TiO2 / ZnO core-shell material, organic hybrid benzotriazole-ceo2, resin material, and preparation method and lamp

By combining TiO₂/ZnO core-shell materials with organic hybrid benzotriazole-CeO₂, the problem of photodegradation of lamp materials under the full spectrum is solved, achieving full-spectrum absorption and improved stability, thus extending the lifespan of the lamps.

CN123152170APending Publication Date: 2026-11-24NINGBO GONEO PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510662913.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing lighting materials are prone to photodegradation under the full spectrum of ultraviolet-visible-near infrared light, resulting in a shortened lifespan. Furthermore, existing improvement measures cannot effectively resist photodegradation caused by the full spectrum.

Method used

By using TiO₂/ZnO core-shell materials and organic hybrid benzotriazole-CeO₂, the photoresponse range is broadened to the near-infrared band through interfacial synergistic effects and the formation of defect energy levels by oxygen vacancies. Furthermore, through chemical bonding, synergistic effects of ultraviolet absorption and free radical quenching are achieved, thus preparing a full-spectrum aging-resistant resin material.

Benefits of technology

It achieves absorption of the entire spectrum, improves the light and heat stability of resin materials, reduces the generation of free radicals, and extends the service life and safety of lamps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005414365400000191
    Figure BDA0005414365400000191
  • Figure BDA0005414365400000192
    Figure BDA0005414365400000192
  • Figure BDA0005414365400000201
    Figure BDA0005414365400000201
Patent Text Reader

Abstract

The application relates to a TiO2 / ZnO core-shell material, an organic hybrid benzotriazole-CeO2, a resin material and a preparation method and a lamp. The resin material comprises a base resin and a full-spectrum absorber; the full-spectrum absorber comprises the TiO2 / ZnO core-shell material and the organic hybrid benzotriazole-CeO2; or the full-spectrum absorber comprises the TiO2 / ZnO core-shell material and a benzotriazole derivative. The TiO2 / ZnO core-shell material can realize continuous absorption from ultraviolet light (200-400 nm) to visible light (400-700 nm); meanwhile, the introduction of cerium ions forms a defect energy level through oxygen vacancies, widens the light response range to a near-infrared band (700-1000 nm), so that the TiO2 / ZnO core-shell material can resist photo-degradation caused by full-spectrum light; the organic hybrid benzotriazole-CeO2 can coordinate ultraviolet absorption and free radical quenching, and improve the problem that the resin material is prone to aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, and more specifically, to TiO2 / ZnO core-shell materials, organic hybrid benzotriazole-CeO2, resin materials, their preparation methods, and lamps. Background Technology

[0002] As users' demand for eye protection increases, the demand for full-spectrum eye-protection lamps is constantly rising. The core design concept of full-spectrum eye-protection lamps is to simulate the natural light spectrum, reduce the proportion of short-wavelength blue light (400-500nm), and enhance beneficial red light (600-700nm) and near-infrared light (700-1000nm) to relieve visual fatigue and improve comfort.

[0003] However, the PP (polypropylene) material provided by the related technology for manufacturing lamps is difficult to resist photodegradation caused by the ultraviolet-visible-near-infrared full spectrum, and is prone to surface powdering, which leads to a shortened lifespan of the lamps. Summary of the Invention

[0004] The purpose of this invention is to provide TiO2 / ZnO core-shell materials, organic hybrid benzotriazole-CeO2, resin materials, their preparation methods, and lamps. Both TiO2 / ZnO core-shell materials and organic hybrid benzotriazole-CeO2 can be used to prepare resin materials suitable for lamp manufacturing. Specifically, the TiO2 / ZnO core-shell material achieves continuous absorption from ultraviolet (200-400 nm) to visible light (400-700 nm), and its optical and thermal stability can be optimized through interfacial synergistic effects. Simultaneously, the introduction of cerium ions, through the formation of defect energy levels via oxygen vacancies, broadens the photoresponse range to the near-infrared band (700-1000 nm), enabling the TiO2 / ZnO core-shell material to resist photodegradation induced across the entire spectrum. The organic hybrid benzotriazole-CeO2 can synergistically combine ultraviolet absorption with free radical quenching to capture excited-state free radicals, reduce molecular chain breakage, and improve the problem of easy aging of resin materials.

[0005] This invention is implemented as follows:

[0006] In a first aspect, the present invention provides a method for preparing a TiO2 / ZnO core-shell material, comprising:

[0007] Add titanium dioxide precursor donor dropwise to an alcoholic solution of zinc oxide precursor donor;

[0008] Then, the first hydrothermal synthesis was performed, followed by separation and washing to obtain the TiO2 / ZnO core-shell product;

[0009] A silane coupling agent was added dropwise to an alcoholic solution of the TiO2 / ZnO core-shell product, followed by a second hydrothermal synthesis, separation, and washing to obtain an aminated modified product on the surface of the TiO2 / ZnO core-shell product.

[0010] A mixture of TiO2 / ZnO core-shell surface aminated modification products and cerium ion-containing solution is evaporated at a first set temperature and then calcined to obtain TiO2 / ZnO core-shell material.

[0011] In an optional embodiment, the zinc oxide precursor donor includes at least one of zinc nitrate, zinc chloride, and zinc sulfate; and / or,

[0012] Titanium oxide precursor donors include at least one of tetrabutyl titanate, titanium tetrachloride, titanium sulfate, and isopropyl titanate; and / or,

[0013] Solutions containing cerium ions include at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or,

[0014] The temperature for the first hydrothermal synthesis is 170-190℃; and / or,

[0015] The heating rate for the first hydrothermal synthesis is 8-12 °C / min; and / or,

[0016] The temperature for the second hydrothermal synthesis is 70±2℃; and / or,

[0017] The first set temperature is 60±5℃; and / or,

[0018] The first calcination includes segmented calcination, wherein the segmented calcination includes calcination at a temperature of 300±50℃, calcination at a temperature of 500±50℃, and calcination at a temperature of 700±50℃ in sequence.

[0019] Secondly, the present invention provides a TiO2 / ZnO core-shell material, which is prepared by the preparation method of the TiO2 / ZnO core-shell material described in the foregoing embodiments.

[0020] Thirdly, the present invention provides a method for preparing an organic hybrid benzotriazole-CeO2, comprising:

[0021] A cerium salt solution and citric acid were mixed and reacted at a second set temperature, then dried and calcined a second time to obtain carboxylated CeO2 nanomaterials.

[0022] A mixture of carboxylated CeO2 nanomaterials, benzotriazole derivatives, and dimethylformamide solution was reacted at a third set temperature to form amide bonds. The mixture was then cooled, washed, and dried to obtain a benzotriazole-CeO2 hybrid product.

[0023] The benzotriazole-CeO2 hybrid product was mixed with hyperbranched polyester and tetrahydrofuran and reacted at a fourth set temperature to obtain organic hybrid benzotriazole-CeO2.

[0024] In optional embodiments, the cerium salt solution includes at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or,

[0025] The second set temperature is 80±5℃; and / or,

[0026] A cerium salt solution and citric acid are mixed and reacted at a second set temperature. After cooling, ammonia is added dropwise to adjust the pH to form a sol, which is then dried at 60±5℃; and / or,

[0027] The temperature of the second calcination is 500±50℃; and / or,

[0028] The third set temperature is 80±5℃; and / or,

[0029] The fourth set temperature is 120±10℃.

[0030] Fourthly, the present invention provides an organic hybrid benzotriazole-CeO2, which is prepared by the preparation method of the organic hybrid benzotriazole-CeO2 described in the foregoing embodiments.

[0031] Fifthly, the present invention provides a full-spectrum aging-resistant resin material, the raw materials of which include: a matrix resin and a full-spectrum absorbent; wherein,

[0032] Full-spectrum absorbers include TiO2 / ZnO core-shell materials and organic hybrid benzotriazole-CeO2; or,

[0033] Full-spectrum absorbers include TiO2 / ZnO core-shell materials and benzotriazole derivatives.

