent. Then, N,N-dimethylbenzylamine (BDMA, 415μL) was added as a curing accelerator to obtain a homogeneous prepolymer. This prepolymer was transferred to a silicone mold and cured in a vacuum oven. Curing process: Vacuum degassing was performed at 60℃ for 15 min, followed by devastation and curing at 140℃ for 10 h. After demolding, epoxy resin EP was obtained. MeTHPA This serves as a raw material for subsequent degradation reactions. The formulation is consistent with the epoxy resin formulation used in transformer winding casting. Figure 2 The infrared spectrum showed no epoxy group signal (910 cm⁻¹). -1 The absence of an absorption peak at the wavenumber indicates that the resin was fully cured under these conditions, and its structure is rich in ester bonds (1733 cm⁻¹). -1 (Strong absorption peak at wavenumber).

[0111] Degradation of cured epoxy resin: The cured EP MeTHPA The sample was crushed into small particles. 1.0 g of EP was weighed. MeTHPA Particles (5.33 mmol ester bond, particle size range: 30-100 mesh) and 0.74 g TBD were added to 400 μL of water and 4 ml of tetrahydrofuran, respectively, and the reaction was carried out by stirring at room temperature.

[0112] Within 12 hours, EP MeTHPA The degradation is considered complete when the resin completely dissolves in the solution, yielding a solution of degradation products (the degradation solution). The hydrolysis process of anhydride-cured epoxy resin is as follows: Figure 3The state of the degradation residues during hydrolysis and their mass percentage relative to the initial particle mass are shown in the figure. Figure 4 As shown in the image.

[0113] The infrared spectra of the hydrolysis products are as follows.

[0114] (1) After the degradation reaction was completed, tetrahydrofuran was recovered by rotary evaporation, and the remaining water was dried in a vacuum oven at 70°C. The dried degradation product was subjected to infrared spectroscopy using an ATR accessory with air as the background. Here, the degradation product in its alkaline form was detected.

[0115] (2) In order to obtain the degradation product in acidic form, the degradation solution was dissolved and diluted with water after removing the solvent, and hydrochloric acid was added to adjust the pH to about 2~3. Then the water was removed and dried to obtain the degradation product in acidic form. Infrared spectroscopy was performed in the same way as in (1).

[0116] like Figure 5 As shown, under alkaline conditions, the product at 1570 cm⁻¹ -1 and 1400cm -1 The presence of a strong absorption peak near the wavenumber, while the absence of this absorption peak in the product under acidic conditions, indicates the presence of carboxyl groups in the hydrolysis product.

[0117] <Example 2: Room temperature heterogeneous hydrolysis of anhydride-cured epoxy resin>

[0118] Weigh the EP used in Example 1 MeTHPA 1.0 g of granules and 0.74 g of TBD were weighed out and added to 400 μL of water and 4 ml of dichloromethane, respectively. The mixture was stirred at room temperature to allow the reaction to proceed. Within 2 hours, EP... MeTHPA It dissolves completely in the solution, resulting in a clear and transparent solution.

[0119] Since dichloromethane has a particularly significant activating effect on the epoxy resin network, even though a heterogeneous reaction is used in this embodiment, its reaction rate is even higher than that of the homogeneous degradation reaction when tetrahydrofuran, acetone, or acetonitrile are used as co-solvents.

[0120] <Example 3: Room temperature degradation of anhydride-cured epoxy resin in a ternary mixed solvent>

[0121] Weigh the EP used in Example 1 MeTHPA 1.0 g of granules and 0.74 g of TBD were weighed and added to 150 μL of methanol, 1.5 mL of dichloromethane, and 70 μL of water, respectively. The mixture was stirred at room temperature to allow the reaction to proceed. Within 1 hour, EP... MeTHPA It dissolves completely in the solution, resulting in a clear and transparent solution.

[0122] This method, by adding an alcohol solvent, weakens the kinetic hindrance caused by the phase separation between water and dichloromethane, allowing the degradation reaction to proceed in a homogeneous solvent, thereby improving the reaction efficiency of the hydrolysis reaction. Infrared spectroscopy of the degradation products shows that the products are concentrated at 1570 cm⁻¹. -1 and 1400cm -1 The presence of a strong absorption peak near the wavenumber indicates that the product structure is still that of a hydrolysis product. For example... Figure 6 As shown, when the solvent composition is a ternary system of water-methanol-dichloromethane, the degradation products are at 1570 cm⁻¹. -1 The presence of a significant infrared signal attributable to the carboxylate ion indicates that the degradation follows a hydrolysis mechanism in the presence of water, and the resulting product contains a carboxyl group structure generated by the hydrolysis of ester bonds.