[0034] In an optional embodiment, the method for preparing the TiO2 / ZnO core-shell material includes:

[0035] Add titanium dioxide precursor donor dropwise to an alcoholic solution of zinc oxide precursor donor;

[0036] Then, the first hydrothermal synthesis was performed, followed by separation and washing to obtain the TiO2 / ZnO core-shell product;

[0037] A silane coupling agent was added dropwise to an alcoholic solution of the TiO2 / ZnO core-shell product, followed by a second hydrothermal synthesis, separation, and washing to obtain an aminated modified product on the surface of the TiO2 / ZnO core-shell product.

[0038] A mixture of TiO2 / ZnO core-shell surface aminated modification products and cerium ion-containing solution is evaporated at a first set temperature and then calcined to obtain TiO2 / ZnO core-shell material.

[0039] In an optional embodiment, the zinc oxide precursor donor includes at least one of zinc nitrate, zinc chloride, and zinc sulfate; and / or,

[0040] Titanium oxide precursor donors include at least one of tetrabutyl titanate, titanium tetrachloride, titanium sulfate, and isopropyl titanate; and / or,

[0041] Solutions containing cerium ions include at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or,

[0042] The temperature for the first hydrothermal synthesis is 170-190℃; and / or,

[0043] The heating rate for the first hydrothermal synthesis is 8-12 °C / min; and / or,

[0044] The temperature for the second hydrothermal synthesis is 70±2℃; and / or,

[0045] The first set temperature is 60±5℃; and / or,

[0046] The first calcination includes segmented calcination, wherein the segmented calcination includes calcination at a temperature of 300±50℃, calcination at a temperature of 500±50℃, and calcination at a temperature of 700±50℃ in sequence.

[0047] In an optional embodiment, the method for preparing the organic hybrid benzotriazole-CeO2 includes:

[0048] A cerium salt solution and citric acid were mixed and reacted at a second set temperature, then dried and calcined a second time to obtain carboxylated CeO2 nanomaterials.

[0049] A mixture of carboxylated CeO2 nanomaterials, benzotriazole derivatives, and dimethylformamide solution was reacted at a third set temperature to form amide bonds. The mixture was then cooled, washed, and dried to obtain a benzotriazole-CeO2 hybrid product.

[0050] The benzotriazole-CeO2 hybrid product was mixed with hyperbranched polyester and tetrahydrofuran and reacted at a fourth set temperature to obtain organic hybrid benzotriazole-CeO2.

[0051] In optional embodiments, the cerium salt solution includes at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or,

[0052] The second set temperature is 80±5℃; and / or,

[0053] A cerium salt solution and citric acid are mixed and reacted at a second set temperature. After cooling, ammonia is added dropwise to adjust the pH to form a sol, which is then dried at 60±5℃; and / or,

[0054] The temperature of the second calcination is 500±50℃; and / or,

[0055] The third set temperature is 80±5℃; and / or,

[0056] The fourth set temperature is 120±10℃.

[0057] In an optional embodiment, the raw materials for the full-spectrum aging-resistant resin material, by mass percentage, include: 95-97.5% matrix resin, 1.5-3% full-spectrum absorber; 0.5-1.0% hyperbranched polyester anti-migration agent, 0.3-0.5% auxiliary antioxidant, and 0.2-0.5% processing aid; wherein,

[0058] The mass ratio of TiO2 / ZnO core-shell material to organic hybrid benzotriazole-CeO2 is 7:(2-4).

[0059] In a sixth aspect, the present invention provides a method for preparing a full-spectrum aging-resistant resin material as described in any of the foregoing embodiments, comprising: mixing raw materials of the full-spectrum aging-resistant resin material and extruding and granulating them using a screw extruder.

[0060] In a seventh aspect, the present invention provides a lamp, wherein the raw material for manufacturing the lamp housing or lampshade includes a full-spectrum aging-resistant resin material of any of the foregoing embodiments.

[0061] The present invention has the following beneficial effects:

[0062] The method for preparing the TiO2 / ZnO core-shell material of this invention produces a composite structure formed by the interfacial bonding of two semiconductor materials, titanium dioxide (TiO2) and zinc oxide (ZnO). This composite structure exhibits a band gradient difference, which enhances light absorption and carrier separation efficiency. Through the band gradient design between TiO2 (Eg = 3.2 eV) and ZnO (Eg = 3.37 eV), continuous absorption from ultraviolet (200-400 nm) to visible light (400-700 nm) is achieved. Simultaneously, cerium ions (Ce) are introduced. 3+ By forming defect energy levels through oxygen vacancies, the optical response range is broadened to the near-infrared band (700-1000nm).

[0063] The method for preparing TiO2 / ZnO core-shell material of the present invention forms a core-shell structure, which is a composite particle composed of a "core" and a "shell" (i.e., TiO2 core + ZnO shell), and can also optimize light and thermal stability through interface synergistic effect.

[0064] Moreover, the preparation method of this TiO2 / ZnO core-shell material uses hydrothermal synthesis to precisely control the crystal morphology and size, ensuring that ZnO can grow uniformly on the TiO2 surface.

[0065] The TiO2 / ZnO core-shell material of the present invention can achieve absorption across the entire spectrum (ultraviolet-visible-near infrared) and has good optical and thermal stability.

[0066] In the preparation method of the organic hybrid benzotriazole-CeO2 of the present invention, the benzotriazole derivative used can absorb ultraviolet light (200-400nm) through an intramolecular charge transfer mechanism and quench free radicals (i.e., inhibit the generation of free radicals). That is, the organic hybrid benzotriazole-CeO2 prepared by this method can achieve synergistic ultraviolet absorption and free radical quenching through chemical bonding.

[0067] Meanwhile, the addition of dimethylformamide (DMF) helps to ensure the hybridization uniformity of benzotriazole derivatives and carboxylated CeO2 nanomaterials.

[0068] The organic hybrid benzotriazole-CeO2 of the present invention can absorb ultraviolet light (200-400nm) and quench free radicals through an intramolecular charge transfer mechanism.

[0069] The full-spectrum aging-resistant resin material of the present invention is formulated by compounding TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 in the matrix resin. By utilizing TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2, the resin material can resist full-spectrum photodegradation, improve light and heat stability, reduce the generation of free radicals, and effectively improve the aging resistance of the resin material.

[0070] The preparation method of the full-spectrum aging-resistant resin material of the present invention is a one-step extrusion granulation method, which is simple and easy to operate.

[0071] The housing or lampshade of the lamp of the present invention is made of the aforementioned full-spectrum aging-resistant resin material, which can resist full-spectrum photodegradation, improve light and heat stability, reduce the generation of free radicals, and effectively improve anti-aging properties. That is, it can delay the occurrence of phenomena such as powdering of the housing or lampshade of the lamp, which is conducive to extending the service life of the lamp and improving the safety of the lamp. Detailed Implementation

[0072] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0073] The inventors discovered that when antioxidants (e.g., hindered phenols) are used to modify PP (polypropylene) materials to delay thermo-oxidative aging, they cannot resist photodegradation caused by the ultraviolet-visible-near-infrared full spectrum, still leading to surface pulverization of the PP material. Even with the addition of UV additives (e.g., UV-326), only the 280-400nm ultraviolet band can be absorbed. In full-spectrum lighting, the proportion of low-wavelength light is extremely small, and the high proportion of visible light (400-700nm) and near-infrared light (>700nm) will still cause PP molecular chain breakage, accelerating the failure of PP materials. Moreover, during high-temperature processing or long-term use, anti-aging additives easily migrate to the surface of PP materials, further causing a decrease in protective performance.

[0074] Further research by the inventors revealed that while using a TiO2 / ZnO composite can improve the weather resistance of PP materials, it can only absorb ultraviolet light (280-400nm) and cannot achieve full-spectrum absorption (i.e., it cannot cover the absorption of light with wavelengths above 400-700nm and near-infrared light above 700nm), making it still prone to photodegradation. Furthermore, while using a benzotriazole UV absorber (e.g., UV-360) combined with nano-CeO2 can achieve absorption of ultraviolet-visible light (280-600nm), it still cannot absorb near-infrared light, causing PP materials to still easily age under the influence of infrared thermal radiation.

[0075] To address the aforementioned issues, this invention provides a full-spectrum aging-resistant resin material that overcomes the bottlenecks of PP materials in terms of spectral matching, chalking resistance, and long-term stability. It resists photodegradation induced by the entire spectrum, improves light and heat stability, reduces free radical generation, minimizes molecular chain breakage, and alleviates the aging problem of resin materials. This full-spectrum aging-resistant resin material can be used to manufacture lamp housings or lampshades, which helps extend the service life of the corresponding lamps and improves their safety.

[0076] The raw materials of the full-spectrum aging-resistant resin material of the present invention include: a matrix resin and a full-spectrum absorber; wherein, the full-spectrum absorber includes TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2.

[0077] The full-spectrum aging-resistant resin material of the present invention is formulated by compounding TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 in the matrix resin. By utilizing TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2, the resin material can resist full-spectrum photodegradation, improve light and heat stability, reduce the generation of free radicals, and effectively improve the aging resistance of the resin material.

[0078] Of course, in other embodiments, the full-spectrum absorber may also be a TiO2 / ZnO core-shell material and an unhybridized benzotriazole derivative.

[0079] Optionally, the preparation method of TiO2 / ZnO core-shell material includes:

[0080] Add titanium dioxide precursor donor dropwise to an alcoholic solution of zinc oxide precursor donor;

[0081] Then, the first hydrothermal synthesis was performed, followed by separation and washing to obtain the TiO2 / ZnO core-shell product;

[0082] A silane coupling agent was added dropwise to an alcoholic solution of the TiO2 / ZnO core-shell product, followed by a second hydrothermal synthesis, separation, and washing to obtain an aminated modified product on the surface of the TiO2 / ZnO core-shell product.

[0083] A mixture of TiO2 / ZnO core-shell surface amylation modification products and a cerium ion-containing solution is evaporated at a first set temperature and then calcined to obtain a TiO2 / ZnO core-shell material (i.e., a core-shell heterojunction TiO2 / ZnO-Ce). 3+ ).

[0084] The prepared TiO2 / ZnO core-shell material, a composite structure formed by the interfacial bonding of titanium dioxide (TiO2) and zinc oxide (ZnO), exhibits a band gradient difference, which enhances light absorption and carrier separation efficiency. Through the band gradient design between TiO2 (Eg = 3.2 eV) and ZnO (Eg = 3.37 eV), continuous absorption from ultraviolet (200-400 nm) to visible light (400-700 nm) is achieved. Simultaneously, cerium ions (Ce) are introduced. 3+ By forming defect energy levels through oxygen vacancies, the optical response range is broadened to the near-infrared band (700-1000nm).

[0085] The method for preparing TiO2 / ZnO core-shell material of the present invention forms a core-shell structure, which is a composite particle composed of a "core" and a "shell" (i.e., TiO2 core + ZnO shell), and can also optimize light and thermal stability through interface synergistic effect.

[0086] Moreover, the preparation method of this TiO2 / ZnO core-shell material uses hydrothermal synthesis to precisely control the crystal morphology and size, ensuring that ZnO can grow uniformly on the TiO2 surface.

[0087] The TiO2 / ZnO core-shell material of the present invention can achieve absorption across the entire spectrum (ultraviolet-visible-near infrared) and has good optical and thermal stability.

[0088] Optionally, the zinc oxide precursor donor includes at least one of zinc nitrate, zinc chloride, and zinc sulfate. For example, zinc nitrate (e.g., grade ZN-01) can refer to Zn(NO3)2·6H2O, which is a colorless tetragonal crystal with a purity ≥99.5%, water solubility: readily soluble, and decomposition temperature: 105℃ (loss of water of crystallization). Zinc nitrate provides the ZnO precursor, and a ZnO shell is formed through hydrothermal synthesis, forming a heterojunction with TiO2.

[0089] Optionally, the titanium dioxide precursor donor includes at least one selected from tetrabutyl titanate, titanium tetrachloride, titanium sulfate, and isopropyl titanate. For example, tetrabutyl titanate (e.g., tetrabutyl titanate with the designation T-7) can be hydrolyzed to generate high-purity nano-TiO2 cores as a precursor, which is a colorless to pale yellow transparent liquid with a purity ≥99.9% and a density of 1.05 g / cm³. 3 Hydrolysis activity: High (requires ethanol inhibition).

[0090] Optionally, the cerium-containing solution includes at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution. For example, the cerium nitrate solution (e.g., grade CN-4G) can be used with a purity ≥99.99% and a cerium content (Ce) of ≥99.99%. 3+ ): ≥99.9% cerium nitrate, wherein cerium nitrate is readily soluble in water.

[0091] There are no specific limitations on the selection of silane coupling agents. For example, the silane coupling agent (e.g., brand KBE-903) has an amino content of 0.8 mmol / g and a density of 1.02 g / cm³. 3 The decomposition temperature is 250℃. Surface amino modification using silane coupling agents can enhance the interfacial bonding between TiO2 / ZnO core-shell materials and PP materials, inhibit agglomeration, and improve raw material dispersibility.

[0092] Optionally, the preparation method of the alcohol solution of zinc oxide precursor donor includes: adding zinc oxide precursor donor to deionized water in a high-pressure reactor, stirring magnetically (stirring speed: 300±20 rpm) until completely dissolved, and then adding ethanol solution.

[0093] Optionally, when preparing an alcoholic solution of zinc oxide precursor donor, the mass ratio of zinc oxide precursor donor to deionized water is 85-90:1 (g / L), for example: 85:1, 88:1, 88.89:1, 90:1, etc.

[0094] Optionally, when preparing the alcohol solution of the zinc oxide precursor donor, the volume ratio of the ethanol solution to deionized water is 2.5-3.5:1, for example: 2.5:1, 3:1, 3.5:1, etc.

[0095] Optionally, the ethanol solution is prepared from anhydrous ethanol (purity ≥99.8%, i.e., GC detection, water content ≤0.02%; boiling point 78.5℃, e.g., grade 100092683) and water in a volume ratio of 2-4:1 (e.g., 2:1, 3:1, 4:1). The use of ethanol can reduce the water activity of the titanium dioxide precursor donor, thereby hydrolyzing the titanium dioxide precursor donor, and can also disperse the core-shell powder, preventing agglomeration.

[0096] Optionally, the titanium dioxide precursor donor is added dropwise under stirring, and the dropping rate is controlled to be ≤5 mL / min, for example: 5 mL / min, 4.5 mL / min, 4 mL / min, 3.5 mL / min, etc.

[0097] Optionally, the volume ratio of the titanium dioxide precursor donor to the deionized water used in the alcohol solution for preparing the zinc oxide precursor donor is 0.12-0.2:1, for example: 0.12:1, 0.16:1, 0.20:1, etc.

[0098] Optionally, after adding the titanium dioxide precursor donor, the pH can be adjusted to 9.5 ± 0.2 with ammonia. Adjusting the pH of the reaction solution allows for better control of the TiO2 / ZnO core-shell growth rate.

[0099] Optionally, the concentration of ammonia (e.g., grade A112931) is 25-28% (w / w), and the pH is adjusted in the range of 8.5-10.0.

[0100] Optionally, the temperature of the first hydrothermal synthesis is 170-190℃ (e.g., 170℃, 180℃, 190℃, etc.), the reaction time is 10-15h (e.g., 10h, 12h, 15h, etc.), and the heating rate of the first hydrothermal synthesis is 8-12℃ / min (e.g., 8℃ / min, 10℃ / min, 12℃ / min, etc.).

[0101] Optionally, after the first hydrothermal synthesis is completed, the product is naturally cooled to room temperature, and the solid product is separated using a high-speed centrifuge (e.g., 8000±100 rpm, 10±1 min). The product is then washed successively with ethanol and deionized water to remove unreacted ions, yielding the TiO2 / ZnO core-shell product.