[0123] <Reference Example>

[0124] The degradation was carried out in the same manner as in Example 3, except that the solvent system (150 μL methanol, 1.5 mL dichloromethane, and 70 μL water) in Example 3 was replaced with 150 μL methanol and 1.5 mL dichloromethane. Within 2 hours, EP... MeTHPA It dissolves completely in the solution, resulting in a clear and transparent solution.

[0125] Infrared spectroscopy was also performed on the degradation products. For example... Figure 6 As shown, when the solvent composition is a methanol-dichloromethane binary system, the degradation products are at 1570 cm⁻¹ -1 The absence of infrared signals indicates that the alcoholysis mechanism is followed.

[0126] <Comparative Example>

[0127] Weigh 1.0g of the EP prepared in Example 1. MeTHPA 0.74g of epoxy resin granules and 0.74g of TBD were added to 4ml of water and stirred at room temperature to carry out the reaction. The reaction was carried out at room temperature (25-30°C) with stirring for at least 10 days, and no significant dissolution or reduction of epoxy resin granules was observed.

[0128] Example 4: Recovery of Organic Amine Catalysts

[0129] The degradation solution obtained in Example 1 was subjected to solvent removal using a rotary evaporator and then dried in a vacuum oven at 70°C to remove residual moisture. The dried component was dissolved again in 30 mL of deionized water, and the pH was adjusted with 1 M hydrochloric acid. A white precipitate was formed during the acidification process. When no more white precipitate formed, the addition of hydrochloric acid solution was stopped; at this point, the pH of the solution was approximately 3. The solution was centrifuged, and the supernatant was collected. NaOH solution was added to the clear supernatant until the solution became alkaline. The water in the alkaline aqueous solution was removed using a rotary evaporator and then dried in a vacuum oven at 70°C. The dried solid was ultrasonically washed with 100 mL of ethyl acetate in an ultrasonic cleaner, and then the ethyl acetate solution was collected by filtration. The ethyl acetate solution was subjected to solvent removal using a rotary evaporator to obtain a white crystalline solid, which is the recovered and regenerated catalyst. The catalyst recovery rate was calculated as the ratio of the recovered mass to the mass of catalyst added in the degradation reaction.

[0130] The recovered catalyst was subjected to 1H NMR spectroscopy to verify the purity of its active ingredients. The results are as follows: Figure 7 As shown, the 1H NMR spectrum signals of the recovered TBD (regenerated TBD) and the original TBD are almost identical, indicating that the recovery method can recover organic amine catalysts with high purity and recovery rate, further improving the economics of this room temperature depolymerization and recycling plastic scheme.

[0131] It should be noted that although the technical solution of the present invention has been described with specific examples, those skilled in the art will understand that the present invention should not be limited thereto.

[0132] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or technical improvements to the embodiments in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A method for degrading epoxy resin containing ester bonds, characterized in that, The degradation method includes: reacting the epoxy resin containing ester bonds with a reactive solvent in a co-solvent in the presence of an organic amine catalyst. The reactive solvent is water. The cosolvent comprises a polar solvent and does not react with the epoxy resin containing ester bonds.

2. The degradation method according to claim 1, characterized in that, The organic amine catalyst is selected from at least one of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]non-5-ene (DBN), 1,5,7-triazabicyclo[4.4.0]decen-5-ene (TBD), tetramethylguanidine (TMG) or 7-methyl-1,5,7-triazabicyclo[4.4.0]decen-5-ene (MTBD).

3. The degradation method according to claim 1 or 2, characterized in that, The mass ratio of the organic amine catalyst to the epoxy resin containing ester bonds is (0.30~2.00):1; The amount of the organic amine catalyst used is in a mass ratio of 1:1 to 1:15 to the total amount of the reactive solvent and the co-solvent.

4. The degradation method according to any one of claims 1 to 3, characterized in that, The polar solvent is selected from at least one of chlorinated alkane solvents, ketone solvents, nitrile solvents, and ether solvents.

5. The degradation method according to any one of claims 1 to 4, characterized in that, The volume ratio of the reactive solvent to the co-solvent is 1 / 2 to 1 / 30.

6. The degradation method according to any one of claims 1 to 5, characterized in that, The amount of epoxy resin containing ester bonds is 100% to 800% by mass relative to 100% by mass of the reactive solvent.

7. The degradation method according to any one of claims 1 to 6, characterized in that, The degradation method is carried out at room temperature.

8. A solution composition for degrading epoxy resins containing ester bonds, characterized in that, The solution composition comprises an organic amine catalyst, a reactive solvent, and a co-solvent. The reactive solvent is water. The cosolvent comprises a polar solvent and does not react with the epoxy resin containing ester bonds.