[0102] Optionally, the above washing can be performed by washing with ethanol 1-5 times and then washing with deionized water 1-5 times.

[0103] Optionally, the method for preparing the alcohol solution of the TiO2 / ZnO core-shell product includes: adding the TiO2 / ZnO core-shell product (powder) to anhydrous ethanol at a solid-liquid ratio of 1:45-55 (i.e., the mass ratio of TiO2 / ZnO core-shell product to anhydrous ethanol is 1:45-55), magnetically stirring, and ultrasonically treating (e.g., 30±5 min, frequency 40±5 kHz, power 300±50 W).

[0104] Optionally, the mass of the added silane coupling agent is 3 ± 0.5 wt% of the mass of the TiO2 / ZnO core-shell product (powder).

[0105] Optionally, the dropping rate of the silane coupling agent is ≤10 mL / min, for example: 10 mL / min, 9 mL / min, 8 mL / min, etc.

[0106] Optionally, after the silane coupling agent has been added, the pH can be adjusted to 8.5-9.0 using ammonia.

[0107] Optionally, the temperature for the second hydrothermal synthesis is 70±2℃ (e.g., 68℃, 70℃, 72℃).

[0108] Optionally, the second hydrothermal synthesis is carried out under stirring conditions, with a stirring speed of 300±50 rpm (e.g., 250 rpm, 300 rpm, 350 rpm, etc.) and a second hydrothermal synthesis time of 4±0.4 h, e.g., 3.5 h, 4 h, 4.5 h.

[0109] Optionally, after the second hydrothermal synthesis, the product is naturally cooled to room temperature and separated using a high-speed centrifuge (e.g., 8000±500 rpm, 10±2 min). The product is then washed sequentially with ethanol and deionized water to remove the physically adsorbed silane coupling agent and byproducts, yielding TiO2 / ZnO core-shell surface aminated modified powder (i.e., TiO2 / ZnO core-shell surface aminated modified product).

[0110] Alternatively, the washing method using ethanol and deionized water can be the same as the washing method used to prepare TiO2 / ZnO core-shell products.

[0111] Optionally, the molar concentration of the solution containing cerium ions is 0.1 ± 0.02 mol / L, for example: 0.08 mol / L, 0.1 mol / L, 0.12 mol / L, etc.

[0112] Optionally, the solid-liquid ratio of the TiO2 / ZnO core-shell surface aminated modified product to the cerium ion-containing solution is 1:(18-22), that is, the mass ratio of the TiO2 / ZnO core-shell surface aminated modified product to the cerium ion-containing solution is 1:(18-22), for example: 1:18, 1:20, 1:22, etc.

[0113] Optionally, the first set temperature is 60±5℃, for example: 55℃, 60℃, 65℃, etc.

[0114] Optionally, the first calcination includes segmented calcination, wherein the segmented calcination includes sequential calcination at temperatures of 300±50℃ (e.g., 250℃, 280℃, 300℃, 320℃, 350℃, etc.), calcination at temperatures of 500±50℃ (e.g., 450℃, 480℃, 500℃, 520℃, 550℃, etc.), and calcination at temperatures of 700±50℃ (e.g., 650℃, 680℃, 700℃, 720℃, 750℃, etc.). Segmented gradient calcination can gradually control lattice defects in the material and improve doping uniformity, while retaining sufficient Ce. 3+ The crystal lattice ensures that the prepared TiO2 / ZnO core-shell material can effectively resist full-spectrum photodegradation and ensure that the TiO2 / ZnO core-shell material has good optical and thermal stability.

[0115] Optionally, the calcination time at 300±50℃ can be 2±0.5h, during which organic residues can be effectively removed; the calcination time at 500±50℃ can be 3±0.5h, during which Ce can be ensured. 3+ Uniform doping of the crystal lattice; calcination at 700±50℃ for 1±0.5h can stabilize the crystal form.

[0116] Optionally, the first calcination described above can be carried out in a tube furnace under nitrogen protection.

[0117] Optionally, a method for preparing organic hybrid benzotriazole-CeO2 includes:

[0118] A cerium salt solution and citric acid were mixed and reacted at a second set temperature, then dried and calcined a second time to obtain carboxylated CeO2 nanomaterials.

[0119] A mixture of carboxylated CeO2 nanomaterials, benzotriazole derivatives, and dimethylformamide solution was reacted at a third set temperature to form amide bonds. The mixture was then cooled, washed, and dried to obtain a benzotriazole-CeO2 hybrid product.

[0120] The benzotriazole-CeO2 hybrid product was mixed with hyperbranched polyester and tetrahydrofuran and reacted at a fourth set temperature to obtain organic hybrid benzotriazole-CeO2.

[0121] In the preparation method of organic hybrid benzotriazole-CeO2, the benzotriazole derivative used can absorb ultraviolet light (200-400nm) through an intramolecular charge transfer mechanism and quench free radicals (i.e., inhibit the generation of free radicals). In other words, the organic hybrid benzotriazole-CeO2 prepared by this method can achieve synergistic ultraviolet absorption and free radical quenching through chemical bonding.

[0122] Meanwhile, the addition of dimethylformamide (DMF) helps to ensure the hybridization uniformity of benzotriazole derivatives and carboxylated CeO2 nanomaterials.

[0123] The organic hybrid benzotriazole-CeO2 of the present invention can absorb ultraviolet light (200-400nm) and quench free radicals through an intramolecular charge transfer mechanism.

[0124] Optionally, the cerium salt solution includes at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution. Exemplarily, the cerium nitrate solution (e.g., cerium nitrate of grade CN-4G) can be used with a purity ≥99.99%, Ce... 3+ It is prepared by dissolving ≥99.9% cerium nitrate (easily soluble in water, solubility at 25℃: 200g / 100mL) in water. The cerium salt solution is used to supply Ce. 3+ Source, through Ce doping 3+ Source, to broaden near-infrared absorption (700-1000nm).

[0125] Optionally, the citric acid (e.g., grade C0752) has a purity of ≥99.5%, a carboxyl group content of 3 per molecule, and a decomposition temperature of 175°C (without residue). Citric acid can carboxylate the CeO2 surface to provide chemical grafting sites.

[0126] Optionally, the molar ratio of cerium salt to citric acid in preparing the cerium salt solution is 1:(0.8-1.2), for example: 1:0.8, 1:1, 1:1.2, etc.

[0127] Optionally, the second set temperature is 80±5℃, for example: 75℃, 80℃, 85℃, etc.; the reaction time at the second set temperature is 4±0.5h.

[0128] Optionally, the cerium salt solution and citric acid are mixed and reacted at a second set temperature, then cooled, and ammonia is added dropwise to adjust the pH to generate a sol. The sol is then dried at a temperature of 60±5℃.

[0129] Optionally, after the reaction is completed at the second set temperature, the mixture can be naturally cooled to room temperature, and ammonia water can be added dropwise to adjust the pH to 7.0 neutral to generate a sol, followed by drying and other steps.

[0130] Optionally, the drying time can be 12±2 hours.

[0131] Optionally, the temperature of the second calcination is 500±50℃, for example: 450℃, 500℃, 550℃, etc.; the time of the second calcination can be 2±0.5h.

[0132] Optionally, the second calcination can be carried out under nitrogen protection.

[0133] Optionally, the mass ratio of carboxylated CeO2 nanomaterials to benzotriazole derivatives is 7:(2.5-3.5), for example: 7:2.5, 7:3, 7:3.5, etc.

[0134] Optionally, the dimethylformamide solution (e.g., grade D0790) has a purity ≥99.9% and a boiling point of 153℃; wherein the mass ratio of the total mass of carboxylated CeO2 nanomaterials and benzotriazole derivatives to the mass of the DMF solution is (14-16):1, that is, the solid content ratio of the carboxylated CeO2 nanomaterials and benzotriazole derivatives to the DMF solution is (14-16):1, for example: 14:1, 15:1, 16:1, etc. Dimethylformamide can promote the amide bond reaction between benzotriazole and CeO2, ensuring uniform hybridization.

[0135] Optionally, after mixing the carboxylated CeO2 nanomaterials, benzotriazole derivatives, and dimethylformamide solution, the mixture can be dispersed by magnetic stirring and ultrasonication for 30±5 min, wherein the ultrasonic frequency is 40±5 kHz and the power is 300±50 W.

[0136] Optionally, the third set temperature is 80±5℃, for example: 75℃, 80℃, 85℃, etc.

[0137] Optionally, when reacting at the third set temperature, the reaction can be carried out under nitrogen protection with stirring. The stirring rate can be 300±50 rpm and the reaction time can be 8±1 h.

[0138] Optionally, after the reaction is completed at the third set temperature, cool to room temperature, centrifuge (8000±500 rpm, 10±2 min), wash with DMF, and vacuum dry at 60±5℃.

[0139] Optionally, DMF can be used for washing 1-5 times, such as 1 time, 3 times, 5 times, etc.

[0140] Optionally, the benzotriazole derivative can be UV-360 (e.g., Tinuvin 360), with an absorption band of 200-400 nm, a melting point of 140-145 °C, and a volatility (TGA) of <1% (250 °C). The addition of the benzotriazole derivative can supplement UV absorption and quench free radicals through excited-state proton transfer.

[0141] Optionally, the hyperbranched polyester (HBP, e.g., Boltorn H2004) has a molecular weight of 5000-8000, a hydroxyl value of 12 mmol / g, and a glass transition temperature (Tg) of 45°C. The hyperbranched polyester can coat hybrid particles, inhibiting additive migration through physical entanglement and chemical bonding.

[0142] Optionally, the tetrahydrofuran (HTF, e.g., grade 401757) has a purity of ≥99.9% and a boiling point of 66°C. Tetrahydrofuran can dissolve hyperbranched polyesters and organic hybrid particles.

[0143] Optionally, the mass ratio of benzotriazole-CeO2 hybrid product (particles) to hyperbranched polyester is 1:(0.1-0.3), for example: 1:0.1, 1:0.2, 1:0.3, etc.

[0144] Optionally, the total mass ratio of benzotriazole-CeO2 hybrid product and hyperbranched polyester to tetrahydrofuran is (9-11):1, that is, the solid content ratio of benzotriazole-CeO2 hybrid product and hyperbranched polyester to tetrahydrofuran is (9-11):1, for example: 9:1, 10:1, 11:1, etc.

[0145] Optionally, the fourth set temperature is 120±10℃, for example: 110℃, 120℃, 130℃, etc.; the reaction time at the fourth set temperature can be 4±1h.

[0146] Optionally, after reacting at the fourth set temperature, the mixture is naturally cooled to room temperature, centrifuged (8000±500 rpm, 10±2 min), washed with DMF, and vacuum dried at 60±5℃ to obtain organic hybrid benzotriazole-CeO2 (coated particles).

[0147] Optionally, DMF can be used for washing 1-5 times, such as 1 time, 3 times, 5 times, etc.

[0148] The method for preparing the organic hybrid benzotriazole-CeO2 of the present invention achieves chemical bonding and hybridization of benzotriazole and CeO2 through a three-step process: carboxylation CeO2 synthesis (i.e., preparation of carboxylation CeO2 nanomaterials) → in-situ grafting (i.e., preparation of benzotriazole-CeO2 hybrid products) → hyperbranched polyester coating (i.e., preparation of organic hybrid benzotriazole-CeO2). This overcomes the limitation that physical mixing still cannot achieve absorption of near-infrared light, resulting in PP materials still being prone to aging under the influence of infrared thermal radiation.

[0149] Optionally, the raw materials for the full-spectrum aging-resistant resin material, by mass percentage, include: 95-97.5% of the matrix resin (e.g., 95%, 96%, 97%, 97.5%, etc.), 1.5-3% of the full-spectrum absorber (e.g., 1.5%, 2%, 2.5%, 3%, etc.); 0.5-1.0% of the hyperbranched polyester anti-migration agent (e.g., 0.5%, 0.7%, 1.0%, etc.), 0.3-0.5% of the auxiliary antioxidant (e.g., 0.3%, 0.4%, 0.5%, etc.), and 0.2-0.5% of the processing aid (e.g., 0.2%, 0.3%, 0.4%, 0.5%, etc.); wherein the mass ratio of TiO2 / ZnO core-shell material to organic hybrid benzotriazole-CeO2 is 7:(2-4), for example, 7:2, 7:3, 7:4, etc.

[0150] Optionally, the matrix resin includes homopolymer PP and copolymer PP, with a mass ratio of 6:(3-5), such as 2:1, 3:2, 6:5, etc.; wherein, the homopolymer PP has a high melt index of 36 g / 10 min (230℃, 2.16 kg) and a notched impact strength of 4.5 kJ / m. 2 The copolymer PP has a melt index of 8 g / 10 min (230℃, 2.16 kg) and an impact strength of 21 kJ / m. 2 The combination of the two can balance the injection molding performance and toughness of the material. That is, the combination of homopolymer PP and copolymer PP as the main structure of the material can ensure processing performance and mechanical strength.

[0151] Optionally, the hyperbranched polyester anti-migration agent has a hyperbranched structure (e.g., the hyperbranched polyester anti-migration agent of brand name Boltorn H2004), with a molecular weight Mn of 5000-8000 and a hydroxyl value of 12 mmol / g. The hyperbranched polyester anti-migration agent can fix the additives through physical entanglement and chemical grafting, inhibiting high-temperature migration (migration rate <0.1%), thereby improving the problem of additives migrating to the material surface and causing a decrease in protective performance.

[0152] Optionally, the auxiliary antioxidant is dilaurate thiodipropionate (DLTDP, for example, the auxiliary antioxidant of brand Irganox PS 802), with a melting point of 40-45℃ and low volatility (VOC <50ppm); the auxiliary antioxidant can synergistically capture residual free radicals and delay thermo-oxidative aging.

[0153] Optionally, the processing aid is a silicone masterbatch (containing siloxane segments, such as the processing aid of grade MB50-002), which reduces interfacial tension, D90 < 80 nm, and transmittance > 92%; the processing aid can be used to improve dispersibility, that is, reduce melt viscosity and improve the uniformity of dispersion of nano-additives in PP.

[0154] Optionally, the preparation method of the full-spectrum aging-resistant resin material includes: mixing the raw materials of the full-spectrum aging-resistant resin material and granulating them by extrusion using a screw extruder.

[0155] The preparation method of the full-spectrum aging-resistant resin material of the present invention is a one-step extrusion granulation method, which is simple and easy to operate.

[0156] Optionally, the matrix resin, full-spectrum absorber, hyperbranched polyester, auxiliary antioxidant, and processing aid are placed in a high-speed mixer (speed 1000±200 rpm, time 5±1 min) for premixing; the above premixed materials are added from the main feed port of a twin-screw extruder, melt-blended in the twin-screw extruder, then extruded, and pelletized in a pelletizer to obtain full-spectrum aging-resistant PP material.

[0157] Optionally, the screw diameter of the above-mentioned twin-screw extruder is less than 35 mm, and the length-to-diameter ratio is 40-44; the main engine speed of the twin-screw extruder is 250-500 r / min, the barrel temperature is 180-210℃, the water tank temperature is 20-60℃, and the pelletizer speed is 400-700 r / min.

[0158] The present invention will be further described in detail below with reference to the embodiments.

[0159] Example 1-1

[0160] Preparation of TiO2 / ZnO core-shell materials:

[0161] In a 5L high-pressure reactor, 100.0g of Zn(NO3)2·6H2O was added to 1.125L of deionized water and magnetically stirred (stirring speed: 300rpm) until completely dissolved. Then, 3.375L of ethanol (ethanol:water volume ratio = 3:1) was added. While stirring, 180mL of TTIP was added dropwise to the above ethanol mixture at a rate of 5mL / min. Ammonia was added to adjust the pH to 9.5, and the reactor temperature was adjusted to 180℃ (heating rate: 10℃ / min). After the temperature stabilized, the reaction was allowed to proceed for 12 hours. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The solid product was separated using a high-speed centrifuge (8000rpm, 10min). The product was washed three times with ethanol and then three times with deionized water to remove unreacted ions, yielding TiO2 / ZnO core-shell powder.

[0162] Will ZnO powder was added to anhydrous ethanol at a solid-liquid ratio of 1:50, then placed in a magnetically stirred reactor and sonicated for 30 minutes (frequency 40kHz, power 300W) to ensure uniform dispersion of the powder. KH550 was then added... Weigh 3 wt% of the ZnO powder and slowly add it dropwise to the powder dispersion at a rate of 10 mL / min. Add ammonia to adjust the pH to 8.5. Turn on the magnetic stirrer (300 rpm) and set the temperature to 70℃ for 4 h. After the reaction is complete, allow it to cool naturally to room temperature. Use a high-speed centrifuge (8000 rpm, 10 min) to separate the solid product. Wash it three times with ethanol and deionized water to remove physically adsorbed KH550 and byproducts, and obtain TiO2 / ZnO core-shell surface aminated modified powder.

[0163] TiO2 / ZnO core-shell surface aminated modified powder was immersed in 0.1 mol / L cerium nitrate solution (solid-liquid ratio 1:20) and evaporated to dryness at 60℃. The dried powder was then placed in a tube furnace and calcined under nitrogen protection in a gradient: 300℃×2h (to remove residual organic matter) → 500℃×3h (to remove cerium nitrate). 3 +Lattice doping) → 700℃×1h (stable crystal form), and after cooling, TiO2 / ZnO core-shell material is obtained.

[0164] Preparation of organic hybrid benzotriazole-CeO2:

[0165] Ce(NO3)3·6H2O (0.1 mol) was dissolved in deionized water (200 mL) and citric acid (0.1 mol), and added to a magnetically stirred reactor. The reactor was stirred at 80 °C (300 rpm) for 4 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and ammonia was added dropwise to adjust the pH to 7.0 neutral, forming a sol. The sol was dried at 60 °C for 12 h and then calcined at 500 °C under nitrogen protection for 2 h to obtain carboxylated products. Nanoparticles.

[0166] Carboxylation UV-360 is mixed with DMF solvent at a mass ratio of 7:3 (carboxylation) The UV-360 solvent (solid content ratio of DMF to UV-360) was added to a magnetically stirred reactor and ultrasonically dispersed for 30 min (frequency 40 kHz, power 300 W). Under nitrogen protection, the mixture was heated to 80 °C and stirred (300 rpm) for 8 h to form amide bonds. After the reaction was complete, the mixture was cooled to room temperature, centrifuged (8000 rpm × 10 min), washed three times with DMF, and vacuum dried at 60 °C to obtain benzotriazole-CeO2 hybrid particles.

[0167] Benzotriazole-CeO2 hybrid particles and hyperbranched polyester (at a mass ratio of 1:0.2) were dissolved in HTF tetrahydrofuran (the solid content ratio of benzotriazole-CeO2 hybrid particles, hyperbranched polyester and HTF was 10:1). The mixture was reacted at 120℃ for 4 h. After the reaction was completed, the mixture was naturally cooled to room temperature, centrifuged (8000 rpm × 10 min), washed three times with DMF, and dried under vacuum at 60℃ to obtain organic hybrid benzotriazole-CeO2 coated particles.

[0168] Preparation of full-spectrum aging-resistant resin materials:

[0169] The PP matrix resin, full-spectrum absorber (TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2), hyperbranched polyester, auxiliary antioxidant, and processing aids were premixed in a high-speed mixer (1000 rpm, 5 min).

[0170] The above premixed material is added to the main feed port of a twin-screw extruder, melt-blended in the twin-screw extruder, then extruded, and pelletized in a pelletizer to obtain a full-spectrum aging-resistant PP material.

[0171] The mass percentages of the full-spectrum aging-resistant resin material prepared in Example 1-1 are shown in Table 1.

[0172] The differences between Examples 1-2, Comparative Examples 1, 2, and 3 and Example 1, as well as the mass percentage of the raw materials, are shown in Table 1.

[0173] Table 1

[0174]

[0175] Performance tests were conducted on Examples 1-1, 1-2, Comparative Examples 1, 2, and 3. Full-spectrum absorbance was tested according to ASTM E903-20; ΔYI and elongation at break after 5000h QUV aging were tested according to ASTM E313-10; chalking life at 150℃ was tested according to ASTM D3045-18; transmittance was tested according to GB / T 2410-2008; and migration was tested according to ENISO 177:2017. The test results are shown in Table 2.

[0176] Table 2

[0177]

[0178]

[0179] According to Table 2, comparing Examples 1-1 with Comparative Examples 1, 2, and 3, incorporating the TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 prepared by the method of this invention into the PP matrix resin effectively improves the full-spectrum absorption rate of the resin material and makes it less prone to yellowing. In other words, it exhibits excellent anti-yellowing performance (demonstrated by a lower ΔYI value after 5000h QUV aging in Example 1). After aging tests, it maintains good flexibility and ductility (demonstrated by a higher elongation at break after 5000h QUV aging in Example 1), and has a longer chalking life; that is, the resin of Example 1 only shows chalking after a longer aging time. Simultaneously, incorporating the TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 prepared by the method of this invention into the PP matrix resin also ensures good light transmittance of the resin material and reduces the migration rate of additives, thus mitigating the problem of reduced protective performance caused by additive migration to the surface of the PP material.

[0180] Comparing Examples 1-1 and Comparative Example 3, it can be seen that when the total amount of TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 is greater than 3%, the full-spectrum absorption rate of the prepared resin material is reduced, and the anti-yellowing and anti-aging properties are reduced. At the same time, the powdering life is shortened, the light transmittance is reduced, and the migration rate of the additives is increased.

[0181] Comparing Examples 1-1 and 1-2, it can be seen that using TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 to prepare resin material results in improved full-spectrum absorption, improved resistance to yellowing and aging, longer powdering life, increased light transmittance, and reduced migration of additives compared to using TiO2 / ZnO core-shell material and unhybridized benzotriazole-CeO2.

[0182] Example 2

[0183] In a 5L high-pressure reactor, 100.0g of zinc chloride was added to 1.125L of deionized water and magnetically stirred (stirring speed: 300rpm) until completely dissolved. Then, 3.375L of ethanol (ethanol:water volume ratio = 3:1) was added. While stirring, 180mL of titanium tetrachloride (purity ≥99.9%) was added dropwise to the above ethanol mixture at a rate of 5mL / min. Ammonia was added to adjust the pH to 9.5, and the reactor temperature was adjusted to 190℃ (heating rate: 9℃ / min). After the temperature stabilized, the reaction was allowed to proceed for 11 hours. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The solid product was separated using a high-speed centrifuge (8000rpm, 10min). The product was washed three times with ethanol and then three times with deionized water to remove unreacted ions, yielding TiO2 / ZnO core-shell powder.

[0184] Will ZnO powder was added to anhydrous ethanol at a solid-liquid ratio of 1:50, then placed in a magnetically stirred reactor and sonicated for 30 minutes (frequency 40kHz, power 300W) to ensure uniform dispersion of the powder. KH550 was then added... Weigh 3 wt% of the ZnO powder and slowly add it dropwise to the powder dispersion at a rate of 10 mL / min. Add ammonia to adjust the pH to 8.5. Turn on the magnetic stirrer (300 rpm) and set the temperature to 68℃ for 4 h. After the reaction is complete, allow it to cool naturally to room temperature. Use a high-speed centrifuge (8000 rpm, 10 min) to separate the solid product. Wash it three times with ethanol and deionized water to remove physically adsorbed KH550 and byproducts, and obtain TiO2 / ZnO core-shell surface aminated modified powder.

[0185] TiO2 / ZnO core-shell surface aminated modified powder was immersed in 0.1 mol / L cerium chloride solution (solid-liquid ratio 1:20) and evaporated to dryness at 55℃. The dried powder was then placed in a tube furnace and calcined under nitrogen protection in a gradient: 250℃×2h (to remove residual organic matter) → 450℃×3h (Ce 3 +Lattice doping) → 650℃×1h (stable crystal form), and after cooling, TiO2 / ZnO core-shell material is obtained.

[0186] Preparation of organic hybrid benzotriazole-CeO2:

[0187] Cerium chloride (0.1 mol) was dissolved in deionized water (200 mL) and citric acid (0.1 mol), and the mixture was added to a magnetically stirred reactor. The reactor was stirred at 75 °C (300 rpm) for 4 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and ammonia was added dropwise to adjust the pH to 7.0 neutral, forming a sol. The sol was dried at 55 °C for 12 h and then calcined at 450 °C under nitrogen protection for 2 h to obtain carboxylated cerium chloride. Nanoparticles.

[0188] Carboxylation UV-360 was mixed with DMF solvent at a mass ratio of 7:2.5 (carboxylation). The UV-360 and DMF solvent (solid content ratio 14:1) were added to a magnetically stirred reactor and ultrasonically dispersed for 30 min (frequency 40 kHz, power 300 W). Under nitrogen protection, the mixture was heated to 75 °C and stirred (300 rpm) for 8 h to form amide bonds. After the reaction was complete, the mixture was cooled to room temperature, centrifuged (8000 rpm × 10 min), washed three times with DMF, and vacuum dried at 60 °C to obtain benzotriazole-CeO2 hybrid particles.

[0189] Benzotriazole-CeO2 hybrid particles and hyperbranched polyester (at a mass ratio of 1:0.1) were dissolved in HTF tetrahydrofuran (the solid content ratio of benzotriazole-CeO2 hybrid particles, hyperbranched polyester and HTF was 9:1). The mixture was reacted at 110℃ for 4 hours. After the reaction was completed, the mixture was naturally cooled to room temperature, centrifuged (8000 rpm × 10 min), washed three times with DMF, and dried under vacuum at 60℃ to obtain organic hybrid benzotriazole-CeO2 coated particles.

[0190] Preparation of full-spectrum aging-resistant resin materials:

[0191] The PP matrix resin, full-spectrum absorber (TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 in a mass ratio of 7:4), hyperbranched polyester, auxiliary antioxidant, and processing aids were premixed in a high-speed mixer (1000 rpm for 5 min).

[0192] The above premixed material is added to the main feed port of a twin-screw extruder, melt-blended in the twin-screw extruder, then extruded, and pelletized in a pelletizer to obtain a full-spectrum aging-resistant PP material.

[0193] Example 3

[0194] In a 5L high-pressure reactor, 100.0g of zinc sulfate was added to 1.125L of deionized water and magnetically stirred (stirring speed: 300rpm) until completely dissolved. Then, 3.375L of ethanol (ethanol:water volume ratio = 3:1) was added. While stirring, 180mL of titanium sulfate (purity ≥99.9%) was added dropwise to the ethanol mixture at a rate of 5mL / min. Ammonia was added to adjust the pH to 9.5, and the reactor temperature was adjusted to 170℃ (heating rate: 8℃ / min). After the temperature stabilized, the reaction was allowed to proceed for 13 hours. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The solid product was separated using a high-speed centrifuge (8000rpm, 10min). The product was washed three times with ethanol and then three times with deionized water to remove unreacted ions, yielding TiO2 / ZnO core-shell powder.

[0195] Will ZnO powder was added to anhydrous ethanol at a solid-liquid ratio of 1:50, then placed in a magnetically stirred reactor and sonicated for 30 minutes (frequency 40kHz, power 300W) to ensure uniform dispersion of the powder. KH550 was then added... Weigh 3 wt% of the ZnO powder and slowly add it dropwise to the powder dispersion at a rate of 10 mL / min. Add ammonia to adjust the pH to 8.5. Turn on the magnetic stirrer (300 rpm) and set the temperature to 72℃ for 4 h. After the reaction is complete, allow it to cool naturally to room temperature. Use a high-speed centrifuge (8000 rpm, 10 min) to separate the solid product. Wash it three times with ethanol and deionized water to remove physically adsorbed KH550 and byproducts, and obtain TiO2 / ZnO core-shell surface aminated modified powder.

[0196] TiO2 / ZnO core-shell surface aminated modified powder was immersed in 0.1 mol / L cerium sulfate solution (solid-liquid ratio 1:20) and evaporated to dryness at 65℃. The dried powder was then placed in a tube furnace and calcined under nitrogen protection in a gradient: 350℃×2h (to remove residual organic matter) → 550℃×3h (to remove cerium sulfate residue). 3 +Lattice doping) → 750℃×1h (stable crystal form), and after cooling, TiO2 / ZnO core-shell material is obtained.

[0197] Preparation of organic hybrid benzotriazole-CeO2:

[0198] Cerium sulfate (0.1 mol) was dissolved in deionized water (200 mL) and citric acid (0.1 mol), and the mixture was added to a magnetically stirred reactor. The reactor was stirred at 85 °C (300 rpm) for 4 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and ammonia was added dropwise to adjust the pH to 7.0 neutral, forming a sol. The sol was dried at 65 °C for 12 h and then calcined at 550 °C under nitrogen protection for 2 h to obtain carboxylated products. Nanoparticles.

[0199] Carboxylation UV-360 was mixed with DMF solvent at a mass ratio of 7:3.5 (carboxylation). The UV-360 solvent (solid content ratio of DMF to UV-360) was added to a magnetically stirred reactor and ultrasonically dispersed for 30 min (frequency 40 kHz, power 300 W). Under nitrogen protection, the mixture was heated to 85 °C and stirred (300 rpm) for 8 h to form amide bonds. After the reaction was complete, the mixture was cooled to room temperature, centrifuged (8000 rpm × 10 min), washed three times with DMF, and vacuum dried at 60 °C to obtain benzotriazole-CeO2 hybrid particles.

[0200] Benzotriazole-CeO2 hybrid particles and hyperbranched polyester (at a mass ratio of 1:0.3) were dissolved in HTF tetrahydrofuran (the solid content ratio of benzotriazole-CeO2 hybrid particles, hyperbranched polyester and HTF was 11:1). The mixture was reacted at 130℃ for 4 hours. After the reaction was completed, the mixture was naturally cooled to room temperature, centrifuged (8000 rpm × 10 min), washed three times with DMF, and dried under vacuum at 60℃ to obtain organic hybrid benzotriazole-CeO2 coated particles.

[0201] Preparation of full-spectrum aging-resistant resin materials:

[0202] The PP matrix resin, full-spectrum absorber (TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 in a mass ratio of 7:2), hyperbranched polyester, auxiliary antioxidant, and processing aids were premixed in a high-speed mixer (1000 rpm for 5 min).

[0203] The above premixed material is added to the main feed port of a twin-screw extruder, melt-blended in the twin-screw extruder, then extruded, and pelletized in a pelletizer to obtain a full-spectrum aging-resistant PP material.

[0204] In summary, the TiO2 / ZnO core-shell material and organic hybrid benzotriazole-CeO2 of this invention can enhance the full-spectrum protection capability, extending the resin's light absorption range from the traditional ultraviolet band (200-400nm) to the full spectrum of 200-1000nm (ultraviolet + visible light + near-infrared), thus blocking multi-band synergistic aging. Specifically, the ultraviolet-visible-near-infrared spectrum shows an average absorption rate ≥90%, while related technologies can only absorb ultraviolet light with an absorption rate ≤30%.

[0205] It can also improve the resin's resistance to chalking; among them, benzotriazole derivatives capture excited free radicals and reduce molecular chain breakage; the hyperbranched polyester coating layer uniformly disperses stress and avoids chalking caused by microcracks; the chalking life is improved by ≥3 times compared with related technologies.

[0206] It can also reduce the migration rate of additives; among them, hyperbranched polyester achieves a migration rate of <0.1% through the dual effects of physical entanglement and chemical grafting.

[0207] The TiO2 / ZnO core-shell material and the organic hybrid benzotriazole-CeO2 of the present invention have a high degree of dispersion, and the screw extrusion method for preparing the resin can further ensure the uniformity of dispersion. Therefore, the prepared resin material has good light transmittance.

[0208] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a TiO2 / ZnO core-shell material, characterized in that, include: Add titanium dioxide precursor donor dropwise to an alcoholic solution of zinc oxide precursor donor; Then, the first hydrothermal synthesis was performed, followed by separation and washing to obtain the TiO2 / ZnO core-shell product; A silane coupling agent was added dropwise to an alcoholic solution of the TiO2 / ZnO core-shell product, followed by a second hydrothermal synthesis, separation, and washing to obtain an aminated modified product on the surface of the TiO2 / ZnO core-shell product. The TiO2 / ZnO core-shell surface aminated modification product and cerium ion-containing solution are mixed, evaporated at a first set temperature, and then calcined to obtain the TiO2 / ZnO core-shell material.

2. The method for preparing the TiO2 / ZnO core-shell material according to claim 1, characterized in that, The zinc oxide precursor donor includes at least one of zinc nitrate, zinc chloride, and zinc sulfate; and / or, The titanium dioxide precursor donor includes at least one selected from tetrabutyl titanate, titanium tetrachloride, titanium sulfate, and isopropyl titanate; and / or, The cerium-containing solution includes at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or, The temperature of the first hydrothermal synthesis is 170-190℃; and / or, The heating rate for the first hydrothermal synthesis is 8-12 °C / min; and / or, The temperature for the second hydrothermal synthesis is 70±2℃; and / or, The first set temperature is 60±5℃; and / or, The first calcination includes segmented calcination, wherein the segmented calcination includes calcination at a temperature of 300±50℃, calcination at a temperature of 500±50℃, and calcination at a temperature of 700±50℃ in sequence.

3. A TiO2 / ZnO core-shell material, characterized in that, It is prepared by the method for preparing TiO2 / ZnO core-shell material as described in claim 1 or 2.

4. A method for preparing an organic hybrid benzotriazole-CeO2, characterized in that, include: A cerium salt solution and citric acid were mixed and reacted at a second set temperature, then dried and calcined a second time to obtain carboxylated CeO2 nanomaterials. The carboxylated CeO2 nanomaterial, benzotriazole derivative, and dimethylformamide solution were mixed and reacted at a third set temperature to form amide bonds. After cooling, washing, and drying, the benzotriazole-CeO2 hybrid product was obtained. The benzotriazole-CeO2 hybrid product was mixed with hyperbranched polyester and tetrahydrofuran and reacted at a fourth set temperature to obtain organic hybrid benzotriazole-CeO2.

5. The method for preparing the organic hybrid benzotriazole-CeO2 according to claim 4, characterized in that, The cerium salt solution includes at least one selected from cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or, The second set temperature is 80±5℃; and / or, The cerium salt solution and the citric acid are mixed and reacted at the second set temperature. After cooling, ammonia is added dropwise to adjust the pH to form a sol, which is then dried at 60±5℃; and / or, The second calcination temperature is 500±50℃; and / or, The third set temperature is 80±5℃; and / or, The fourth set temperature is 120±10℃.

6. An organic hybrid benzotriazole-CeO2, characterized in that, It is prepared by the method for preparing organic hybrid benzotriazole-CeO2 as described in claim 4 or 5.

7. A full-spectrum aging-resistant resin material, characterized in that, The raw materials for the full-spectrum aging-resistant resin material include: a matrix resin and a full-spectrum absorbent; wherein, The full-spectrum absorber includes TiO2 / ZnO core-shell materials and organic hybrid benzotriazole-CeO2; or... The full-spectrum absorber includes TiO2 / ZnO core-shell materials and benzotriazole derivatives.

8. The full-spectrum aging-resistant resin material according to claim 7, characterized in that, The preparation method of the TiO2 / ZnO core-shell material includes: Add titanium dioxide precursor donor dropwise to an alcoholic solution of zinc oxide precursor donor; Then, the first hydrothermal synthesis was performed, followed by separation and washing to obtain the TiO2 / ZnO core-shell product; A silane coupling agent was added dropwise to an alcoholic solution of the TiO2 / ZnO core-shell product, followed by a second hydrothermal synthesis, separation, and washing to obtain an aminated modified product on the surface of the TiO2 / ZnO core-shell product. The TiO2 / ZnO core-shell surface aminated modification product and cerium ion-containing solution are mixed, evaporated at a first set temperature, and then calcined to obtain the TiO2 / ZnO core-shell material.

9. The full-spectrum aging-resistant resin material according to claim 8, characterized in that, The zinc oxide precursor donor includes at least one of zinc nitrate, zinc chloride, and zinc sulfate; and / or, The titanium dioxide precursor donor includes at least one selected from tetrabutyl titanate, titanium tetrachloride, titanium sulfate, and isopropyl titanate; and / or, The cerium-containing solution includes at least one of cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or, The temperature of the first hydrothermal synthesis is 170-190℃; and / or, The heating rate for the first hydrothermal synthesis is 8-12 °C / min; and / or, The temperature for the second hydrothermal synthesis is 70±2℃; and / or, The first set temperature is 60±5℃; and / or, The first calcination includes segmented calcination, wherein the segmented calcination includes calcination at a temperature of 300±50℃, calcination at a temperature of 500±50℃, and calcination at a temperature of 700±50℃ in sequence.

10. The full-spectrum aging-resistant resin material according to claim 7, characterized in that, The method for preparing the organic hybrid benzotriazole-CeO2 includes: A cerium salt solution and citric acid were mixed and reacted at a second set temperature, then dried and calcined a second time to obtain carboxylated CeO2 nanomaterials. The carboxylated CeO2 nanomaterial, benzotriazole derivative, and dimethylformamide solution were mixed and reacted at a third set temperature to form amide bonds. After cooling, washing, and drying, the benzotriazole-CeO2 hybrid product was obtained. The benzotriazole-CeO2 hybrid product was mixed with hyperbranched polyester and tetrahydrofuran and reacted at a fourth set temperature to obtain organic hybrid benzotriazole-CeO2.

11. The full-spectrum aging-resistant resin material according to claim 10, characterized in that, The cerium salt solution includes at least one selected from cerium nitrate solution, cerium chloride solution, and cerium sulfate solution; and / or, The second set temperature is 80±5℃; and / or, The cerium salt solution and the citric acid are mixed and reacted at the second set temperature. After cooling, ammonia is added dropwise to adjust the pH to form a sol, which is then dried at 60±5℃; and / or, The second calcination temperature is 500±50℃; and / or, The third set temperature is 80±5℃; and / or, The fourth set temperature is 120±10℃.

12. The full-spectrum aging-resistant resin material according to any one of claims 7-11, characterized in that, The raw materials for the full-spectrum aging-resistant resin material, by mass percentage, include: 95-97.5% of the matrix resin, 1.5-3% of the full-spectrum absorber; 0.5-1.0% of the hyperbranched polyester anti-migration agent, 0.3-0.5% of the auxiliary antioxidant, and 0.2-0.5% of the processing aid; wherein, The mass ratio of the TiO2 / ZnO core-shell material to the organic hybrid benzotriazole-CeO2 is 7:(2-4).

13. The method for preparing the full-spectrum aging-resistant resin material according to any one of claims 7-12, characterized in that, include: The raw materials of the full-spectrum aging-resistant resin material are mixed and extruded and granulated using a screw extruder.

14. A lamp, characterized in that, The raw materials used to manufacture the housing or lampshade of the lamp include the full-spectrum aging-resistant resin material as described in any one of claims 7-12.